Preparation method of hot-pressable mixed-weave fabric, mixed-weave fabric and application thereof
By using a three-layer interwoven fabric method combining polyester yarn and TPU yarn, the problems of easy peeling of heterogeneous material interfaces and poor breathability during the hot pressing and shaping process of polyester mesh fabric have been solved. This method achieves a three-dimensional shaping, soft feel and high breathability blended fabric, which is suitable for shoe uppers, bags and seat covers.
Patent Information
- Application Number
- CN202611557149.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional polyester mesh fabrics suffer from problems such as easy peeling of heterogeneous material interfaces, poor air permeability, complex processing and high cost during hot pressing and shaping, making it difficult to simultaneously achieve three-dimensional shaping, soft hand feel and high air permeability.
A method for preparing blended fabric using three layers of polyester yarn and TPU yarn is adopted. The TPU yarn is completely embedded between the polyester yarn layers. The TPU yarn is plastically flowed through hot pressing to form a three-dimensional shape while maintaining the fiber shape of the polyester yarn. After cooling and setting, a blended fabric that can be hot-pressed and shaped is obtained.
It achieves a non-heterogeneous bonding interface, good breathability, three-dimensional shaping ability and soft hand feel, simplifies the processing process and reduces production costs, and is suitable for shoe uppers, bags and seat covers.
Smart Images

Figure CN123133076A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of textile materials technology, and in particular to a method for preparing a heat-pressable blended fabric, the blended fabric, and its applications. Background Technology
[0002] Taking shoe upper applications as an example, traditional polyester mesh is a two-dimensional flexible fabric that lacks the ability to be thermoformed, making it difficult to create durable three-dimensional patterns or three-dimensional curved surfaces in molds. To address these issues, existing technologies generally employ the following two methods to composite polyester mesh: Method 1: Polyester mesh fabric composite with TPU film. A thermoplastic polyurethane (TPU) film is hot-pressed onto the surface of a polyester mesh fabric. Utilizing the thermoplasticity of the TPU film, the composite material can be molded under heating conditions. However, this method has the following drawbacks: First, the TPU film and the polyester mesh fabric are heterogeneous materials, bonded solely by hot pressing, which can easily lead to peeling and delamination under long-term use or in humid and hot environments. Second, the TPU film has a continuous, dense structure that completely covers the yarn pores on the mesh fabric surface, significantly reducing the breathability of the composite material and affecting wearing comfort.
[0003] Method 2: Polyester mesh fabric composite with artificial leather or genuine leather. This method combines sheets of artificial leather or genuine leather with mesh fabric using adhesives or stitching to achieve a leather-like appearance and texture. However, this method has the following drawbacks: artificial leather and genuine leather themselves lack a mesh structure, resulting in poor breathability; additionally, the overall thickness of the composite material increases, its softness decreases, the processing steps become more complex, and the material cost is higher.
[0004] In summary, existing technologies still lack an ideal solution that simultaneously addresses four dimensions: three-dimensional shaping, soft feel, high breathability, and no risk of peeling. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing a heat-pressable blended fabric, the blended fabric itself, and its applications, thereby solving the aforementioned technical problems.
[0006] To achieve the above objectives, the present invention provides a method for preparing a heat-pressable blended fabric, comprising the following steps: S1. Fabric weaving: Polyester yarn and TPU yarn are woven together to form a three-layer blended fabric. The three-layer blended fabric includes an outer layer and an inner layer woven from polyester yarn, and an inner layer woven from TPU yarn located between the outer layer and the inner layer. The TPU yarn is completely embedded between the outer layer and the inner layer woven from polyester yarn and is not exposed on the upper and lower surfaces of the three-layer blended fabric. S2. Hot pressing: The three-layer blended preform is arranged in the mold cavity and hot pressed. While the polyester yarns of the surface and bottom layers maintain their fiber shape, the TPU yarns of the middle layer are softened by heat and undergo plastic flow, forming a three-dimensional shape in the mold. S3. Cooling and Shaping: Cooling and shaping the fabric after hot pressing to obtain a blended fabric that can be hot-pressed and shaped.
[0007] Preferably, step S1 uses warp knitting, weft knitting, or circular knitting techniques for weaving, employing a double-sided or spaced fabric structure. Polyester yarn is used to weave the surface and bottom layers, while TPU yarn is used as the intermediate connecting yarn or filling yarn to participate in the weaving. This allows the three layers of yarn to interweave synchronously during the weaving process, forming an integrated multi-layered blended structure. During weaving, the amount of warp feed or yarn feeding is differentiated and correlated with the polyester yarn forming the surface layer, the polyester yarn forming the bottom layer, and the TPU yarn forming the middle layer, so that they are distributed in the middle layer of the fabric and not exposed on the surface and bottom layers.
[0008] Preferably, when using a double-needle bed warp-knitted spacer fabric process, the warp feed rate is set independently for the surface polyester guide bar, the bottom polyester guide bar, and the TPU intermediate connecting guide bar. The formula for calculating the warp feed rate is as follows: ; in, ; Constraints: ; In the formula, For the surface layer polyester comb bar, the amount of warp feed is; For the bottom layer polyester comb bar, the amount of warp feed is... For the TPU intermediate connecting comb, the amount of warp feed is; The number of repeating rows in the fabric structure; For the surface layer of polyester comb bar Length of yarn used in the horizontal row; For the bottom layer of polyester comb bar Length of yarn used in the horizontal row; The length of the outer layer polyester coil arc; The length of the bottom polyester coil arc; For TPU combing Length of yarn used in the horizontal row; This refers to the length of the interlayer extension line of the TPU yarn; The needle pitch of the knitting machine; The number of stitches shifted laterally between adjacent rows of padding yarn in the TPU comb bar; This refers to the distance between the front and rear needle beds on a double-needle bed machine. This refers to the actual working elongation of the TPU yarn. The geometric length of the extension line of TPU yarn in its free state; The maximum safe elongation allowed for TPU yarn; Weft knitting and circular knitting processes achieve differentiated correlation control by controlling the yarn feeding length of each 100 stitches.
[0009] Preferably, in step S1, the polyester yarn is polyester filament or polyester staple fiber yarn with a specification of 75D-350D; the TPU yarn is TPU monofilament or TPU multifilament yarn with a specification of 300D-1200D; the melting point of the TPU yarn is lower than that of the polyester yarn or its softening point.
[0010] Preferably, in step S1, the mass ratio of polyester yarn to TPU yarn is 40:60.
[0011] Preferably, in step S2, the mold temperature during hot pressing is 190℃-250℃, the pressure is 6T-18T, and the holding time is 30 seconds-60 seconds; and the mold cavity surface is provided with one or any combination of simulated leather texture, artificial leather texture, embossed texture, brand logo, and three-dimensional curved surface structure, so that after hot pressing, the surface of the blended fabric forms a three-dimensional texture or three-dimensional shape corresponding to the surface of the mold cavity.
[0012] A blended fabric, prepared by a method for preparing blended fabrics that can be heat-pressed and shaped.
[0013] Application of blended fabrics in shoe uppers, bags, or seat upholstery.
[0014] Therefore, the present invention, employing the above-mentioned method for preparing a heat-pressable blended fabric, the blended fabric itself, and its application, has the following beneficial effects: 1. This invention uses a three-layer synchronous interlacing weaving of polyester yarn and TPU yarn. The TPU yarn is completely embedded between the polyester surface layer and the bottom layer, abandoning the traditional surface composite solution of TPU film bonding and leather adhesive bonding. There is no heterogeneous bonding interface, eliminating the risk of delamination and peeling in humid and hot environments from the root. 2. The entire upper and lower surfaces of the fabric are made of polyester yarn, without continuous dense coating. The fabric mesh can be retained, and the fabric has good breathability, which improves the comfort of wearing and using the product. 3. The hot pressing processing window is constructed by utilizing the difference in melting points between TPU and polyester. During the hot pressing process, the intermediate TPU layer softens and flows plastically to replicate the three-dimensional shape of the mold cavity, while the surface and bottom polyester yarns maintain the fiber shape. The fabric has both three-dimensional shaping ability and a soft hand feel. The mold can directly form simulated leather texture, simplifying subsequent processing procedures and reducing production costs. 4. The fabric can be directly used for shoe uppers, bags, and seat covers. The mold cavity can be flexibly set with concave and convex textures, logos, and three-dimensional curved surfaces, allowing for a high degree of freedom in product design.
[0015] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0016] Figure 1 This is a flowchart of a method for preparing a heat-pressable blended fabric according to the present invention. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are merely illustrative of the embodiments of the present invention and are not intended to limit the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of this application. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout.
[0018] It should be noted that the terms "comprising" and "having" and any variations thereof are intended to cover non-exclusive inclusion, such as a process, method, system, product, or server that includes a series of steps or units, not necessarily limited to those steps or units that are explicitly listed, but may include other steps or units that are not explicitly listed or that are inherent to such processes, methods, products, or devices.
[0019] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0020] like Figure 1 As shown, a method for preparing a heat-pressable blended fabric includes the following steps: S1. Fabric weaving: Polyester yarn and TPU yarn are woven together to form a three-layer blended fabric. The three-layer blended fabric includes an outer layer and an inner layer woven from polyester yarn, and an inner layer woven from TPU yarn located between the outer layer and the inner layer. The TPU yarn is completely embedded between the outer layer and the inner layer woven from polyester yarn and is not exposed on the upper and lower surfaces of the three-layer blended fabric. S2. Hot pressing: The three-layer blended preform is arranged in the mold cavity and hot pressed. While the polyester yarns of the surface and bottom layers maintain their fiber shape, the TPU yarns of the middle layer are softened by heat and undergo plastic flow, forming a three-dimensional shape in the mold. S3. Cooling and Shaping: Cooling and shaping the fabric after hot pressing to obtain a blended fabric that can be hot-pressed and shaped.
[0021] Step S1 involves weaving using warp knitting, weft knitting, or circular knitting techniques. A double-sided or spaced fabric structure is used, with polyester yarns weaving the surface and bottom layers, and TPU yarns as intermediate connecting or filling yarns participating in the weaving. This allows the three layers of yarns to interweave synchronously during the weaving process, forming an integrated multi-layered blended structure. During weaving, the amount of warp feed or yarn feeding is differentiated and correlated with the polyester yarns forming the surface layer, the polyester yarns forming the bottom layer, and the TPU yarns forming the middle layer, so that they are distributed in the middle layer of the fabric and not exposed on the surface and bottom layers.
[0022] When using a double-needle bed warp-knitted spacer fabric process, the warp feed rate is set independently for the surface polyester guide bar, the bottom polyester guide bar, and the TPU intermediate connecting guide bar. The formula for calculating the warp feed rate is as follows: ; in, ; Constraints: ; In the formula, For the surface layer polyester comb bar, the amount of warp feed is; For the bottom layer polyester comb bar, the amount of warp feed is... For the TPU intermediate connecting comb, the amount of warp feed is; The number of repeating rows in the fabric structure; For the surface layer of polyester comb bar Length of yarn used in the horizontal row; For the bottom layer of polyester comb bar Length of yarn used in the horizontal row; The length of the outer layer polyester coil arc; The length of the bottom polyester coil arc; For TPU combing Length of yarn used in the horizontal row; This refers to the length of the interlayer extension line of the TPU yarn; The needle pitch of the knitting machine; The number of stitches shifted laterally between adjacent rows of padding yarn in the TPU comb bar; This refers to the distance between the front and rear needle beds on a double-needle bed machine. This refers to the actual working elongation of the TPU yarn. The geometric length of the extension line of TPU yarn in its free state; The maximum safe elongation allowed for TPU yarn; Weft knitting and circular knitting processes achieve differentiated correlation control by controlling the yarn feeding length of each 100 stitches.
[0023] In step S1, the polyester yarn is polyester filament or polyester staple fiber yarn with a specification of 75D-350D; the TPU yarn is TPU monofilament or TPU multifilament yarn with a specification of 300D-1200D; the melting point of the TPU yarn is lower than that of the polyester yarn or its softening point.
[0024] In step S1, the mass ratio of polyester yarn to TPU yarn is 40:60.
[0025] In step S2, the mold temperature during hot pressing is 190℃-250℃, the pressure is 6T-18T, and the holding time is 30 seconds-60 seconds. The mold cavity surface is provided with one of the following: simulated leather texture, artificial leather texture, embossed texture, brand logo, three-dimensional curved surface structure, or any combination thereof. After hot pressing, the surface of the blended fabric forms a three-dimensional texture or three-dimensional shape corresponding to the surface of the mold cavity.
[0026] Example 1 A method for preparing a heat-pressable blended fabric, comprising the following steps: S1. Yarn Preparation: 200D polyester filament is selected as the outer and bottom layer raw materials; 600D TPU multifilament is selected as the middle layer raw material. The melting point range of TPU is 160℃-220℃, while the melting point of polyester is approximately 255℃, ensuring that the melting point of TPU is lower than that of polyester. The mass ratio of polyester to TPU yarn is 40:60. The yarn is warped and packaged using a double-needle bed warp knitting machine with an interlocking fabric structure. Polyester yarn is used to knit the outer and bottom layers on both the front and back needle beds respectively; TPU yarn is used as an interlocking yarn, forming interlayer extension lines only between the two layers and not participating in loop formation on the front and back sides. The number of repeat rows is determined based on the fabric padding yarn number. Substitute the values into the warp feed formula to calculate the target warp feed of the TPU comb, adjust the warp feed mechanism of the machine, and control the TPU yarn extension lines to be distributed only between the two layers of polyester, without exposing the upper and lower surfaces of the fabric; the three layers of yarn are interwoven synchronously to form a single unit, and the three-layer blended fabric is obtained after the machine is removed.
[0027] S2. Hot pressing: The blended fabric is placed into the mold cavity with simulated leather texture; the mold temperature is set to 210℃, the press pressure is 12T, and the holding time is 45s; during the hot pressing process, the intermediate TPU yarn softens and undergoes plastic flow due to heat, replicating the simulated leather texture of the mold; the surface and bottom polyester yarns maintain the fiber shape.
[0028] S3. Cooling and shaping: The fabric is cooled by freezing in a freezer. After the TPU inside the fabric is completely cured, it is demolded to obtain the heat-pressable and shape-forming blended fabric of this embodiment.
[0029] The blended fabric obtained in this embodiment is an integrally interwoven fabric without any bonding interface. The surface retains polyester mesh holes, and after hot pressing, it is formed into a simulated leather three-dimensional texture. It has a soft feel and no risk of peeling.
[0030] Example 2 A method for preparing a heat-pressable blended fabric, comprising the following steps: S1. 150D polyester staple fiber is selected as the outer layer bottom yarn and 450D TPU monofilament is selected as the middle layer yarn. Double-sided weft knitting circular knitting machine is used for double-sided weaving. Polyester yarn is woven into the upper bottom layer and TPU yarn is used as filling yarn to run between the two layers. By controlling the length of each yarn feed, the TPU yarn is completely embedded between the two polyester layers to obtain a three-layer blended fabric.
[0031] S2. Place the blank into the mold cavity with the brand logo, mold temperature 220℃, pressure 9T, holding time 40s, hot press to form a three-dimensional logo shape.
[0032] S3. After freezing and cooling in a freezer to set the shape, the fabric is demolded to obtain the blended fabric.
[0033] The blended fabrics obtained in Examples 1 and 2 were used in the preparation of shoe uppers.
[0034] Comparative Example 1 (Prior Art): A TPU film was hot-pressed onto the surface of a polyester mesh to obtain a composite fabric; Comparative Example 2 (Prior Art): A composite fabric was obtained by bonding polyester mesh with artificial leather.
[0035] Performance comparison tests were conducted on the fabrics of Example 1, Comparative Example 1, and Comparative Example 2. Test indicators included: porosity, drape coefficient, cantilever bending stiffness, bending modulus, yarn friction coefficient, interlayer peel strength, and air permeability. The tests verified that the fabric of this invention combines three-dimensional shaping, a soft hand feel, and high breathability, and does not pose a risk of heterogeneous layer peeling.
[0036] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a heat-pressable blended fabric, characterized in that: Includes the following steps: S1. Fabric weaving: Polyester yarn and TPU yarn are woven together to form a three-layer blended fabric; wherein, the three-layer blended fabric includes an outer layer and an inner layer woven from polyester yarn, and an inner layer woven from TPU yarn located between the outer layer and the inner layer, with the TPU yarn completely embedded between the outer layer and the inner layer woven from polyester yarn. S2. Hot pressing: The three-layer blended preform is arranged in the mold cavity and hot pressed. While the polyester yarns of the surface and bottom layers maintain their fiber shape, the TPU yarns of the middle layer are softened by heat and undergo plastic flow, forming a three-dimensional shape in the mold. S3. Cooling and Shaping: Cooling and shaping the fabric after hot pressing to obtain a blended fabric that can be hot-pressed and shaped.
2. The method for preparing a heat-pressable blended fabric according to claim 1, characterized in that: Step S1 involves weaving using warp knitting, weft knitting, or circular knitting techniques. A double-sided or spaced fabric structure is used, with polyester yarns weaving the surface and bottom layers, and TPU yarns as intermediate connecting or filling yarns participating in the weaving. This allows the three layers of yarns to interweave synchronously during the weaving process, forming an integrated multi-layered blended structure. During weaving, the amount of warp feed or yarn feeding is differentiated and correlated with the polyester yarns forming the surface layer, the polyester yarns forming the bottom layer, and the TPU yarns forming the middle layer, so that they are distributed in the middle layer of the fabric and not exposed on the surface and bottom layers.
3. The method for preparing a heat-pressable blended fabric according to claim 2, characterized in that: When using a double-needle bed warp-knitted spacer fabric process, the warp feed rate is set independently for the surface polyester guide bar, the bottom polyester guide bar, and the TPU intermediate connecting guide bar. The formula for calculating the warp feed rate is as follows: ; in, ; Constraints: ; In the formula, For the surface layer polyester comb bar, the amount of warp feed is; For the bottom layer polyester comb bar, the amount of warp feed is... For the TPU intermediate connecting comb, the amount of warp feed is [not specified]. The number of repeating rows in the fabric structure; For the surface layer of polyester comb bar Length of yarn used in the horizontal row; For the bottom layer of polyester comb bar Length of yarn used in the horizontal row; The length of the outer layer polyester coil arc; The length of the bottom polyester coil arc; For TPU combing Length of yarn used in the horizontal row; This refers to the length of the interlayer extension line of the TPU yarn; The needle pitch of the knitting machine; The number of stitches shifted laterally between adjacent rows of padding yarn in the TPU comb bar; This refers to the distance between the front and rear needle beds on a double-needle bed machine. This refers to the actual working elongation of the TPU yarn. The geometric length of the extended line of the TPU yarn in its free state; For the maximum safe elongation allowed for TPU yarn; Weft knitting and circular knitting processes achieve differentiated correlation control by controlling the yarn feeding length of each 100 stitches.
4. The method for preparing a heat-pressable blended fabric according to claim 2, characterized in that: In step S1, the polyester yarn is polyester filament or polyester staple fiber yarn with a specification of 75D-350D; the TPU yarn is TPU monofilament or TPU multifilament yarn with a specification of 300D-1200D; the melting point of the TPU yarn is lower than that of the polyester yarn or its softening point.
5. The method for preparing a heat-pressable blended fabric according to claim 1, characterized in that: In step S1, the mass ratio of polyester yarn to TPU yarn is 40:
60.
6. The method for preparing a heat-pressable blended fabric according to claim 1, characterized in that: In step S2, the mold temperature during hot pressing is 190℃-250℃, the pressure is 6T-18T, and the holding time is 30 seconds-60 seconds. The mold cavity surface is provided with one of the following: simulated leather texture, artificial leather texture, embossed texture, brand logo, three-dimensional curved surface structure, or any combination thereof. After hot pressing, the surface of the blended fabric forms a three-dimensional texture or three-dimensional shape corresponding to the surface of the mold cavity.
7. A blended fabric, characterized in that: It is prepared by the method for preparing heat-pressable woven fabric according to any one of claims 1-6.
8. The application of the blended fabric as described in claim 7 in shoe uppers, bags, or seat upholstery.