High-porosity functional membrane cloth with strong fiber permeability and preparation method and application thereof
The highly porous fiber permeable functional membrane fabric prepared by electrospinning technology solves the problems of traditional membrane fabrics in terms of skin adhesion, absorption efficiency, water retention and active functionality, and achieves higher essence utilization and beauty effect.
Patent Information
- Application Number
- CN202611143866.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional mask sheet materials have shortcomings in terms of skin adhesion, absorption efficiency, water retention, active functionality, and adaptability to high-temperature care scenarios, resulting in low serum utilization, dry skin, and safety risks.
High-porosity fiber permeability functional membrane fabric is prepared using electrospinning technology. By combining modified silicone oil, sulfonated graphene oxide and polyamic acid precursor, the fiber diameter and pore size are controlled, and electromagnetic waves are used to promote microcirculation.
The membrane fabric has improved flexibility, hydrophilicity, and breathability, enhancing the penetration efficiency and water-locking ability of the essence, providing active therapeutic functions, and improving the beauty and skincare effects.
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional fiber membrane materials technology, specifically to a highly porous fiber permeable functional membrane fabric, its preparation method, and its application. Background Technology
[0002] With the rapid development of the functional skincare and minimally invasive medical aesthetics market, consumers have increasingly higher demands for skincare consumables such as mask substrates, medical dressings, and materials for beauty devices. Traditional mask materials (such as non-woven fabrics, silk masks, Tencel masks, cupro fiber masks, etc.) have the following technical shortcomings:
[0003] First, it lacks skin adhesion and delivery efficiency: Traditional mask sheets have relatively large fiber diameters (usually >10μm) and uneven pore structure, resulting in limited adhesion to the skin surface. The essence is mainly delivered through gravity penetration rather than targeted delivery, leading to low utilization of effective ingredients and a large amount of essence evaporation and waste.
[0004] Secondly, their water-locking and moisturizing capabilities are limited: Traditional mask sheets are mostly single-layered, and their water-retention capacity relies on the absorption of external essence, lacking an active water-locking function. Some mask sheets exhibit a "reverse absorption" phenomenon during use, meaning that the mask sheet will absorb moisture from the skin's surface during the drying process, exacerbating skin dryness.
[0005] Third, there is a lack of active functionality: most existing membrane sheets are inert carriers, only providing the function of carrying essence, and do not have additional functions such as active therapy, microcirculation promotion, and warm care. Although some products attempt to impart far-infrared functions by adding ceramic powder, there are problems such as powder shedding and questionable safety.
[0006] Fourth, poor adaptability to high-temperature care scenarios: Products such as hot compress masks and heating films for beauty instruments have high requirements for the heat resistance, flexibility, and insulation of the materials. Traditional fabric materials are prone to aging and deformation after repeated heating and use, posing safety hazards.
[0007] In view of this, the present invention is hereby proposed. Summary of the Invention
[0008] The purpose of this invention is to provide a highly porous fiber permeable functional membrane fabric, its preparation method, and its application. The highly porous fiber permeable functional membrane fabric prepared by this invention has excellent flexibility, hydrophilicity, breathability, and mechanical properties, and can be better used in beauty and skin care products.
[0009] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:
[0010] The first aspect of this invention provides a method for preparing a highly porous fiber permeable functional membrane fabric, the method comprising the following steps:
[0011] (a) A modified silicone oil was obtained by reacting amino-terminated silicone oil with 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone.
[0012] (b) Under nitrogen protection, 4,4'-diaminodiphenyl ether and p-phenylenediamine were dissolved in N,N-dimethylacetamide, and then modified silicone oil was added to obtain a diamine solution;
[0013] (c) Under ice bath conditions, pyromellitic dianhydride was added to the diamine solution and stirred. After the reaction was completed, sulfonated graphene oxide and tetrabutylammonium chloride were added and ultrasonically dispersed to obtain the spinning solution.
[0014] (d) Electrospinning the spinning solution to obtain a polyamic acid precursor fiber membrane, followed by thermal imidization and shaping to obtain the highly porous fiber permeable functional membrane fabric.
[0015] Preferably, in step (a), the molar ratio of amino-terminated silicone oil to 1-(3-allyl-2,4-dihydroxyphenyl)ethyl ketone is 1:1.
[0016] Preferably, in step (a), the reaction temperature is 40~60℃ and the time is 4~6h.
[0017] Preferably, in step (b), the mass ratio of 4,4'-diaminodiphenyl ether, p-phenylenediamine and modified silicone oil is (80~95):(5~20):(2~15).
[0018] Preferably, in step (c), the mass ratio of pyromellitic dianhydride to 4,4'-diaminodiphenyl ether is (18~22):(16~19).
[0019] The mass ratio of pyromellitic dianhydride, sulfonated graphene oxide, and tetrabutylammonium chloride is (90~110):(0.05~0.3):(0.5~2).
[0020] Preferably, in step (c), the stirring reaction temperature is no higher than 10°C and the time is 3~5h.
[0021] Preferably, in step (d), the electrospinning parameters are as follows: voltage 15~25kV, receiving distance 12~18cm, spinning solution flow rate 0.3~0.7mL / h, ambient temperature 20~30℃, relative humidity 40%~60%, and the diameter of the electrospun fiber is 0.3~0.8μm.
[0022] Preferably, in step (d), the thermal imidization includes: first heating to 170~190℃ and holding for 12~18 min, then heating to 280~320℃ and holding for 18~22 min, and finally heating to 370~390℃ and holding for 6~10 min.
[0023] A second aspect of the present invention provides a highly porous fiber permeable functional membrane fabric prepared by the above-described preparation method.
[0024] The third aspect of the present invention provides an application of the highly porous fiber permeable functional membrane fabric prepared by the above-mentioned preparation method in the preparation of beauty and skin care products, wherein the beauty and skin care products include a facial mask substrate, a medical cold compress substrate, a beauty instrument hot compress mask, and an eye hot compress.
[0025] Compared with the prior art, the beneficial effects of the present invention include at least the following:
[0026] The highly porous fiber permeable functional membrane fabric prepared by this invention possesses excellent flexibility, hydrophilicity, breathability, and mechanical properties, making it better suited for use in beauty and skincare products. Specifically, the introduction of modified silicone oil imparts better flexibility and wrinkle resistance to the fiber membrane, while maintaining the high strength characteristics of polyimide and regulating the membrane fabric's amphiphilic wettability and breathability to water-based essences and oil-based active ingredients. The sulfonate group (-SO3H) on the surface of sulfonated graphene oxide endows the fiber membrane with excellent liquid absorption and wettability, significantly reducing the essence contact angle and greatly improving penetration efficiency. Simultaneously, the two-dimensional planar structure of graphene oxide undergoes π-π conjugated interaction with the polyimide molecular chains, orienting along the fiber axis under the shearing action during spinning, thus improving the tensile strength of the fiber membrane. Furthermore… PPDA introduces a rigid benzene ring structure, increasing the rigidity of the molecular chain and improving tensile strength; ODA provides flexible ether bonds to ensure spinning processability. The two work together to give the membrane fabric both high strength and good flexibility. By using electrospinning technology and adding sulfonated graphene oxide and tetrabutylammonium chloride, the charge density of the jet during electrospinning can be controlled, the fiber diameter and distribution can be controlled to be more uniform, and the pore size is more uniform.
[0027] The beauty and skincare products prepared from the highly porous fiber permeable functional membrane fabric of this invention can be used in conjunction with electromagnetic waves. Through the promoting effect of electromagnetic waves on human microcirculation and metabolism, the effective ingredients of the beauty and skincare products are absorbed by the skin, resulting in better beauty effects. Detailed Implementation
[0028] The embodiments of the technical solution of the present invention will be described in detail below with reference to the examples. The following embodiments are only used to illustrate the technical solution of the present invention more clearly, and are therefore only examples, and should not be used to limit the scope of protection of the present invention.
[0029] It should be noted that, unless otherwise stated, the technical or scientific terms used in this application should have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.
[0030] This invention provides a method for preparing a highly porous fiber permeable functional membrane fabric, the preparation method comprising the following steps:
[0031] (a) A modified silicone oil was obtained by reacting amino-terminated silicone oil with 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone.
[0032] (b) Under nitrogen protection, 4,4'-diaminodiphenyl ether and p-phenylenediamine were dissolved in N,N-dimethylacetamide, and then modified silicone oil was added to obtain a diamine solution;
[0033] (c) Under ice bath conditions, pyromellitic dianhydride was added to the diamine solution and stirred. After the reaction was completed, sulfonated graphene oxide and tetrabutylammonium chloride were added and ultrasonically dispersed to obtain the spinning solution.
[0034] (d) Electrospinning the spinning solution to obtain a polyamic acid precursor fiber membrane, followed by thermal imidization and shaping to obtain the highly porous fiber permeable functional membrane fabric.
[0035] In one embodiment, in step (a), the molar ratio of the amino-terminated silicone oil and 1-(3-allyl-2,4-dihydroxyphenyl)ethyl ketone is 1:1.
[0036] In one embodiment, in step (a), the reaction temperature is 40~60°C and the time is 4~6h.
[0037] In one embodiment, in step (b), the mass ratio of 4,4'-diaminodiphenyl ether, p-phenylenediamine and modified silicone oil is (80~95):(5~20):(2~15).
[0038] In one embodiment, in step (c), the mass ratio of pyromellitic dianhydride to 4,4'-diaminodiphenyl ether is (18~22):(16~19).
[0039] The mass ratio of pyromellitic dianhydride, sulfonated graphene oxide, and tetrabutylammonium chloride is (90~110):(0.05~0.3):(0.5~2).
[0040] In one embodiment, in step (c), the stirring reaction temperature is no higher than 10°C, and the time is 3-5 hours.
[0041] In one embodiment, the electrospinning parameters in step (d) are as follows: voltage 15~25kV, receiving distance 12~18cm, spinning solution flow rate 0.3~0.7mL / h, ambient temperature 20~30℃, relative humidity 40%~60%, and the diameter of the electrospun fiber is 0.3~0.8μm.
[0042] In one embodiment, step (d) of thermal imidization includes: first heating to 170~190°C and holding for 12~18 min, then heating to 280~320°C and holding for 18~22 min, and finally heating to 370~390°C and holding for 6~10 min.
[0043] Another embodiment of the present invention provides a highly porous fiber permeable functional membrane fabric prepared by the above preparation method.
[0044] Another embodiment of the present invention provides the application of the highly porous fiber permeable functional membrane fabric prepared by the above preparation method in the preparation of beauty and skin care products, wherein the beauty and skin care products include a facial mask substrate, a medical cold compress substrate, a beauty instrument hot compress mask, and an eye hot compress.
[0045] The technical solution of the present invention will be further described in detail below through specific embodiments.
[0046] Example 1
[0047] This embodiment describes a method for preparing a highly porous fiber permeable functional membrane fabric, the preparation method comprising the following steps:
[0048] (a) A amino-terminated silicone oil (8069 amino-terminated small molecule silicone oil) and 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone were reacted at a temperature of 40°C for 6 hours to obtain modified silicone oil, wherein the molar ratio of amino-terminated silicone oil to 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone was 1:1;
[0049] (b) Under nitrogen protection, 4,4'-diaminodiphenyl ether and p-phenylenediamine are dissolved in N,N-dimethylacetamide, and then modified silicone oil is added to obtain a diamine solution, wherein the mass ratio of 4,4'-diaminodiphenyl ether, p-phenylenediamine and modified silicone oil is 80:5:2;
[0050] (c) Under ice bath conditions, pyromellitic dianhydride was added to the diamine solution and stirred for 3 hours (temperature not exceeding 10°C). After the reaction was completed, sulfonated graphene oxide and tetrabutylammonium chloride were added and ultrasonically dispersed to obtain the spinning solution. The mass ratio of pyromellitic dianhydride to 4,4'-diaminodiphenyl ether was 18:19; the mass ratio of pyromellitic dianhydride, sulfonated graphene oxide and tetrabutylammonium chloride was 90:0.3:0.5.
[0051] (d) The spinning solution is electrospun to obtain a polyamic acid precursor fiber membrane, which is then subjected to thermal imidization and calendering to obtain the high-porosity fiber permeability functional membrane fabric. The electrospinning parameters are as follows: voltage 15kV, receiving distance 18cm, spinning solution flow rate 0.3mL / h, ambient temperature 30℃, relative humidity 40%, and the diameter of the electrospun fiber is 0.5μm.
[0052] The thermal imidization process includes: first heating to 170℃ and holding for 18 min, then heating to 280℃ and holding for 22 min, and finally heating to 390℃ and holding for 10 min.
[0053] Example 2
[0054] This embodiment describes a method for preparing a highly porous fiber permeable functional membrane fabric, the preparation method comprising the following steps:
[0055] (a) A amino-terminated silicone oil (8069 amino-terminated small molecule silicone oil) and 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone were reacted at a temperature of 60°C for 4 hours to obtain modified silicone oil, wherein the molar ratio of amino-terminated silicone oil to 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone was 1:1;
[0056] (b) Under nitrogen protection, 4,4'-diaminodiphenyl ether and p-phenylenediamine are dissolved in N,N-dimethylacetamide, and then modified silicone oil is added to obtain a diamine solution, wherein the mass ratio of 4,4'-diaminodiphenyl ether, p-phenylenediamine and modified silicone oil is 95:20:15;
[0057] (c) Under ice bath conditions, pyromellitic dianhydride was added to the diamine solution and stirred for 5 h (temperature not higher than 10℃). After the reaction was completed, sulfonated graphene oxide and tetrabutylammonium chloride were added and ultrasonically dispersed to obtain the spinning solution. The mass ratio of pyromellitic dianhydride to 4,4'-diaminodiphenyl ether was 22:16; the mass ratio of pyromellitic dianhydride, sulfonated graphene oxide and tetrabutylammonium chloride was 110:0.05:2.
[0058] (d) The spinning solution is electrospun to obtain a polyamic acid precursor fiber membrane, which is then subjected to thermal imidization and calendering to obtain the high-porosity fiber permeability functional membrane fabric. The electrospinning parameters are as follows: voltage 25kV, receiving distance 12cm, spinning solution flow rate 0.7mL / h, ambient temperature 20℃, relative humidity 60%, and the diameter of the electrospun fiber is 0.5μm.
[0059] The thermal imidization process includes: first heating to 190℃ and holding for 12 minutes, then heating to 320℃ and holding for 18 minutes, and finally heating to 370℃ and holding for 6 minutes.
[0060] Example 3
[0061] This embodiment describes a method for preparing a highly porous fiber permeable functional membrane fabric, the preparation method comprising the following steps:
[0062] (a) A amino-terminated silicone oil (8069 amino-terminated small molecule silicone oil) and 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone were reacted at a temperature of 50°C for 5 h to obtain modified silicone oil, wherein the molar ratio of amino-terminated silicone oil to 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone was 1:1;
[0063] (b) Under nitrogen protection, 4,4'-diaminodiphenyl ether and p-phenylenediamine are dissolved in N,N-dimethylacetamide, and then modified silicone oil is added to obtain a diamine solution, wherein the mass ratio of 4,4'-diaminodiphenyl ether, p-phenylenediamine and modified silicone oil is 90:15:10;
[0064] (c) Under ice bath conditions, pyromellitic dianhydride was added to the diamine solution and stirred for 4 hours (temperature not higher than 10°C). After the reaction was completed, sulfonated graphene oxide and tetrabutylammonium chloride were added and ultrasonically dispersed to obtain the spinning solution. The mass ratio of pyromellitic dianhydride to 4,4'-diaminodiphenyl ether was 20:18; the mass ratio of pyromellitic dianhydride, sulfonated graphene oxide and tetrabutylammonium chloride was 100:0.2:1.
[0065] (d) The spinning solution is electrospun to obtain a polyamic acid precursor fiber membrane, which is then subjected to thermal imidization and calendering to obtain the high-porosity fiber permeability functional membrane fabric. The electrospinning parameters are as follows: voltage 20kV, receiving distance 15cm, spinning solution flow rate 0.5mL / h, ambient temperature 25℃, relative humidity 50%, and the diameter of the electrospun fiber is 0.5μm.
[0066] The thermal imidization process includes: first heating to 180°C and holding for 15 minutes, then heating to 300°C and holding for 20 minutes, and finally heating to 380°C and holding for 8 minutes.
[0067] Comparative Example 1
[0068] This comparative example is a method for preparing a highly porous fiber permeable functional membrane fabric. The preparation method is basically the same as that in Example 3, except that sulfonated graphene oxide is not added in step (c).
[0069] Comparative Example 2
[0070] This comparative example is a method for preparing a highly porous fiber permeable functional membrane fabric. The preparation method is basically the same as that in Example 3, except that in step (b), p-phenylenediamine is replaced with an equal amount of 4,4'-diaminodiphenyl ether.
[0071] Comparative Example 3
[0072] This comparative example is a method for preparing a highly porous fiber permeable functional membrane fabric. The preparation method is basically the same as that in Example 3, except that modified silicone oil is not added in step (b).
[0073] Experimental Example
[0074] High-porosity fiber permeable functional membrane fabrics were prepared according to the preparation methods of Example 3 and Comparative Examples 1-3, respectively.
[0075] The performance of the prepared high-porosity fiber permeable functional membrane fabric was tested (3 replicates). The test methods are shown in Table 1, and the results were statistically analyzed as shown in Table 2.
[0076] Table 1
[0077] detection indicators Test methods / standards illustrate Fiber tensile strength (MPa) GB / T 1040.3-2006 Tensile properties of plastics, film / sheet specimens, 50 mm / min Liquid permeation time (s) FZ / T 60017-93 Liquid permeability test of nonwoven fabrics Serum carrying capacity (times) Self-built method Immerse the sample in the essence until saturated, remove and let stand for 30 seconds, then weigh and calculate: (wet weight - dry weight) / dry weight Breathability (mm / s) GB / T 5453-1997 The air permeability of textiles was tested with a pressure difference of 100 Pa and a test area of 20 cm². Porosity (%) Density method Sample bulk density / skeletal density × 100%, refer to GB / T 24218.18 Hydrophilicity (contact angle, °) GB / T 30693-2014 The water contact angle was determined using the static drop method with distilled water at 25°C.
[0078] Table 2
[0079] detection indicators Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Fiber tensile strength (MPa) 9.2 ± 0.4 6.8 ± 0.3 5.6 ± 0.3 7.1 ± 0.4 Liquid permeation time (s) 1.6 ± 0.1 3.5 ± 0.2 2.8 ± 0.2 1.9 ± 0.1 Serum carrying capacity (times) 15.2 ± 0.5 11.4 ± 0.4 12.8 ± 0.5 13.5 ± 0.4 Breathability (mm / s) 92 ± 5 78 ± 4 68 ± 4 85 ± 4 Porosity (%) 88.5 ± 1.2 82.3 ± 1.5 84.1 ± 1.3 86.2 ± 1.2 Hydrophilicity (contact angle, °) 18.5 ± 2.1 42.3 ± 2.5 35.6 ± 2.8 22.4 ± 2.3
[0080] As shown in Table 2:
[0081] Compared to the comparative example, the highly porous fiber permeable functional membrane fabric prepared in this application has excellent hydrophilicity, breathability and mechanical properties, and can be better used in beauty and skin care products to meet market demand.
[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.
Claims
1. A method for preparing a highly porous fiber permeable functional membrane fabric, characterized in that, The preparation method includes the following steps: (a) A modified silicone oil was obtained by reacting amino-terminated silicone oil with 1-(3-allyl-2,4-dihydroxyphenyl) ethyl ketone. (b) Under nitrogen protection, 4,4'-diaminodiphenyl ether and p-phenylenediamine were dissolved in N,N-dimethylacetamide, and then modified silicone oil was added to obtain a diamine solution; (c) Under ice bath conditions, pyromellitic dianhydride was added to the diamine solution and stirred. After the reaction was completed, sulfonated graphene oxide and tetrabutylammonium chloride were added and ultrasonically dispersed to obtain the spinning solution. (d) Electrospinning the spinning solution to obtain a polyamic acid precursor fiber membrane, followed by thermal imidization and shaping to obtain the highly porous fiber permeable functional membrane fabric.
2. The preparation method according to claim 1, characterized in that, In step (a), the molar ratio of amino-terminated silicone oil to 1-(3-allyl-2,4-dihydroxyphenyl)ethyl ketone is 1:
1.
3. The preparation method according to claim 1, characterized in that, In step (a), the reaction temperature is 40~60℃ and the time is 4~6h.
4. The preparation method according to claim 1, characterized in that, In step (b), the mass ratio of 4,4'-diaminodiphenyl ether, p-phenylenediamine and modified silicone oil is (80~95):(5~20):(2~15).
5. The preparation method according to claim 1, characterized in that, In step (c), the mass ratio of pyromellitic dianhydride to 4,4'-diaminodiphenyl ether is (18~22):(16~19). The mass ratio of pyromellitic dianhydride, sulfonated graphene oxide, and tetrabutylammonium chloride is (90~110):(0.05~0.3):(0.5~2).
6. The preparation method according to claim 1, characterized in that, In step (c), the stirring reaction temperature is no higher than 10°C, and the time is 3-5 hours.
7. The preparation method according to claim 1, characterized in that, In step (d), the electrospinning parameters are as follows: voltage 15~25kV, receiving distance 12~18cm, spinning solution flow rate 0.3~0.7mL / h, ambient temperature 20~30℃, relative humidity 40%~60%, and the diameter of the electrospun fiber is 0.3~0.8μm.
8. The preparation method according to claim 1, characterized in that, In step (d), thermal imidization includes: first heating to 170~190℃ and holding for 12~18 min, then heating to 280~320℃ and holding for 18~22 min, and finally heating to 370~390℃ and holding for 6~10 min.
9. A highly porous fiber permeable functional membrane fabric prepared by any of the preparation methods described in claims 1 to 8.
10. The application of the highly porous fiber permeable functional membrane fabric prepared by any one of claims 1 to 8 in the preparation of cosmetic and skincare products, characterized in that, The beauty and skincare products include facial mask substrates, medical cold compress substrates, beauty device hot compress masks, and eye hot compress patches.