Production process of bacteriostatic spunbond nonwoven fabric and product thereof
By using an extended die head and an ultrasonic treatment device in the production process of spunbond nonwoven fabric, the gelation problem caused by polyquaternium salts was solved, achieving high-quality nonwoven fabric drawing and improving production efficiency and product quality.
Patent Information
- Application Number
- CN202611573829.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-20
AI Technical Summary
In the process of preparing spunbond nonwoven fabric by blending and melting polyquaternium salt as an antibacterial agent, how to improve the local gelation phenomenon during the processing, avoid the formation of gel particles during the drawing process, and improve the drawing effect?
By employing an extended die head and an ultrasonic treatment device, the extruded raw material is subjected to ultrasonic vibration treatment between the screw extruder outlet and the spinneret orifice. Combined with a special internal flow channel design, including a feeding section, a vibration section, and a discharge section, the cavitation effect and mechanical vibration effect of ultrasound are used to refine gel particles and improve melt uniformity.
This effectively avoids the formation of gel particles, improves the fiber drawing effect, and ensures the quality and consistency of spunbond nonwoven fabric.
Abstract
Description
Technical Field
[0001] This invention relates to the field of nonwoven fabrics, and in particular to a production process and product of antibacterial spunbond nonwoven fabric. Background Technology
[0002] With the increasing global awareness of medical and personal protective equipment, the demand for medical protective equipment such as medical masks and protective clothing has surged. As a core material for these products, nonwoven fabrics have also seen a significant increase in market demand. At the same time, the production process of nonwoven fabrics has been continuously improved, resulting in significant increases in production efficiency and product quality. Spunbond nonwoven fabrics, as a common type of nonwoven fabric, have also experienced rapid development.
[0003] As development deepens, spunbond nonwoven fabrics with special properties are constantly emerging in the market. For example, Chinese invention patent application number "202310751844.9", entitled "An Antibacterial Spunbond Nonwoven Fabric and Its Preparation Method", discloses an antibacterial spunbond nonwoven fabric and its preparation method. It involves adding a zinc-based antibacterial agent to a polypropylene substrate. The zinc-based antibacterial agent, combined with a dispersant and a coupling agent, forms an antibacterial masterbatch. The dispersant and coupling agent promote the uniform bonding of the zinc-based antibacterial agent with the polypropylene. The resulting polypropylene-based antibacterial masterbatch has good compatibility with the polypropylene spunbond nonwoven fabric, allowing them to bond uniformly during the melting process. This promotes the uniform dispersion of the antibacterial components in the spunbond nonwoven fabric system, improving its dispersibility. However, this solution involves the addition of metal ions, which may cause irritation upon skin contact, such as redness, swelling, and itching. Furthermore, some users may be allergic to certain metal ions, experiencing allergic reactions such as rashes and allergic dermatitis upon contact.
[0004] Therefore, recently, technologies that apply polyquaternary ammonium salts to spunbond nonwoven fabrics have emerged on the market. For example, the application with application number "202311697178.1" and title "A guanidine quaternary ammonium salt antibacterial polymer and its preparation method and application" proposes a guanidine quaternary ammonium salt antibacterial polymer, which covalently grafts the commonly used human-safe disinfectant polyhexamethylene biguanide and quaternary ammonium salt together, which can achieve a better synergistic antibacterial effect. Moreover, this graft copolymer compound has high heat resistance and antibacterial properties, and can be blended and melt-prepared with polymer materials to prepare antibacterial nonwoven fabrics and other products.
[0005] However, the introduction of polyquaternium salts can affect the molecular weight distribution of polypropylene, and the change in molecular weight can affect the crystallinity and crystallization rate of polypropylene. Such inhomogeneity can lead to local gelation of the melt during processing, which in turn can result in gel particles during the fiber drawing process, thus affecting the fiber drawing effect. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the technical problem to be solved by this invention is: how to improve the localized gelation phenomenon that occurs during the processing of spunbond nonwoven fabrics by using polyquaternary ammonium salts as antibacterial agents in blending and melting, thereby minimizing the formation of gel particles during the drawing process and improving the drawing effect.
[0007] To address the aforementioned problems, this invention proposes a production process for antibacterial spunbond nonwoven fabric, comprising the following steps in sequence: S1: Raw material preparation, taking polypropylene substrate and antibacterial granules (the antibacterial granules are polyquaternium salts), premixing the polypropylene substrate and antibacterial granules, and adding additives to obtain a mixed raw material; S2: Melt spinning, feeding the mixed raw material into a screw extruder, heating and stirring the mixed raw material in the screw extruder to form an extruded raw material, which is then extruded through a spinneret to form fibers; S3: Cooling and stretching, cooling the fibers with air and performing fiber stretching... S4: Laying and bonding, laying the fibers into a web, and then hot-rolling the web to melt and bond the fibers to obtain a nonwoven fabric; S5: Post-treatment, performing surface treatment on the nonwoven fabric as required, and then winding and collecting the surface-treated nonwoven fabric; The feature is that in the S2 melt spinning step, an extended die head is provided between the outlet of the screw extruder and the spinneret hole, the extruded raw material flows through the inner channel in the middle of the extended die head, and an ultrasonic treatment device is provided on the outside of the extended die head, which performs ultrasonic vibration treatment on the extruded raw material that continuously passes through the extended die head.
[0008] In this field, common practices to address the polypropylene crystallinity issue caused by the addition of polyquaternium salts include: premixing with a high-speed mixer or twin-screw extruder during the raw material mixing stage to ensure thorough mixing of the polyquaternium salt and polypropylene; setting up precise temperature control systems in each heating zone of the extruder and meltblown die to ensure temperature stability and uniformity; and installing online monitoring equipment, such as temperature sensors, pressure sensors, and fiber diameter monitors, to monitor key parameters in real time and adjust process conditions promptly. However, these practices are either limited in effectiveness or require high levels of production control. The present invention utilizes the cavitation and mechanical vibration effects of ultrasound to refine gel particles in the polypropylene melt, improve melt uniformity, and avoids the drawbacks of the conventional methods described above.
[0009] Preferably, the mass ratio of polypropylene substrate to polyquaternium salt is 97:3. The addition of polyquaternium salt alters the crystallinity of polypropylene, thus affecting fiber formation during the subsequent filament drawing process; therefore, the proportion of polyquaternium salt should not be too high. On the other hand, a higher polyquaternium salt content can improve the antibacterial effect of spunbond nonwoven fabric; therefore, this ratio is preferred in this design.
[0010] Furthermore, the extruded material travels at least 30 cm through the extended die head's inner flow channel. This inner flow channel includes a feeding section, a vibrating section, and a discharging section. The feeding section has a gradually increasing orifice diameter along the flow direction of the extruded material, while the vibrating section has a constant orifice diameter. The discharging section has a gradually decreasing orifice diameter along the flow direction of the extruded material. The extruded material's flow rate slows down in the feeding section, resulting in pressure reduction. It undergoes ultrasonic vibration in the vibrating section and is pressurized in the discharging section due to the reduced orifice diameter. Firstly, the minimum 30 cm travel distance ensures sufficient ultrasonic treatment of the extruded material. Secondly, designing the inner flow channel as a three-section (feeding, vibrating, and discharging) with a variable diameter structure allows for some pressure relief in the vibrating section, enhancing the vibration effect, while the pressure in the discharging section ensures the extruded material regains its compactness, resulting in a continuous and compact process.
[0011] Preferably, the length ratio of the feed section to the discharge section through which the extruded raw material flows in the extended die head is 1:0.3-0.5, and the length ratio of the vibration section to the discharge section is 1:4-6. Since this process involves decompression, vibration, and pressurization, any segmentation of the extended die head can lead to changes in product properties. Experiments have shown that the product properties obtained by the above-mentioned segmentation are better.
[0012] At this point, the ultrasonic frequency of the ultrasonic processing device is set to 30-50 kHz, and the ultrasonic power is set to 100-200 W. The frequency of ultrasonic processing is typically between 20-100 kHz, and the power range is typically between 100-500 W. For the mixed system of polypropylene and polyquaternary ammonium salt, a low-frequency processing of 20-40 kHz can be used, along with a relatively low power of 100-300 W to enhance the mechanical and cavitation effects. However, because this scheme uses the aforementioned special extended head, the processing frequency can be appropriately increased for more precise material processing. Furthermore, higher frequency ultrasonic energy is more concentrated, causing less damage to the material structure, thus allowing for a more appropriate reduction in power selection.
[0013] Regarding the temperature issue in the extended die head area, the first solution is to implement temperature control in the extended die head, within a range of 220℃-225℃. The extrusion temperature of a screw extruder is typically controlled at 230℃. The residence time of the extruded material in the extended die head is limited, and the ultrasonic treatment device exerts energy on the melt. Controlling the extended die head temperature between 220℃ and 225℃ ensures that the ultrasonic waves provide sufficient vibration without affecting the melt's fluidity.
[0014] The second approach involves adding triphenyl phosphate as an additive in the S1 raw material preparation step, and controlling the temperature of the extended die head within a range of 235℃-240℃. Higher temperatures allow for more thorough refinement of the gel particles in the extruded raw material under ultrasonic action. However, due to the high temperature, special additives are needed to improve the material's thermal stability. Simultaneously, these additives must avoid affecting the antibacterial effect of the polyquaternium salt; therefore, triphenyl phosphate is chosen.
[0015] Specifically, the polyquaternary ammonium salt is a guanidine quaternary ammonium salt antibacterial polymer. Guanidine quaternary ammonium salt antibacterial polymers have dual antibacterial groups of quaternary ammonium salt and guanidine salt, exhibiting excellent antibacterial properties. At the same time, they have high heat resistance and resistance to decomposition, and a wide processing temperature window, making them suitable for melt blending with polymer granules to prepare antibacterial nonwoven fabrics.
[0016] As an alternative, hyperbranched polyquaternium salts are preferred. Hyperbranched polyquaternium salts exhibit good antibacterial properties and biocompatibility.
[0017] The present invention also proposes an antibacterial spunbond nonwoven fabric, which is produced according to the antibacterial spunbond nonwoven fabric production process described above.
[0018] In summary, this antibacterial spunbond nonwoven fabric production process and its products, under the premise of using polyquaternary ammonium salt as an antibacterial agent for blending and melting to prepare spunbond nonwoven fabric, can improve the local gelation phenomenon that occurs during processing, thereby minimizing the formation of gel particles during the drawing process and improving the drawing effect. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below.
[0020] A process for producing antibacterial spunbond nonwoven fabric includes the following steps in sequence: S1: Raw material preparation, taking polypropylene substrate and antibacterial granules, the antibacterial granules being polyquaternary ammonium salt, premixing the polypropylene substrate and antibacterial granules, and adding auxiliaries to obtain a mixed raw material; S2: Melt spinning, feeding the mixed raw material into a screw extruder, the screw extruder heating and stirring the mixed raw material to form an extruded raw material, which is then extruded through a spinneret to form fibers; S3: Cooling and stretching, the fibers are cooled by air and stretched; S4: S5: Web laying and bonding, the fibers are laid into a web, and the web is hot-rolled to melt and bond the fibers to obtain nonwoven fabric; S6: Post-treatment, the nonwoven fabric is surface-treated as required, and the surface-treated nonwoven fabric is wound and collected; The feature is that: in the S2 melt spinning step, an extended die head is provided between the outlet of the screw extruder and the spinneret hole, the extruded raw material flows through the inner flow channel in the middle of the extended die head, and an ultrasonic treatment device is provided on the outside of the extended die head, the ultrasonic treatment device performs ultrasonic vibration treatment on the extruded raw material that continuously passes through the extended die head.
[0021] In this field, common practices to address the polypropylene crystallinity issue caused by the addition of polyquaternium salts include: premixing with a high-speed mixer or twin-screw extruder during the raw material mixing stage to ensure thorough mixing of the polyquaternium salt and polypropylene; setting up precise temperature control systems in each heating zone of the extruder and meltblown die to ensure temperature stability and uniformity; and installing online monitoring equipment, such as temperature sensors, pressure sensors, and fiber diameter monitors, to monitor key parameters in real time and adjust process conditions promptly. However, these practices are either limited in effectiveness or require high levels of production control. The present invention utilizes the cavitation and mechanical vibration effects of ultrasound to refine gel particles in the polypropylene melt, improve melt uniformity, and avoids the drawbacks of the conventional methods described above.
[0022] In this embodiment, the mass ratio of polypropylene substrate to polyquaternium salt is 97:3. The addition of polyquaternium salt alters the crystallinity of polypropylene, thus affecting fiber formation during the subsequent filament drawing process; therefore, the proportion of polyquaternium salt cannot be too high. On the other hand, a higher polyquaternium salt content can improve the antibacterial effect of spunbond nonwoven fabric; therefore, this ratio is preferred in this embodiment.
[0023] Furthermore, the extruded material travels at least 30 cm through the inner channel of the extended die head. This inner channel includes a feeding section, a vibrating section, and a discharging section. The diameter of the orifice in the feeding section gradually increases along the flow direction of the extruded material, while the diameter in the vibrating section remains constant. The diameter of the orifice in the discharging section gradually decreases along the flow direction of the extruded material. The flow velocity of the extruded material slows down as it passes through the feeding section. The extruded material undergoes ultrasonic vibration treatment as it passes through the vibrating section, and it is compressed as it passes through the discharging section due to the reduced orifice diameter. In this embodiment, the inner channel travels at least 50 cm. Firstly, a travel distance of at least 30 cm ensures that the extruded material undergoes sufficient ultrasonic treatment. Secondly, designing the inner channel as a three-section (feeding, vibrating, and discharging) with a variable diameter structure allows for some pressure relief on the extruded material in the vibrating section, enhancing the vibration effect. Simultaneously, the material is compressed in the discharging section, ensuring the extruded material regains its compactness, resulting in a continuous and compact process.
[0024] Preferably, the length ratio of the feed section to the discharge section through which the extruded raw material flows in the extended die head is 1:0.3-0.5, and the length ratio of the vibration section to the discharge section is 1:4-6. In this embodiment, the length ratio of the feed section to the discharge section is 1:0.4, and the length ratio of the vibration section to the discharge section is 1:5. Since this process involves decompression, vibration, and pressurization, any segmentation of the extended die head can lead to changes in product properties. Experiments have shown that the product properties obtained by the above-mentioned segmentation are better.
[0025] Preferably, the ultrasonic frequency of the ultrasonic processing device is set to 30-50kHz, and the ultrasonic power is set to 100-200W. In this embodiment, the frequency is selected as 40kHz, and the power is set to 150W. The frequency of ultrasonic processing is usually between 20-100kHz, and the power range is usually between 100-500W. For the mixed system of polypropylene and polyquaternary ammonium salt, a low-frequency processing of 20-40kHz can be used, along with a relatively low power of 100-300W, to enhance the mechanical and cavitation effects. However, since this scheme uses the aforementioned special extended head, the processing frequency can be appropriately increased for more detailed material processing. Moreover, the high-frequency ultrasonic energy is more concentrated, causing less damage to the material structure, so the power selection can be appropriately reduced.
[0026] Regarding the temperature issue in the extended head section, this embodiment can adopt two solutions:
[0027] The first approach is to extend the die head for temperature control, with a range of 220℃-225℃. The extrusion temperature of a screw extruder is typically controlled at 230℃. The residence time of the extruded material in the extended die head is limited, and the ultrasonic treatment device exerts energy on the melt. Controlling the extended die head temperature at 220℃-225℃ ensures that the ultrasonic waves effectively vibrate without affecting the melt's fluidity.
[0028] The second option is to add triphenyl phosphate as an additive in the S1 raw material preparation step, and to control the temperature of the extended die head within the range of 235℃-240℃. Higher temperatures allow for more thorough refinement of the gel particles in the extruded raw material under ultrasonic action. However, due to the high temperature, special additives are needed to improve the material's thermal stability. Simultaneously, this substance must avoid affecting the antibacterial effect of the polyquaternium salt; therefore, triphenyl phosphate is chosen.
[0029] In this embodiment, the polyquaternary ammonium salt is a guanidine quaternary ammonium salt antibacterial polymer or a hyperbranched polyquaternary ammonium salt. Guanidine quaternary ammonium salt antibacterial polymers possess both quaternary ammonium salt and guanidine salt antibacterial groups, exhibiting excellent antibacterial properties. They also possess high heat resistance and resistance to decomposition, and have a wide processing temperature window, making them suitable for melt blending with polymer granules to prepare antibacterial nonwoven fabrics. Hyperbranched polyquaternary ammonium salts, on the other hand, exhibit good antibacterial properties and biocompatibility.
[0030] The present invention also proposes an antibacterial spunbond nonwoven fabric, which is produced according to the antibacterial spunbond nonwoven fabric production process described above.
[0031] In summary, this antibacterial spunbond nonwoven fabric production process and its products, under the premise of using polyquaternary ammonium salt as an antibacterial agent for blending and melting to prepare spunbond nonwoven fabric, can improve the local gelation phenomenon that occurs during processing, thereby minimizing the formation of gel particles during the drawing process and improving the drawing effect.
[0032] In summary, the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A process for producing antibacterial spunbond nonwoven fabric, comprising the following steps in sequence: S1: Raw material preparation: Take polypropylene substrate and antibacterial granules, wherein the antibacterial granules are polyquaternary ammonium salts. Premix the polypropylene substrate and antibacterial granules and add additives to obtain mixed raw materials. S2: Melt spinning, the mixed raw materials are fed into a screw extruder, the screw extruder heats and stirs the mixed raw materials evenly to form extruded raw materials, which are then extruded through spinnerets to form fibers; S3: Cooling and stretching, the fiber is cooled by air and stretched; S4: Web laying and bonding, the fibers are laid into a web, and the web is hot-rolled to melt and bond the fibers to obtain a nonwoven fabric; S5: Post-processing, the non-woven fabric is surface-treated as required, and the surface-treated non-woven fabric is wound and collected. Its features are: In the S2 melt spinning step, an extended die head is provided between the outlet of the screw extruder and the spinneret, so that the extruded raw material flows through the inner channel in the middle of the extended die head, and ultrasonic vibration is applied to the extended die head using an ultrasonic treatment device.
2. The antibacterial spunbond nonwoven fabric production process according to claim 1, characterized in that: The mass ratio of the polypropylene substrate to the polyquaternary ammonium salt is 97:
3.
3. The antibacterial spunbond nonwoven fabric production process according to claim 2, characterized in that: The extruded material travels for at least 30 centimeters through the inner channel of the extended die head. The inner channel includes a feeding section, a vibrating section, and a discharging section. The diameter of the feeding section gradually increases along the flow direction of the extruded material, while the diameter of the vibrating section remains constant. The diameter of the discharging section gradually decreases along the flow direction of the extruded material. The flow rate of the extruded material slows down in the feeding section, resulting in pressure reduction. The extruded material undergoes ultrasonic vibration treatment when passing through the vibrating section. The extruded material is pressurized when passing through the discharging section due to the reduced diameter.
4. The antibacterial spunbond nonwoven fabric production process according to claim 3, characterized in that: The length ratio of the feed section to the discharge section through which the extruded raw material flows in the extended die head is 1:0.3-0.5, and the length ratio of the vibration section to the discharge section is 1:4-6.
5. The antibacterial spunbond nonwoven fabric production process according to claim 4, characterized in that: The ultrasonic frequency of the ultrasonic processing device is set to 30-50kHz, and the ultrasonic power is set to 100-200W.
6. The antibacterial spunbond nonwoven fabric production process according to claim 5, characterized in that: The extended head is temperature controlled within a range of 220℃-225℃.
7. The antibacterial spunbond nonwoven fabric production process according to claim 5, characterized in that: The additives added in the S1 raw material preparation step include triphenyl phosphate, and the extended die head is temperature controlled within a range of 235℃-240℃.
8. The antibacterial spunbond nonwoven fabric production process according to any one of claims 1-7, characterized in that: The polyquaternary ammonium salt is a guanidine quaternary ammonium salt antibacterial polymer.
9. The antibacterial spunbond nonwoven fabric production process according to any one of claims 1-7, characterized in that: The polyquaternary ammonium salt is a hyperbranched polyquaternary ammonium salt.
10. An antibacterial spunbond nonwoven fabric, characterized in that: The antibacterial spunbond nonwoven fabric is produced according to the production process described in claims 1-9.
Citation Information
Patent Citations
Antibacterial spunbond non-woven fabric and preparation method thereof
CN116988226A
Guanidine quaternary ammonium salt antibacterial polymer as well as preparation method and application thereof
CN117624590A