A plane-wire heterostructure MXene / CNT coating fabric and a preparation method and application thereof
By alternating deposition of MXene and aminated CNTs on fabric using electrostatic layer-by-layer assembly technology, a surface-to-line heterostructure is constructed, which solves the problems of high density, poor flexibility and insufficient conductivity of existing electromagnetic shielding materials. This achieves high-efficiency electromagnetic shielding and good flexibility, and is suitable for wearable electronic devices, smart clothing, military stealth and aerospace electronic protection.
Patent Information
- Application Number
- CN202611581791.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-20
AI Technical Summary
Existing electromagnetic shielding materials suffer from problems such as high density, poor flexibility, and easy corrosion. Traditional conductive composite materials have insufficient conductivity and limited shielding effect. Pure MXene coatings are prone to reduced conductive pathways due to van der Waals forces, resulting in low mechanical strength. Traditional deposition methods lead to uneven distribution of conductive materials and poor adhesion.
Electrostatic layer-by-layer assembly technology was used to alternately deposit negatively charged MXene nanosheets and positively charged aminated CNTs on alkali-treated cotton knitted fabrics to construct a surface-to-line heterostructure, forming a highly interconnected three-dimensional conductive network, which enhances interfacial bonding and electromagnetic shielding effectiveness.
While maintaining the softness and breathability of the fabric, it significantly enhances the electromagnetic shielding effectiveness, improves the carrier migration capability and multiple reflection loss, thereby improving the electromagnetic shielding effectiveness, and at the same time improves the adhesion between the coating and the fiber matrix.
Smart Images

Figure CN123133162A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional textile technology, specifically relating to a surface-to-line heterostructure MXene / CNT coated fabric, its preparation method, and its application. Background Technology
[0002] With the increasing integration of electronic devices and the widespread adoption of 5G communication, electromagnetic radiation pollution poses a growing threat to the precise operation of electronic devices and human health. Traditional electromagnetic shielding materials mainly include metal-based materials (such as copper, aluminum, and silver) and ferrites. While they offer good shielding effectiveness, they generally suffer from high density, poor flexibility, and susceptibility to corrosion, making it difficult to meet the demands of modern electronic devices for lightweight and high performance. Conductive composite materials achieve a certain level of conductivity by incorporating carbon black or metal powder, but their conductivity is far inferior to that of metals, resulting in limited shielding effectiveness and insufficient flexibility. Textiles, being soft, lightweight, and breathable, offer the potential to achieve electromagnetic shielding while maintaining comfort by loading conductive functional materials onto their surface. In recent years, novel conductive fillers such as silver nanowires, graphene, carbon nanotubes (CNTs), and MXene have been successively used in fabric coatings.
[0003] MXene is a two-dimensional transition metal carbide / nitride, with Ti3C2T X Represented by MXene, it possesses a layered structure, high conductivity, and good solution processability. Its surface contains functional groups such as –OH, –F, and –O, making it both hydrophilic and prone to forming stable colloids. It disperses stably in water and can be deposited onto flexible fabrics through impregnation, spraying, vacuum filtration, or electrophoretic deposition to form conductive coatings. However, pure MXene coatings are prone to irreversible stacking due to van der Waals forces during film formation, leading to a reduction in effective conductive pathways and a decrease in specific shielding effectiveness. Simultaneously, its mechanical strength is low, making it prone to peeling under repeated bending or friction, limiting its long-term stability. CNTs, on the other hand, possess a one-dimensional hollow tubular structure, extremely high aspect ratio, and excellent mechanical properties, allowing for the formation of continuous conductive networks even with low addition amounts. Combining two-dimensional MXene sheets with one-dimensional CNTs creates a "surface-to-line" heterostructure, which improves carrier migration efficiency and overall conductivity while introducing heterojunctions and defect sites at the interface, enhancing dielectric loss, interfacial polarization, and multiple internal reflections, thereby significantly improving electromagnetic shielding effectiveness. However, traditional dip-coating or spray-coating methods often result in uneven distribution of conductive materials, poor adhesion, and easy detachment during use. Therefore, there is an urgent need to develop a surface-to-wire heterostructure MXene / CNT coated fabric and its controllable preparation method that combines efficient shielding, good conductivity, flexibility, and breathability. Summary of the Invention
[0004] In view of the shortcomings of the prior art, this invention provides a surface-to-linear heterostructure MXene / CNT coated fabric, its preparation method, and its application. This invention uses alkali-treated cotton knitted fabric as a flexible substrate and employs electrostatic layer-by-layer assembly technology to alternately deposit negatively charged MXene nanosheets and positively charged aminated CNTs on the fiber surface, constructing a surface-to-linear heterostructure. By adjusting the MXene concentration, CNT concentration, and number of impregnation cycles, coated fabrics with different structures are obtained, preserving the fabric's softness and breathability while ensuring efficient electromagnetic shielding.
[0005] The technical solution of the present invention is as follows:
[0006] A method for preparing a surface-to-line heterostructure MXene / CNT coated fabric includes the following steps:
[0007] S1. Alkali-treated cotton knitwear: Place the pure cotton knitwear in a NaOH solution and treat it at 100℃ for 2 hours to remove the surface wax, making it more hydrophilic and conducive to the adhesion of subsequent coatings; after alkali treatment, rinse the fabric with water and air dry.
[0008] S2. Preparation of MXene dispersion: Ti3C2T was prepared by wet etching technique. X MXene dispersion was prepared by ultrasonic dispersion treatment to obtain a few-layer MXene dispersion;
[0009] S3. Preparation of aminated CNT dispersion: Take an appropriate amount of aminated CNT powder and add it to deionized water for ultrasonic dispersion to prepare a CNT dispersion.
[0010] S4. Electrostatic Layer-by-Layer Assembly: Immerse the alkali-treated cotton knitted fabric in an MXene dispersion, leave it at room temperature for 10 minutes, then remove it and dry it in a 60°C oven. Next, immerse the fabric in an aminated CNT dispersion, leave it to stand for 10 minutes, then remove it and dry it in a 60°C oven, completing one MXene / CNT bilayer deposition cycle. Repeat the above operation to obtain a multilayer MXene / CNT coated fabric.
[0011] In some embodiments of the present invention, in step S2, the concentration of the MXene dispersion is 1~20 mg / mL.
[0012] In some embodiments of the present invention, in step S3, the concentration of the CNT dispersion is 0.1~0.5 mg / mL.
[0013] In some embodiments of the present invention, in step S4, the MXene / CNT bilayer deposition cycle is 1 to 20 times.
[0014] In a second aspect, the present invention provides a surface-to-line heterostructure MXene / CNT coated fabric prepared by the above-described preparation method.
[0015] A third aspect of the present invention provides an application of the above-described MXene / CNT coated fabric in the field of electromagnetic shielding.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0017] This invention employs electrostatic layer-by-layer assembly technology, utilizing the electrostatic attraction between the negative charge of MXene and the positive charge of aminated CNTs to achieve orderly and alternating deposition of nanomaterials on the fiber surface. This avoids the aggregation and shedding of conductive components and enhances the interfacial bonding between the coating and the fiber matrix. Two-dimensional sheet-like MXene and one-dimensional linear CNTs form a "surface-line" heterostructure, constructing a highly interconnected, multi-directionally extending three-dimensional conductive network at the microscale. This strengthens free electron migration and multiple reflection loss paths, achieving excellent electromagnetic shielding performance with a low filler loading. Simultaneously, the coated fabric prepared by this invention maintains good flexibility and breathability, making it suitable for wearable electronic devices, smart clothing, military stealth applications, medical monitoring, and aerospace electronic protection. Attached Figure Description
[0018] Figure 1 The images shown are SEM images of the MXene / CNT composite coated fabric prepared in Example 1; where (a) is magnified by 1000x and (b) is magnified by 10000x.
[0019] Figure 2 The figures show the surface resistance of the coated fabrics prepared in Examples 1-5 and Comparative Examples 1-2; wherein, (a) the figure shows the surface resistance of fabrics with different MXene concentrations; (b) the figure shows the surface resistance of fabrics with different CNT concentrations; and (c) the figure shows the surface resistance of pure MXene, pure CNT and MXene / CNT composite coated fabrics.
[0020] Figure 3 The figure shows the average SE in the X-band for the coated fabrics prepared in Examples 1-5 and Comparative Examples 1-2; wherein, (a) the figure shows the average SE in the X-band for fabrics with different MXene concentrations; (b) the figure shows the average SE in the X-band for fabrics with different CNT concentrations; and (c) the figure shows the average SE in the X-band for pure MXene, pure CNT and MXene / CNT composite coated fabrics. Detailed Implementation
[0021] The technical solution of the present invention will be further described in detail below through embodiments and in conjunction with the accompanying drawings. In this specification, the same or similar reference numerals indicate the same or similar components. The following description of the embodiments of the present invention with reference to the accompanying drawings is intended to explain the overall inventive concept of the present invention and should not be construed as a limitation thereof.
[0022] It should be noted that the terms used in this application are generally those commonly used by those skilled in the art. If there is any inconsistency with commonly used terms, the terms used in this application shall prevail.
[0023] An embodiment of the first aspect of the present invention provides a method for preparing an MXene / CNT composite coated fabric, comprising the following steps:
[0024] S1. Alkali-treated cotton knitwear: Place the pure cotton knitwear in a NaOH solution and treat it at 100℃ for 2 hours to remove the surface wax, making it more hydrophilic and conducive to the adhesion of subsequent coatings; after alkali treatment, rinse the fabric with water and air dry.
[0025] S2. Preparation of MXene dispersion: Ti3C2T was prepared by wet etching technique. X MXene dispersion was prepared by ultrasonic dispersion treatment to obtain a few-layer MXene dispersion;
[0026] S3. Preparation of aminated CNT dispersion: Take an appropriate amount of aminated CNT powder and add it to deionized water for ultrasonic dispersion to prepare a CNT dispersion.
[0027] S4. Electrostatic Layer-by-Layer Assembly: Immerse the alkali-treated cotton knitted fabric in an MXene dispersion, leave it at room temperature for 10 minutes, then remove it and dry it in a 60°C oven. Next, immerse the fabric in an aminated CNT dispersion, leave it to stand for 10 minutes, then remove it and dry it in a 60°C oven, completing one MXene / CNT bilayer deposition cycle. Repeat the above operation to obtain a multilayer MXene / CNT coated fabric.
[0028] In some embodiments of the present invention, in step S2, the concentration of the MXene dispersion is 1~20 mg / mL.
[0029] In some embodiments of the present invention, in step S3, the concentration of the CNT dispersion is 0.1~0.5 mg / mL.
[0030] In some embodiments of the present invention, in step S4, the MXene / CNT bilayer deposition cycle is 1 to 20 times.
[0031] In a second aspect, the present invention provides a surface-to-line heterostructure MXene / CNT coated fabric prepared by the above-described preparation method.
[0032] A third aspect of the present invention provides an application of the above-described MXene / CNT coated fabric in the field of electromagnetic shielding.
[0033] Example 1
[0034] (1) Alkali treatment of cotton knitted fabrics: Put pure cotton knitted fabrics into NaOH solution and treat them at 100°C for 2 hours to remove surface wax and enhance hydrophilicity. Then rinse them with water and dry them.
[0035] (2) Preparation of MXene dispersion: Mix 10 mL of water and 30 mL of concentrated hydrochloric acid in a polytetrafluoroethylene bottle, add 2 g of LiF, stir in a water bath for 30 min; add 2 g of Ti3AlC2 MAX phase powder, react at 35 °C for 48 h; centrifuge and wash until the pH of the supernatant is close to neutral; redisperse the precipitate in deionized water, sonicate in an ice-water bath at 300 W for 1 h; dilute to 15 mg / mL.
[0036] (3) Preparation of aminated CNT dispersion: Weigh the aminated CNT powder and add it to deionized water to make the CNT concentration 0.1 mg / mL; stir at room temperature for 30 min, and sonicate at 200 W for 30 min to obtain a uniform black dispersion.
[0037] (4) Electrostatic layer-by-layer assembly: The alkali-treated cotton knitted fabric was immersed in MXene dispersion, dried at room temperature for 10 min, and then dried at 60℃; then immersed in aminated CNT dispersion, dried at room temperature for 10 min, and dried at 60℃; one double-layer cycle was completed. This was repeated 4 times. The resulting coated fabric has the following microstructure: Figure 1 As shown in (ab), after alternating impregnation with MXene and CNT, the fiber retains its original ribbon shape, and the fiber surface is completely covered by the coating; CNTs are interspersed between the MXene sheets in the coating, forming a three-dimensional network of "surface-line" interweaving.
[0038] Example 2
[0039] Steps (1), (3), and (4) are the same as in Example 1, except that the concentration of the MXene dispersion prepared in step (2) is 5 mg / mL.
[0040] Example 3
[0041] Steps (1), (3), and (4) are the same as in Example 1, except that the concentration of the MXene dispersion prepared in step (2) is 10 mg / mL.
[0042] Example 4
[0043] Steps (1), (2), and (4) are the same as in Example 1, except that the concentration of the CNT dispersion in step (3) is 0.3 mg / mL.
[0044] Example 5
[0045] Steps (1), (2), and (4) are the same as in Example 1, except that the concentration of the CNT dispersion in step (3) is 0.5 mg / mL.
[0046] Comparative Example 1
[0047] Steps (1) and (2) are the same as in Example 1;
[0048] The difference is that in step (3): the alkali-treated cotton knitted fabric is immersed in MXene dispersion, kept at room temperature for 10 min, and dried at 60°C. The immersion and drying operation is repeated 4 times.
[0049] Comparative Example 2
[0050] Step (1) is the same as in Example 1;
[0051] The difference is that in step (2): weigh the aminated CNT powder and add it to deionized water to make the CNT concentration 0.1 mg / mL; stir at room temperature for 30 min, and sonicate at 200 W for 30 min to obtain a uniform black dispersion.
[0052] Step (3): Immerse the alkali-treated cotton knitted fabric in the aminated CNT dispersion, at room temperature for 10 min, and dry at 60°C. Repeat the immersion and drying process 4 times.
[0053] Figure 2 The surface resistivity of seven coated fabrics. From Figure 2 (a) shows that when the CNT concentration is maintained at 0.1 mg / mL, the surface resistivity of the fabric decreases with increasing MXene concentration; simultaneously, with increasing impregnation cycles, the surface resistivity of coated fabrics with different MXene concentrations all decreases. Figure 2 (b) shows that when the MXene concentration is maintained at 15 mg / mL, the fabric surface resistivity is lowest at a CNT concentration of 0.5 mg / mL during the first impregnation. However, as the number of impregnations increases, the fabric surface resistivity is lowest at a CNT concentration of 0.1 mg / mL. After four impregnations, the surface resistivity of the fabric is 3 Ω / sq. From... Figure 2 (c) It can be seen that the surface resistance of the MXene / CNT composite coated fabric is lower than that of the pure MXene and pure CNT coated fabrics.
[0054] Test Example 1
[0055] The scattering parameters (SL) of macroporous GNP / PLA composite materials prepared by the methods shown in all examples and comparative examples in the X-band (8.2–12.4 GHz) were analyzed using a vector network analyzer (P5004A, Agilent). 11 S 22 S 12 S 21 The test is conducted. The total electromagnetic shielding efficiency (SE) can be calculated using the following formula:
[0056] Through testing and calculation, the average SE of fabrics coated with different MXene concentrations in the X-ray band was obtained when the CNT concentration was 0.1 mg / mL. Figure 3 As shown in (a), with an MXene concentration of 15 mg / mL, the average SE of coated fabrics with different CNT concentrations in the X-band is as follows: Figure 3 As shown in (b), the average SE in the X-band for pure MXene-coated fabric, pure CNT-coated fabric, and MXene / CNT-coated fabric is as follows: Figure 3 As shown in (c), the SE value of the composite coating showed a gradual upward trend as the concentration of MXene dispersion gradually increased from 5 mg / mL to 15 mg / mL. Specifically, the fabric with 5 mg / mL MXene had an average SE of 11.8 dB after four impregnations, while the fabric with 15 mg / mL MXene had an average SE of 34.7 dB after four impregnations, showing an increase of 22.9 dB. Figure 3 (a)); and for composite coated fabrics with different CNT concentrations, the SE value reached its highest (34.7 dB) at a CNT concentration of 0.1 mg / mL. Figure 3 (b)); from Figure 3 As can be seen in (c), the SE value of the MXene / CNT composite coated fabric is higher than that of the pure MXene coated fabric and the CNT coated fabric under the same concentration and number of impregnations.
[0057] Table 1 shows the air permeability (100 Pa pressure difference) and flexural stiffness of the coated samples after four immersions. As can be seen from the table, although there are some differences in air permeability and flexural stiffness among the different coated samples, they all maintain high air permeability and good flexural stiffness, indicating that the coated fabric obtained by this method can retain the softness and air permeability of the fabric while ensuring efficient electromagnetic shielding.
[0058] While some embodiments of the present general inventive concept have been shown and described, those skilled in the art will understand that changes may be made to these embodiments without departing from the principles and spirit of the present general inventive concept, the scope of which is defined by the claims and their equivalents.
Claims
1. A method for preparing a surface-to-linear heterostructure MXene / CNT coated fabric, comprising the following steps: S1. Alkali-treated cotton knitwear: Pure cotton knitwear is pretreated in NaOH solution to remove surface wax, making it more hydrophilic and facilitating the adhesion of subsequent coatings; the alkali-treated fabric is then rinsed with water and dried. S2. Preparation of MXene dispersion: Ti3C2T was prepared by wet etching technique. X MXene dispersion was prepared by ultrasonic dispersion treatment to obtain a few-layer MXene dispersion; S3. Preparation of aminated CNT dispersion: Take an appropriate amount of aminated CNT powder, add it to deionized water, and ultrasonically disperse it to prepare a CNT dispersion; S4. Electrostatic layer-by-layer assembly: After immersing the alkali-treated cotton knitted fabric in MXene dispersion for a period of time; The fabric is then immersed in an aminated CNT dispersion to complete one MXene / CNT bilayer deposition cycle; the above operation is repeated to obtain a multilayer MXene / CNT coated fabric.
2. The preparation method according to claim 1, characterized in that, In step S1, the pretreatment conditions for pure cotton knitted fabric in NaOH solution are: treatment at 100℃ for 2 hours.
3. The preparation method according to claim 1, characterized in that, In step S2, the concentration of the MXene dispersion is 1~20 mg / mL.
4. The preparation method according to claim 1, characterized in that, In step S3, the concentration of the CNT dispersion is 0.1~0.5 mg / mL.
5. The preparation method according to claim 1, characterized in that, In step S4, the MXene / CNT bilayer deposition cycle is 1 to 20 times.
6. The preparation method according to claim 1, characterized in that, In step S4, the treatment conditions for immersing cotton knitted fabric in MXene dispersion are: after being placed at room temperature for 10 minutes, it is taken out and dried in an oven at 60°C; the treatment conditions for immersing fabric in aminated CNT dispersion are: after being left to stand for 10 minutes, it is taken out and dried in an oven at 60°C.
7. A surface-to-line heterostructure MXene / CNT coated fabric prepared by the preparation method according to any one of claims 1-6.
8. The application of the MXene / CNT coated fabric as described in claim 7 in the field of electromagnetic shielding.