PI@zif-8 composite fiber membrane with directional ion transmission channel and application in lithium battery
By employing self-assembly interface modification and low-temperature chemical imidization in lithium-ion batteries, PI@ZIF-8 composite fiber membranes with directional ion transport channels were prepared, solving the problems of ZIF-8 particle agglomeration and weak interfacial bonding, and achieving high efficiency in ion conduction and electrochemical stability.
Patent Information
- Application Number
- CN202611658013.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-20
AI Technical Summary
Existing PI@ZIF-8 composite fiber membranes suffer from problems such as ZIF-8 particle agglomeration, weak interfacial bonding, incompatible process temperatures, and disordered ion transport, making it difficult to simultaneously achieve high safety, high ion conduction efficiency, and long cycle life.
Using polyamic acid (PAA) nanofiber membranes as a substrate, a PI@ZIF-8 composite fiber membrane with directional ion transport channels was formed by self-assembly interfacial modification and induction of ZIF-8 crystal directional growth, combined with low-temperature chemical imidization.
Chemical bonding between ZIF-8 and the PAA matrix was achieved, constructing a continuous directional ion transport channel, which significantly improved the ion conduction performance and electrochemical stability of lithium-ion batteries. The ion conductivity reached 1.84×10⁻⁴-2.01×10⁻⁴ S/cm, the lithium-ion transference number reached 0.75-0.79, and the cycle stability was excellent.
Smart Images

Figure CN123133166A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a PI@ZIF-8 composite fiber membrane with directional ion transport channels and its application in lithium batteries, belonging to the field of lithium-ion battery material technology. Background Technology
[0002] Lithium-ion batteries are widely used in portable electronic devices, new energy vehicles, and energy storage power stations. Commercial systems mostly use organic liquid electrolytes, which pose safety hazards such as leakage, flammability, and explosion, hindering the development of high-energy-density lithium metal batteries. Quasi-solid-state electrolytes combine the high ionic conductivity of liquid electrolytes with the high safety of solid electrolytes, representing the core development direction for next-generation high-safety lithium batteries. The separator, as a key battery material, plays a crucial role in isolating the positive and negative electrodes, supporting the electrolyte, and regulating lithium-ion transport; its structural performance directly determines the battery's safety and electrochemical performance.
[0003] Polyimide (PI) possesses ultra-high thermal stability (thermal decomposition temperature > 400℃), excellent mechanical strength, and electrochemical inertness. Compared to traditional polyolefin separators, it exhibits stronger resistance to thermal shrinkage and mechanical shock, making it an ideal substrate for fabricating high-performance battery separators. ZIF-8, as a typical metal-organic framework (MOF) material, possesses a regular porous structure and Lewis acid active sites, enabling it to both construct lithium-ion transport channels and anchor TFSI in the electrolyte. - Anions increase the lithium-ion transference number and are therefore often used to modify PI membranes to prepare high-performance PI@ZIF-8 composite fiber membranes.
[0004] Currently, PI@ZIF-8 composite fiber membranes are mainly prepared through physical blending, electrospinning doping, and surface coating, but these processes have many inherent drawbacks: (1) Powdered ZIF-8 is very easy to agglomerate in the PI matrix and cannot form a continuous ion transport channel. Lithium ions are transported in a hopping manner, and the interfacial impedance is significantly increased.
[0005] (2) Physical blending only achieves the bonding of the two-phase interface without chemical bonding. During long-term battery cycling, ZIF-8 is easy to fall off from the PI fiber surface, resulting in membrane structure failure and battery capacity decay.
[0006] (3) PI preparation requires high-temperature thermal imidization treatment above 300℃, while the thermal stability limit of ZIF-8 is only 200℃. Under high-temperature conditions, its crystal skeleton will collapse and fail, forming a bottleneck in process adaptability.
[0007] (4) In conventional preparation methods, ZIF-8 grows randomly on the PI surface, resulting in disordered pore orientation, tortuous lithium-ion transport paths, and high resistance, which makes it impossible to achieve directional and efficient conduction and limits the improvement of battery rate performance.
[0008] In summary, existing PI@ZIF-8 composite fiber membranes suffer from technical challenges such as particle agglomeration, weak interfacial bonding, incompatible process temperatures, and disordered ion transport, making it difficult to simultaneously achieve high safety, high ion conduction efficiency, and long cycle life. Summary of the Invention
[0009] To address the aforementioned problems, this invention provides a PI@ZIF-8 composite fiber membrane with directional ion transport channels and its application in lithium-ion batteries. Specifically, this invention first uses a polyamic acid (PAA) nanofiber membrane as a substrate, and then modifies the PAA nanofiber membrane through self-assembly and interfacial modification; subsequently, it induces ZIF-8 crystals to grow directionally along the PAA fiber surface, and finally converts PAA to PI through low-temperature chemical imidization, obtaining a PI@ZIF-8 composite fiber membrane with directional ion transport channels. Using the prepared PI@ZIF-8 composite fiber membrane as a separator in lithium-ion batteries significantly improves the ion conduction performance and electrochemical stability of the lithium-ion batteries.
[0010] The first objective of this invention is to provide a method for preparing a PI@ZIF-8 composite fiber membrane with directional ion transport channels, comprising the following steps: (1) The polyamic acid (PAA) nanofiber membrane was immersed in a solution containing self-assembled monolayer (SAMs) precursors at pH 4.0-5.5 and reacted at 15-35℃ (room temperature) for 6-48 h. After the reaction was completed, the membrane was washed and dried to obtain the polyamic acid (PAA) nanofiber membrane modified with aminopropyl functionalized self-assembled monolayer (SAMs). The solution containing the self-assembled monolayer (SAMs) precursor is either a 3-aminopropyltriethoxysilane (APTES) solution or a 3-mercaptopropyltrimethoxysilane (MPTMS) solution. (2) The polyamic acid (PAA) nanofiber membrane modified with SAMs was immersed in the ZIF-8 precursor growth solution and grown in situ at 15-50℃ for 2-48 h. After washing and drying, the PAA@ZIF-8 composite fiber membrane was obtained. (3) The PAA@ZIF-8 composite fiber membrane was immersed in a mixed solution of acetic anhydride / pyridine / N,N-dimethylacetamide (DMAc) and chemically imidized at 60-120℃ for 2-12 h. After the reaction was completed, the membrane was washed and dried to obtain the PI@ZIF-8 composite fiber membrane with directional ion transport channels.
[0011] In one embodiment of the present invention, the polyamic acid (PAA) nanofiber membrane in step (1) is prepared by electrospinning, with a fiber diameter of 200-500 nm and a membrane thickness of 10-60 μm; The specific preparation method is as follows: Polyamic acid (PAA) is dissolved in N,N-dimethylacetamide (DMAc) to obtain a spinning solution with a mass fraction of 8%-12%. The spinning solution was electrospun to obtain a polyamic acid (PAA) nanofiber membrane; Among them, the number-average molecular weight of polyamic acid (PAA) is approximately 80,000-120,000; Dissolution is carried out by stirring at 15-35 ℃ and 500-1000 rpm for 3-10 hours; The parameters for electrospinning include: voltage 15-25 kV, receiving distance 15-20 cm, feed speed 0.5-1.5 mL / h; roller speed 100-200 r / min, spinneret lateral oscillation amplitude 20-40 cm, oscillation speed 0.4-0.6 cm / min; and spinning time 3-5 h.
[0012] In one embodiment of the present invention, after the polyamic acid (PAA) nanofiber membrane is prepared in step (1), it can be ultrasonically cleaned with anhydrous ethanol and water for 10-20 min each, and then dried to remove some impurities on the surface.
[0013] In one embodiment of the present invention, the impregnation in step (1) is to completely immerse the polyamic acid (PAA) nanofiber membrane in a solution containing a self-assembled monolayer (SAMs) precursor.
[0014] In one embodiment of the present invention, the solvent of the solution containing the self-assembled monolayer (SAMs) precursor in step (1) is anhydrous ethanol with a concentration of 5-20 mM.
[0015] In one embodiment of the present invention, the pH of the solution containing the self-assembled monolayer (SAMs) precursor in step (1) is adjusted using acetic acid.
[0016] In one embodiment of the present invention, the reaction in step (1) is a static reaction.
[0017] In one embodiment of the present invention, the washing in step (1) is repeated rinsing with anhydrous ethanol, and the drying is drying at 50-70 ℃ for 4-10 hours.
[0018] In one embodiment of the present invention, the preparation method of the ZIF-8 precursor growth solution in step (2) is as follows: Zinc nitrate hexahydrate is dissolved in methanol to obtain a zinc nitrate hexahydrate solution; 2-Methylimidazole was dissolved in methanol to obtain a 2-methylimidazole solution; The ZIF-8 precursor growth solution was obtained by mixing zinc nitrate hexahydrate solution and 2-methylimidazole solution and stirring until homogeneous. In the zinc nitrate hexahydrate solution, the ratio of zinc nitrate hexahydrate to methanol is 1-3 g: 40 mL; The ratio of 2-methylimidazole to methanol in the 2-methylimidazole solution is 2-8 g: 40 mL; The molar ratio of zinc nitrate hexahydrate to 2-methylimidazole is 1:8-9; Stirring is performed at room temperature and 500-1000 rpm for 0.5-1 h.
[0019] In one embodiment of the present invention, the impregnation in step (2) is to completely immerse the modified polyamic acid (PAA) nanofiber membrane in the ZIF-8 precursor growth solution.
[0020] In one embodiment of the present invention, the reaction in step (2) is a static reaction.
[0021] In one embodiment of the present invention, the washing in step (2) is repeated rinsing with methanol, and the drying is drying at 50-70 ℃ for 10-20 h.
[0022] In one embodiment of the present invention, the volume ratio of acetic anhydride, pyridine, and N,N-dimethylacetamide (DMAc) in the acetic anhydride / pyridine / N,N-dimethylacetamide (DMAc) mixed solution in step (3) is 0.5-2:0.5-2:5-10.
[0023] In one embodiment of the present invention, the impregnation in step (3) is to completely immerse the PAA@ZIF-8 composite fiber membrane in a mixed solution of acetic anhydride / pyridine / N,N-dimethylacetamide (DMAc).
[0024] In one embodiment of the present invention, the washing in step (3) is repeated rinsing with DMAc and anhydrous ethanol, and the drying is drying at 50-70 °C for 10-20 h.
[0025] The second objective of this invention is to prepare a PI@ZIF-8 composite fiber membrane with directional ion transport channels using the method described herein.
[0026] The third objective of this invention is to provide a quasi-solid-state electrolyte membrane, wherein the PI@ZIF-8 composite fiber membrane with directional ion transport channels described in this invention is employed.
[0027] In one embodiment of the present invention, the quasi-solid-state electrolyte membrane is prepared as follows: Lithium bis(trifluoromethanesulfonate)imide (LiTFSI) was dissolved in a mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME), and LiPF6 was added as an initiator. The mixture was stirred until homogeneous to obtain a quasi-solid-state electrolyte precursor solution. The PI@ZIF-8 composite fiber membrane with directional ion transport channels was immersed in a quasi-solid electrolyte precursor solution and adsorbed at 15-35 °C for 10-20 h. After removal, excess quasi-solid electrolyte precursor solution was removed to obtain the quasi-solid electrolyte membrane. The volume ratio of the mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME) is 1:1. The concentration of lithium bis(trifluoromethanesulfonate)imide (LiTFSI) in the quasi-solid electrolyte precursor solution was 0.5-1.5 M; the mass concentration of LiPF6 was 1%-3%.
[0028] The fourth objective of this invention is to provide a lithium-ion symmetric battery, wherein the PI@ZIF-8 composite fiber membrane or quasi-solid electrolyte membrane with directional ion transport channels described in this invention is employed.
[0029] In one embodiment of the present invention, the lithium-ion symmetric battery includes a Li electrode, a quasi-solid-state electrolyte membrane, and a Li symmetric electrode.
[0030] The sixth objective of this invention is to provide a lithium-ion full battery in which a PI@ZIF-8 composite fiber membrane or a quasi-solid electrolyte membrane with directional ion transport channels as described in this invention is employed.
[0031] In one embodiment of the present invention, the lithium-ion full battery is a coin cell assembled with LiFePO4 as the positive electrode and lithium metal as the negative electrode.
[0032] The seventh objective of this invention is to provide a method for improving the ion conduction performance and electrochemical stability of lithium-ion batteries, wherein the PI@ZIF-8 composite fiber membrane with directional ion transport channels described in this invention is used.
[0033] The eighth object of the present invention is to provide a battery for forklifts, wherein the PI@ZIF-8 composite fiber membrane or quasi-solid electrolyte membrane with directional ion transport channels described in the present invention is used.
[0034] [Beneficial Effects] (1) This invention constructs a continuous directional ion transport channel. By inducing ZIF-8 crystals to align axially along PAA fibers using SAMs interfacial chemistry, the pore direction of ZIF-8 is aligned with the fiber axis, forming a one-dimensional ion "highway" that connects end to end, significantly reducing the tortuosity of ion transport.
[0035] (2) This invention achieves chemical bonding anchoring between ZIF-8 and the PAA matrix. The carboxyl groups (-COOH) on the surface of PAA fibers form coordination bonds with ZIF-8. Combined with the bridging effect of SAMs, chemical bonding between ZIF-8 and the PAA matrix is achieved, effectively solving the problem of ZIF-8 shedding.
[0036] (3) The present invention uses low-temperature chemical imidization to completely preserve the structure of ZIF-8. Chemical imidization at 80-120℃ achieves PAA→PI conversion, avoiding the damage to the ZIF-8 pore structure caused by traditional 300℃ thermal imidization.
[0037] (4) The ion conduction performance of the PI@ZIF-8 composite fiber membrane with directional ion transport channels of the present invention is significantly improved. This invention utilizes oriented ZIF-8 channels combined with ZIF-8 Lewis acid sites to anchor anions, achieving an ionic conductivity of up to 1.84 × 10⁻⁶. -4 -2.01×10 -4 The S / cm ratio and lithium-ion transference number can reach 0.75-0.79.
[0038] (5) The PI@ZIF-8 composite fiber membrane with directional ion transport channels of the present invention has excellent electrochemical stability. The PI fiber framework endows the composite fiber membrane with excellent electrochemical performance and thermal stability, achieving a lithium-ion symmetric battery cycle stability of >1500 h (0.2 mA / cm²). 2 Critical current density > 2.0 mA / cm² 2 The capacity retention rate of the LiFePO4 / Li full cell is >83% after 400 cycles at 0.5C. Attached Figure Description
[0039] Figure 1 This is a flowchart illustrating the preparation process of PI@ZIF-8 composite fiber membranes with directional ion transport channels.
[0040] Figure 2 The images are scanning electron microscope (SEM) images of the polyamic acid (PAA) nanofiber membrane, the PAA@ZIF-8 composite fiber membrane, and the PI@ZIF-8 composite fiber membrane with directional ion transport channels in Example 1.
[0041] Figure 3 The image shows the XRD pattern of the PI@ZIF-8 composite fiber membrane with directional ion transport channels prepared in Example 1.
[0042] Figure 4The graph shows a comparison of ionic conductivity and lithium-ion transference number for Examples 1-3 and Comparative Examples 1-4.
[0043] Figure 5 For Li / QSE-1 / Li symmetric cells at 0.2 mA / cm 2 The cyclic stability curve is shown below.
[0044] Figure 6 The cycling performance curves of the LiFePO4 / QSE-1 / Li full cell at 0.5C rate are shown. Detailed Implementation
[0045] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explanation of the present invention and are not intended to limit the present invention.
[0046] Test method: 1. XRD orientation characterization: The composite fiber membrane was characterized by X-ray diffraction. The orientation degree of the ZIF-8 crystal was characterized by calculating the intensity ratio I(110) / I(002) of the diffraction peak of the (110) crystal plane and the diffraction peak of the (002) crystal plane.
[0047] 2. Ionic conductivity test: The measurements were performed using electrochemical impedance spectroscopy (EIS) at 30°C, with a frequency range of 1 Hz to 1 MHz and an amplitude of 10 mV.
[0048] A quasi-solid-state electrolyte membrane is sandwiched between two stainless steel blocking electrodes to assemble a coin cell. The ionic conductivity is calculated using the following formula: σ=L / (R b ×S); Where σ: ionic conductivity, S / cm; L: electrolyte membrane thickness, cm; R b Electrolyte bulk impedance (volume resistance), ohms; S: Effective contact area, cm² 2 .
[0049] 3. Lithium-ion transference number test: The method was determined by a combination of potentiostatic polarization and AC impedance spectroscopy.
[0050] Assemble a symmetric cell with a Li electrode, a quasi-solid electrolyte membrane, and a Li symmetric electrode, apply a constant potential polarization of 10 mV, and calculate the lithium-ion transference number according to the Bruce-Vincent formula.
[0051] 4. Cycle stability test of lithium symmetric battery: At 0.2 mA / cm 2 Constant current charge-discharge cycles were performed at the current density, and the cycle time before a short circuit occurred was recorded.
[0052] 5. Critical current density test: At 0.1 mA / cm 2 The initial current density is increased by 0.1 mA / cm² every 30 minutes. 2 Until a short circuit occurs, record the maximum current density before the short circuit.
[0053] 6. Full battery cycle performance test: A CR2032 coin cell was assembled using LiFePO4 as the positive electrode, lithium metal as the negative electrode, and a quasi-solid-state electrolyte membrane as the electrolyte. Constant current charge-discharge was performed at 0.5C, with a voltage window of 2.5-4.2 V, and the capacity retention was recorded after 400 cycles.
[0054] Raw materials used in the examples: Polyamic acid (PAA) powder, number average molecular weight Mn≈80000-120000; N,N-Dimethylacetamide (DMAc), anhydrous ethanol, 3-aminopropyltriethoxysilane (APTES), zinc nitrate hexahydrate, 2-methylimidazole, acetic anhydride, pyridine, etc. are commonly used experimental raw materials, all of which are from Sinopharm Chemical Reagent Co., Ltd.
[0055] The preparation method of ZIF-8 powder is as follows: Zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 1.19 g, 4.0 mmol) was dissolved in 40 mL of methanol to obtain a zinc nitrate hexahydrate solution; 2-methylimidazole (HmIm, 2.63 g, 32.0 mmol) was dissolved in 40 mL of methanol to obtain a 2-methylimidazole solution; the zinc nitrate hexahydrate solution and the 2-methylimidazole solution were mixed and stirred at 500 rpm for 0.5 h to obtain a homogeneous ZIF-8 precursor growth solution; the ZIF-8 precursor growth solution was stirred at 600 rpm for 6 h at room temperature, the white precipitate was collected by centrifugation, washed three times with methanol, and dried under vacuum at 60 °C for 12 h to obtain ZIF-8 powder (particle size 50-150 nm).
[0056] The preparation method of PI film is as follows: Weigh 10.0 g of polyamic acid (PAA) powder and dissolve it in 90 g of N,N-dimethylacetamide (DMAc). Stir mechanically at 35°C and 500 rpm for 10 h until completely dissolved to obtain a spinning solution with a mass fraction of 10%. The spinning solution was injected into a syringe with a stainless steel spinneret (0.8 mm inner diameter); the receiving device was a cylindrical roller wrapped with aluminum foil (12 cm diameter, 30 cm length), the receiving distance was 18 cm, the applied voltage was 20 kV, the feed speed was 0.5 ml / h, the roller speed was 150 r / min, the spinneret lateral oscillation amplitude was 30 cm, and the oscillation speed was 0.5 cm / min; the ambient temperature was controlled at 25 ± 2℃, and the relative humidity was 30%; electrospinning was carried out for 5 h. After spinning, the fiber membrane was peeled off the aluminum foil and dried in a vacuum drying oven at 60°C for 12 h to obtain a polyamic acid (PAA) nanofiber membrane with a fiber diameter of 200-500 nm and a thickness of 30 μm. Acetic anhydride, pyridine, and N,N-dimethylacetamide (DMAc) were mixed in a volume ratio of 1:1:8. PAA nanofiber membranes were immersed in the above mixed solution and chemically imidized at 80°C for 6 h. After the reaction, the membranes were washed three times with DMAc and anhydrous ethanol, and then vacuum dried at 60°C for 12 h to obtain PI nanofiber membranes.
[0057] Room temperature refers to 15-35℃.
[0058] Immersion means complete immersion.
[0059] Example 1 A method for preparing a PI@ZIF-8 composite fiber membrane with directional ion transport channels includes the following steps: (1) Weigh 10 g of polyamic acid (PAA) powder and dissolve it in 90 g of N,N-dimethylacetamide (DMAc). Stir mechanically at 35°C and 500 rpm for 10 h until completely dissolved to obtain a spinning solution with a mass fraction of 10%. The spinning solution was injected into a syringe with a stainless steel spinneret with an inner diameter of 0.8 mm. The receiving device was a cylindrical roller wrapped with aluminum foil (12 cm in diameter and 30 cm in length), with a receiving distance of 18 cm. The applied voltage was 18 kV, the feed rate was 1.0 mL / h, the roller speed was 200 r / min, the spinneret lateral oscillation amplitude was 40 cm, and the oscillation speed was 0.6 cm / min. The ambient temperature was controlled at 25 ± 2℃ and the relative humidity was 30%. Electrospinning was carried out for 4.0 h. After spinning, the fiber membrane was peeled off the aluminum foil and dried in a vacuum drying oven at 60°C for 12 h to obtain a polyamic acid (PAA) nanofiber membrane with a fiber diameter of 200-500 nm and a thickness of 40 μm. Before use, polyamic acid (PAA) nanofiber membranes need to be cleaned by ultrasonic cleaning with anhydrous ethanol and water for 15 minutes each, then dried with nitrogen, and then cut into 5 cm × 5 cm square pieces. (2) Dissolve 3-aminopropyltriethoxysilane (APTES) in anhydrous ethanol and adjust the pH to 4.5 with acetic acid to obtain a 5 mM 3-aminopropyltriethoxysilane (APTES) solution. Polyamic acid (PAA) nanofiber membranes were immersed in a solution of 3-aminopropyltriethoxysilane (APTES) and allowed to stand at 25°C for 24 h to allow APTES molecules to self-assemble on the surface of PAA fibers to form aminopropyl-functionalized self-assembled monolayers (SAMs). After removal, the membranes were rinsed three times with anhydrous ethanol and dried under vacuum at 60°C for 6 h to obtain SAMs-modified PAA fiber membranes. (3) Zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 1.00 g, 3.36 mmol) was dissolved in 40 mL of methanol to obtain a zinc nitrate hexahydrate solution; 2-methylimidazole (HmIm, 2.21 g, 26.92 mmol) was dissolved in 40 mL of methanol to obtain a 2-methylimidazole solution; the zinc nitrate hexahydrate solution and the 2-methylimidazole solution were mixed and stirred at 600 rpm for 0.5 h to obtain a ZIF-8 precursor growth solution; The SAMs-modified PAA fiber membrane was immersed in ZIF-8 precursor growth solution, and then grown in situ at 30°C for 12 h. After being repeatedly washed with methanol three times, it was vacuum dried at 60°C for 12 h to obtain PAA@ZIF-8 composite fiber membrane. (4) Acetic anhydride, pyridine, and N,N-dimethylacetamide (DMAc) are mixed evenly in a volume ratio of 0.5:0.5:10 to obtain an acetic anhydride / pyridine / DMAc mixed solution; The PAA@ZIF-8 composite fiber membrane was immersed in a mixed solution of acetic anhydride / pyridine / N,N-dimethylacetamide (DMAc) and chemically imidized at 30 °C for 6 h. After the reaction, it was repeatedly washed three times with DMAc and anhydrous ethanol, and then vacuum dried at 60 °C for 12 h to obtain a PI@ZIF-8 composite fiber membrane with directional ion transport channels (thickness of 40 μm).
[0060] Example 2 A method for preparing a PI@ZIF-8 composite fiber membrane with directional ion transport channels includes the following steps: (1) Weigh 12 g of polyamic acid (PAA) powder and dissolve it in 88 g of N,N-dimethylacetamide (DMAc). Stir mechanically at 35°C and 800 rpm for 6 h until completely dissolved to obtain a spinning solution with a mass fraction of 12%. The spinning solution was injected into a syringe with a stainless steel spinneret (0.8 mm inner diameter); the receiving device was a cylindrical roller wrapped with aluminum foil (12 cm diameter, 30 cm length), the receiving distance was 15 cm, the applied voltage was 20 kV, the feed rate was 1.50 mL / h, the roller speed was 150 r / min, the spinneret lateral oscillation amplitude was 30 cm, and the oscillation speed was 0.5 cm / min; the ambient temperature was controlled at 25 ± 2℃, and the relative humidity was 30%; electrospinning was carried out for 3 h. After spinning, the fiber membrane was peeled off the aluminum foil and dried in a vacuum drying oven at 60°C for 12 h to obtain a polyamic acid (PAA) nanofiber membrane with a fiber diameter of 200-500 nm and a thickness of 50 μm. Before use, polyamic acid (PAA) nanofiber membranes need to be cleaned by ultrasonic cleaning with anhydrous ethanol and water for 15 minutes each, then dried with nitrogen, and then cut into 5 cm × 5 cm square pieces. (2) Dissolve 3-aminopropyltriethoxysilane (APTES) in anhydrous ethanol and adjust the pH to 4.0 with acetic acid to obtain a 10 mM solution of 3-aminopropyltriethoxysilane (APTES). Polyamic acid (PAA) nanofiber membranes were immersed in a solution of 3-aminopropyltriethoxysilane (APTES) and allowed to stand at 25°C for 48 h to allow APTES molecules to self-assemble on the surface of PAA fibers to form aminopropyl-functionalized self-assembled monolayers (SAMs). After removal, the membranes were rinsed three times with anhydrous ethanol and dried under vacuum at 60°C for 6 h to obtain SAMs-modified PAA fiber membranes. (3) Zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 2.00 g, 6.72 mmol) was dissolved in 40 mL of methanol to obtain a zinc nitrate hexahydrate solution; 2-methylimidazole (HmIm, 4.42 g, 53.84 mmol) was dissolved in 40 mL of methanol to obtain a 2-methylimidazole solution; the zinc nitrate hexahydrate solution and the 2-methylimidazole solution were mixed and stirred at 600 rpm for 0.5 h to obtain a ZIF-8 precursor growth solution; The SAMs-modified PAA fiber membrane was immersed in ZIF-8 precursor growth solution, and then grown in situ at 40°C for 2 hours. After being repeatedly washed with methanol 3 times, it was vacuum dried at 60°C for 12 hours to obtain PAA@ZIF-8 composite fiber membrane. (4) Mix acetic anhydride, pyridine, and N,N-dimethylacetamide (DMAc) in a volume ratio of 1:1:8 to obtain a mixed solution of acetic anhydride / pyridine / DMAc; The PAA@ZIF-8 composite fiber membrane was immersed in a mixed solution of acetic anhydride / pyridine / N,N-dimethylacetamide (DMAc) and chemically imidized at 90℃ for 6 h. After the reaction, it was repeatedly washed three times with DMAc and anhydrous ethanol, and then vacuum dried at 60℃ for 12 h to obtain a PI@ZIF-8 composite fiber membrane with directional ion transport channels (thickness of 50 μm).
[0061] Example 3 A method for preparing a PI@ZIF-8 composite fiber membrane with directional ion transport channels includes the following steps: (1) Weigh 10 g of polyamic acid (PAA) powder and dissolve it in 90 g of N,N-dimethylacetamide (DMAc). Stir mechanically at 25°C and 1000 rpm for 3 h until completely dissolved to obtain a spinning solution with a mass fraction of 10%. The spinning solution was injected into a syringe with a stainless steel spinneret with an inner diameter of 0.8 mm. The receiving device was a cylindrical roller wrapped with aluminum foil (12 cm in diameter and 30 cm in length), with a receiving distance of 18 cm. The applied voltage was 15 kV, the feed rate was 0.5 mL / h, the roller speed was 100 r / min, the spinneret lateral oscillation amplitude was 40 cm, and the oscillation speed was 0.4 cm / min. The ambient temperature was controlled at 25 ± 2℃ and the relative humidity was 30%. Electrospinning was carried out for 5 h. After spinning, the fiber membrane was peeled off the aluminum foil and dried in a vacuum drying oven at 60°C for 12 h to obtain a polyamic acid (PAA) nanofiber membrane with a fiber diameter of 200-500 nm and a thickness of 30 μm. Before use, polyamic acid (PAA) nanofiber membranes need to be cleaned by ultrasonic cleaning with anhydrous ethanol and water for 20 minutes each, then dried with nitrogen, and then cut into 5 cm × 5 cm square pieces. (2) Dissolve 3-mercaptopropyltrimethoxysilane (MPTMS) in anhydrous ethanol and adjust the pH to 5.5 with acetic acid to obtain a 20 mM 3-mercaptopropyltrimethoxysilane (MPTMS) solution. Polyamic acid (PAA) nanofiber membranes were immersed in 3-mercaptopropyltrimethoxysilane (MPTMS) solution and allowed to stand at 25°C for 6 h. After removal, the membranes were rinsed three times with anhydrous ethanol and dried under vacuum at 60°C for 6 h to obtain SAMs-modified PAA fiber membranes. (3) Zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 3.00 g, 10.08 mmol) was dissolved in 40 mL of methanol to obtain a zinc nitrate hexahydrate solution; 2-methylimidazole (HmIm, 6.62 g, 80.83 mmol) was dissolved in 40 mL of methanol to obtain a 2-methylimidazole solution; the zinc nitrate hexahydrate solution and the 2-methylimidazole solution were mixed and stirred at 600 rpm for 0.5 h to obtain a ZIF-8 precursor growth solution; The SAMs-modified PAA fiber membrane was immersed in ZIF-8 precursor growth solution, and then grown in situ at 25°C for 12 h. After being repeatedly washed with methanol three times, it was vacuum dried at 60°C for 12 h to obtain PAA@ZIF-8 composite fiber membrane. (4) Mix acetic anhydride, pyridine, and N,N-dimethylacetamide (DMAc) in a volume ratio of 2:2:5 to obtain a mixed solution of acetic anhydride / pyridine / DMAc; The PAA@ZIF-8 composite fiber membrane was immersed in a mixed solution of acetic anhydride / pyridine / N,N-dimethylacetamide (DMAc) and chemically imidized at 120℃ for 2 h. After the reaction, it was repeatedly washed three times with DMAc and anhydrous ethanol, and then vacuum dried at 60℃ for 12 h to obtain a PI@ZIF-8 composite fiber membrane with directional ion transport channels (thickness of 30 μm).
[0062] Comparative Example 1: Interface without SAMs (Self-Enhancing Features) Step (2) in Example 1 is omitted, and everything else remains the same as in Example 1 to obtain a composite fiber membrane.
[0063] Comparative Example 2: Conventional thermal imidization Adjust step (4) in Example 1 as follows: The PAA@ZIF-8 composite fiber membrane was placed in a muffle furnace and subjected to gradient heating thermal imidization under nitrogen protection: the temperature was increased from room temperature to 100℃ at a heating rate of 2℃ / min and held for 30 min; then increased to 200℃ at a heating rate of 2℃ / min and held for 30 min; finally increased to 300℃ at a heating rate of 2℃ / min and held for 60 min; and then naturally cooled to room temperature to obtain the PI@ZIF-8 composite fiber membrane.
[0064] Comparative Example 3: Blending Electrospinning A method for preparing a composite fiber membrane includes the following steps: (1) Weigh 10.0 g of polyamic acid (PAA) powder and dissolve it in 90 g of N,N-dimethylacetamide (DMAc). Stir mechanically at 25°C and 1000 rpm for 6 h until completely dissolved to obtain a polyamic acid solution. ZIF-8 nanoparticles (1.0 g, 50-150 nm) were dispersed in 15 mL of DMAc and ultrasonically dispersed for 30 min to obtain a ZIF-8 dispersion. The ZIF-8 dispersion was added to the polyamic acid solution, and the mixture was stirred at 600 rpm for 2 h to obtain the spinning solution. The spinning solution was injected into a syringe with a stainless steel spinneret (0.8 mm inner diameter); the receiving device was a cylindrical roller wrapped with aluminum foil (12 cm diameter, 30 cm length), the receiving distance was 18 cm, the applied voltage was 20 kV, the feed speed was 0.5 ml / h, the roller speed was 150 r / min, the spinneret lateral oscillation amplitude was 30 cm, and the oscillation speed was 0.5 cm / min; the ambient temperature was controlled at 25 ± 2℃, and the relative humidity was 30%; electrospinning was carried out for 5 h. After spinning, the fiber membrane was peeled off the aluminum foil and dried in a vacuum drying oven at 60°C for 12 h to obtain a polyamic acid (PAA) nanofiber membrane containing ZIF-8, with a fiber diameter of 200-500 nm and a thickness of 30 μm. Before use, the polyamic acid (PAA) nanofiber membrane containing ZIF-8 needs to be cleaned by ultrasonic cleaning with anhydrous ethanol and water for 15 min each, then dried with nitrogen, and then cut into 5 cm × 5 cm square pieces. Then, imidization was performed according to step (4) of Example 1 to obtain PI / ZIF-8 composite fiber membrane.
[0065] Comparative Example 4: ZIF-8 / PVDF-HFP blade-coated film without PI fiber skeleton. A method for preparing a ZIF-8 / PVDF-HFP composite membrane includes the following steps: (1) Weigh 7.0 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and add it to 90.0 g of N-methylpyrrolidone (NMP). Stir mechanically at 60 °C and 600 rpm for 4 h to obtain a homogeneous polymer solution. (2) Weigh 3.0 g of ZIP-8 powder (50-150 nm) and add it to the above PVDF-HFP solution. First, ultrasonically disperse it for 10 min, and then mechanically stir it at 600 rpm for 1 h to make ZIF-8 uniformly dispersed and obtain ZIF-8 / PVDF-HFP mixed slurry. (3) The obtained mixed slurry was uniformly coated on the surface of a clean glass plate by scraping method. After vacuum degassing, it was vacuum dried at 60℃ for 12 h to obtain ZIF-8 / PVDF-HFP composite film (thickness of 40 μm). The mass ratio of ZIF-8 powder to PVDF-HFP is 3:7, the mass ratio of ZIF-8, PVDF-HFP and NMP is 3:7:90, and the mass fraction of solid components in the mixed slurry is 10 wt%.
[0066] Example 4 A method for preparing a quasi-solid-state electrolyte membrane includes the following steps: (1) Lithium bis(trifluoromethanesulfonate)imide (LiTFSI) was dissolved in a mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME), and LiPF6 was added as an initiator. The mixture was stirred at 600 rpm to obtain a quasi-solid electrolyte precursor solution. The volume ratio of the mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME) is 1:1. The concentration of lithium bis(trifluoromethanesulfonate) (LiTFSI) in the quasi-solid-state electrolyte precursor solution was 1 M; the mass concentration of LiPF6 was 2%. (2) In a glove box filled with argon (H2O<0.1 ppm, O2<0.1 ppm), the composite membranes prepared in Examples 1-3 and Comparative Examples 1-4 were cut into circular diaphragm sheets with a diameter of 19 mm and placed in a vacuum oven to dry at 80°C for 12 h. (3) The dried composite membranes prepared in Examples 1-3 and Comparative Examples 1-4 were immersed in a quasi-solid electrolyte precursor solution and adsorbed at 25°C for 12 h. After removal, excess liquid on the surface was gently absorbed with filter paper to obtain a quasi-solid electrolyte membrane.
[0067] The obtained quasi-solid electrolyte membrane was subjected to performance testing, and the test results are as follows: Table 1
[0068] As can be seen from Table 1: (1) Comparison of Example 1 and Comparative Example 1: SAMs interface modification increased the orientation degree of ZIF-8 from 0.98 to 2.87 and the ionic conductivity from 0.92 × 10⁻⁶ to 2.87. -4 Increased to 1.84×10 -4 S / cm, tLi + The improvement from 0.58 to 0.77 demonstrates that the directional alignment induced by SAMs is the key to the performance enhancement.
[0069] (2) Comparison of Example 1 and Comparative Example 2: Traditional 300℃ thermal imidization destroys the ZIF-8 structure. Although a certain orientation (1.85) is preserved, the ionic conductivity (0.65×10) is reduced. -4 S / cm) and tLi +(0.51) is much lower than that of Example 1 (chemical imidization at 80°C), demonstrating the necessity of low-temperature chemical imidization for MOF structure protection.
[0070] (3) Comparison of Example 1 and Comparative Example 3: The ZIF-8 orientation degree of the blending method was the lowest (0.75), and the ionic conductivity was (0.58×10). -4 S / cm) and tLi + (0.48) are significantly lower than those in Example 1, demonstrating the advantages of the "directed growth first, then conversion" process.
[0071] (4) Comparison of Example 1 and Comparative Example 4: The ZIF-8 / PVDF-HFP membrane without PI fiber skeleton had the worst performance (ionic conductivity 0.41×10). -4 (S / cm, cyclic stability 180 h), demonstrating the irreplaceable nature of the key mechanical support and three-dimensional interconnected network structure provided by the PI fiber skeleton.
[0072] (5) In Example 2, by optimizing the concentration of SAMs and the growth time, the orientation degree reached 3.12 and the ionic conductivity reached 2.01 × 10⁻⁶. -4 S / cm is the optimal solution.
[0073] (6) In Example 3, MPTMS was used instead of APTES, and the same good results were achieved.
[0074] Figure 2 These are scanning electron microscope (SEM) images of the polyamic acid (PAA) nanofiber membrane, the PAA@ZIF-8 composite fiber membrane, and the PI@ZIF-8 composite fiber membrane with directional ion transport channels from Example 1. Figure 2 It can be seen that the surface of unmodified PAA nanofibers is relatively smooth and flat, with the fibers interwoven to form a continuous porous network structure. After SAMs interface modification and in-situ growth of ZIF-8, a large number of particulate ZIF-8 crystals are continuously distributed along the fiber contour and attached to the fiber surface. After further low-temperature chemical imidization, the fiber network structure remains intact, and the ZIF-8 particles remain stably loaded on the fiber surface without significant large-scale shedding or fiber structure collapse. This indicates that SAMs interface modification can promote the in-situ nucleation and continuous growth of ZIF-8 on the PAA fiber surface, while low-temperature chemical imidization can better maintain the ZIF-8 and fiber porous structure during the PAA to PI conversion, providing a structural basis for the formation of continuous ion transport channels along the fiber direction.
[0075] Figure 3 XRD pattern of the PI@ZIF-8 composite fiber membrane with directional ion transport channels prepared in Example 1. Figure 3It can be seen that, compared with the pure PI membrane, the APTES-PI@ZIF-8 composite fiber membrane exhibits diffraction signals corresponding to the main characteristic diffraction peaks of ZIF-8, indicating that ZIF-8 with a crystalline structure exists in the composite fiber membrane, and that the main crystal structure characteristics of ZIF-8 are still retained after compositing.
[0076] Figure 4 This is a comparison graph showing the ionic conductivity versus lithium-ion transference number for Examples 1-3 and Comparative Examples 1-4. From... Figure 4 It can be seen that the ionic conductivity of Examples 1-3 is 1.84 × 10⁻⁶. -4 S / cm, 2.01×10 -4 S / cm and 1.72×10 -4 The S / cm and lithium-ion transference numbers were 0.77, 0.79, and 0.75, respectively, all significantly higher than those of Comparative Examples 1-4. Among them, Example 2 exhibited the highest ionic conductivity and lithium-ion transference number, reaching 2.01 × 10⁻⁶. -4 S / cm and 0.79. Comparing Example 1 and Comparative Example 1, after omitting the SAMs interface modification, the ionic conductivity increased from 1.84 × 10⁻⁶ to 0.79. -4 S / cm decreased to 0.92×10 -4 The S / cm ratio and lithium-ion transference number decreased from 0.77 to 0.58. This indicates that the ordered in-situ growth of ZIF-8 induced by SAMs on the fiber surface can reduce the tortuosity of the lithium-ion transport path, and combined with the confinement effect of ZIF-8 on anions, effectively improve the ion conductivity and lithium-ion migration capacity of the composite fiber membrane.
[0077] Figure 5 For Li / QSE-1 / Li symmetric cells at 0.2 mA / cm 2 The cyclic stability curve is shown below. Figure 5 It can be seen that the Li / Li symmetric batteries corresponding to Examples 1, 2 and 3 can be stably cycled for about 2000 h, 1800 h and 1600 h respectively. During the cycle, the polarization voltage remains stable overall, and no obvious voltage change or short circuit phenomenon occurs. The PI@ZIF-8 composite fiber membrane constructed in this invention can improve the uniform transport of lithium ions in the electrolyte membrane, which is beneficial to stabilizing the lithium metal deposition / stripping interface, reducing local ion concentration difference and short circuit risk, thereby significantly improving the long-term cycle stability of lithium metal symmetric batteries.
[0078] Figure 6 The cycling performance curves of the LiFePO4 / QSE-1 / Li full cell at 0.5C rate are shown. Figure 6It can be seen that the full cells corresponding to Examples 1-3 all exhibit good cycle stability, with the coulombic efficiency generally remaining close to 100% during cycling. After 400 cycles, the capacity retention rates of Examples 1, 2, and 3 are 85%, 90%, and 83%, respectively, with Example 2 showing the best cycle retention performance. This indicates that the PI@ZIF-8 composite fiber membrane with directional ion transport channels can promote Li + Rapid and uniform transport reduces interfacial polarization during cycling, which is beneficial to improving the long-term cycling stability and capacity retention of LiFePO4 / Li full cells.
[0079] Comparative Example 5 In step (2) of Example 1, 3-aminopropyltriethoxysilane (APTES) was changed to methyltriethoxysilane (MTES), while the rest remained the same as in Example 1.
[0080] The results showed that although MTES could form a silane-modified layer on the PAA fiber surface after interface modification, the MTES terminal methyl group lacked the ability to effectively adsorb or coordinate Zn. 2+ The reduced number and continuous loading of ZIF-8 nucleation sites on the fiber surface due to the absence of active functional groups resulted in decreased crystal distribution uniformity and orientation, leading to lower ionic conductivity and lithium-ion transference number in the resulting composite fiber membrane compared to Example 1. This indicates that the formation of a self-assembled interface layer is not the only condition; the ends of self-assembled molecules possess the ability to promote Zn... 2+ Enrichment, nucleation, and growth of active functional groups at the ZIF-8 interface are important factors in obtaining highly oriented ZIF-8 composite fiber membranes.
[0081] Comparative Example 6 Direct in-situ growth of ZIF-8 crystals from PI fiber membranes includes the following steps: Zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 1.19 g, 4.0 mmol) was dissolved in 40 mL of methanol to obtain a zinc nitrate hexahydrate solution; 2-methylimidazole (HmIm, 2.63 g, 32.0 mmol) was dissolved in 40 mL of methanol to obtain a 2-methylimidazole solution; the zinc nitrate hexahydrate solution and the 2-methylimidazole solution were mixed and stirred at 600 rpm for 0.5 h to obtain the ZIF-8 precursor growth solution; PI nanofiber membranes were directly immersed in ZIF-8 precursor growth solution and allowed to stand at 25°C for 6 h. After the reaction, the membranes were washed three times with methanol and dried under vacuum at 60°C for 12 h to obtain PI composite fiber membranes with directly grown ZIF-8.
[0082] The results showed that, compared with Example 1, when ZIF-8 was grown directly on the surface of the PI fiber membrane in situ, the ZIF-8 crystal loading on the fiber surface decreased, the crystal distribution became discontinuous, and random nucleation and local aggregation occurred to a certain extent, with a significant reduction in orientation. This is because PAA, after imidization to PI, can participate in Zn... 2+ The reduced number of adsorption and coordination active sites, coupled with the lack of interfacial nucleation and anchoring effects provided by SAMs, makes it difficult to achieve continuous and directional growth of ZIF-8 along the fiber surface. This indicates that the preparation sequence of "SAMs interfacial modification and in-situ growth of ZIF-8 during the PAA stage, followed by low-temperature chemical imidization" plays a crucial role in constructing continuous and stable ZIF-8 ion transport channels.
[0083] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.
Claims
1. A method for preparing a PI@ZIF-8 composite fiber membrane with directional ion transport channels, characterized in that, Includes the following steps: (1) The polyamic acid nanofiber membrane was immersed in a solution containing a self-assembled monolayer precursor at pH 4.0-5.5 and reacted at 15-35℃ for 6-48 h. After the reaction was completed, the membrane was washed and dried to obtain the polyamic acid nanofiber membrane modified with aminopropyl functionalized self-assembled monolayer. The solution containing the self-assembled monolayer precursor is either a 3-aminopropyltriethoxysilane solution or a 3-mercaptopropyltrimethoxysilane solution. (2) The polyamic acid nanofiber membrane modified with aminopropyl functionalized self-assembled monolayer was immersed in ZIF-8 precursor growth solution and grown in situ at 15-50℃ for 2-48h. After washing and drying, PAA@ZIF-8 composite fiber membrane was obtained. (3) The PAA@ZIF-8 composite fiber membrane was immersed in a mixed solution of acetic anhydride / pyridine / N,N-dimethylacetamide and chemically imidized at 25-40℃ for 2-12h. After the reaction was completed, it was washed and dried to obtain the PI@ZIF-8 composite fiber membrane with directional ion transport channels.
2. The method according to claim 1, characterized in that, In step (1), the polyamic acid nanofiber membrane is prepared by electrospinning, with a fiber diameter of 200-500 nm and a membrane thickness of 10-60 μm.
3. The method according to claim 1, characterized in that, The solvent for the solution containing the self-assembled monolayer precursor in step (1) is anhydrous ethanol with a concentration of 5-20 mM.
4. The method according to claim 1, characterized in that, In step (3), the volume ratio of acetic anhydride, pyridine, and N,N-dimethylacetamide in the acetic anhydride / pyridine / N,N-dimethylacetamide mixed solution is 0.5-2:0.5-2:5-10.
5. The PI@ZIF-8 composite fiber membrane with directional ion transport channels prepared by the method according to any one of claims 1-4.
6. A quasi-solid-state electrolyte membrane, characterized in that, The PI@ZIF-8 composite fiber membrane with directional ion transport channels as described in claim 5 was used.
7. A lithium-ion symmetric battery, characterized in that, The PI@ZIF-8 composite fiber membrane with directional ion transport channels as described in claim 5 or the quasi-solid electrolyte membrane as described in claim 6 were used.
8. A lithium-ion full battery, characterized in that, The PI@ZIF-8 composite fiber membrane with directional ion transport channels as described in claim 5 or the quasi-solid electrolyte membrane as described in claim 6 were used.
9. A method for improving the ion conductivity and electrochemical stability of lithium-ion batteries, characterized in that, The PI@ZIF-8 composite fiber membrane with directional ion transport channels as described in claim 5 was used.
10. A battery for forklifts, characterized in that, The PI@ZIF-8 composite fiber membrane with directional ion transport channels as described in claim 5 or the quasi-solid electrolyte membrane as described in claim 6 were used.