Water-voltaic nanogenerator fabric material, preparation method and application thereof
By introducing a stacked structure of hydrophilic fiber substrate, cationic polymer layer and porous conductive layer into the hydrovoltaic nano-power generation fabric material, and utilizing graphene oxide and sodium polystyrene sulfonate to form a highly efficient ion conduction channel, the problems of low output current and poor stability of existing fabric materials are solved, and higher electrical signal output and better flexibility and breathability are achieved.
Patent Information
- Application Number
- CN202611257034.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-20
AI Technical Summary
Existing hydrovolt nanofiber power generation fabric materials have low output current, are prone to performance degradation, and have poor cycle stability, making it difficult to meet the needs of energy harvesting and wearable electronic devices.
The structure employs a stacked structure of hydrophilic fiber substrate, cationic polymer layer, composite functional layer and porous conductive layer. The composite functional layer contains graphene oxide and sodium polystyrene sulfonate, which form high-density fixed negative charge and mobile ion conduction channels through electrostatic adsorption. Combined with fiber gaps and nanochannels, it synergistically promotes liquid capillary transport.
It significantly improves electrical signal output performance and cycle stability, enhances flexibility and breathability, and is suitable for energy harvesting and wearable electronic devices.
Smart Images

Figure CN123133175A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of self-powered material preparation technology, specifically to a water-voltaic nanofiber power generation fabric material, its preparation method, and its application. Background Technology
[0002] Mechanical-to-electrical energy conversion has become a key method for energy harvesting, self-powered devices, and wearable electronic devices. Traditional mechanical-to-electrical energy conversion mechanisms mainly include electromagnetic effects, piezoelectricity, and triboelectric nanogenerators. Hydrovoltaic generators are a novel energy conversion device that relies on the directional migration of ions as liquid flows within nanochannels to generate an electric field, offering a new alternative for low-frequency energy harvesting and flexible self-powered electronic devices.
[0003] Human sweat is rich in various electrolyte ions (Na+). + K + Cl - The continuous evaporation of moisture and capillary transport on the skin surface provide natural conditions for hydrovoltaic power generation. Although various ion-conducting materials such as graphene oxide (GO) films and carbon nanotube films have been reported to exhibit the hydrovoltaic effect, their electrical signal output is still limited to tens of millivolts or a few microamps, making it difficult to directly utilize this electrical energy. Existing fabric-based hydrovoltaic devices have the following main drawbacks: the ionization degree of carboxyl groups (-COOH) on the GO surface is limited, the surface negative charge density is low, and the interlayer channels of GO tend to stack densely, leading to the accumulation of mobile counterions (mainly H+). + Insufficient concentration and obstructed ion transport paths result in generally low output current (typically below microamperes). Furthermore, existing devices are prone to performance degradation and poor cycle stability during repeated dry-wet cycles (sweating-drying).
[0004] Therefore, further improving the electrical signal output of hydroelectric power generation is of great significance. Considering that the electrical signal originates from the directional migration of ions under liquid flow, introducing high-density fixed charges and mobile ions into the ion conduction channel is a feasible strategy. Summary of the Invention
[0005] The purpose of this invention is to overcome the problems of generally low output current, easy performance degradation, and poor cycle stability of existing water-voltaic nanofiber power generation fabrics, and to provide a water-voltaic nanofiber power generation fabric material, its preparation method, and its applications. This water-voltaic nanofiber power generation fabric material significantly improves the electrical signal output performance and enhances cycle stability, while also possessing excellent flexibility, breathability, and wearable integration adaptability, showing broad application prospects in energy harvesting, self-powered devices, or wearable electronic devices.
[0006] To achieve the above objectives, the present invention provides a hydrovoltaic nanofiber power generation fabric material, which includes a hydrophilic fiber substrate, a cationic polymer layer, a composite functional layer and a porous conductive layer stacked sequentially, wherein the composite functional layer contains graphene oxide and sodium polystyrene sulfonate.
[0007] Preferably, the cationic polymer layer, the composite functional layer, and the porous conductive layer are arranged symmetrically on both sides of the hydrophilic fiber substrate.
[0008] Preferably, relative to 100 parts by weight of the hydrophilic fiber substrate, the content of the cationic polymer layer is 50-200 parts by weight, the content of the composite functional layer is 10-60 parts by weight, and the content of the porous conductive layer is 1-10 parts by weight.
[0009] Preferably, in the composite functional layer, the mass ratio of graphene oxide to sodium polystyrene sulfonate is 1:0.1-10, more preferably 1:0.25-4.
[0010] Preferably, the hydrophilic fiber substrate is selected from at least one of cleanroom fabric, natural fiber, modified synthetic fiber, and blended fabric.
[0011] Preferably, the cationic polymer layer is selected from at least one of polyethyleneimine, polydiallyldimethylammonium chloride, and polyacrylamide-copolymer-dimethyldiallylammonium chloride.
[0012] Preferably, the porous conductive layer contains at least one of carbon black, carbon nanotubes, and conductive polymer materials.
[0013] A second aspect of this invention provides a method for preparing a water-voltaic nanofiber power generation fabric material, the method comprising the following steps: (1) The hydrophilic fiber substrate is immersed in a solution containing a cationic polymer to form a cationic polymer layer on both sides of the hydrophilic fiber substrate; (2) The material obtained in step (1) is immersed in a mixture containing graphene oxide and sodium polystyrene sulfonate to form a composite functional layer on the surface of the cationic polymer layer; (3) The material obtained in step (2) is immersed in a mixture containing porous conductive material to form a porous conductive layer in the composite functional layer.
[0014] Preferably, in step (1), the mass ratio of the hydrophilic fiber substrate to the cationic polymer is 1:0.5-2.
[0015] Preferably, the concentration of the solution containing the cationic polymer is 10-50 g / L.
[0016] Preferably, the cationic polymer is selected from at least one of polyethyleneimine, polydiallyldimethylammonium chloride, and polyacrylamide-copolymer-dimethyldiallylammonium chloride.
[0017] Preferably, the hydrophilic fiber substrate is selected from at least one of cleanroom fabric, natural fiber, modified synthetic fiber, and blended fabric.
[0018] Preferably, the mass ratio of the hydrophilic fiber substrate to the total amount of graphene oxide and sodium polystyrene sulfonate is 1:0.1-0.6.
[0019] Preferably, in the mixture containing graphene oxide and sodium polystyrene sulfonate, the mass ratio of graphene oxide to sodium polystyrene sulfonate is 1:0.1-10, more preferably 1:0.25-4.
[0020] Preferably, the mass ratio of the hydrophilic fiber substrate to the porous conductive material is 1:0.01-0.1.
[0021] Preferably, the porous conductive material is selected from at least one of carbon black, carbon nanotubes, and conductive polymer materials.
[0022] Preferably, the mixture containing the porous conductive material further contains a dispersant, and the mass ratio of the conductive material to the dispersant is 1:1-5.
[0023] More preferably, the dispersant is selected from at least one of sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, and hexadecyltrimethylammonium bromide.
[0024] Preferably, in step (1), the impregnation conditions include: a temperature of 40-80°C and a time of 0.5-2h.
[0025] Preferably, in step (2), the impregnation conditions include: a temperature of 20-40°C and a time of 5-60 min.
[0026] Preferably, in step (3), the impregnation conditions include: a temperature of 20-40°C and a time of 5-60 min.
[0027] A third aspect of the present invention provides a water-voltaic nanofiber power generation fabric material prepared by the method described above.
[0028] The fourth aspect of this invention provides the application of the aforementioned water-voltaic nanofiber power generation fabric material in the fabrication process of flexible self-powered devices.
[0029] The hydrovoltaic nanofiber power generation fabric material of this invention comprises a hydrophilic fiber substrate, a cationic polymer layer, a composite functional layer, and a porous conductive layer stacked sequentially. The composite functional layer contains graphene oxide and sodium polystyrene sulfonate. The sodium polystyrene sulfonate in the composite functional layer provides a high-density sulfonic acid group to fix negative charges and cationic carriers, forming a bicontinuous network with the graphene oxide, significantly improving ion conduction efficiency and output current. Simultaneously, the micron-scale flow channels formed by the interfiber gaps of the hydrophilic fiber substrate synergistically with the interlayer nanochannels of the graphene oxide to promote capillary transport of liquid. Compared to traditional fabrics coated with pure graphene oxide, the photovoltaic nanofiber fabric material described in this invention exhibits significantly improved electrical signal output and enhanced cycle stability. Furthermore, compared to other photovoltaic materials (such as pure graphene oxide films and carbon nanotube films), the micron-level voids between the fibers of the cleanroom fabric, the nanochannels between the GO / PSSNa layers, and the porous structure of the carbon black conductive layer together form a three-dimensional breathable network, resulting in better flexibility, breathability, and wearable integration. This makes the material promising for applications in energy harvesting, self-powered devices, or wearable electronic devices. Attached Figure Description
[0030] Figure 1 These are scanning electron microscope (SEM) images of (a) a cleanroom cloth, (b) the water-voltaic nanofiber fabric material prepared in Comparative Example 1, and (c) the water-voltaic nanofiber fabric material prepared in Example 1. Figure 2 This is a voltage output diagram of the water-volt nano-power generation fabric material prepared in Comparative Example 3; Figure 3 The voltage output diagrams of the water-volt nano-power generation fabric materials prepared in Comparative Example 1 and Comparative Example 2 are shown. Figure 4 The current output diagrams of the water-volt nano-power generation fabric materials prepared in Comparative Example 1 and Comparative Example 2 are shown. Figure 5 These are voltage output diagrams of the water-volt nanofiber power generation fabric materials prepared in Examples 1 and 4-8; Figure 6 These are the current output diagrams of the water-voltaic nanofiber power generation fabric materials prepared in Examples 1 and 4-8; Figure 7 This is a stability output diagram of the water-voltaic nano-power generation fabric material prepared in Example 1 after 10 dry-wet cycles. Detailed Implementation
[0031] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0032] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0033] The hydrovoltaic nano-power generation fabric material of the present invention comprises a hydrophilic fiber substrate, a cationic polymer layer, a composite functional layer and a porous conductive layer stacked sequentially, wherein the composite functional layer contains graphene oxide (GO) and sodium polystyrene sulfonate (PSSNa).
[0034] In the aforementioned hydrovoltaic nanofiber power generation fabric material, the cationic polymer layer, the composite functional layer, and the porous conductive layer are symmetrically arranged on both sides of the hydrophilic fiber substrate. It can be understood that the hydrovoltaic nanofiber power generation fabric material has a sandwich structure, with the hydrophilic fiber substrate as the core inner layer, and the cationic polymer layer, composite functional layer, and porous conductive layer sequentially stacked on both sides of the substrate from the inside out.
[0035] In some embodiments, relative to 100 parts by weight of the hydrophilic fiber substrate, the content of the cationic polymer layer is 50-200 parts by weight, preferably 75-175 parts by weight, and more preferably 100-150 parts by weight; the content of the composite functional layer is 10-60 parts by weight, preferably 20-40 parts by weight, and more preferably 25-35 parts by weight; and the content of the porous conductive layer is 1-10 parts by weight, preferably 2-8 parts by weight, and more preferably 3-7 parts by weight. As a specific example, relative to 100 parts by weight of the hydrophilic fiber substrate, the content of the cationic polymer layer can be 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, or 150 parts by weight; the content of the composite functional layer can be 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, or 35 parts by weight; and the content of the porous conductive layer can be 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, or 7 parts by weight. In this invention, the content of each component is based on the amount of each component raw material added during the preparation process.
[0036] In some embodiments, in the composite functional layer, the sulfonic acid groups of PSSNa provide a high density of fixed negative charges and mobile metal cations, while GO provides two-dimensional nanochannels and a structural framework. The mass ratio of graphene oxide to sodium polystyrene sulfonate is 1:0.1-10, preferably 1:0.25-4, more preferably 1:1-4, and even more preferably 1:1.5-2.5. As a specific example, in the composite functional layer, the mass ratio of graphene oxide to sodium polystyrene sulfonate can be 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, or 1:2.5.
[0037] In this invention, the hydrophilic fiber substrate has natural fiber gaps, which can form micron-level flow channels. Preferably, the hydrophilic fiber substrate is selected from at least one of cleanroom fabric (polypropylene / polyimide composite fiber), natural fibers, modified synthetic fibers, and blended fabrics. The natural fibers can be cotton, linen, bamboo fiber, wool, etc.; the modified synthetic fibers can be plasma-treated or hydrophilically modified polyester, nylon, etc.; and the blended fabrics can be cotton / polyester blends, cotton / spandex blends, etc.
[0038] In this invention, the cationic polymer layer can form a positively charged layer on the fiber surface through electrostatic adsorption, thereby strongly attracting and fixing negatively charged graphene oxide (GO) and sodium polystyrene sulfonate (PSSNa), improving the loading and stability of the functional layer. Preferably, the cationic polymer layer is selected from at least one of polyethyleneimine, polydiallyldimethylammonium chloride, and polyacrylamide-copolymer-dimethyldiallylammonium chloride. More preferably, the cationic polymer layer is polyethyleneimine, and the weight-average molecular weight of the polyethyleneimine is 500-1000.
[0039] In this invention, the porous conductive layer can collect the charge generated by the composite functional layer and form a current through an external circuit. Simultaneously, its porous structure allows sweat / solution to pass freely without affecting capillary action and evaporation processes. Preferably, the porous conductive layer contains at least one of carbon black, carbon nanotubes (single-walled or multi-walled), and conductive polymer materials (such as poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonate), polyaniline, or polypyrrole). In a further preferred embodiment, the porous conductive layer is carbon black.
[0040] This invention also provides a method for preparing a water-voltaic nanofiber power generation fabric material, the method comprising the following steps: (1) The hydrophilic fiber substrate is immersed in a solution containing a cationic polymer to form a cationic polymer layer on both sides of the hydrophilic fiber substrate; (2) The material obtained in step (1) is immersed in a mixture containing graphene oxide and sodium polystyrene sulfonate to form a composite functional layer on the surface of the cationic polymer layer; (3) The material obtained in step (2) is immersed in a mixture containing porous conductive material to form a porous conductive layer in the composite functional layer.
[0041] In some embodiments, in step (1), the mass ratio of the hydrophilic fiber substrate to the cationic polymer is 1:0.5-2, preferably 1:0.75-1.75, and more preferably 1:1-1.5. As a specific example, the mass ratio of the hydrophilic fiber substrate to the cationic polymer can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, or 1:1.5.
[0042] In the method described in this invention, the hydrophilic fiber substrate has natural fiber gaps that can form micron-level flow channels. Preferably, the hydrophilic fiber substrate is selected from at least one of cleanroom fabric (polypropylene / polyimide composite fiber), natural fibers, modified synthetic fibers, and blended fabrics. The natural fibers can be cotton, linen, bamboo fiber, wool, etc.; the modified synthetic fibers can be plasma-treated or hydrophilically modified polyester, nylon, etc.; and the blended fabrics can be cotton / polyester blends, cotton / spandex blends, etc.
[0043] In the method described in this invention, the cationic polymer can form a positively charged layer on the fiber surface through electrostatic adsorption, thereby strongly attracting and fixing negatively charged graphene oxide (GO) and sodium polystyrene sulfonate (PSSNa), improving the loading and stability of the functional layer. Preferably, the cationic polymer is selected from at least one of polyethyleneimine, polydiallyldimethylammonium chloride, and polyacrylamide-copolymer-dimethyldiallylammonium chloride. More preferably, the cationic polymer is polyethyleneimine, and the weight-average molecular weight of the polyethyleneimine is 500-1000.
[0044] In some embodiments, in step (1), the concentration of the solution containing the cationic polymer is 10-50 g / L, preferably 20-40 g / L. Within this concentration range, the cationic polymer can be uniformly adsorbed and coated on the surface of the hydrophilic fiber substrate. This ensures that the fiber surface is fully grafted with positively charged active sites, effectively improving the interfacial bonding force of the subsequent composite functional layer. It also avoids the agglomeration and accumulation of the polymer due to excessively high concentration, which would block the fiber pores, or the insufficient charge sites due to excessively low concentration. This ensures that the prepared hydrovoltaic nanofiber power generation fabric has stable interfacial charge transport performance and hydrovoltaic power generation efficiency.
[0045] In some embodiments, the conditions for impregnation in step (1) include: a temperature of 40-80°C, preferably 50-70°C; and a time of 0.5-2h, preferably 1-1.5h.
[0046] In some embodiments, the specific process of step (1) further includes drying the impregnated material at 50-70°C.
[0047] In some embodiments, the mass ratio of the hydrophilic fiber substrate to the total amount of graphene oxide and sodium polystyrene sulfonate is 1:0.1-0.6, preferably 1:0.2-0.4, and more preferably 1:0.25-0.35. As specific examples, the mass ratio of the hydrophilic fiber substrate to the total amount of graphene oxide and sodium polystyrene sulfonate can be 1:0.25, 1:0.26, 1:0.27, 1:0.28, 1:0.29, 1:0.3, 1:0.31, 1:0.32, 1:0.33, 1:0.34, or 1:0.35.
[0048] In the method described in this invention, in step (2), the graphene oxide and the sodium polystyrene sulfonate form a nanochannel network through self-assembly. The sulfonic acid groups of PSSNa provide a high density of fixed negative charges and mobile metal cations, while GO provides two-dimensional nanochannels and a structural framework. The fixed negative charges attract cations to form an electrical double layer. Driven by capillary flow, the cations migrate directionally along the nanochannels, generating a flow potential. GO and PSSNa form a bicontinuous network, synergistically enhancing ion selectivity and conductivity efficiency.
[0049] The graphene oxide and sodium polystyrene sulfonate can be commercially available products or prepared using conventional methods in the art. In some embodiments, the graphene oxide has a multilayer structure and a purity ≥98%, and the sodium polystyrene sulfonate has a weight-average molecular weight of 70,000-80,000.
[0050] In some embodiments, in step (2), in the mixture containing graphene oxide and sodium polystyrene sulfonate, the mass ratio of graphene oxide to sodium polystyrene sulfonate is 1:0.1-10, preferably 1:0.25-4, more preferably 1:1-4, and even more preferably 1:1.5-2.5. As a specific example, in the mixture containing graphene oxide and sodium polystyrene sulfonate, the mass ratio of graphene oxide to sodium polystyrene sulfonate can be 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, or 1:2.5.
[0051] In some embodiments, step (2) further includes preparing the mixture containing graphene oxide and sodium polystyrene sulfonate according to the following process: mixing the aqueous solution of graphene oxide and sodium polystyrene sulfonate with a solvent, and then sonicating the cells for 0.5-2 hours. The solvent is a commonly used solvent in the art, such as deionized water.
[0052] In some embodiments, in step (2), the conditions for impregnation include: a temperature of 20-40°C, preferably 25-35°C; and a time of 5-60 min, preferably 10-30 min.
[0053] In some embodiments, the specific process of step (2) further includes drying the impregnated material at 50-70°C.
[0054] In the method described in this invention, in step (2), to achieve uniform loading and full deposition of graphene oxide and sodium polystyrene sulfonate on the surface of the cationic polymer layer, strengthen the interlayer interface bonding strength, and simultaneously control the thickness, pore structure, and charge transport performance of the composite functional layer, step (2) can be repeated 1-4 times according to actual needs. Through multiple cycles of coating-deposition, problems such as insufficient single-cycle loading and uneven functional layer coverage can be effectively avoided, water molecule adsorption and transport channels can be optimized, thereby improving the final water-voltaic power generation output performance and structural stability of the fabric material.
[0055] In some embodiments, the mass ratio of the hydrophilic fiber substrate to the porous conductive material is 1:0.01-0.1, preferably 1:0.02-0.08, and more preferably 1:0.03-0.07. As specific examples, the mass ratio of the hydrophilic fiber substrate to the porous conductive material can be 1:0.03, 1:0.04, 1:0.05, 1:0.06, or 1:0.07.
[0056] In the method described in this invention, in step (3), the porous conductive material can collect the charge generated by the composite functional layer and form a current through the external circuit. Simultaneously, its porous structure allows sweat / solution to pass freely without affecting capillary action and evaporation processes. Preferably, the porous conductive material contains at least one of carbon black, carbon nanotubes (single-walled or multi-walled), and conductive polymers (such as poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonate), polyaniline, or polypyrrole). In a further preferred embodiment, the porous conductive material is carbon black.
[0057] In some embodiments, in step (3), the mixture containing the porous conductive material also contains a dispersant, and the mass ratio of the conductive material to the dispersant is 1:1-5, preferably 1:1-3.
[0058] In the method described in this invention, in step (3), the dispersant is selected from at least one of sodium dodecylbenzenesulfonate (SDBS), sodium dodecyl sulfate (SDS), and hexadecyltrimethylammonium bromide (CTAB).
[0059] In some embodiments, in step (3), the conditions for impregnation include: a temperature of 20-40°C, preferably 25-35°C; and a time of 5-60 min, preferably 10-30 min.
[0060] In some embodiments, the specific process of step (3) further includes drying the impregnated material at 50-70°C.
[0061] This invention also provides a hydrovoltaic nanofiber power generation fabric material prepared by the method described above. This hydrovoltaic nanofiber power generation fabric material comprises a hydrophilic fiber substrate, a cationic polymer layer, a composite functional layer, and a porous conductive layer stacked sequentially. The composite functional layer contains graphene oxide and sodium polystyrene sulfonate. The sodium polystyrene sulfonate in the composite functional layer provides a high-density sulfonic acid group to fix negative charges and cationic charge carriers, forming a bicontinuous network with the graphene oxide, significantly improving ion conduction efficiency and output current. Simultaneously, the micron-scale flow channels formed by the interfiber gaps of the hydrophilic fiber substrate synergistically with the interlayer nanochannels of the graphene oxide to promote capillary transport of liquid.
[0062] This invention further provides the application of the aforementioned water-voltaic nanofiber power generation fabric material in the fabrication process of flexible self-powered devices. Compared with traditional pure graphene oxide-coated fabrics, the water-voltaic nanofiber power generation fabric material of this invention significantly improves the electrical signal output and enhances the cycle stability. Moreover, compared with other water-voltaic materials (such as pure graphene oxide films, carbon nanotube films, etc.), the micron-level voids between the fibers of the cleanroom fabric, the nanochannels between the GO / PSSNa layers, and the porous structure of the carbon black conductive layer together form a three-dimensional breathable network, giving the material better flexibility, breathability, and wearable integration. It has broad application prospects in the fields of energy harvesting, self-powered devices, or wearable electronic devices.
[0063] In some embodiments, the water-voltaic nanofiber power-generating fabric material can be applied to low-power electronic paper displays. Electronic paper features power-off display persistence and extremely low refresh power consumption, with some products requiring only tens of microamps of current per refresh. When integrated into sportswear, it can be paired with external sensors to visualize data such as exercise duration, sweat level, and heart rate zone; and the displayed content can be stably retained after power failure, requiring no continuous power supply.
[0064] In some embodiments, the hydrovoltaic nanofiber power-generating fabric material can be used for intermittent power replenishment of smartwatches and wristbands. When the human body sweats during exercise, the fabric activates power generation, trickle-charging the device's battery and effectively improving battery life. In practical applications, a micro supercapacitor can be integrated inside the smart wearable device, with the power-generating fabric placed in the strap / wristband; under sweating conditions, the fabric first stores energy for the supercapacitor, and after the voltage accumulates to a set value, it then supplies power to the device's main battery, thereby extending the device's charging cycle.
[0065] In some embodiments, the hydrovoltaic nanofiber power generation fabric material can be applied to military and outdoor emergency power supply scenarios. The sweat produced by combat personnel and outdoor workers during their movements can soak into the power generation fabric array embedded in their uniforms, thereby providing emergency power to portable electronic devices such as walkie-talkies, GPS devices, and miniature sensors. This solution can effectively reduce the battery load and extend the equipment's operational endurance.
[0066] In some implementations, this hydrovoltaic nanofiber power generation fabric material is suitable for self-powered scenarios in extreme environments for aviation pilots, possessing significant advantages: it has wide temperature range adaptability, can operate using both sweat and condensation as energy sources, and also features flexible wearability, intrinsic safety, and stable and long-lasting output. This technology can overcome the problem of insufficient power supply for critical equipment during long-haul missions, providing a new energy solution for next-generation intelligent flight suits and aviation wearable systems.
[0067] The following examples further illustrate the water-voltaic nanofiber power generation fabric material, its preparation method, and its application according to the present invention. These examples are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following examples.
[0068] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.
[0069] In the following examples and comparative examples, the polyethyleneimine was purchased from Aladdin Company and had a weight-average molecular weight of 700. The graphene oxide was purchased from Shanghai Yuanye Biotechnology Co., Ltd., and has a multilayer sheet structure with a purity of 98%. The sodium polystyrene sulfonate was purchased from Shanghai Yingxin Laboratory Equipment Co., Ltd., and its weight-average molecular weight was 70,000.
[0070] Example 1 (1) Cut the cleanroom cloth into 2×5cm pieces (about 2g), immerse the cleanroom cloth in 100mL of 30 g / L polyethyleneimine (PEI) aqueous solution, soak it in a 65℃ water bath for 1h, and then dry it at 60℃. (2) Add 200 mg of graphene oxide and 2 mL of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.25 g / mL) to 40 mL of deionized water, and sonicate the cells for 1 h to obtain a mixture containing graphene oxide and sodium polystyrene sulfonate. (3) Immerse the material obtained in step (1) into the above-mentioned mixture containing graphene oxide and sodium polystyrene sulfonate at 25°C for 15 minutes, take it out and dry it at 60°C, and repeat step (3) 3 times. (4) Add 0.1 g of carbon black and 0.2 g of SDBS to 40 mL of deionized water and ultrasonically disperse for 1 h to obtain a mixture containing porous conductive material; then immerse the material obtained in step (3) in the mixture containing porous conductive material for 15 min, take it out and dry it at 60 °C to obtain water-volt nano-power generation fabric material.
[0071] in, Figure 1 Scanning electron microscope (SEM) images of (a) a cleanroom cloth, (b) a water-voltaic nanofiber fabric material prepared in Comparative Example 1, and (c) a water-voltaic nanofiber fabric material prepared in Example 1 are shown. The results show that the cleanroom cloth exhibits a smooth fiber structure; on the surface of the water-voltaic nanofiber fabric material prepared in Comparative Example 1, GO sheets are attached in discontinuous sheet form, and the surface is relatively rough; the fibers of the GO / PSSNa composite fabric of the water-voltaic nanofiber fabric material prepared in Example 1 are tightly wrapped by a continuous, smooth, and uniform polymer film, and the pores between the fibers also form a beneficial bridging network.
[0072] Example 2 (1) Cut the cleanroom cloth into 2×5cm pieces (about 2g), immerse the cleanroom cloth in 100mL of 20 g / L polyethyleneimine (PEI) aqueous solution, soak in a 50℃ water bath for 1.5h, and then dry at 60℃. (2) Add 200 mg of graphene oxide and 1.5 mL of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) to 40 mL of deionized water, and sonicate the cells for 1 h to obtain a mixture containing graphene oxide and sodium polystyrene sulfonate. (3) Immerse the material obtained in step (1) into the above-mentioned mixture containing graphene oxide and sodium polystyrene sulfonate at 25°C for 30 minutes, take it out and dry it at 60°C, and repeat step (3) 3 times. (4) Add 0.06 g of Kelvin black carbon black and 0.12 g of SDBS to 40 mL of deionized water and ultrasonically disperse for 1 h to obtain a mixture containing porous conductive material; then immerse the material obtained in step (3) in the mixture containing porous conductive material for 30 min, take it out and dry it at 60 °C to obtain water-volt nano-power generation fabric material.
[0073] Example 3 (1) Cut the cleanroom cloth into 2×5cm pieces (about 2g), immerse the cleanroom cloth in 100mL of 25 g / L polyethyleneimine (PEI) aqueous solution, soak in a 70℃ water bath for 0.5h, and then dry at 60℃. (2) Add 200 mg of graphene oxide and 2.5 mL of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) to 40 mL of deionized water, and sonicate the cells for 1 h to obtain a mixture containing graphene oxide and sodium polystyrene sulfonate. (3) Immerse the material obtained in step (1) into the above-mentioned mixture containing graphene oxide and sodium polystyrene sulfonate at 25°C for 10 minutes, take it out and dry it at 60°C, and repeat step (3) 3 times. (4) Add 0.14 g of Kelvin black carbon black and 0.28 g of SDBS to 40 mL of deionized water and ultrasonically disperse for 1 h to obtain a mixture containing porous conductive material; then immerse the material obtained in step (3) in the mixture containing porous conductive material for 10 min, take it out and dry it at 60°C to obtain water-volt nano-power generation fabric material.
[0074] Example 4 The method described in Example 1 is implemented, except that in step (2), the volume of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) added is 0.5 mL.
[0075] Example 5 The method described in Example 1 is implemented, except that in step (2), the volume of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) added is 1 mL.
[0076] Example 6 The method described in Example 1 is implemented, except that in step (2), the volume of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) added is 3 mL.
[0077] Example 7 The method described in Example 1 is implemented, except that in step (2), the volume of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) added is 4 mL.
[0078] Example 8 The method described in Example 1 is implemented, except that in step (2), the volume of sodium polystyrene sulfonate (20 wt%, with a concentration of approximately 0.2 g / mL) added is 11 mL.
[0079] Comparative Example 1 The method described in Example 1 is implemented, except that sodium polystyrene sulfonate is not added in step (2).
[0080] Comparative Example 2 The method described in Example 1 is implemented, except that graphene is not added in step (2).
[0081] Comparative Example 3 The method described in Example 1 is implemented, except that steps (2) and (3) are omitted.
[0082] Test case Test Example 1 (1) The present invention uses the following methods to test the power generation performance of the water-voltaic nanofiber power generation fabric materials prepared in the examples and comparative examples. The specific test process is as follows: Add 50 mL of 50 mM NaCl solution to one end of the material, while keeping the other end dry. Use capillary action to drive the solution flow. Under the conditions of room temperature (25℃) and relative humidity of 30%, use an electrometer to test the open circuit voltage and short circuit current. The results are shown in Table 1.
[0083] in, Figure 2 The voltage output diagram of the water-volt nano-powered fabric material prepared in Comparative Example 3 is shown; it can be seen that the voltage output is only 0.093V, which is much lower than that in Examples 1-8; Figure 3 The voltage output diagrams of the water-volt nano-power generation fabric materials prepared in Comparative Example 1 and Comparative Example 2 are shown. The results show that the voltage output of Comparative Example 1 with only GO attached and Comparative Example 2 with only PSSNa attached is improved compared to Comparative Example 3, but is still lower than that of Examples 1-8. Figure 4 The current output diagrams of the water-volt nano-power generation fabric materials prepared in Comparative Example 1 and Comparative Example 2 are shown. The results show that the current output effect of only GO attached in Comparative Example 1 and only PSSNa attached in Comparative Example 2 is improved compared with Comparative Example 3, but is still lower than that of Examples 1-8. Figure 5 The voltage output diagrams of the water-voltaic nanofiber power generation fabric materials prepared in Examples 1 and 4-8 are shown. The results show that the optimal ratio of GO:PSSNa is 1:2, which achieves the highest output value and is a significant improvement compared to the single component. Figure 6The current output diagrams of the water-voltaic nanofiber power generation fabric materials prepared in Examples 1 and 4-8 are shown. The results show that the optimal ratio of GO:PSSNa is 1:2, which achieves the highest output value and is significantly improved compared to the single component. Figure 7 The stability output diagram of the water-voltaic nano-power generation fabric material prepared in Example 1 after 10 dry-wet cycles is shown. The results show that when the optimal ratio of GO:PSSNa=1:2 is reached, the performance retention rate of the water-voltaic nano-power generation fabric after 10 dry-wet cycles is greater than 90%, indicating that no functional layer is detached after repeated soaking and drying, the functional layer and fiber are firmly bonded, and the chemical properties of the material are stable.
[0084] Table 1
[0085] Test Example 2 This invention conducts series and parallel tests on the water-voltaic nanofiber power generation fabric material prepared in Example 1. The specific test procedure is as follows: Multiple pieces of the same size water-voltaic nanofiber power generation fabric prepared in Example 1 are taken, and one end (anode) of multiple devices is connected to the other end (cathode) sequentially to form a series assembly; the anodes and cathodes of multiple devices are connected to each other to form a parallel assembly. One end of the series or parallel device assembly is added to 50 μL of 50 mM NaCl solution, while the other end remains dry. Under room temperature (25°C) and relative humidity of 30%, the open-circuit voltage and short-circuit current are measured using an electrometer (Keithley 6514). The output performance of different numbers of devices (1, 2, 3, and 4) connected in series / parallel is recorded to evaluate the scalability and integration capability of the devices. The results are shown in Table 2.
[0086] Table 2
[0087] The results in Tables 1 and 2 show a significant synergistic enhancement effect between GO and PSSNa: PSSNa provides a high density of sulfonic acid groups (-SO3). - Fixed negative charge and mobile Na + The charge carriers, GO, provide two-dimensional nanochannels and a structural framework, forming a dual continuous network that effectively improves ion transport efficiency and charge separation capability. Furthermore, series connection can multiply the device's output voltage, and parallel connection can multiply the output current, demonstrating that the water-voltaic nanofiber power generation fabric of this invention has good scalability and integration capabilities. The output performance of the device can be flexibly configured according to actual load requirements, meeting the power supply requirements of different wearable electronic devices.
[0088] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A water-based photovoltaic nanofiber power generation fabric material, characterized in that, The hydrovoltaic nano-power generation fabric material comprises a hydrophilic fiber substrate, a cationic polymer layer, a composite functional layer, and a porous conductive layer stacked sequentially, wherein the composite functional layer contains graphene oxide and sodium polystyrene sulfonate.
2. The water-volt nano-power generation fabric material according to claim 1, characterized in that, The cationic polymer layer, the composite functional layer, and the porous conductive layer are symmetrically arranged on both sides of the hydrophilic fiber substrate.
3. The water-volt nano-power generation fabric material according to claim 1 or 2, characterized in that, Relative to 100 parts by weight of the hydrophilic fiber substrate, the content of the cationic polymer layer is 50-200 parts by weight, the content of the composite functional layer is 10-60 parts by weight, and the content of the porous conductive layer is 1-10 parts by weight.
4. The water-volt nano-power generation fabric material according to any one of claims 1-3, characterized in that, In the composite functional layer, the mass ratio of graphene oxide to sodium polystyrene sulfonate is 1:0.1-10, preferably 1:0.25-4.
5. The water-volt nano-power generation fabric material according to any one of claims 1-3, characterized in that, The hydrophilic fiber substrate is selected from at least one of cleanroom fabrics, natural fibers, modified synthetic fibers, and blended fabrics; and / or The cationic polymer layer is selected from at least one of polyethyleneimine, polydiallyldimethylammonium chloride, and polyacrylamide-copoly-dimethyldiallylammonium chloride; and / or The porous conductive layer contains at least one of carbon black, carbon nanotubes, and conductive polymer materials.
6. A method for preparing a water-voltaic nanofiber power generation fabric material, characterized in that, The method includes the following steps: (1) The hydrophilic fiber substrate is immersed in a solution containing a cationic polymer to form a cationic polymer layer on both sides of the hydrophilic fiber substrate; (2) The material obtained in step (1) is immersed in a mixture containing graphene oxide and sodium polystyrene sulfonate to form a composite functional layer on the surface of the cationic polymer layer; (3) The material obtained in step (2) is immersed in a mixture containing porous conductive material to form a porous conductive layer in the composite functional layer.
7. The method according to claim 6, characterized in that, In step (1), the mass ratio of the hydrophilic fiber substrate to the cationic polymer is 1:0.5-2; Preferably, the concentration of the solution containing the cationic polymer is 10-50 g / L; Preferably, the cationic polymer is selected from at least one of polyethyleneimine, polydiallyldimethylammonium chloride, and polyacrylamide-copolymer-dimethyldiallylammonium chloride; Preferably, the hydrophilic fiber substrate is selected from at least one of cleanroom fabric, natural fiber, modified synthetic fiber, and blended fabric.
8. The method according to claim 6 or 7, characterized in that, The mass ratio of the hydrophilic fiber substrate to the total amount of graphene oxide and sodium polystyrene sulfonate is 1:0.1-0.6; and / or In the mixture containing graphene oxide and sodium polystyrene sulfonate, the mass ratio of graphene oxide to sodium polystyrene sulfonate is 1:0.1-10, preferably 1:0.25-4.
9. The method according to any one of claims 6-8, characterized in that, The mass ratio of the hydrophilic fiber substrate to the porous conductive material is 1:0.01-0.1; Preferably, the porous conductive material is selected from at least one of carbon black, carbon nanotubes, and conductive polymer materials; Preferably, the mixture containing the porous conductive material further contains a dispersant, and the mass ratio of the conductive material to the dispersant is 1:1-5; More preferably, the dispersant is selected from at least one of sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, and hexadecyltrimethylammonium bromide.
10. The method according to any one of claims 6-9, characterized in that, In step (1), the impregnation conditions include: a temperature of 40-80°C and a time of 0.5-2 hours; and / or In step (2), the impregnation conditions include: a temperature of 20-40°C and a time of 5-60 min; and / or In step (3), the conditions for impregnation include: a temperature of 20-40°C and a time of 5-60 min.
11. A water-voltaic nanofiber fabric material prepared by the method according to any one of claims 6-10.
12. The application of the water-voltaic nano-powered fabric material according to any one of claims 1-5 and 11 in the preparation process of flexible self-powered devices.