High-flame-retardant wear-resistant mine plastic coated cloth and preparation method thereof
By grafting molybdate-type polyimidazolium onto the surface of alumina, a modified alumina with wear resistance, antistatic properties, and smoke suppression was prepared. This modified alumina was then differentially configured into a flexible flame-retardant anchoring layer and a highly wear-resistant flame-retardant layer, solving the problem of unstable interfacial bonding in mining plastic coated fabrics and achieving excellent comprehensive performance.
Patent Information
- Application Number
- CN202611320756.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
AI Technical Summary
In existing mining plastic coated fabrics, there is a lack of stable interfacial bonding between wear-resistant fillers, flame retardants, and antistatic components, which leads to easy detachment of hard alumina and loss of antistatic agents. Furthermore, a single formulation is insufficient to maintain long-term wear resistance and antistatic properties.
Modified alumina with wear resistance, antistatic properties and smoke suppression functions was prepared by grafting molybdate-type polyimidazolium onto the surface of alumina. It was then incorporated into a flexible flame-retardant anchoring layer and a high wear-resistant flame-retardant layer in a differentiated manner. Through continuous coating and plasticizing, a stable interfacial bond was formed.
It improves the dispersibility and interfacial bonding of alumina in PVC coatings, reduces particle shedding and ionic component migration during abrasion, maintains low surface resistance of the coated fabric after immersion in water and abrasion, and has excellent abrasion resistance, antistatic durability, interlayer adhesion, flame retardancy and smoke suppression.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of mining polymer composite materials technology, and in particular to a highly flame-retardant and wear-resistant mining plastic coated fabric and its preparation method. Background Technology
[0002] Mining-grade plastic-coated fabric typically uses polyester fiber fabric as the base, coated with polyvinyl chloride paste resin, and then gelled, plasticized, and cooled to set. It is widely used in mine ventilation ducts, air-sealing facilities, and protective tarpaulins. Due to the presence of equipment friction, dust erosion, and potential ignition sources in the mining environment, the coated fabric, in addition to good adhesion and flexibility to the base fabric, must also possess flame-retardant, abrasion-resistant, and antistatic properties. Existing research mainly improves coating toughness by adding nitrile rubber, enhances abrasion resistance by using inorganic fillers such as alumina and calcium carbonate, and improves flame-retardant and antistatic properties by incorporating phosphorus-containing flame retardants, nitrogen-containing flame retardants, stannates, conductive carbon black, or quaternary ammonium salt antistatic agents. Some technologies also employ multi-layer coating structures, adjusting the formulation and thickness of each coating to improve the adhesion and surface protection properties of the base fabric.
[0003] However, in existing technologies, wear-resistant fillers, flame retardants, and antistatic components are typically directly mixed into PVC coatings as independent powders or small-molecule additives, lacking stable interfacial bonds between the components. Hard alumina has poor compatibility with flexible resin matrices, easily becoming stress concentration points and detaching from the coating under friction; migrating antistatic agents may be lost due to heat, water immersion, or continuous wear, leading to a gradual increase in surface resistance. Molybdate and other smoke-suppressing components, when added directly, are prone to agglomeration or migration, making it difficult to maintain a uniform distribution around the wear-resistant particles. Furthermore, while increasing hard fillers improves surface wear resistance with a single, uniform formulation, it easily reduces the wettability, interlayer adhesion, and flexural properties of the base fabric; reducing fillers makes it difficult to maintain long-term wear resistance and antistatic properties after wear. Therefore, how to stably combine wear-resistant particles, fixed ionic components, and smoke-suppressing components, and differentiate their distribution according to the different functions of the anchoring layer and the surface wear-resistant layer, is a core technical problem that needs to be solved for mining plastic coated fabrics. Summary of the Invention
[0004] To address the aforementioned problems, this invention proposes a highly flame-retardant and wear-resistant mining plastic-coated fabric and its preparation method. By grafting molybdate-type polyimidazolium onto the surface of double-bonded alumina, a modified alumina with wear resistance, antistatic properties, and smoke suppression is obtained. This modified alumina is then differentially incorporated into a flexible flame-retardant anchoring layer and a highly wear-resistant and flame-retardant layer. Through continuous coating and plasticizing composite processes, a mining plastic-coated fabric with excellent comprehensive performance is obtained.
[0005] This invention can be achieved through the following technical solutions: A method for preparing a highly flame-retardant and wear-resistant mining plastic-coated fabric includes the following steps: S1. Acetonitrile, 1-vinylimidazolium and 2-bromoethanol are added to a flask and mixed to carry out a quaternization reaction. The resulting imidazolium bromide is prepared into an aqueous solution and subjected to anion exchange to obtain imidazolium hydroxide. Molybdenum acid is added at a molar ratio of imidazolium hydroxide to molybdate at 2:1 to carry out the reaction. The pH of the reaction endpoint is controlled at 6.5-7.2 to obtain a monomer solution containing bis[1-vinyl-3-(2-hydroxyethyl)imidazolium]molybdate. S2. α-alumina is surface-treated with γ-aminopropyltriethoxysilane, and then the surface-treated α-alumina is reacted with glycidyl methacrylate to obtain alumina with polymerizable double bonds on the surface. S3. Using 100 parts by weight of the alumina obtained in S2 as a reference, under the condition of free radical initiator, 6-12 parts by weight of bis[1-vinyl-3-(2-hydroxyethyl)imidazolium]molybdate (based on the effective component) in the monomer solution obtained in S1 are grafted onto the surface of alumina and then subjected to filtration, washing and drying to obtain molybdate-type polyimidazolium modified alumina. S4. Prepare flexible flame-retardant anchoring layer coating material and high abrasion-resistant flame-retardant layer coating material respectively; based on 100 parts by weight of polyvinyl chloride paste resin contained in each of the two coating materials, the amount of modified alumina in the flexible flame-retardant anchoring layer coating material is 1-4 parts, and the amount of modified alumina in the high abrasion-resistant flame-retardant layer coating material is 8-15 parts; coat the flexible flame-retardant anchoring layer coating material on both sides of the polyester fiber base fabric, pre-gel at 130-150℃ for 30-90 s, then coat the high abrasion-resistant flame-retardant layer coating material, plasticize and melt at 165-185℃ for 1-3 min, and cool and solidify to obtain a high flame-retardant and abrasion-resistant mining plastic coated fabric.
[0006] Preferably, the molar ratio of 1-vinylimidazole to 2-bromoethanol is 1:(1.02-1.08), the quaternization reaction temperature is 55-70℃, and the reaction time is 12-24 h; the anion exchange is carried out using an OH-type strong basic anion exchange resin, and the exchange temperature is 0-5℃.
[0007] Preferably, the particle size D50 of the α-alumina is 2-6 μm; based on 100 parts by weight of α-alumina, the amount of γ-aminopropyltriethoxysilane is 2-5 parts; the surface treatment is carried out in an ethanol aqueous solution with a pH of 4.5-5.5, at a treatment temperature of 70-80°C, and for a treatment time of 3-5 h.
[0008] Preferably, in step S2, based on 100 parts by weight of α-alumina treated with γ-aminopropyltriethoxysilane, the amount of glycidyl methacrylate is 1.5 to 4 parts; the glycidyl methacrylate and the surface-treated α-alumina are reacted in isopropanol at a reaction temperature of 50 to 65°C for a reaction time of 4 to 8 hours.
[0009] Preferably, in step S3, based on 100 parts by weight of alumina containing polymerizable double bonds on its surface, the amount of free radical initiator is 0.05 to 0.20 parts; the free radical initiator is ammonium persulfate, and the graft polymerization is carried out at 55 to 65°C for 4 to 8 hours under nitrogen protection.
[0010] Preferably, the molybdate-type polyimidazolium-modified alumina obtained in S3 has a molybdate content of 0.8% to 2.5% by mass, and the particle size D50 of the modified alumina is 3 to 7 μm.
[0011] Preferably, in step S4, based on 100 parts by weight of polyvinyl chloride paste resin, the flexible flame-retardant anchoring layer coating material further includes the following raw materials in parts by weight: 8-15 parts of powdered nitrile rubber, 25-40 parts of polyester plasticizer, 8-15 parts of isopropyltriphenyl phosphate, 8-16 parts of melamine polyphosphate, 3-8 parts of zinc hydroxystannate, 2-4 parts of conductive carbon black, 2-5 parts of epoxidized soybean oil, and 2-4 parts of calcium-zinc composite stabilizer.
[0012] Preferably, in step S4, based on 100 parts by weight of polyvinyl chloride paste resin, the high wear-resistant and flame-retardant coating material further includes the following raw materials in parts by weight: 15-25 parts of powdered nitrile rubber, 20-32 parts of polyester plasticizer, 5-10 parts of isopropyltriphenyl phosphate, 6-12 parts of melamine polyphosphate, 2-5 parts of zinc hydroxystannate, 2-5 parts of conductive carbon black, 2-5 parts of epoxidized soybean oil, 2-4 parts of calcium-zinc composite stabilizer, and 0.3-1.5 parts of calcium stearate.
[0013] Preferably, the mass fraction of acrylonitrile in the powdered nitrile rubber is 26% to 33%; the polyester plasticizer is a condensation product of adipic acid and 1,4-butanediol, with a number average molecular weight of 1500 to 3000.
[0014] Preferably, the unit area mass of the polyester fiber base fabric is 150-300 g / m2; the thickness of the flexible flame-retardant anchoring layer on each side of the polyester fiber base fabric is 0.10-0.25 mm, and the thickness of the high abrasion-resistant flame-retardant layer is 0.15-0.35 mm; in S4, after the flexible flame-retardant anchoring layer is pre-gelled, its surface temperature is kept not lower than 80°C, and the high abrasion-resistant flame-retardant coating material is applied within 60 s.
[0015] The beneficial effects of this invention are: This invention does not simply combine alumina, antistatic agents, and molybdenum-based smoke suppressants. Instead, it first introduces polymerizable double bonds onto the alumina surface, and then grafts vinylimidazolium monomers with molybdate as the para-anion onto the alumina surface in situ. This results in a stable composite functional particle formed by the wear-resistant inorganic core, ionicly conductive groups, and molybdenum-based smoke suppressant components. This grafting structure improves the dispersibility and interfacial bonding of alumina in PVC coatings, reduces particle shedding during abrasion, and ionic component migration during immersion in water. This reduces abrasion losses while maintaining a low surface resistance after immersion and repeated abrasion. The molybdate groups are fixed in the polyimidazolium graft layer, and during combustion, they synergistically promote char layer formation and suppress smoke release with phosphorus-containing flame retardants, nitrogen-containing flame retardants, and zinc hydroxystannate, achieving a smoke suppressant effect exceeding that of individual abrasion-resistant or antistatic modifications. Furthermore, this invention incorporates a smaller amount of modified alumina into the flexible flame-retardant anchoring layer to maintain the coating's flexibility and its adhesion strength to the base fabric, while a larger amount of modified alumina is incorporated into the highly abrasion-resistant flame-retardant layer to concentrate its abrasion resistance, durable antistatic properties, and flame-retardant and smoke-suppressing effects. Continuous hot coating and plasticizing after pre-gelling ensure a strong bond between the inner and outer coatings. Thus, the specific grafting method of the modified alumina, the differentiated configuration of the inner and outer layers, and the continuous layering process mutually constrain and work together, balancing abrasion resistance, durable antistatic properties, interlayer adhesion, flame retardancy, and smoke suppression. This avoids the migration, loss, interface weakening, and performance sacrifices caused by simply stacking conventional functional additives. Detailed Implementation
[0016] The following provides a detailed description of the embodiments of the present invention: These embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation methods and processes. However, the scope of protection of the present invention is not limited to the following embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions.
[0017] Example 1: A method for preparing a high flame-retardant and wear-resistant mining plastic-coated fabric, comprising the following steps: S1. Add 100 mL of acetonitrile, 9.41 g of 1-vinylimidazole, and 12.75 g of 2-bromoethanol to a flask and stir at 55 °C for 12 h. After the reaction is complete, remove the acetonitrile under reduced pressure and wash with ethyl acetate to obtain imidazolium bromide. Prepare a 15% aqueous solution of the obtained imidazolium bromide and pass it through 120 mL of OH-type D201 strong basic anion exchange resin at 0 °C. Collect the exchange solution to obtain an imidazolium hydroxide solution. Add molybdate at a molar ratio of imidazolium hydroxide to molybdate of 2:1 and stir for 2 h. Control the pH of the reaction endpoint to 6.5, and then add water to adjust the mass fraction of bis[1-vinyl-3-(2-hydroxyethyl)imidazolium]molybdate to 20% to obtain a monomer solution. S2. Take 100 g of α-alumina with a particle size D50 of 2 μm, disperse it in a mixture of 950 mL of ethanol and 50 mL of deionized water, add 2 g of γ-aminopropyltriethoxysilane, adjust the pH to 4.5 with acetic acid, stir and react at 70 °C for 3 h, filter, wash with ethanol and dry at 70 °C for 8 h to obtain aminated alumina; take 100 g of aminated alumina and disperse it in 500 mL of isopropanol, add 1.5 g of glycidyl methacrylate, react at 50 °C for 4 h, filter, wash with isopropanol and vacuum dry at 60 °C for 12 h to obtain alumina with polymerizable double bonds on the surface; S3. Take 100 g of the alumina obtained from S2 and disperse it in a mixture of 640 mL of deionized water and 160 mL of ethanol. Add the monomer solution obtained from S1 containing 6 g of active ingredient, stir and disperse for 20 min, and then purge with nitrogen for 30 min. Add 0.05 g of ammonium persulfate and perform graft polymerization at 55 °C for 4 h. After the reaction is complete, filter the solution, wash it three times with deionized water and twice with ethanol, and then vacuum dry it at 70 °C for 12 h to obtain molybdate-type polyimidazolium-modified alumina. The mass fraction of Mo in the obtained modified alumina is 0.8%, and the particle size D50 is 3 μm. S4, the flexible flame-retardant anchoring layer coating material comprises the following raw materials in parts by weight: 100 parts polyvinyl chloride paste resin, 8 parts powdered nitrile rubber, 25 parts polyester plasticizer, 8 parts isopropylated triphenyl phosphate, 8 parts melamine polyphosphate, 3 parts zinc hydroxystannate, 1 part modified alumina obtained from S3, 2 parts conductive carbon black, 2 parts epoxidized soybean oil, and 2 parts calcium-zinc composite stabilizer; the high wear-resistant flame-retardant layer coating material comprises the following raw materials in parts by weight: 100 parts polyvinyl chloride paste resin, 15 parts powdered nitrile rubber, 20 parts polyester plasticizer, 5 parts isopropylated triphenyl phosphate, 6 parts melamine polyphosphate, 2 parts zinc hydroxystannate, 8 parts modified alumina obtained from S3, 2 parts conductive carbon black, 2 parts epoxidized soybean oil, 2 parts calcium-zinc composite stabilizer, and 0.3 parts calcium stearate; the liquid components of the two coating materials are mixed separately, and then polyvinyl chloride paste resin and the remaining powder raw materials are added, and stirred at 800 r / min for 20 minutes. The material was vacuum degassed at -0.09 MPa for 15 min; a polyester fiber base fabric with a unit area mass of 150 g / m2 was used, and a flexible flame-retardant anchoring layer coating was applied to both sides of the base fabric, with the thickness of the anchoring layer on each side controlled to be 0.10 mm. It was pre-gelled at 130℃ for 30 s; the surface temperature of the anchoring layer was kept not lower than 80℃, and a high abrasion-resistant flame-retardant layer coating was applied to its surface within 60 s, with the thickness of the high abrasion-resistant flame-retardant layer on each side controlled to be 0.15 mm. Then it was plasticized and melted at 165℃ for 1 min, and after cooling and shaping, a mining plastic coated fabric was obtained; the acrylonitrile mass fraction of the powdered nitrile rubber used was 26%, and the polyester plasticizer was an adipic acid-1,4-butanediol condensate with a number average molecular weight of 1500.
[0018] Example 2: A method for preparing a high flame-retardant and wear-resistant mining plastic-coated fabric, comprising the following steps: S1. Add 100 mL of acetonitrile, 9.41 g of 1-vinylimidazolium and 13.12 g of 2-bromoethanol to a flask, and stir the mixture at 62.5 °C for 18 h. Perform solvent removal and washing according to the method in Example 1, and prepare a 15% (w / w) aqueous solution of the obtained imidazolium bromide. Pass the solution through 120 mL of OH-type D201 strong basic anion exchange resin at 2.5 °C. Add molybdenum acid at a molar ratio of imidazolium hydroxide to molybdenum acid of 2:1, stir the mixture for 2 h, control the final pH of the reaction at 6.85, and then add water to adjust the target monomer mass fraction to 20% to obtain the monomer solution. S2. Take 100 g of α-alumina with a particle size D50 of 4 μm, disperse it in a mixture of 950 mL of ethanol and 50 mL of deionized water, add 3.5 g of γ-aminopropyltriethoxysilane, adjust the pH to 5.0 with acetic acid, and react at 75 °C for 4 h. After filtration, washing and drying, obtain aminated alumina. Take 100 g of aminated alumina, disperse it in 500 mL of isopropanol, add 2.75 g of glycidyl methacrylate, and react at 57.5 °C for 6 h. After filtration, washing and drying, obtain alumina with polymerizable double bonds on the surface. S3. Take 100 g of the alumina obtained from S2 and disperse it in a mixture of 640 mL of deionized water and 160 mL of ethanol. Add the monomer solution obtained from S1 containing 9 g of active ingredient, stir and disperse for 20 min, and then purge with nitrogen for 30 min. Add 0.125 g of ammonium persulfate and graft polymerize at 60 °C for 6 h. After filtration, washing, and vacuum drying at 70 °C for 12 h, molybdate-type polyimidazolium-modified alumina is obtained. The mass fraction of Mo in the obtained modified alumina is 1.55%, and the particle size D50 is 5 μm. S4, the flexible flame-retardant anchoring layer coating material comprises the following raw materials in parts by weight: 100 parts polyvinyl chloride paste resin, 11.5 parts powdered nitrile rubber, 32.5 parts polyester plasticizer, 11.5 parts isopropyltriphenyl phosphate, 12 parts melamine polyphosphate, 5.5 parts zinc hydroxystannate, 2.5 parts modified alumina obtained from S3, 3 parts conductive carbon black, 3.5 parts epoxidized soybean oil, and 3 parts calcium-zinc composite stabilizer; the high wear-resistant flame-retardant layer coating material comprises the following raw materials in parts by weight. Materials: 100 parts polyvinyl chloride paste resin, 20 parts powdered nitrile rubber, 26 parts polyester plasticizer, 7.5 parts isopropyltriphenyl phosphate, 9 parts melamine polyphosphate, 3.5 parts zinc hydroxystannate, 11.5 parts S3-modified alumina, 3.5 parts conductive carbon black, 3.5 parts epoxidized soybean oil, 3 parts calcium-zinc composite stabilizer, and 0.9 parts calcium stearate; Mixed, stirred, and degassed according to the method in Example 1; using a unit area mass of 225... A polyester fiber base fabric with a density of g / m2 is coated with a flexible flame-retardant anchoring layer on both sides, with the thickness of the anchoring layer on each side controlled at 0.175 mm. The fabric is then pre-gelled at 140℃ for 60 s. The surface temperature of the anchoring layer is maintained at no less than 80℃, and a high abrasion-resistant flame-retardant layer is applied within 60 s, with the thickness of the high abrasion-resistant flame-retardant layer on each side controlled at 0.25 mm. Subsequently, the fabric is plasticized and melted at 175℃ for 2 min, and then cooled and shaped to obtain a mining plastic-coated fabric. The acrylonitrile mass fraction of the powdered nitrile rubber used is 29.5%, and the polyester plasticizer is an adipic acid-1,4-butanediol condensate with a number average molecular weight of 2250.
[0019] Example 3: A method for preparing a high flame-retardant and wear-resistant mining plastic-coated fabric, comprising the following steps: S1. Add 100 mL of acetonitrile, 9.41 g of 1-vinylimidazolium and 13.50 g of 2-bromoethanol to a flask and stir at 70 °C for 24 h. Remove the solvent and wash according to the method in Example 1, and prepare an aqueous solution of the obtained imidazolium bromide with a mass fraction of 15%. Pass the solution through 120 mL of OH-type D201 strong basic anion exchange resin at 5 °C. Add molybdenum acid at a molar ratio of imidazolium hydroxide to molybdenum acid of 2:1, stir and react for 2 h, control the pH of the reaction endpoint to 7.2, and then add water to adjust the target monomer mass fraction to 20% to obtain the monomer solution. S2. Take 100 g of α-alumina with a particle size D50 of 6 μm, disperse it in a mixture of 950 mL of ethanol and 50 mL of deionized water, add 5 g of γ-aminopropyltriethoxysilane, adjust the pH to 5.5 with acetic acid, react at 80 °C for 5 h, filter, wash and dry to obtain aminated alumina; take 100 g of aminated alumina, disperse it in 500 mL of isopropanol, add 4 g of glycidyl methacrylate, react at 65 °C for 8 h, filter, wash and dry to obtain alumina with polymerizable double bonds on the surface; S3. Take 100 g of the alumina obtained from S2 and disperse it in a mixture of 640 mL of deionized water and 160 mL of ethanol. Add the monomer solution obtained from S1 containing 12 g of active ingredient, stir and disperse for 20 min, and then purge with nitrogen for 30 min. Add 0.20 g of ammonium persulfate and graft polymerize at 65 °C for 8 h. After filtration, washing, and vacuum drying at 70 °C for 12 h, molybdate-type polyimidazolium-modified alumina is obtained. The mass fraction of Mo in the obtained modified alumina is 2.3%, and the particle size D50 is 7 μm. S4, the flexible flame-retardant anchoring layer coating material comprises the following raw materials in parts by weight: 100 parts polyvinyl chloride paste resin, 15 parts powdered nitrile rubber, 40 parts polyester plasticizer, 15 parts isopropylated triphenyl phosphate, 16 parts melamine polyphosphate, 8 parts zinc hydroxystannate, 4 parts modified alumina obtained in S3, 4 parts conductive carbon black, 5 parts epoxidized soybean oil, and 4 parts calcium-zinc composite stabilizer; the high wear-resistant flame-retardant layer coating material comprises the following raw materials in parts by weight: 100 parts polyvinyl chloride paste resin, 25 parts powdered nitrile rubber, 32 parts polyester plasticizer, 10 parts isopropylated triphenyl phosphate, 12 parts melamine polyphosphate, 5 parts zinc hydroxystannate, 15 parts modified alumina obtained in S3, 5 parts conductive carbon black, 5 parts epoxidized soybean oil, 4 parts calcium-zinc composite stabilizer, and 1.5 parts calcium stearate; mixed, stirred, and degassed according to the method of Example 1; using a unit area mass of 300 A polyester fiber base fabric with a density of g / m2 is coated with a flexible flame-retardant anchoring layer on both sides, with the thickness of the anchoring layer on each side controlled at 0.25 mm. The fabric is then pre-gelled at 150℃ for 90 s. The surface temperature of the anchoring layer is maintained at no less than 80℃, and a high abrasion-resistant flame-retardant layer is applied within 60 s, with the thickness of the high abrasion-resistant flame-retardant layer on each side controlled at 0.35 mm. Subsequently, the fabric is plasticized and melted at 185℃ for 3 min, and then cooled and shaped to obtain a mining plastic-coated fabric. The acrylonitrile mass fraction of the powdered nitrile rubber used is 33%, and the polyester plasticizer is an adipic acid-1,4-butanediol condensate with a number average molecular weight of 3000.
[0020] Comparative Example 1: The difference between this comparative example and Example 1 is that α-alumina without surface double bond modification and molybdate-type polyimidazolium graft modification is used to replace the modified alumina in Example 1 by the same mass.
[0021] The preparation method of the plastic-coated fabric in this comparative example includes the following steps: S1. By weight, 100 parts of polyvinyl chloride paste resin, 8 parts of nitrile rubber, 25 parts of polyester plasticizer, 8 parts of isopropyltriphenyl phosphate, 8 parts of melamine polyphosphate, 3 parts of zinc hydroxystannate, 1 part of α-alumina, 2 parts of conductive carbon black, 2 parts of epoxidized soybean oil, and 2 parts of calcium-zinc composite stabilizer are added to a mixing device; wherein, the α-alumina is not silanized, double-bonded, or polyimidazolium grafted, and its D50 is 3 μm; the mixture is stirred at 800 r / min for 20 min, and then vacuum degassed at -0.09 MPa for 15 min to obtain a flexible flame-retardant anchoring layer coating material; S2. By weight, add 100 parts of polyvinyl chloride paste resin, 15 parts of nitrile rubber, 20 parts of polyester plasticizer, 5 parts of isopropyltriphenyl phosphate, 6 parts of melamine polyphosphate, 2 parts of zinc hydroxystannate, 8 parts of α-alumina, 2 parts of conductive carbon black, 2 parts of epoxidized soybean oil, 2 parts of calcium-zinc composite stabilizer and 0.3 parts of calcium stearate to a mixing device, stir at 800 r / min for 20 min, and then degas under vacuum at -0.09 MPa for 15 min to obtain a high wear-resistant and flame-retardant coating material. S3. Select a polyester fiber base fabric with a unit area mass of 150 g / m2. Apply a flexible flame-retardant anchoring layer coating material to both sides of the polyester fiber base fabric to form a flexible flame-retardant anchoring layer with a thickness of 0.10 mm on each side. Then, pre-gel at 130℃ for 30 s. After pre-geling, keep the coating surface temperature not lower than 80℃, and apply a high abrasion-resistant flame-retardant layer coating material to the surface of the flexible flame-retardant anchoring layer on both sides within 60 s to form a high abrasion-resistant flame-retardant layer with a thickness of 0.15 mm on each side. Finally, plasticize at 165℃ for 1 min, cool, and roll up to obtain a mining plastic-coated fabric.
[0022] Comparative Example 2: The difference between this comparative example and Example 1 is that the molybdate-type polyimidazolium and α-alumina are only physically mixed, and double bonds are not introduced on the surface of alumina through silane coupling agent and glycidyl methacrylate, nor is a polyimidazolium layer formed in situ on the surface of alumina.
[0023] The preparation method of the plastic-coated fabric in this comparative example includes the following steps: S1. Perform the operation as described in S1 of Example 1, that is, using 1-vinylimidazolium and 2-bromoethanol as raw materials, and through quaternization, hydroxide-type anion exchange and molybdate neutralization reaction, to prepare a bis[1-vinyl-3-(2-hydroxyethyl)imidazolium]molybdate monomer solution with an effective ingredient content of 20 wt%. S2. Take 30 g of molybdate-type imidazolium monomer solution, of which 6 g is the effective monomer component, and add it to a mixed solvent consisting of 640 mL of deionized water and 160 mL of ethanol. After stirring evenly, purge with nitrogen for 30 min. Add 0.05 g of ammonium persulfate and react at 55 °C for 4 h to allow the molybdate-type imidazolium monomer to polymerize. After the reaction, use a dialysis bag with a molecular weight cutoff of 3500 Da to dialyze with deionized water for 24 h, changing the deionized water every 4 h. Then freeze-dry to obtain free molybdate-type polyimidazolium. Determine the molybdenum content in the molybdate-type polyimidazolium using inductively coupled plasma atomic emission spectrometry (ICP-AES), and calculate the amount added based on the final physical composite molybdenum content of 0.8 wt%. When the molybdenum content in the molybdate-type polyimidazolium is 21.9 wt%, take 96.35 g of unmodified α-alumina with a D50 of 3 μm and 3.65 g of... g of molybdate-type polyimidazolium was mixed at 1000 r / min for 10 min to obtain physically composite alumina; S3. Replace the modified alumina in Example 1 with physical composite alumina of equal mass; in the flexible flame-retardant anchoring layer coating, add 1 part by weight of physical composite alumina for every 100 parts by weight of polyvinyl chloride paste resin; in the high wear-resistant flame-retardant layer coating, add 8 parts by weight of physical composite alumina for every 100 parts by weight of polyvinyl chloride paste resin; the other raw materials and their amounts in the two coatings are the same as in Example 1; stir each raw material at 800 r / min for 20 min, and then degas under vacuum at -0.09 MPa for 15 min to obtain the flexible flame-retardant anchoring layer coating and the high wear-resistant flame-retardant layer coating; S4. Perform the coating process according to Example 1: Coat both sides of a polyester fiber base fabric with a unit area mass of 150 g / m2 with a flexible flame-retardant anchoring layer coating material, so that the thickness of the anchoring layer on each side is 0.10 mm, and pre-gel at 130°C for 30s; keep the coating surface temperature not lower than 80°C, and coat with a high wear-resistant flame-retardant layer coating material within 60s, so that the thickness of the wear-resistant layer on each side is 0.15 mm; finally, plasticize at 165°C for 1 min, cool, and roll up to obtain a mining plastic coated fabric.
[0024] Comparative Example 3: The difference between this comparative example and Example 1 is that the 1 part by weight and 8 parts by weight of modified alumina used in Example 1 for the flexible flame-retardant anchoring layer and the high wear-resistant flame-retardant layer, respectively, are adjusted to 4.5 parts by weight in both layers, and the differentiated distribution of modified alumina between the inner and outer layers is eliminated; when each of the two coating materials is prepared with 100 parts by weight of polyvinyl chloride paste resin, the total amount of modified alumina added remains unchanged.
[0025] The preparation method of the plastic-coated fabric in this comparative example includes the following steps: S1. Following the procedures in S1 to S3 of Example 1, molybdate-type imidazolium monomer solution, double-bonded alumina, and molybdate-type polyimidazolium modified alumina are prepared sequentially; the resulting modified alumina has a molybdenum content of 0.8 wt% and a D50 of 3 μm; S2. By weight, add 100 parts of polyvinyl chloride paste resin, 8 parts of nitrile rubber, 25 parts of polyester plasticizer, 8 parts of isopropyltriphenyl phosphate, 8 parts of melamine polyphosphate, 3 parts of zinc hydroxystannate, 4.5 parts of modified alumina, 2 parts of conductive carbon black, 2 parts of epoxidized soybean oil, and 2 parts of calcium-zinc composite stabilizer to a mixing device, stir at 800 r / min for 20 min, and then degas under vacuum at -0.09 MPa for 15 min to obtain a flexible flame-retardant anchoring layer coating material; by weight, add 100 parts of polyvinyl chloride paste resin, 15 parts of nitrile rubber, 20 parts of polyester plasticizer, 5 parts of isopropyltriphenyl phosphate, 6 parts of melamine polyphosphate, 2 parts of zinc hydroxystannate, 4.5 parts of modified alumina, 2 parts of conductive carbon black, 2 parts of epoxidized soybean oil, 2 parts of calcium-zinc composite stabilizer, and 0.3 parts of calcium stearate to a mixing device, stir at 800 r / min for 20 min. min, then vacuum degassing at -0.09 MPa for 15 min to obtain a high wear-resistant and flame-retardant coating material; S3. Select a polyester fiber base fabric with a unit area mass of 150 g / m2. Apply a flexible flame-retardant anchoring layer coating material to both sides of the polyester fiber base fabric to form a flexible flame-retardant anchoring layer with a thickness of 0.10 mm on each side. Pre-gel at 130℃ for 30 s. Keep the coating surface temperature not lower than 80℃, and apply a high abrasion-resistant flame-retardant coating material to the surface of the flexible flame-retardant anchoring layer on both sides within 60 s to form a high abrasion-resistant flame-retardant layer with a thickness of 0.15 mm on each side. Finally, plasticize at 165℃ for 1 min, cool, and roll up to obtain a mining plastic-coated fabric.
[0026] Performance testing 1. Wear resistance The test was conducted according to GB / T 30314-2021 standard. Circular specimens with a diameter of 105 mm were cut from different locations along the sample. A mounting hole with a diameter of 6.35 mm was made in the center of each specimen. The initial mass m0 of the specimen was weighed, accurate to 0.1 mg. The specimen was mounted on the Taber abrasion tester with the high-wear-resistant and flame-retardant layer facing the grinding wheel. An H-18 grinding wheel was used, with a 1 kg load applied to each wheel at a rotation speed of 60 r / min for 1000 revolutions. After the test, the abrasion debris on the specimen surface was removed, and the specimen mass m1 was re-weighed. The abrasion mass loss was calculated using the following formula: Δm = m0 - m1; In the formula, Δm is the wear mass loss in mg; m0 is the mass before wear in mg; and m1 is the mass after wear in mg.
[0027] 2. Antistatic properties and their retention properties Tests were conducted in accordance with the MT 113-1995 standard.
[0028] Using brass inner cylindrical electrodes and concentric ring electrodes, the electrodes were placed on the surface of the high wear-resistant and flame-retardant layer of the sample. A DC voltage of 100 V was applied, and the surface resistance value was read after 60 s of energization. This value was recorded as the initial surface resistance R0.
[0029] Take another batch of samples and perform the following pretreatments respectively: (1) Water immersion pretreatment: The sample was completely immersed in deionized water at a temperature of 23±2℃ for 24 h. After taking it out, the surface was rinsed with deionized water and placed at a temperature of 23±2℃ and a relative humidity of 50±5% for 24 h. The surface resistance was measured according to the above method and recorded as the surface resistance Rw after immersion. (2) Wear pretreatment: The test was carried out in accordance with GB / T 19089-2012 standard. The surface of the high wear-resistant flame retardant layer was worn 20,000 times under a load of 12 kPa using a Martindale wear tester. After removing the wear debris and leaving it for 2 hours, the surface resistance was measured at the center of the wear area according to the above method and recorded as the surface resistance Ra after wear.
[0030] Record R0, Rw, and Ra respectively, and calculate the resistance increase factor after immersion in water Kw=Rw / R0 and the resistance increase factor after wear Ka=Ra / R0.
[0031] 3. Coating layer adhesion strength Tests were conducted according to HG / T 3052-2022 standard. Strip specimens with a length of not less than 200 mm and a width of 50 ± 0.5 mm were cut along both the warp and weft directions of the coated fabric, with five specimens in each direction. The coating layer was pre-separated from the polyester fiber base fabric by approximately 50 mm at one end of each specimen. The specimens were then clamped in the upper and lower fixtures of a universal testing machine and peeled at a speed of 100 mm / min. The average peel force within the stable peeling range was recorded. The adhesive strength of the coating layer in both the warp and weft directions was calculated, and the lower of the average values in both directions was taken as the adhesive strength of the coating layer for that group of samples.
[0032] Table 1. Test results of wear resistance, antistatic properties, and coating adhesion.
[0033] 4. Flame retardant properties Tests were conducted in accordance with GB / T 20105-2006 and MT 113-1995 standards. Six specimens, each 360 mm long and 50 mm wide, were cut from each set of coated fabric. The specimen thickness was the actual thickness of the coated fabric. The specimens were then vertically mounted in the combustion test chamber.
[0034] An ethanol-methanol mixture with a volume ratio of 95:5 was used as fuel. The flame temperature of the alcohol torch was controlled at 960±60℃ and the flame height at 150–180 mm. The torch was applied to the lower end of the sample for 30 seconds, and then removed. The flaming and flameless combustion times of each sample were recorded, and the arithmetic mean of the six samples was calculated. Simultaneously, the presence of continuous dripping, large-area peeling of the coating, and flame propagation of the base fabric was observed during combustion.
[0035] 5. Smoke suppression performance The test was conducted according to GB / T 16172-2026 standard. The coated fabric was cut into 100 mm × 100 mm samples. Using the high abrasion-resistant and flame-retardant layer as the exposed surface, the samples were laid flat on a non-combustible calcium silicate liner, and the sides and back of the samples were covered with aluminum foil to fully expose the exposed surface. The radiant heat flux density was set to 35 kW / m², and ignition was performed using an external igniter for 600 s. If the sample extinguished prematurely, recording continued until the smoke parameters stabilized. The total smoke release (TSR) during the sample's combustion process was recorded.
[0036] Table 2. Test results of flame retardant and smoke suppression performance
[0037] The test results show that the wear mass loss of Examples 1-3 was 64.8-112.6 mg, the initial surface resistivity was 2.6×10⁵-8.2×10⁵ Ω, and the resistance increase factors after immersion and wear treatment were only 1.31-1.46 and 1.58-1.95, respectively. This indicates that after the molybdate-type polyimidazolium is fixed on the alumina surface by in-situ polymerization, it not only improves the interfacial bonding between alumina and polyvinyl chloride coating, but also enables the ionic conductive sites to remain relatively stable after immersion and mechanical wear. The coating adhesion strength of Examples 1-3 reached 84-94 N / 50mm, the average flaming combustion time and the average flameless combustion time were 0.7-1.6 s and 1.2-3.1 s, respectively, and the total smoke release was 3.2-4.8 m2. This shows that by using less modified alumina in the flexible flame-retardant anchoring layer and more modified alumina in the high wear-resistant flame-retardant layer, the surface wear resistance, antistatic properties and flame-retardant and smoke-suppressing properties can be enhanced while maintaining the adhesion performance of the base fabric.
[0038] Compared with Example 1, in Comparative Example 1, after replacing modified alumina with unmodified alumina, the wear mass loss increased to 169.4 mg, the surface resistivity after wear increased to 1.4 × 10⁷ Ω, the coating adhesion strength decreased to 76 N / 50 mm, the total smoke release increased to 7.6 m², and the average flaming combustion time reached 3.5 s. This indicates that unmodified alumina is prone to loosening or falling off during the wear process due to insufficient interfacial bonding, and it cannot provide polyimidazolium conductive sites and molybdate smoke suppression effect. In Comparative Example 2, since the polyimidazolium and alumina are only physically combined, the surface resistivity increases to 6.2 × 10⁶ Ω and 8.3 × 10⁶ Ω after immersion in water and after wear, respectively, with resistance increases of 8.99 and 12.03 times. At the same time, the wear mass loss, coating adhesion strength and total smoke emission are significantly deteriorated. This proves that the effect achieved by the present invention does not come from a simple mixture of alumina, polyimidazolium and molybdate, but is directly related to the in-situ grafting and fixation of polyimidazolium on the surface of double-bonded alumina. In Comparative Example 3, after the modified alumina was evenly distributed in the two layers, the insufficient modified alumina in the wear-resistant layer increased the wear mass loss to 146.2 mg and the surface resistivity after wear to 7.6 × 10⁶ Ω. At the same time, the excessive modified alumina in the anchoring layer reduced the coating adhesion strength to 61 N / 50 mm and increased the total smoke emission to 5.7 m². This shows that the differentiated distribution of modified alumina in the inner and outer layers can simultaneously avoid the rigidity of the anchoring layer and the insufficient functional filler in the wear-resistant layer, thereby forming a coordinated technical effect of wear resistance, durable antistatic properties, interlayer adhesion, and flame retardancy and smoke suppression.
[0039] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a high flame-retardant and wear-resistant mining plastic-coated fabric, characterized in that, Includes the following steps: S1. Acetonitrile, 1-vinylimidazolium and 2-bromoethanol are added to a flask and mixed to carry out a quaternization reaction. The resulting imidazolium bromide is prepared into an aqueous solution and subjected to anion exchange to obtain imidazolium hydroxide. Molybdenum acid is added at a molar ratio of imidazolium hydroxide to molybdate at 2:1 to carry out the reaction. The pH of the reaction endpoint is controlled at 6.5-7.2 to obtain a monomer solution containing bis[1-vinyl-3-(2-hydroxyethyl)imidazolium]molybdate. S2. α-alumina is surface-treated with γ-aminopropyltriethoxysilane, and then the surface-treated α-alumina is reacted with glycidyl methacrylate to obtain alumina with polymerizable double bonds on the surface. S3. Using 100 parts by weight of the alumina obtained in S2 as a reference, under the condition of free radical initiator, 6-12 parts by weight of bis[1-vinyl-3-(2-hydroxyethyl)imidazolium]molybdate (based on the effective component) in the monomer solution obtained in S1 are grafted onto the surface of alumina and then subjected to filtration, washing and drying to obtain molybdate-type polyimidazolium modified alumina. S4. Prepare flexible flame-retardant anchoring layer coating material and high wear-resistant flame-retardant layer coating material respectively; based on 100 parts by weight of polyvinyl chloride paste resin contained in each of the two coating materials, the amount of modified alumina in the flexible flame-retardant anchoring layer coating material is 1 to 4 parts, and the amount of modified alumina in the high wear-resistant flame-retardant layer coating material is 8 to 15 parts. Flexible flame-retardant anchoring layer coating is applied to both sides of polyester fiber base fabric, pre-gelled at 130-150℃ for 30-90 s, then coated with high abrasion-resistant flame-retardant layer coating, plasticized and melted at 165-185℃ for 1-3 min, and cooled and shaped to obtain high flame-retardant and abrasion-resistant mining plastic coated fabric.
2. The preparation method of the high flame-retardant and wear-resistant mining plastic coated fabric according to claim 1, characterized in that, The molar ratio of 1-vinylimidazole to 2-bromoethanol is 1:(1.02-1.08), the quaternization reaction temperature is 55-70℃, and the reaction time is 12-24 h; the anion exchange is carried out using an OH-type strong basic anion exchange resin, and the exchange temperature is 0-5℃.
3. The method for preparing the high flame-retardant and wear-resistant mining plastic coated fabric according to claim 1, characterized in that, The particle size D50 of the α-alumina is 2-6 μm; based on 100 parts by weight of α-alumina, the amount of γ-aminopropyltriethoxysilane is 2-5 parts; the surface treatment is carried out in an ethanol aqueous solution with a pH of 4.5-5.5, at a treatment temperature of 70-80℃, and for a treatment time of 3-5 h.
4. The method for preparing the high flame-retardant and wear-resistant mining plastic-coated fabric according to claim 1, characterized in that, In step S2, based on 100 parts by weight of α-alumina treated with γ-aminopropyltriethoxysilane, the amount of glycidyl methacrylate is 1.5 to 4 parts; the glycidyl methacrylate and the surface-treated α-alumina are reacted in isopropanol at a reaction temperature of 50 to 65°C for 4 to 8 hours.
5. The method for preparing high flame-retardant and wear-resistant mining plastic coated fabric according to claim 1, characterized in that, In S3, based on 100 parts by weight of alumina with polymerizable double bonds on its surface, the amount of free radical initiator is 0.05 to 0.20 parts; the free radical initiator is ammonium persulfate, and the graft polymerization is carried out at 55 to 65°C for 4 to 8 hours under nitrogen protection.
6. The method for preparing the high flame-retardant and wear-resistant mining plastic-coated fabric according to claim 1, characterized in that, The molybdate-type polyimidazolium-modified alumina obtained by S3 has a molybdate element mass fraction of 0.8% to 2.5% and a particle size D50 of 3 to 7 μm.
7. The method for preparing the high flame-retardant and wear-resistant mining plastic coated fabric according to claim 1, characterized in that, In step S4, based on 100 parts by weight of polyvinyl chloride paste resin, the flexible flame-retardant anchoring layer coating material also includes the following raw materials in parts by weight: 8-15 parts of powdered nitrile rubber, 25-40 parts of polyester plasticizer, 8-15 parts of isopropyltriphenyl phosphate, 8-16 parts of melamine polyphosphate, 3-8 parts of zinc hydroxystannate, 2-4 parts of conductive carbon black, 2-5 parts of epoxidized soybean oil, and 2-4 parts of calcium-zinc composite stabilizer.
8. The method for preparing the high flame-retardant and wear-resistant mining plastic coated fabric according to claim 1, characterized in that, In S4, based on 100 parts by weight of polyvinyl chloride paste resin, the high wear-resistant and flame-retardant coating material also includes the following raw materials in parts by weight: 15-25 parts of powdered nitrile rubber, 20-32 parts of polyester plasticizer, 5-10 parts of isopropyltriphenyl phosphate, 6-12 parts of melamine polyphosphate, 2-5 parts of zinc hydroxystannate, 2-5 parts of conductive carbon black, 2-5 parts of epoxidized soybean oil, 2-4 parts of calcium-zinc composite stabilizer, and 0.3-1.5 parts of calcium stearate.
9. The method for preparing the high flame-retardant and wear-resistant mining plastic-coated fabric according to claim 8, characterized in that, The mass fraction of acrylonitrile in the powdered nitrile rubber is 26% to 33%; the polyester plasticizer is a condensation product of adipic acid and 1,4-butanediol, with a number average molecular weight of 1500 to 3000.
10. The method for preparing the high flame-retardant and wear-resistant mining plastic-coated fabric according to claim 1, characterized in that, The unit area mass of the polyester fiber base fabric is 150-300 g / m2; the thickness of the flexible flame-retardant anchoring layer on each side of the polyester fiber base fabric is 0.10-0.25 mm, and the thickness of the high abrasion-resistant flame-retardant layer is 0.15-0.35 mm; in S4, after the flexible flame-retardant anchoring layer is pre-gelled, its surface temperature is kept not lower than 80℃, and the high abrasion-resistant flame-retardant coating material is applied within 60 s.