Preparation method of home-use flocked high-stain-resistant synthetic leather

By using a closed isocyanate main crosslinking system and temperature-sensitive catalyst microcapsule technology, molecular-level bonding between fibers and adhesive layers is achieved, solving the problems of stain penetration and mold growth at the fiber roots in flocked synthetic leather, improving stain resistance and flocking fastness, while maintaining the fabric's softness.

CN123133192APending Publication Date: 2026-11-20ZHEJIANG HEXIN NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611030148.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing flocked synthetic leather has problems with stain penetration and mold growth caused by micro-gaps at the fiber roots when used in home furnishings. Conventional stain-resistant technologies cannot completely solve this problem and may increase production costs and defect rates.

Method used

By employing a closed isocyanate main crosslinking system and temperature-sensitive catalyst microcapsule technology, molecular-level bonding between fibers and adhesive layers is achieved through covalent crosslinking and targeted pore sealing, thereby blocking capillary permeation channels.

Benefits of technology

It effectively prevents stain penetration and mold growth, improves flocking fastness, reduces the risk of shedding, and maintains the fabric's softness and stain resistance for a long time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123133192A_ABST
    Figure CN123133192A_ABST
Patent Text Reader

Abstract

The application relates to the field of synthetic leather technology, in particular to a preparation method of a home flocked high-stain-resistant synthetic leather, and specifically comprises the following steps: pre-activation and modification are carried out on flocked fibers to obtain modified fibers; an adhesive based on a closed isocyanate main crosslinking system is prepared into microcapsules containing catalysts and microcapsules of pore sealing agents; a base is pretreated, then the adhesive and the modified fibers are used for coating and electrostatic flocking to obtain a semi-finished product; the semi-finished product is placed and pre-dried to promote the migration of the microcapsules to the root of the modified fibers; the semi-finished product after the migration and enrichment is crosslinked, sealed and cured, and then is finished to obtain a flocked synthetic leather product, so that the stain resistance of the fiber root and the adhesive interface is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of synthetic leather technology, and in particular to a method for preparing flocked, highly stain-resistant synthetic leather for home use. Background Technology

[0002] Flocked synthetic leather is the mainstream base material for sofa fabrics, background wall upholstery, wall decoration fabrics and home textiles in home settings. However, in daily life, the fabric inevitably comes into frequent contact with various liquid pollutants such as red wine, soy sauce, coffee, sweat stains and pet stains. Ordinary flocked synthetic leather has problems such as weak stain resistance, easy penetration of stains, difficulty in cleaning, and easy mold and blackening after long-term use.

[0003] Stain-resistant synthetic leather is usually achieved by applying a stain-resistant coating to the surface. For example, the stain-resistant and anti-graffiti semi-silicone synthetic leather and its manufacturing process, which is announced in CN115157818B, is a three-layer composite structure consisting of a base fabric layer, a polymer layer, and an organosilicon film layer. The organosilicon chain segments are intertwined with the polyurethane or polyvinyl chloride molecular chains by the swelling effect of cyclohexanone on the polymer layer.

[0004] The flocked fiber itself can also be modified to be stain-resistant. For example, a wear-resistant composite flocked fabric and its preparation method can be referred to in CN117166263B. A two-component system composed of modified wax emulsion and modified organosilicon emulsion is used to impregnate and finish nylon and viscose flocked fibers. The reaction of phenylboronic acid and hydroxyl groups generates borate ester covalent bonds, which firmly bond the hydrophobic and stain-resistant components to the fiber surface. After baking, a dense stain-resistant wax film is formed.

[0005] However, the above-mentioned stain-resistant technologies only target the hydrophobic stain resistance of the fiber body and the surface of synthetic leather. Electrostatic flocking, on the other hand, involves vertically implanting fibers into the surface of a base fabric coated with adhesive, followed by baking and curing to fix the fibers. However, due to factors such as adhesive leveling properties, uniform fiber implantation depth, and shrinkage of the cured adhesive layer, micron-sized annular micro-gaps of 5-20 μm inevitably form between the fiber roots and the adhesive. In a home setting, liquid stains can quickly penetrate into these micro-gaps through capillary action. Conventional surface wiping can only remove stains from the fiber surface and cannot reach the residual contaminants within these micro-gaps.

[0006] Long-term residue in the gaps at the root of the flocked leather can cause the root to turn black and moldy, producing an irritating odor and breeding bacteria and mold, which can harm the health of the indoor environment. Furthermore, stains and mold can accelerate the degradation of the adhesive layer, leading to a significant decrease in flocking strength and causing problems such as shedding and exposure of the substrate. If crude methods such as increasing the thickness of the adhesive coating or raising the baking temperature are used, it will not only increase the cost of raw materials and production energy consumption, but also easily cause problems such as glue penetration, flocking clumping and fabric hardening, resulting in an increase in the product defect rate and failing to fundamentally solve the problem of stain prevention at the fiber root and adhesive interface. Summary of the Invention

[0007] To better address the issue of stain resistance at the fiber root and adhesive interface, this application provides a method for preparing flocked, highly stain-resistant synthetic leather for home use.

[0008] The present application provides a method for preparing flocked, highly stain-resistant synthetic leather for home use, which adopts the following technical solution.

[0009] A method for preparing flocked, highly stain-resistant synthetic leather for home use includes the following steps.

[0010] S1. Pre-activate and modify the flocked fibers to obtain modified fibers;

[0011] S2. An adhesive containing catalyst microcapsules and sealing agent microcapsules was prepared based on a closed isocyanate main crosslinking system;

[0012] S3. Pre-treat the substrate, then apply adhesive and modified fibers for coating and electrostatic flocking to obtain a semi-finished product;

[0013] S4. Allow the semi-finished product to stand and pre-dry to promote the migration and enrichment of microcapsules into the roots of the modified fibers.

[0014] S5. The semi-finished product that has completed migration and enrichment is cross-linked, sealed, and cured, and then finished to obtain flocked synthetic leather product.

[0015] By adopting the above technical solution, the molecular-level bonding between the fiber and the adhesive layer is achieved through covalent cross-linking, thereby achieving targeted sealing of the root. This solves the industry problem that existing technologies can only achieve surface anti-fouling but cannot eradicate capillary penetration pollution at the fiber root, thus eliminating the problems of blackening, mold, and odor at the root caused by stain residue in home settings.

[0016] Optionally, the modifying liquid required for modification in S1 comprises, by weight: 5-9 parts of monovinyl-terminated polydimethylsiloxane, 2.5-4.5 parts of 4-vinylphenylboronic acid, 3-5 parts of octadecyl methacrylate, 1-3 parts of acrylamide, 2-3 parts of nonionic emulsifier, 0.0002-0.0004 parts of aqueous selective polymerization inhibitor, 0.3-0.5 parts of oxidant, 0.1-0.3 parts of reducing agent, 16-20 parts of anhydrous ethanol, 0.1-0.5 parts of glacial acetic acid, and 66-70 parts of deionized water.

[0017] By adopting the above technical solution, the dual hydrophobic backbone design of monovinyl-terminated polydimethylsiloxane and octadecyl methacrylate synergistically reduces the surface energy of the fiber, giving the fiber body superhydrophobic and stain-resistant properties. Common household stains such as red wine, soy sauce, coffee and sweat stains are not easy to adhere to, and surface stains can be removed by wiping with water without residue.

[0018] By introducing 4-vinylphenylboronic acid active monomers, crosslinkable groups are anchored on the fiber surface, which can then form covalent bonds with hydroxyl groups in the adhesive. This eliminates the inherent interface gaps between the fiber and the adhesive layer at the molecular level, reduces capillary penetration channels at the source, and significantly improves flocking fastness, thus reducing the risk of flocking during home use.

[0019] Nonionic emulsifiers and anhydrous ethanol construct a stable oil-in-water emulsion system. The weakly acidic formulation system inhibits the self-complexation of phenylboronic acid, ensuring the long-term stability of active groups.

[0020] The polymerization inhibitor system selectively suppresses the homopolymerization reaction of free monomers in the aqueous phase without affecting the heterogeneous grafting polymerization of active sites on the fiber surface. While reducing impurities in the homopolymer and improving the stability of the modified liquid, it maximizes the efficiency of the grafting reaction.

[0021] Optionally, the modified liquid is prepared by first mixing and stirring anhydrous ethanol, nonionic emulsifier, and monovinyl-terminated polydimethylsiloxane to form a pre-emulsion, then adding 4-vinylphenylboronic acid, octadecyl methacrylate, acrylamide, an aqueous selective polymerization inhibitor, and an oxidant and stirring. Then, glacial acetic acid is added to adjust the pH of the system to 5.5-6.0 to obtain the modified liquid base material. Before impregnation of the pre-activated flocked fibers, the modified liquid base material is heated to a predetermined temperature, and then a reducing agent is added and stirred.

[0022] By adopting the above technical solution, a uniform pre-emulsion is first prepared to ensure that the hydrophobic monomers are completely dispersed in the aqueous phase and to avoid uneven fiber modification caused by oil phase agglomeration. After heating to the reaction temperature, a reducing agent is added to ensure that the redox system is stably initiated under optimal conditions, and graft polymerization is preferentially triggered at the active sites on the fiber surface, further improving the grafting rate and modification uniformity.

[0023] The stepwise feeding and pH pre-adjustment process ensures that the initiation system reacts in a stable weakly acidic environment, resulting in a stable free radical generation rate and avoiding the problems of rapid agglomeration of the aqueous phase and sudden increase in the viscosity of the modified liquid caused by one-time feeding.

[0024] Optionally, the adhesive comprises, by weight: 68-72 parts of hydroxyl-terminated waterborne polyurethane prepolymer, 6-10 parts of blocked isocyanate crosslinking agent, 5-9 parts of plasticizer, 1-5 parts of stabilizer, 0.2-0.6 parts of silicone leveling agent, 4-8 parts of temperature-sensitive catalyst microcapsules, 6-10 parts of temperature-sensitive sealing agent microcapsules, and 11-15 parts of deionized water.

[0025] Optionally, in step S4, the sample is left to stand at room temperature and pressure for 60 seconds, and then pre-dried at 80°C for 30 seconds.

[0026] By adopting the above technical solution, and allowing the microcapsules to stand at room temperature and pressure, the low surface energy microcapsules spontaneously migrate to the gas-liquid interface of the colloidal layer, i.e. the fiber root implantation area, driven by thermodynamics.

[0027] The pre-baking temperature of 80℃ is lower than the microcapsule rupture temperature and the crosslinking agent desealing temperature. It only temporarily reduces the viscosity of the adhesive layer to increase the migration rate of microcapsules. It will not trigger microcapsule rupture and adhesive layer crosslinking in advance, ensuring that the microcapsules migrate completely to the fiber root area and avoiding premature reaction failure inside the adhesive layer.

[0028] Low-temperature pre-baking can also gently remove free moisture from the surface of the adhesive layer, avoiding defects such as pinholes, bubbles or shrinkage cavities during subsequent high-temperature curing, improving the density of the adhesive layer, and further reducing the channels for stain penetration.

[0029] Optionally, in step S5, the cross-linking sealing process involves first baking at 88-92°C for 6 minutes, followed by cross-linking curing at 115°C for 10 minutes.

[0030] By adopting the above technical solution, baking and sealing causes the microcapsule paraffin shell to rupture and the closed isocyanate to unseal. Simultaneously, four core reactions are achieved: initiation of main cross-linking of the adhesive layer, release of functional components by microcapsule rupture, covalent cross-linking of fiber-adhesive layer interface, and in-situ sealing and filling of root gaps. Multiple composite sealing is completed in one step, completely blocking the capillary permeation channels at the fiber root.

[0031] The polyurethane adhesive layer is fully cross-linked and cured at 115℃ for 10 minutes to ensure the flocking adhesion, water resistance, and aging resistance of the adhesive layer.

[0032] Segmented temperature control avoids the problems of rapid shrinkage of the adhesive layer, fiber flattening, and hardening of the flocked surface caused by one-time high-temperature curing. It ensures the stability of the sealing structure and adhesive layer performance, while retaining the soft and rich core touch of the flocked fabric.

[0033] Optionally, the pre-activation in S1 involves immersing the flocked fibers in a sodium hydroxide solution and stirring, then rinsing until neutral and drying until the moisture content is 10%.

[0034] By adopting the above technical solution, mild alkali etching is used to introduce a large number of hydroxyl and amino active sites on the surface of nylon fibers, which improves the adsorption of the modification liquid on the fiber surface and the grafting reaction efficiency, thus solving the problems of low grafting rate of unactivated fibers and easy peeling of the modified layer.

[0035] By precisely controlling the fiber moisture content to 10%, the fiber resistivity can be stabilized within the optimal range, ensuring the fiber's verticality and uprightness during electrostatic flocking. This allows for vertical fiber implantation into the adhesive layer, resulting in a uniform and full flock surface without issues such as lodging, clumping, or uncontrolled flocking.

[0036] Rinse until neutral to avoid residual alkali affecting the pH of the modification solution, ensuring that the grafting reaction always takes place in an optimal weakly acidic environment, and preventing problems such as unstable grafting rate and uneven modification effect caused by pH fluctuations.

[0037] Optionally, in S3, the substrate is a polyurethane base, and the substrate pretreatment involves cleaning with a mixture of isopropanol and ethanol, followed by plasma treatment.

[0038] By adopting the above technical solutions, the mixture of isopropanol and ethanol can completely remove impurities such as release agents, oil stains and dust from the surface of polyurethane base, avoiding problems such as decreased adhesive strength, bulging or delamination after long-term use caused by impurities; plasma / corona treatment can introduce a large number of polar active groups on the substrate surface, thereby improving the adhesion between the adhesive layer and the substrate.

[0039] Optionally, in S2, the catalyst microcapsule core material is an organotin composite agent and the shell material is paraffin wax, with the shell surface modified by fluorosilane.

[0040] By adopting the above technical solution, the cracking temperature of the paraffin shell material is perfectly matched with the unsealing temperature of the crosslinking agent. After heating, the catalyst is released synchronously upon cracking. It is completely sealed at room temperature and will not release prematurely, which would cause the adhesive to gel or shorten the storage period.

[0041] The organotin composite core material can simultaneously catalyze the polyurethane crosslinking reaction and the silane grafting sealing reaction, achieving dual-system catalysis in one step, which greatly improves the sealing reaction efficiency and the curing speed of the adhesive layer, and shortens the reaction time.

[0042] Surface fluorosilane modification endows microcapsules with low surface energy properties, enabling them to spontaneously migrate and accumulate towards the fiber roots, thereby releasing the catalyst directly in the core area of ​​the sealing pores. This ensures that the sealing reaction occurs in situ inside the pores, resulting in more thorough sealing without any reaction blind zones.

[0043] Optionally, in S2, the core material of the sealing agent microcapsule is a mixture of hydroxyl silicone oil and perfluorohexylethyltriethoxysilane, and the shell material is paraffin wax, with the shell surface modified by fluorosilane.

[0044] By adopting the above technical solution, which also uses paraffin shell material, the catalyst microcapsules are released synchronously, and a grafting reaction occurs in situ in the fiber root gaps to form a superhydrophobic interpenetrating network. This fills the micron-level annular gaps, blocks the capillary permeation channels, and solves the problems of deep stain penetration and root blackening and mold in home environments.

[0045] Hydroxyl silicone oil can form covalent bonds with polyurethane adhesive layers and fiber surface groups, firmly anchoring the sealing network to the substrate without falling off or migrating.

[0046] Perfluorohexylethyltriethoxysilane significantly reduces the surface energy of the sealing area, preventing liquid stains from penetrating and maintaining its anti-fouling properties even after rubbing or washing.

[0047] In summary, this application includes at least the following beneficial effects.

[0048] Sufficient hydroxyl and amino active sites are introduced through a mild alkaline solution pre-activation process for fibers without damaging the mechanical properties of the fibers or the compatibility with flocking.

[0049] The adhesive formulation employs a combination of paraffin shell temperature-sensitive catalyst microcapsules with fluorosilane-modified surface and sealing agent microcapsules, along with a precisely proportioned isocyanate main crosslinking system. This ensures the adhesive's room temperature storage stability, basic bonding strength, and flexibility suitable for home environments, while also providing a controllable functional basis for targeted sealing at the fiber roots.

[0050] The system employs a two-step targeted enrichment process involving room temperature resting and 80℃ pre-baking, enabling efficient and directional migration and enrichment of functional microcapsules in the fiber implantation root region. A segmented heat treatment process, involving baking and sealing at 88-92℃ and complete curing at 115℃, simultaneously completes the construction of the polyurethane main crosslinking network in the adhesive layer, precise microcapsule rupture and release, covalent bonding at the fiber-adhesive layer interface, and in-situ superhydrophobic interpenetrating network sealing of the micron-level annular gaps at the fiber root. This blocks the capillary penetration channels of stains, fundamentally solving long-standing industry pain points in flocked synthetic leather for home furnishings, such as root stain-resistant blind spots, deep-seated mold growth, rapid decline in flocking fastness, and short-lasting stain-resistant performance. Attached Figure Description

[0051] Figure 1 This is a flowchart of the main steps of this application. Detailed Implementation

[0052] The present application will be further described in detail below with reference to the accompanying drawings.

[0053] This application discloses a method for preparing flocked, highly stain-resistant synthetic leather for home use, referring to... Figure 1 Specifically, it includes the following steps.

[0054] S1. Pre-activate and modify the flocked fibers to obtain modified fibers.

[0055] The flocking fiber is selected from standard nylon 6 chopped fibers. Pre-activation involves immersing the flocking fiber in a sodium hydroxide solution for 8 minutes with stirring, then rinsing it with deionized water until neutral, and drying it with hot air at 40°C until the moisture content is 10% to obtain pre-activated fiber. The pre-activated fiber is then immediately fed into the subsequent modification process.

[0056] First, prepare a modified solution, which by weight comprises: 5-9 parts of monovinyl-terminated polydimethylsiloxane, 2.5-4.5 parts of 4-vinylphenylboronic acid, 3-5 parts of octadecyl methacrylate, 1-3 parts of acrylamide, 2-3 parts of nonionic emulsifier, 0.0002-0.0004 parts of aqueous selective polymerization inhibitor, 0.3-0.5 parts of oxidant, 0.1-0.3 parts of reducing agent, 16-20 parts of anhydrous ethanol, 0.1-0.5 parts of glacial acetic acid, and 66-70 parts of deionized water.

[0057] The monovinyl-terminated polydimethylsiloxane has a molecular weight of 800-1500. Its low molecular weight ensures dispersibility, provides a hydrophobic and antifouling backbone, and reduces fiber surface energy. 4-Vinylphenylboronic acid provides reactive crosslinking groups, covalently bonding with adhesive hydroxyl groups and sealing components, and inhibiting self-complexation in a weakly acidic environment. Octadecyl methacrylate enhances hydrophobicity, improves fiber abrasion resistance and smoothness, has strong adsorption to the fiber surface, and improves grafting anchoring efficiency. Acrylamide improves the adhesion between the modified layer and the fiber matrix, promoting monomer adsorption and grafting on the fiber surface. The nonionic emulsifier can be Tween 80, constructing a stable oil-in-water emulsion system with no stratification or oil drift within two to three days, ensuring uniform modification. The aqueous selective polymerization inhibitor can be p-hydroxyanisole. The oxidant can be ammonium persulfate, which rapidly decomposes at 40°C to generate free radicals. The reducing agent can be sodium bisulfite, which, in combination with ammonium persulfate, forms a low-to-medium temperature redox initiation system, efficiently triggering surface grafting at 40°C. Anhydrous ethanol is used as a co-solvent to assist in the dispersion of monovinyl-terminated polydimethylsiloxane and octadecyl methacrylate without affecting the fiber conductivity. Glacial acetic acid is used to create a weakly acidic environment to inhibit the self-complexation of phenylboronic acid and ensure initiation efficiency. Deionized water is the main solvent in the system.

[0058] To prepare the modified liquid, anhydrous ethanol, nonionic emulsifier, and monovinyl-terminated polydimethylsiloxane were first mixed and stirred for 15 min to form a pre-emulsion. Then, 4-vinylphenylboronic acid, octadecyl methacrylate, acrylamide, aqueous selective polymerization inhibitor, and oxidant were added and stirred for 20 min. Finally, glacial acetic acid was added to adjust the pH of the system to 5.5-6.0 to obtain the modified liquid base material.

[0059] Before impregnation of the pre-activated flocked fibers, the modified liquid base material was heated to 40°C and held at that temperature. A reducing agent was added and stirred for 5 minutes, followed by the addition of the pre-activated fibers and impregnation for 15 minutes, with low-speed stirring maintained throughout. During this process, the redox system continuously generates free radicals, preferentially triggering graft polymerization at the active sites on the fiber surface, while p-hydroxyanisole selectively inhibits the homopolymerization of free monomers in the aqueous phase. After impregnation, the fibers were removed and rinsed three times with deionized water at 40°C, then dried at 45°C for 40 minutes to obtain the modified fibers.

[0060] S2. An adhesive containing catalyst microcapsules and sealing agent microcapsules was prepared based on a closed isocyanate main crosslinking system.

[0061] The adhesive comprises, by weight, 68-72 parts of hydroxyl-terminated waterborne polyurethane prepolymer, 6-10 parts of blocked isocyanate crosslinking agent, 5-9 parts of plasticizer, 1-5 parts of stabilizer, 0.2-0.6 parts of silicone leveling agent, 4-8 parts of temperature-sensitive catalyst microcapsules, 6-10 parts of temperature-sensitive sealing agent microcapsules, and 11-15 parts of deionized water.

[0062] The adhesive matrix, consisting of a hydroxyl-terminated waterborne polyurethane prepolymer, provides basic adhesion and has a solid content of 40% with a hydroxyl value of 28 mg KOH / g. The blocked isocyanate crosslinking agent, IPDI type with a deblocking temperature of 90-95℃, is the main crosslinking system. After deblocking, it reacts with the hydroxyl-terminated waterborne polyurethane prepolymer to form a dense polyurethane network, ensuring the mechanical properties of the adhesive layer. The plasticizer can be diisononyl phthalate, which adjusts the flexibility of the adhesive layer to meet the high-frequency bending requirements of home furnishing fabrics. The stabilizer can be dibutyltin dilaurate, which ensures the storage stability of the adhesive and catalyzes the crosslinking and silane grafting reactions. The silicone leveling agent can be BYK-333, which reduces the surface tension of the adhesive layer, assists the migration of microcapsules to the gas-liquid interface (fiber root), and improves the enrichment efficiency under high fiber density.

[0063] The catalyst microcapsule core material is an organotin composite agent, and the shell material is paraffin wax, with the shell surface modified by fluorosilane. The sealing agent microcapsule core material is a mixture of hydroxyl silicone oil and perfluorohexylethyltriethoxysilane, and the shell material is paraffin wax, with the shell surface modified by fluorosilane. The paraffin wax shell has a rupture temperature of 88-90℃. The particle size of both the catalyst microcapsule and the sealing agent microcapsule is 1-3 μm, and the fluorosilane can be 1H,1H,2H,2H-perfluorodecyltriethoxysilane.

[0064] In the preparation of the adhesive, hydroxyl-terminated waterborne polyurethane prepolymer is first added to a reactor. Under low-speed stirring, plasticizer, stabilizer, silicone leveling agent, and blocked isocyanate crosslinking agent are added sequentially, and stirring continues for 25 minutes until the system is completely homogeneous. Then, while maintaining low-speed stirring, catalyst microcapsules and sealing agent microcapsules are slowly added, and stirring continues for 30 minutes. Finally, deionized water is added to adjust the solid content of the system to 35%, achieving a coating viscosity of 800-1200 mPa. s, filter through a 200-mesh sieve to remove impurities, maintain low-speed stirring throughout the process to avoid premature rupture of microcapsules due to high shear force, obtain adhesive, seal and store for later use.

[0065] S3. Pre-treat the substrate, then apply adhesive and modified fibers for coating and electrostatic flocking to obtain a semi-finished product.

[0066] Polyurethane substrate can be used. For substrate pretreatment, first wash the substrate surface with a 1:1 mixture of isopropanol and ethanol to remove oil and mold release agent residue. Avoid using strong solvents such as cyclohexanone and xylene to prevent swelling and deformation of the polyurethane substrate. After cleaning, perform low-temperature plasma treatment at a power of 2-3 kW and a processing speed of 10-15 m / min to increase the surface energy and active sites of the polyurethane substrate, further enhancing the adhesion between the adhesive layer and the substrate. The adhesive application must be completed within 30 minutes after treatment to avoid surface activity degradation.

[0067] The adhesive is then applied to the pretreated substrate surface to a thickness of 0.2-0.3 mm. The electrostatic flocking process follows the conventional top-mount electrostatic flocking process, with the fiber implantation depth controlled at 0.1-0.15 mm.

[0068] S4. Allow the semi-finished product to stand and pre-dry to promote the migration and enrichment of microcapsules into the roots of the modified fibers.

[0069] First, the microcapsules are left to stand at room temperature and pressure for 60 seconds, allowing them to migrate spontaneously to the gas-liquid interface of the gel layer (the fiber root implantation area) under thermodynamic drive. Then, they are pre-baked at 80°C for 30 seconds to temporarily reduce the viscosity of the gel layer, significantly increasing the migration speed of the microcapsules without triggering microcapsule rupture or desealing of the crosslinking agent.

[0070] S5. The semi-finished product that has completed migration and enrichment is cross-linked, sealed, and cured, and then finished to obtain flocked synthetic leather product.

[0071] First, a baking and sealing process is performed at 88-92℃ for 6 minutes. During this process, the blocked isocyanate crosslinking agent is desealed and reacts with the hydroxyl-terminated waterborne polyurethane prepolymer to form the main crosslinking network of polyurethane, laying the mechanical foundation for the adhesive layer. The catalyst microcapsules and sealing agent microcapsules are precisely ruptured sequentially, and the released catalyst accelerates the crosslinking reaction. The phenylboronic acid groups on the fiber surface undergo covalent crosslinking with the hydroxyl groups of the adhesive to form a molecular-level interface bond, eliminating the inherent interface gaps between the fiber and the adhesive layer. The hydroxyl silicone oil and fluorosilane in the sealing agent undergo grafting reactions with the polyurethane molecular chains and fiber surface groups to form a continuous superhydrophobic interpenetrating network at the fiber root, filling the remaining micron-level annular gaps and completely sealing the capillary permeation channels.

[0072] Then, cross-linking curing is carried out at 115℃ for 10 minutes to ensure complete cross-linking and curing of the polyurethane adhesive layer, guaranteeing the flocking firmness and mechanical properties of the adhesive layer, while also allowing the sealing interpenetrating network to fully set and achieve long-term stability. After curing, the product is allowed to cool naturally to room temperature, and the surface loose flocking is removed by brushing with a brush roller. Then, it is brushed, ironed, rolled up, and slit to obtain the final synthetic leather product.

[0073] The following provides a detailed description of each embodiment and comparative example.

[0074] Example 1:

[0075] S1. Pre-activate and modify the flocked fibers to obtain modified fibers.

[0076] The modified liquid comprises, by weight: 5 parts of monovinyl-terminated polydimethylsiloxane, 2.5 parts of 4-vinylphenylboronic acid, 3 parts of octadecyl methacrylate, 1 part of acrylamide, 2 parts of nonionic emulsifier, 0.0002 parts of aqueous selective polymerization inhibitor, 0.3 parts of oxidant, 0.1 parts of reducing agent, 16 parts of anhydrous ethanol, 0.1 parts of glacial acetic acid, and 66 parts of deionized water.

[0077] S2. An adhesive containing catalyst microcapsules and sealing agent microcapsules was prepared based on a closed isocyanate main crosslinking system.

[0078] The adhesive comprises, by weight: 68 parts of hydroxyl-terminated waterborne polyurethane prepolymer, 6 parts of blocked isocyanate crosslinking agent, 5 parts of plasticizer, 1 part of stabilizer, 0.2 parts of silicone leveling agent, 4 parts of temperature-sensitive catalyst microcapsules, 6 parts of temperature-sensitive sealing agent microcapsules, and 11 parts of deionized water.

[0079] S3. Pre-treat the substrate, then apply adhesive and modified fibers for coating and electrostatic flocking to obtain a semi-finished product.

[0080] S4. Allow the semi-finished product to stand and pre-dry to promote the migration and enrichment of microcapsules into the roots of the modified fibers.

[0081] First, allow the mixture to stand at room temperature and pressure for 60 seconds, then pre-bake it at 80°C for 30 seconds.

[0082] S5. The semi-finished product that has completed migration and enrichment is cross-linked, sealed, and cured, and then finished to obtain flocked synthetic leather product.

[0083] First, bake at 88-92℃ for 6 minutes to seal the pores, then cure at 115℃ for 10 minutes for cross-linking.

[0084] Example 2:

[0085] The difference from Example 1 is that the modified liquid, by weight, comprises: 9 parts of monovinyl-terminated polydimethylsiloxane, 4.5 parts of 4-vinylphenylboronic acid, 5 parts of octadecyl methacrylate, 3 parts of acrylamide, 3 parts of nonionic emulsifier, 0.0004 parts of aqueous selective polymerization inhibitor, 0.5 parts of oxidant, 0.3 parts of reducing agent, 20 parts of anhydrous ethanol, 0.5 parts of glacial acetic acid, and 70 parts of deionized water.

[0086] Example 3:

[0087] The difference from Example 1 is that the adhesive comprises, by weight, 72 parts of hydroxyl-terminated waterborne polyurethane prepolymer, 10 parts of blocked isocyanate crosslinking agent, 9 parts of plasticizer, 5 parts of stabilizer, 0.6 parts of silicone leveling agent, 8 parts of temperature-sensitive catalyst microcapsules, 10 parts of temperature-sensitive sealing agent microcapsules, and 15 parts of deionized water.

[0088] Comparative Example 1:

[0089] The difference from Example 1 is that the adhesive, by weight, comprises: 55 parts n-butyl acrylate, 25 parts ethyl acrylate, 15 parts methyl methacrylate, 13.5 parts diacetone acrylamide, 7.5 parts 4-allyl catechol, 8 parts vinyl silicone oil, 15 parts adipate dihydrazide, 5 parts emulsifier, 0.5 parts initiator, 62 parts deionized water, 1.2 parts sodium bicarbonate, and 8.5 parts acetone. The emulsifier is a mixture of sodium dodecyl sulfate and polyoxyethylene octylphenol ether-10 in a mass ratio of 3:2. The initiator is ammonium persulfate.

[0090] Comparative Example 2:

[0091] The difference from Example 1 is that S4 is left to stand at room temperature and pressure for 60 seconds.

[0092] Comparative Example 3:

[0093] The difference from Example 1 is that S4 is not performed; that is, S5 is performed directly after S3 is completed.

[0094] Comparative Example 4:

[0095] The difference from Example 1 is that S5 did not involve baking and sealing at 88-92°C for 6 minutes.

[0096] The synthetic leather products of the above embodiments and comparative examples were tested for relevant indicators.

[0097] Stain resistance rating was determined according to GB / T 30694-2014 "Test Method for Stain Resistance of Polyurethane Synthetic Leather". Five common household stains were selected: soy sauce, red wine, coffee, ballpoint pen ink, and pet simulated stain (egg yolk: physiological saline = 1:1). 0.5 mL of each stain was added to the sample surface and allowed to stand for 24 hours. The sample was then wiped three times with a clean, lint-free cloth and rated from 1 to 5. Grade 5: no residue; Grade 4: very slight residue; Grade 3: slight residue; Grade 2: obvious residue; Grade 1: severe residue. The arithmetic mean of the five stain ratings was taken.

[0098] To determine the root staining and penetration level, the sample was cut into a 50mm diameter circle with the napped side facing upwards. A 0.5% methylene blue aqueous solution was prepared as the colorimetric tracer solution. An equal volume of tracer solution was dropped onto the sample surface, ensuring that the tracer solution area did not come into contact with the surrounding area of ​​the test, and the sample was allowed to stand for 24 hours. The sample surface was then thoroughly rinsed three times with clean water and dried. A cryostat was then used to slice the sample perpendicular to the fiber. The methylene blue staining in the gum layer area at the fiber root was observed under a microscope and graded from 1 to 5: Grade 5: No staining at the root; Grade 4: Very trace staining not penetrating the gum layer; Grade 3: Slight staining confined to the gum layer surface; Grade 2: Obvious staining penetrating the gum layer; Grade 1: Severe staining penetrating the gum layer.

[0099] The specific results are shown in Table 1.

[0100] Table 1:

[0101]

[0102] Comparative Example 1 removed the core adhesive system of this application and replaced it with a conventional acrylic adhesive. It lacked the blocked isocyanate main crosslinking system and the dual microcapsule design of catalyst and sealing agent. The remaining processes were completely consistent with Example 1. The final measured stain resistance level was 2.7, and the root stain residue rating was 1.5, both of which were severely substandard. At the 2.7 stain resistance level, all tested stains left significant residue after wiping. Soy sauce, red wine, and ballpoint pen ink formed stubborn stains that could not be removed by conventional wiping, completely failing to meet the needs of daily household use. At the 1.5 root residue rating, the colorimetric tracer completely penetrated the adhesive layer, and there was no sealing effect on the fiber root gaps. Stains could completely penetrate into the adhesive layer through capillary effect. The performance defect was due to the lack of a targeted sealing microcapsule system, which could not fill the micron-level gaps at the fiber roots. Simultaneously, the acrylic adhesive and modified fibers lacked covalent crosslinking, resulting in significant interfacial gaps and completely open stain penetration channels.

[0103] Comparative Example 2 removed the pre-drying auxiliary migration process in S4 of this application, retaining only 60 seconds of room temperature and pressure resting. The final measured stain resistance level was 3.8, and the root stain residue rating was 3.0. Both indicators only reached a general level near the pass mark, showing a significant decrease compared to Example 1. At a stain resistance level of 3.8, slight visible traces remained after wiping, indicating a significant reduction in stain resistance. At a root residue rating of 3.0, the colorant only slightly stained the surface of the adhesive layer, not penetrating deep into the adhesive layer, but there were obvious signs of root penetration, resulting in a significant reduction in gap sealing effect. The performance defect is due to the fact that room temperature resting alone cannot achieve efficient enrichment of microcapsules at the fiber roots. Most microcapsules remain dispersed within the adhesive layer, unable to release the sealing agent in situ in the core root area, only achieving partial gap sealing, leading to a significant decrease in root anti-penetration performance.

[0104] Comparative Example 3 omitted the entire targeted enrichment process of S4 (settling and pre-drying) in this application. After electrostatic flocking, it directly entered the S5 cross-linking and curing process. The final measured stain resistance level was 2.9, and the root stain residue rating was 1.8, both of which were severely substandard. The stain resistance performance was not significantly different from conventional commercially available products. At the 2.9 stain resistance level, there was obvious residue after wiping, and the easy-to-clean performance was completely unacceptable. At the 1.8 root residue rating, a large amount of colorant penetrated deep into the adhesive layer, and the fiber root gaps were completely unsealed, with penetration close to that of Comparative Example 1. The performance defect is due to the complete lack of time and conditions for the microcapsules to migrate and enrich towards the fiber roots. The microcapsules were uniformly dispersed throughout the adhesive layer and prematurely ruptured and released within the adhesive layer during curing, failing to form a sealing network at the root gaps. The core targeted sealing technology of this application was completely ineffective.

[0105] Comparative Example 4 omitted the baking and sealing process in S5 of this invention, directly proceeding to high-temperature cross-linking and curing. The final measured stain resistance level was 3.1, and the root stain residue rating was 2.0, both of which were unqualified, indicating a significant failure to meet stain resistance standards. At the 3.1 stain resistance level, visible residue was left after wiping. At the 2.0 root residue rating, the colorant penetrated significantly into the adhesive layer, and the fiber root gaps were not effectively sealed, resulting in significant penetration and contamination problems. The performance defect is due to skipping the low-temperature baking and sealing process, which precisely matches the microcapsule rupture temperature and the cross-linking agent unsealing temperature. Direct high-temperature curing caused rapid cross-linking and shaping of the adhesive layer. The microcapsule rupture, the in-situ reaction of the sealing agent, and the cross-linking of the adhesive layer were completely out of sync, failing to form a continuous sealing network within the root gaps. Simultaneously, the rapid shrinkage of the adhesive layer widened the interface gaps between the fiber and the adhesive layer, further exacerbating stain penetration and completely negating the targeted sealing effect.

[0106] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A method for preparing flocked, highly stain-resistant synthetic leather for home use, characterized in that: Specifically, the following steps are included: S1. Pre-activate and modify the flocked fibers to obtain modified fibers; S2. An adhesive containing catalyst microcapsules and sealing agent microcapsules was prepared based on a closed isocyanate main crosslinking system; S3. Pre-treat the substrate, then apply adhesive and modified fibers for coating and electrostatic flocking to obtain a semi-finished product; S4. Allow the semi-finished product to stand and pre-dry to promote the migration and enrichment of microcapsules into the roots of the modified fibers. S5. The semi-finished product that has completed migration and enrichment is cross-linked, sealed, and cured, and then finished to obtain flocked synthetic leather product.

2. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The modifying solution required for modification in S1 comprises, by weight: 5-9 parts of monovinyl-terminated polydimethylsiloxane, 2.5-4.5 parts of 4-vinylphenylboronic acid, 3-5 parts of octadecyl methacrylate, 1-3 parts of acrylamide, 2-3 parts of nonionic emulsifier, 0.0002-0.0004 parts of aqueous selective polymerization inhibitor, 0.3-0.5 parts of oxidant, 0.1-0.3 parts of reducing agent, 16-20 parts of anhydrous ethanol, 0.1-0.5 parts of glacial acetic acid, and 66-70 parts of deionized water.

3. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 2, characterized in that: The modified liquid is prepared by first mixing and stirring anhydrous ethanol, nonionic emulsifier, and monovinyl-terminated polydimethylsiloxane to form a pre-emulsion, then adding 4-vinylphenylboronic acid, octadecyl methacrylate, acrylamide, an aqueous selective polymerization inhibitor, and an oxidant and stirring. Then, glacial acetic acid is added to adjust the pH of the system to 5.5-6.0 to obtain the modified liquid base material. Before impregnation of the pre-activated flocked fibers, the modified liquid base material is heated to a predetermined temperature, and then a reducing agent is added and stirred.

4. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The adhesive comprises, by weight, 68-72 parts of hydroxyl-terminated waterborne polyurethane prepolymer, 6-10 parts of blocked isocyanate crosslinking agent, 5-9 parts of plasticizer, 1-5 parts of stabilizer, 0.2-0.6 parts of silicone leveling agent, 4-8 parts of temperature-sensitive catalyst microcapsules, 6-10 parts of temperature-sensitive sealing agent microcapsules, and 11-15 parts of deionized water.

5. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: In step S4, the sample is left to stand at room temperature and pressure for 60 seconds, and then pre-dried at 80°C for 30 seconds.

6. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The cross-linking sealing process in S5 involves baking at 88-92°C for 6 minutes, followed by cross-linking curing at 115°C for 10 minutes.

7. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The pre-activation in S1 involves immersing the flocked fibers in a sodium hydroxide solution and stirring, then rinsing until neutral and drying until the moisture content is 10%.

8. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The substrate in S3 is a polyurethane base. The substrate is pretreated by first cleaning with a mixture of isopropanol and ethanol, and then subjected to plasma treatment.

9. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The catalyst microcapsule core material in S2 is an organotin composite agent and the shell material is paraffin wax, with the shell surface modified by fluorosilane.

10. The method for preparing flocked, highly stain-resistant synthetic leather for home use according to claim 1, characterized in that: The core material of the sealing agent microcapsule in S2 is a mixture of hydroxyl silicone oil and perfluorohexylethyltriethoxysilane, and the shell material is paraffin wax with the shell surface modified by fluorosilane.

Citation Information

Patent Citations

  • Stain-resistant and graffiti-resistant semi-silicone synthetic leather and its manufacturing process

    CN115157818B

  • A wear-resistant composite flocking cloth and preparation method thereof

    CN117166263B