Dyeing and finishing process for improving the sweat stain problem of knitted nylon-polyamide fabric

By using the dyeing and finishing process of knitted nylon-spandex fabrics, and employing specific auxiliaries and controlling the temperature and rate, the problem of sweat stains has been solved, improving the appearance and comfort of the garments, making them suitable for use in multiple scenarios.

CN123133196APending Publication Date: 2026-11-20FUJIAN NEW HONGGANG TEXTILE TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611335920.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Knitted nylon-spandex fabrics tend to leave white or light-colored marks after absorbing sweat, affecting the appearance and comfort of clothing, especially noticeable in high-temperature summer conditions.

Method used

An improved dyeing and finishing process for knitted nylon-spandex fabrics is adopted, including pretreatment, dyeing, anti-yellowing, and post-setting steps. Auxiliaries such as anti-staining soap, leveling agent, anti-phenolic yellowing agent, citric acid, and moisture-wicking agent are used to control the heating and cooling rates, reduce the amount of auxiliary agents, and avoid the formation of watermarks.

Benefits of technology

It effectively solves the problem of sweat stains, leaving no obvious color difference or circular marks on the fabric surface, improving the appearance and visual quality of clothing, extending the life of clothing, and keeping the user looking presentable and fresh.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123133196A_ABST
    Figure CN123133196A_ABST
Patent Text Reader

Abstract

The present application relates to a kind of dyeing and finishing processes for improving the problem of knitted brocade sweat stain, the process includes pretreatment: normal temperature cloth, run 5~10min, join anti-staining soaping agent, temperature is raised to 65~75 degrees, keep warm 15~25min, after finishing, temperature is reduced to 50~60 DEG C after drainage;Dyeing: normal temperature cloth, first join level dyeing agent and oil removal agent, run 5~15min after, join dyeing solution, charge time is 20~30min, temperature is raised to 98 DEG C keep warm 15~25min, after keeping warm, temperature is reduced to 50~60 DEG C after drainage.Wash cold water 1~2 cylinders;Anti-yellow: cloth, join anti-phenol yellow change agent, citric acid and moisture absorption sweat agent, normal temperature temperature is raised to 65~75 DEG C, keep warm 15~25min, after keeping warm, temperature is reduced to 45~55 DEG C, wash cold water one cylinder;After fixing: after fixing, over clean water, do process requirement specification.The present application can solve the problem that knitted brocade fabric is prone to sweat stain.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile technology, and in particular to a dyeing and finishing process for improving the problem of sweat stains on knitted nylon-spandex fabrics. Background Technology

[0002] Sweat stains are white or light-colored marks that form on the surface of clothing (especially dark or light-colored work clothes and shirts) after absorbing and drying sweat. This phenomenon is particularly common in the high temperatures of summer. When wearing a shirt, if heat cannot dissipate, sweat stains easily remain on the fabric, causing visual embarrassment and a stiff feeling. Some people (such as girls) tend to sweat more under their arms in summer, and without special breathable design, sweat stains can be very noticeable and uncomfortable. Aesthetically unappealing: Sweat stains are considered an "embarrassing" phenomenon, potentially making clothing look cheap or untidy. They are often accompanied by a sticky, damp feeling, causing the wearer to be hesitant to move around much and reducing comfort. Summary of the Invention

[0003] The purpose of this invention is to provide a dyeing and finishing process that improves the problem of sweat stains on knitted nylon-spandex fabrics, thereby solving the problem of sweat stains on knitted nylon-spandex fabrics.

[0004] To achieve the above objectives, the present invention provides the following technical solution: a dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics, the process comprising the following steps: Step S1, Pretreatment: Place the fabric at room temperature, run for 5-10 minutes, add anti-staining soap, heat to 65-75 degrees Celsius, keep warm for 15-25 minutes, and then cool down to 50-60 degrees Celsius and drain. Step S2, Dyeing: Place the fabric at room temperature, first add leveling agent and degreasing agent, run for 5-15 minutes, then add dye liquor, adding for 20-30 minutes. Heat to 98℃ and hold for 15-25 minutes. After holding, cool to 50-60℃ and drain. Wash with cold water for 1-2 cycles.

[0005] Step S3, Anti-yellowing: Place the fabric in the incubator, add anti-phenolic yellowing agent, citric acid and moisture-wicking agent, heat to 65-75℃ at room temperature, keep warm for 15-25 minutes, after the warming is completed, cool down to 45-55℃, and wash with cold water.

[0006] Step S4, Post-fixing: Perform post-fixing, rinse with clean water, and meet the process requirements and specifications.

[0007] Furthermore, the concentration of the anti-stain soap is 2 g / L.

[0008] Furthermore, the heating rate in both steps S1 and S2 is 1–1.5 °C / min, and the cooling rate is 0.8–1.5 °C / min.

[0009] Furthermore, the leveling agent is a multifunctional acidic and cationic co-bath leveling agent, the concentration of the leveling agent is 1.5 g / L, and the content of acidic dye in the dyeing solution is x.

[0010] Furthermore, the heating rate and cooling rate in step S3 are both 1 to 2 °C / min.

[0011] Furthermore, in step S3, the concentration of the anti-phenolic yellowing agent is 3 g / L, the concentration of citric acid is 0.5 g / L, and the concentration of the moisture-wicking agent is 2 g / L.

[0012] Furthermore, in step S4, the set temperature is 145-155℃ and the vehicle speed is 20-40m / min.

[0013] The beneficial effects of this invention are as follows: This invention effectively and persistently solves the problem of sweat stains. After multiple simulated sweat immersion and drying cycles, there is still no obvious color difference or circular marks on the fabric surface. Fabrics treated with this invention show satisfactory results in standard sweat stain fastness tests. Furthermore, the elimination of sweat stains directly improves the neatness and visual quality of clothing, allowing users to maintain a presentable and fresh image in various scenarios such as social gatherings, work, and sports, extending the lifespan of clothing and protecting personal health. Attached Figure Description

[0014] Figure 1 A fabric pattern obtained in Comparative Example 1; Figure 2 This is a fabric image showing that sweat stains are almost invisible in this embodiment. Figure 3 The image shows the results of the colorfastness test. Figure 4 The image shows the results of the colorfastness test. Figure 5 The image shows the results of the colorfastness test. Detailed Implementation

[0015] The invention will now be further described with reference to the accompanying drawings.

[0016] Please see Figures 1 to 5 The present invention provides an embodiment: a dyeing and finishing process for improving the problem of sweat stains on knitted nylon-spandex fabrics, the process comprising the following steps: Step S1, Pretreatment: Place the fabric at room temperature, run for 5-10 minutes, add anti-staining soap, heat to 65-75 degrees Celsius, keep warm for 15-25 minutes, and then cool down to 50-60 degrees Celsius and drain. Step S2, Dyeing: Place the fabric at room temperature, first add leveling agent and degreasing agent, run for 5-15 minutes, then add dye liquor, adding for 20-30 minutes. Heat to 98℃ and hold for 15-25 minutes. After holding, cool to 50-60℃ and drain. Wash with cold water for 1-2 cycles. Step S3, Anti-yellowing: Place the fabric in the pan, add anti-phenolic yellowing agent, citric acid and moisture-wicking agent, heat to 65-75℃ at room temperature, keep warm for 15-25 minutes, after the heat preservation is completed, cool to 45-55℃, and wash in a tub of cold water. Step S4, Post-setting: Perform post-setting, rinse with clean water, and meet process requirements. In this invention, no softener is added during post-setting. Softeners added during setting will adhere to the fabric fiber surface, leading to uneven fabric transfer and watermarks. This invention adds leveling agents and degreasing agents during the dyeing stage, and does not add any auxiliaries during post-setting, only rinsing with clean water. Compared to conventional processes that add auxiliaries during the setting step, this reduces the amount of auxiliaries used.

[0017] Please continue reading. Figures 2 to 5 As shown, in one embodiment of the present invention, the concentration of the anti-stain soap is 2 g / L.

[0018] Please continue reading. Figures 2 to 5 As shown, in one embodiment of the present invention, the heating rate of steps S1 and S2 is 1 to 1.5 °C / min, and the cooling rate is 0.8 to 1.5 °C / min.

[0019] Please continue reading. Figures 2 to 5 As shown, in one embodiment of the present invention, the leveling agent is a multifunctional acidic and cationic co-bath leveling agent, the concentration of the leveling agent is 1.5 g / L, and the content of acid dye in the dye bath is x%. The model of the multifunctional acidic and cationic co-bath leveling agent is Acid leveling agent RA-11.

[0020] Please continue reading. Figures 2 to 5 As shown, in one embodiment of the present invention, the heating rate and cooling rate in step S3 are both 1-2℃ / min.

[0021] Please continue reading. Figures 2 to 5 As shown, in one embodiment of the present invention, the concentration of the anti-phenolic yellowing agent in step S3 is 3 g / L, the concentration of citric acid is 0.5 g / L, and the concentration of the moisture-wicking agent is 2 g / L.

[0022] Please continue reading. Figures 2 to 5 As shown, in one embodiment of the present invention, the temperature set in step S4 is 145-155°C and the vehicle speed is 20-40 m / min. Specific Implementation

[0023] It is made of a nylon-spandex interwoven knitted fabric, with the following composition: 83% Nylon and 17% Elastane.

[0024] (1) Pre-processing: Formula: Anti-stain soap detergent 2g / L Place the fabric at room temperature, run for 5-10 minutes, add anti-staining soap, heat up to 70 degrees Celsius at a rate of 1-1.5℃ / min, keep warm for 20 minutes, and then cool down to 50-60 degrees Celsius at a rate of 0.8-1.5℃ / min before draining.

[0025] (2) Dyeing: Dye according to the following dyeing formula: Acid dyes x% Multifunctional acidic and cationic leveling agent, 1.5 g / L Degreasing agent 0.3g / L For fabric loading at room temperature, first add leveling agent and degreasing agent at room temperature, run for 5-15 minutes, then add dye liquor and feed for 20-30 minutes. Increase the temperature to 98℃ at a rate of 1-1.5℃ / min, hold for 20 minutes, and after holding, decrease the temperature to 50-60℃ at a rate of 0.8-1.5℃ / min before draining. Wash with cold water for 1-2 cycles.

[0026] (3) Anti-yellowing: After dyeing, an anti-yellowing treatment is performed, and the process is as follows: formula: Anti-phenol yellowing agent 3g / L Citric acid 0.5g / L Moisture-wicking agent 2g / L Add the fabric, anti-phenol yellowing agent, citric acid, and moisture-wicking agent. Heat the fabric to 70°C at a rate of 1-2°C / min from room temperature, keep it warm for 20 minutes, and then cool it down to 50°C at a rate of 1-2°C / min. Wash it in a tub of cold water.

[0027] (4) Final determination: Set the temperature to 150℃, drive at 30m / min, rinse with clean water, and meet the process requirements.

[0028] Comparative Example 1: The dyeing and finishing method disclosed in patent application CN121853263A was adopted. After the greige fabric was fed into the setting machine, an anti-yellowing agent was added to obtain the fabric.

[0029] Figures 1 to 5 As shown, Figure 1 and Figure 2 The comparison shows that Figure 2 After treatment using the method of this invention, sweat stains on the fabric surface are almost invisible. Figures 3 to 5All results are color fastness test results of the treated fabric, and the test results are qualified. It can be seen from the test results that the water stains of the finished product of the present invention are significantly improved, and there is no impact on the color fastness.

[0030] The above description is only a preferred embodiment of the present invention and should not be construed as a limitation of this application. All equivalent changes and modifications made in accordance with the scope of the patent application of the present invention should be included in the scope of the present invention.

Claims

1. A dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics, characterized in that: The process includes the following steps: Step S1, Pretreatment: Place the fabric at room temperature, run for 5-10 minutes, add anti-staining soap, heat to 65-75 degrees Celsius, keep warm for 15-25 minutes, and then cool down to 50-60 degrees Celsius and drain. Step S2, Dyeing: Place the fabric at room temperature, first add leveling agent and degreasing agent, run for 5-15 minutes, then add dye liquor, adding for 20-30 minutes. Heat to 98℃ and hold for 15-25 minutes. After holding, cool to 50-60℃ and drain. Wash with cold water for 1-2 cycles. Step S3, Anti-yellowing: Place the fabric in the pan, add anti-phenolic yellowing agent, citric acid and moisture-wicking agent, heat to 65-75℃ at room temperature, keep warm for 15-25 minutes, after the heat preservation is completed, cool to 45-55℃, and wash in a tub of cold water. Step S4, Post-fixing: Perform post-fixing, rinse with clean water, and meet the process requirements and specifications.

2. The dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics according to claim 1, characterized in that: The concentration of the anti-stain soap is 2 g / L.

3. The dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics according to claim 1, characterized in that: The heating rate in both steps S1 and S2 is 1–1.5 °C / min, and the cooling rate is 0.8–1.5 °C / min.

4. The dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics according to claim 1, characterized in that: The leveling agent is a multifunctional acidic and cationic co-bath leveling agent, the concentration of the leveling agent is 1.5 g / L, and the content of acidic dye in the dyeing solution is x.

5. The dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics according to claim 1, characterized in that: The heating rate and cooling rate in step S3 are both 1-2℃ / min.

6. The dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics according to claim 1, characterized in that: In step S3, the concentration of the anti-phenolic yellowing agent is 3 g / L, the concentration of citric acid is 0.5 g / L, and the concentration of the moisture-wicking agent is 2 g / L.

7. The dyeing and finishing process for improving the problem of perspiration stains on knitted nylon-spandex fabrics according to claim 1, characterized in that: In step S4, the set temperature is 145-155℃ and the vehicle speed is 20-40m / min.

Citation Information

Patent Citations

  • Knitted fabric and preparation method and application thereof

    CN121853263A