An aqueous microsphere foaming ink composition for three-dimensional printing and a method for preparing the same

By using a combination of polyacrylate nanospheres and waterborne polyurethane resin, the adhesion and abrasion resistance issues of waterborne microsphere foaming inks in the footwear industry have been solved, achieving high adhesion and uniform foaming effect for 3D printing. This results in a 3D raised effect and a soft, comfortable feel suitable for athletic and casual shoes.

CN123133199APending Publication Date: 2026-11-20TAIWEI OPTICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611550265.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing water-based microsphere foaming inks suffer from poor adhesion, poor abrasion resistance, and uneven foaming in the footwear material industry, which limits their promotion and application in high-end fields.

Method used

A water-based microsphere foaming ink composition for 3D printing was prepared by using polyacrylate nanospheres as a foaming agent, combined with water-based polyurethane resin as a binder, and incorporating wetting and leveling agents, defoamers, and adhesion promoters.

Benefits of technology

It achieves high ink adhesion, good abrasion resistance, and uniform foaming, meets environmental protection standards, and is suitable for 3D printing of shoe materials in high-intensity application scenarios, meeting the needs of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123133199A_ABST
    Figure CN123133199A_ABST
Patent Text Reader

Abstract

The application discloses a water-based microsphere foaming ink composition for three-dimensional printing and a preparation method thereof, and belongs to the field of shoe material printing process and three-dimensional vamp forming technology.The water-based microsphere foaming ink composition is composed of polyacrylate nano microspheres, a connecting agent water-based polyurethane resin, a wetting and leveling agent, a defoaming agent, an ink adhesion promoter and the like.The polyacrylate nano foaming microspheres are used as the main body, and the water-based polyurethane resin connecting agent is used, so that the comprehensive performance of the water-based foaming ink, such as adhesion, wear resistance and foaming uniformity, is significantly improved, and a new selection is provided for the three-dimensional printing process of the vamp.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of shoe material printing technology and three-dimensional shoe upper molding technology, and specifically discloses an aqueous microsphere foaming ink composition for three-dimensional printing and its preparation method. Background Technology

[0002] Traditional solvent-based inks contain large amounts of volatile organic compounds (VOCs), which not only cause environmental pollution but also harm human health. Water-based microsphere foaming inks, with their low toxicity, harmlessness, non-flammability, and non-explosive environmental protection properties, are gradually becoming the mainstream choice in the footwear materials industry.

[0003] Water-based microsphere foaming ink is a special type of ink made by dispersing microspheres into binders such as acrylate copolymers, utilizing the properties of microspheres. When heated, the ink foams and bulges; upon cooling and solidification, it forms raised text or patterns.

[0004] Water-based microsphere foaming inks have been widely used in footwear materials, apparel printing, packaging decoration, and other fields. In the footwear industry, they can be used for upper patterns and logos on athletic shoes and casual shoes, giving the upper a three-dimensional, raised visual effect and a soft, comfortable feel.

[0005] However, existing technologies still suffer from problems such as poor adhesion, poor abrasion resistance, and uneven foaming, which limit the promotion and application of water-based microsphere foaming inks in high-end fields such as shoe materials. Summary of the Invention

[0006] To address the limitations of existing foaming ink technology, this invention proposes a water-based microsphere foaming ink composition for 3D printing and its preparation method, aiming to develop a water-based microsphere foaming ink with strong adhesion, good abrasion resistance, and uniform foaming.

[0007] This invention uses polyacrylate nanofoamed microspheres as the main body and water-based polyurethane resin as a binder to significantly improve the overall performance of water-based foamed inks, providing a new option for three-dimensional printing processes on shoe uppers.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] A water-based microsphere foaming ink composition for 3D printing, comprising the following parts by weight:

[0010] 10 parts polyacrylate nanospheres, 50-60 parts waterborne polyurethane resin, 0.5-3 parts wetting and leveling agent, 1-2 parts defoamer, 0.5-2 parts waterborne ink adhesion promoter, 2-8 parts waterborne pigment, and 2-12 parts deionized water.

[0011] Preferably, the wetting and leveling agent is any one or a mixture of two of polyether-modified organosilicon and polyether-modified dimethylpolysiloxane.

[0012] Preferably, the defoamer is any one of polydimethylsiloxane or modified polysiloxane.

[0013] Preferably, the adhesion promoter for water-based ink is any one or a mixture of multiple of silane coupling agents, titanate coupling agents, and aluminate coupling agents.

[0014] Preferably, the aqueous color paste is any one of phthalocyanine blue, phthalocyanine green, and quinacridone violet.

[0015] The method for preparing the polyacrylate nanospheres is as follows:

[0016] (1) Preparation of oil phase: Methyl methacrylate, methyl acrylate, azobisisobutyronitrile, 1,4-butanediol dimethacrylate and n-hexane are added to the reaction vessel and stirred to obtain oil phase liquid.

[0017] Preferably, the weight ratio of methyl methacrylate, methyl acrylate, azobisisobutyronitrile, 1,4-butanediol dimethacrylate and n-hexane is (20-100):300:(0.3-2):(4-25):(95-125).

[0018] (2) Preparation of aqueous phase: Add NaOH to deionized water and dissolve it completely. Transfer the solution to a three-necked flask, add sodium dodecyl sulfate, and stir thoroughly for 20-30 min. Add MgCl2·6H2O to distilled water and dissolve it completely for later use. Use a peristaltic pump to add the MgCl2·6H2O solution to the three-necked flask and speed up the stirring to form a relatively stable magnesium hydroxide particle dispersion. Finally, add sodium chloride, sodium nitrite and anhydrous ethanol to the flask and stir thoroughly to obtain an aqueous phase liquid.

[0019] Preferably, the weight ratio of NaOH to MgCl2·6H2O is 1:2-6.

[0020] (3) Preparation of polyacrylate nanospheres: The prepared oil phase liquid is added to the aqueous phase liquid and emulsified by a homogenizer to fully disperse the oil phase liquid in the aqueous phase liquid. The water bath temperature is heated to 60~70℃ and the reaction is carried out for 6~12 hours under mechanical stirring at 150-400 rpm to initially obtain a polyacrylate nanosphere suspension.

[0021] Dilute hydrochloric acid was added dropwise to the polyacrylate nanosphere suspension to adjust the pH to about 3-4. After stirring for a period of time, magnesium hydroxide was removed, and the mixture was washed with water 3-5 times and filtered. After drying, polyacrylate nanospheres were obtained.

[0022] Preferably, the weight ratio of the oil phase liquid to the water phase liquid is 1:2-8.

[0023] The present invention also proposes a method for preparing the aforementioned aqueous microsphere foaming ink composition, comprising the following steps:

[0024] (1) Preparation of polyurethane linking emulsion: Add waterborne polyurethane resin to a dispersion tank and stir at 400 rpm. Add defoamer, wetting agent and other liquid additives in sequence and stir for 3-5 min. Add waterborne color paste and mix evenly.

[0025] (2) Reduce the stirring speed to 200 rpm, slowly add polyacrylate nanospheres to the dispersion tank, maintain the system temperature at 25~40℃, stir for 6~8 min, add an appropriate amount of deionized water, filter with a 200-mesh filter to obtain the water-based microsphere foaming ink composition, the reaction mechanism of which is as follows: Figure 1 As shown.

[0026] Furthermore, the present invention also provides a three-dimensional printing process for shoe uppers based on the aforementioned aqueous microsphere foaming ink composition, the main process of which is as follows:

[0027] (1) Pretreatment of shoe upper material: Use plasma bombardment equipment to bombard the surface of shoe upper material to roughen the surface of the material and increase the surface energy;

[0028] (2) Microsphere foaming ink is applied to the surface of the shoe upper fabric using screen printing.

[0029] (3) After being heated in the drying tunnel, the microsphere foaming ink on the fabric foams and expands rapidly within a few seconds, forming a three-dimensional texture with uneven surfaces;

[0030] (4) After foaming, the temperature is lowered for pre-curing, and a dense nano-sealing layer is formed on the surface of the foamed layer;

[0031] (5) Collect the height data of the three-dimensional texture through 3D scanning, and automatically adjust the amount of digital ink according to the height. Set the top of the raised part of the pattern to spray 8~15% more ink and the recessed part to spray 8~15% less ink.

[0032] (6) Spray ink onto the surface of the fabric, heat it again to allow the ink to penetrate into the fabric, and obtain a three-dimensional print after drying.

[0033] Compared with the prior art, the beneficial effects of the present invention are:

[0034] 1. Environmental friendliness: The ink composition of this invention uses water as the dispersion medium and contains almost no volatile organic solvents, achieving almost zero VOC emissions throughout the entire process, reducing environmental pollution in the production workshop, and meeting the limit requirements of relevant environmental standards of the International Association for Research and Testing in Textile and Leather Ecology.

[0035] 2. Significantly Improved Foaming Uniformity: This invention uses polyacrylate microspheres with controllable particle size distribution as the foaming agent. Through precise control of polymerization process parameters, the microsphere particle size is concentrated within the target range, effectively avoiding inconsistent foaming caused by particle size differences. The microsphere walls are of uniform thickness, and the expansion rate is consistent during heating, avoiding phenomena such as inconsistent cell size and disordered distribution caused by uneven heating. Experimental results show that the water-based microsphere foaming ink prepared by the method of this invention has a regular and dense cell structure, a smooth and uniform foaming surface, and no obvious protrusions or collapsed areas, effectively improving the overall visual effect and performance of the product.

[0036] 3. Significantly Enhanced Pigment Adhesion: This invention uses polyurethane resin as a binder, allowing pigment particles to be uniformly dispersed within the network structure formed by the polyurethane resin, creating a stable pigment-resin composite system. During the foaming and curing process, the polyurethane resin and microspheres simultaneously cross-link and cure, firmly locking the pigment to the cell walls and substrate surface, forming a three-dimensional anchoring structure. This structure prevents the pigment from easily detaching or migrating from the substrate surface, maintaining excellent color integrity and decorative effect even after external forces such as friction and bending.

[0037] 4. Significantly Improved Abrasion Resistance and Durability: Polyurethane resin itself possesses excellent abrasion resistance; its tensile strength, tear strength, and abrasion resistance are all superior to traditional acrylic resins. This invention utilizes these properties of polyurethane resin to give the foam layer excellent abrasion resistance and scratch resistance. During normal use, the surface of the foam layer is not easily scratched or worn down, maintaining a good three-dimensional effect and decorative appearance for a long time. Simultaneously, the strong adhesion between the polyurethane resin and the substrate, achieving an adhesion strength of Grade 1 or higher (cross-cut adhesion test), effectively avoids problems such as delamination and bubbling during use. This significantly improves product durability and reliability, meeting the needs of high-intensity applications such as athletic shoes and casual shoes.

[0038] 5. Water-based microsphere foaming ink has a simple process that does not require large-scale equipment modification, meets the needs of industrial production, and has good market application prospects in the footwear material industry. Attached Figure Description

[0039] Figure 1 This is a schematic diagram of the preparation process of polyacrylate nanospheres and aqueous microsphere foaming ink. Detailed Implementation

[0040] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.

[0041] Preparation Example 1: A method for preparing polyacrylate nanospheres (methyl methacrylate: methyl acrylate = 1:15), the specific process is as follows:

[0042] (1) Preparation of oil phase: 20 g of methyl methacrylate, 300 g of methyl acrylate, 0.3 g of azobisisobutyronitrile, 4 g of 1,4-butanediol dimethacrylate and 95 g of n-hexane were added to the reaction vessel and stirred and mixed evenly to obtain the oil phase liquid.

[0043] (2) Preparation of the aqueous phase: 200 g of NaOH was added to 400 g of deionized water and dissolved completely. The solution was then transferred to a three-necked flask, and 5 g of sodium dodecyl sulfate was added. The mixture was stirred thoroughly for 25 min. 400 g of MgCl2·6H2O was added to 400 g of distilled water and dissolved completely. The MgCl2·6H2O solution was added to the three-necked flask using a peristaltic pump, and the stirring speed was increased until a relatively stable dispersion of magnesium hydroxide particles was formed. Finally, 5 g of sodium chloride, 5 g of sodium nitrite, and 10 g of anhydrous ethanol were added to the flask and stirred thoroughly to obtain the aqueous phase liquid.

[0044] (3) Preparation of polyacrylate nanospheres: The oil phase liquid was added to the aqueous phase liquid at a ratio of 1:2, and emulsified at 4000 rpm for 5 min using a homogenizer to ensure thorough dispersion of the oil phase liquid in the aqueous phase liquid. The system was heated to 60℃ in a water bath and reacted for 12 h under mechanical stirring at 200 rpm to obtain a polyacrylate nanosphere suspension. 5% (w / w) dilute hydrochloric acid was added dropwise to the polyacrylate nanosphere suspension to adjust the pH to 3.5, and the mixture was stirred for 30 min to remove magnesium hydroxide. The nanospheres were washed three times with water and filtered, then dried at 50℃ for 24 h to obtain polyacrylate nanospheres.

[0045] Preparation Example 2: A method for preparing polyacrylate nanospheres (methyl methacrylate: methyl acrylate = 1:5), the specific process is as follows:

[0046] (1) Preparation of oil phase: 60 g of methyl methacrylate, 300 g of methyl acrylate, 1.2 g of azobisisobutyronitrile, 15 g of 1,4-butanediol dimethacrylate and 105 g of n-hexane were added to the reaction vessel and stirred and mixed evenly to obtain the oil phase liquid.

[0047] (2) Preparation of the aqueous phase: 200 g of NaOH was added to 400 g of deionized water and dissolved completely. The solution was then transferred to a three-necked flask, and 5 g of sodium dodecyl sulfate was added. The mixture was stirred thoroughly for 25 min. 800 g of MgCl2·6H2O was added to 400 g of distilled water and dissolved completely. The MgCl2·6H2O solution was added to the three-necked flask using a peristaltic pump, and the stirring speed was increased until a relatively stable dispersion of magnesium hydroxide particles was formed. Finally, 5 g of sodium chloride, 5 g of sodium nitrite, and 10 g of anhydrous ethanol were added to the flask and stirred thoroughly to obtain the aqueous phase liquid.

[0048] (3) Preparation of polyacrylate nanospheres: The oil phase liquid was added to the aqueous phase liquid at a ratio of 1:4.5, and emulsified at 4000 rpm for 5 min using a homogenizer to ensure sufficient dispersion of the oil phase liquid in the aqueous phase liquid. The system was heated to 65℃ in a water bath and reacted for 9 h with mechanical stirring at 200 rpm to obtain a polyacrylate nanosphere suspension. 5% (w / w) dilute hydrochloric acid was added dropwise to the polyacrylate nanosphere suspension to adjust the pH to 3.5, and the mixture was stirred for 30 min to remove magnesium hydroxide. The nanospheres were washed three times with water and filtered, then dried at 50℃ for 24 h to obtain polyacrylate nanospheres.

[0049] Preparation Example 3: A method for preparing polyacrylate nanospheres (methyl methacrylate: methyl acrylate = 1:3), the specific process is as follows:

[0050] (1) Preparation of oil phase: 100 g of methyl methacrylate, 300 g of methyl acrylate, 2 g of azobisisobutyronitrile, 25 g of 1,4-butanediol dimethacrylate and 120 g of n-hexane were added to the reaction vessel and stirred and mixed evenly to obtain the oil phase liquid.

[0051] (2) Preparation of the aqueous phase: 200 g of NaOH was added to 400 g of deionized water and dissolved completely. The solution was then transferred to a three-necked flask, and 5 g of sodium dodecyl sulfate was added. The mixture was stirred thoroughly for 25 min. 1200 g of MgCl2·6H2O was added to 400 g of distilled water and dissolved completely. The MgCl2·6H2O solution was added to the three-necked flask using a peristaltic pump, and the stirring speed was increased until a relatively stable dispersion of magnesium hydroxide particles was formed. Finally, 5 g of sodium chloride, 5 g of sodium nitrite, and 10 g of anhydrous ethanol were added to the flask and stirred thoroughly to obtain the aqueous phase liquid.

[0052] (3) Preparation of polyacrylate nanospheres: The oil phase liquid was added to the aqueous phase liquid at a ratio of 1:8, and emulsified at 4000 rpm for 5 min using a homogenizer to ensure thorough dispersion of the oil phase liquid in the aqueous phase liquid. The system was heated to 70℃ in a water bath and reacted for 6 h under mechanical stirring at 200 rpm to obtain a polyacrylate nanosphere suspension. 5% (w / w) dilute hydrochloric acid was added dropwise to the polyacrylate nanosphere suspension to adjust the pH to 3.5, and the mixture was stirred for 30 min to remove magnesium hydroxide. The mixture was washed three times with water and filtered, then dried at 50℃ for 24 h to obtain polyacrylate nanospheres.

[0053] Preparation of Comparative Example 1: The difference between Comparative Example 1 and Preparation Example 1 is that no initiator was used in the preparation of the polyacrylate nanospheres. The specific process is as follows:

[0054] (1) Preparation of oil phase: 20 g of methyl methacrylate, 300 g of methyl acrylate, 4 g of 1,4-butanediol dimethacrylate and 95 g of n-hexane were added to the reaction vessel and stirred and mixed evenly to obtain an oil phase liquid without the initiator azobisisobutyronitrile.

[0055] (2) Preparation of aqueous phase and preparation of polypropylene nanospheres are the same as in preparation example 1.

[0056] Preparation of Comparative Example 2: The difference between Comparative Example 2 and Preparation Example 1 is that no crosslinking agent was used in the preparation of the polyacrylate nanospheres. The specific preparation process is as follows:

[0057] (1) Preparation of oil phase: 20 g of methyl methacrylate, 300 g of methyl acrylate, 0.3 g of azobisisobutyronitrile and 95 g of n-hexane were added to the reaction vessel and stirred until uniform. No crosslinking agent 1,4-butanediol dimethacrylate was added.

[0058] (2) The preparation of aqueous phase and microspheres are the same as in preparation example 1.

[0059] Preparation of Comparative Example 3: The difference between Comparative Example 3 and Preparation Example 1 is that n-hexane was not used in the preparation of polyacrylate nanospheres. The specific process is as follows:

[0060] (1) Preparation of oil phase: 20 g of methyl methacrylate, 300 g of methyl acrylate, 0.3 g of azobisisobutyronitrile and 4 g of 1,4-butanediol dimethacrylate were added to the reaction vessel and stirred and mixed evenly to obtain the oil phase liquid (without adding n-hexane).

[0061] (2) Preparation of aqueous phase and preparation of polypropylene nanospheres are the same as in preparation example 1.

[0062] The composition and content of the oil phase solution in each preparation example are shown in Table 1:

[0063] Table 1. Composition and content of oil phase solution in preparation examples

[0064] Component dosage test group Methyl methacrylate / g Methyl acrylate / g azobisisobutyronitrile / g 1,4-Butanediol dimethacrylate / g n-Hexane / g Preparation Example 1 20 300 0.3 4 95 Preparation Example 2 60 300 1.2 15 105 Preparation Example 3 100 300 2 25 120 Preparation of Comparative Example 1 20 300 0 4 95 Preparation of Comparative Example 2 20 300 0.3 0 95 Preparation of Comparative Example 3 20 300 0.3 4 0

[0065] Example 1: A method for preparing an aqueous microsphere foaming ink composition (using polyacrylate nanospheres obtained in Preparation Example 1), the specific process of which is as follows:

[0066] A water-based microsphere foaming ink composition has the following composition by weight: 10 parts polyacrylate nanospheres, 50 parts water-based polyurethane resin, 0.5 parts polyether-modified dimethyl polysiloxane (wetting and leveling agent), 1 part polydimethyl siloxane (defoamer), 0.5 parts titanate coupling agent (adhesion promoter for water-based ink), 2 parts phthalocyanine blue (water-based color paste), and 2 parts deionized water.

[0067] Preparation method:

[0068] (1) Preparation of polyurethane linking emulsion: 50 g of waterborne polyurethane resin was added to a dispersion tank and stirred at 400 rpm. 1 g of polydimethylsiloxane and 0.5 g of polyether-modified dimethylpolysiloxane were added slowly in sequence and stirred for 4 min. Then 2 g of phthalocyanine blue paste was added and stirred for another 5 min until homogeneous.

[0069] (2) Reduce the stirring speed to 200 rpm, slowly add 10 g of the polyacrylate nanospheres obtained in Preparation Example 1 into the dispersion tank, maintain the system temperature at 30℃±2℃, and stir for 8 min. Add 2 g of deionized water to adjust the viscosity, filter using a 200-mesh filter to obtain the water-based microsphere foaming ink composition.

[0070] Example 2: Preparation of an aqueous microsphere foaming ink composition (using polyacrylate nanospheres obtained in Preparation Example 2)

[0071] This embodiment provides a water-based microsphere foaming ink composition for three-dimensional printing, which has the following composition by weight: 10 parts polyacrylate nanospheres, 55 parts water-based polyurethane resin, 1.5 parts polyether-modified silicone (wetting and leveling agent), 1.5 parts modified polysiloxane (defoamer), 1.5 parts silane coupling agent (adhesion promoter for water-based ink), 6 parts phthalocyanine green (water-based color paste), and 2 parts deionized water.

[0072] Preparation method:

[0073] (1) Preparation of polyurethane linking emulsion: 55 g of waterborne polyurethane resin was added to a dispersion tank and stirred at 400 rpm. 1.5 g of modified polysiloxane and 1.5 g of polyether-modified organosilicon were added slowly in sequence and stirred for 5 min. Then 6 g of phthalocyanine green paste was added and stirred for 5 min until homogeneous.

[0074] (2) Reduce the stirring speed to 200 rpm, slowly add 10 g of the polyacrylate nanospheres obtained in Preparation Example 2 into the dispersion tank, maintain the system temperature at 35℃±2℃, and stir for 7 min. Add 2 g of deionized water and filter using a 200-mesh filter to obtain the water-based microsphere foaming ink composition.

[0075] Example 3: Preparation of an aqueous microsphere foaming ink composition (using polyacrylate nanospheres prepared in Preparation Example 3)

[0076] This embodiment provides a water-based microsphere foaming ink composition for three-dimensional printing, which has the following composition by weight: 10 parts polyacrylate nanospheres, 60 parts water-based polyurethane resin, 3 parts polyether-modified silicone and polyether-modified dimethyl polysiloxane mixed in a 1:1 weight ratio (wetting and leveling agent), 2 parts polydimethylsiloxane (defoamer), 2 parts titanate and aluminate coupling agent mixed in a 1:1 weight ratio (adhesion promoter for water-based inks), 8 parts quinacridone violet (water-based color paste), and 12 parts deionized water.

[0077] Preparation method:

[0078] (1) Preparation of polyurethane linking emulsion: 60 g of waterborne polyurethane resin was added to a dispersion tank and stirred at 400 rpm. 2 g of polydimethylsiloxane and 3 g of polyether-modified dimethylpolysiloxane were added slowly in sequence and stirred for 3 min. Then 8 g of quinacridone purple paste was added and stirred for 5 min until homogeneous. 2 g of aluminate coupling agent was then added and stirred for 3 min.

[0079] (2) The stirring speed was reduced to 200 rpm, and 10 g of the polyacrylate nanospheres obtained in Preparation Example 3 were slowly added to the dispersion tank. The system temperature was maintained at 40℃±2℃, and the mixture was stirred for 6 min. 12 g of deionized water was added, and the mixture was filtered through a 200-mesh filter to obtain the water-based microsphere foaming ink composition.

[0080] Comparative Example 1 (Polyacrylate-free nanospheres): This comparative example provides an aqueous microsphere foaming ink composition, which is composed of the following parts by weight: 60 parts of aqueous polyurethane resin, 3 parts of polyether-modified dimethyl polysiloxane (wetting and leveling agent), 2 parts of polydimethylsiloxane (defoamer), 2 parts of aluminate coupling agent (adhesion promoter for water-based ink), 8 parts of quinacridone violet (water-based color paste), and 12 parts of deionized water.

[0081] Compared to Example 3, no polyacrylate nanospheres were added.

[0082] The preparation method is the same as in Example 3 (the step of adding polyacrylate nanospheres is omitted).

[0083] Comparative Example 2 (30 parts of polyacrylate nanospheres): This comparative example provides an aqueous microsphere foaming ink composition, the composition of which is as follows by weight: 30 parts of polyacrylate nanospheres, 60 parts of aqueous polyurethane resin, 3 parts of polyether-modified dimethyl polysiloxane (wetting and leveling agent), 2 parts of polydimethylsiloxane (defoamer), 2 parts of aluminate coupling agent (adhesion promoter for water-based ink), 8 parts of quinacridone violet (water-based color paste), and 12 parts of deionized water.

[0084] Compared to Example 3, the amount of polyacrylate nanospheres was increased to 30 parts.

[0085] The preparation method is the same as in Example 3.

[0086] Comparative Example 3 (30 parts of waterborne polyurethane resin binder): This comparative example provides a waterborne microsphere foaming ink composition, the composition of which is as follows by weight: 10 parts of polyacrylate nanospheres, 30 parts of waterborne polyurethane resin binder, 3 parts of polyether-modified dimethyl polysiloxane (wetting and leveling agent), 2 parts of polydimethylsiloxane (defoamer), 2 parts of aluminate coupling agent (adhesion promoter for waterborne ink), 8 parts of quinacridone violet (waterborne color paste), and 12 parts of deionized water.

[0087] Compared to Example 3, the amount of waterborne polyurethane resin binder was reduced to 30 parts.

[0088] The preparation method is the same as in Example 3.

[0089] Comparative Example 4 (without wetting and leveling agent): 10 parts polyacrylate nanospheres, 60 parts waterborne polyurethane resin, 2 parts polydimethylsiloxane (defoamer), 2 parts aluminate coupling agent (adhesion promoter for water-based ink), 8 parts quinacridone violet (waterborne pigment), and 12 parts deionized water.

[0090] Compared to Example 3, no wetting and leveling agent was added.

[0091] The preparation method is the same as in Example 3 (the step of adding the wetting and leveling agent is omitted).

[0092] Comparative Example 5 (without defoamer): 10 parts polyacrylate nanospheres, 60 parts waterborne polyurethane resin, 3 parts polyether-modified dimethyl polysiloxane (wetting and leveling agent), 2 parts aluminate coupling agent (adhesion promoter for water-based ink), 8 parts quinacridone violet (waterborne pigment), and 12 parts deionized water.

[0093] Compared to Example 3, no defoamer was added.

[0094] The preparation method is the same as in Example 3 (the step of adding defoamer is omitted).

[0095] Comparative Example 6 (adhesive for waterless ink): 10 parts polyacrylate nanospheres, 60 parts waterborne polyurethane resin, 3 parts polyether-modified dimethyl polysiloxane (wetting and leveling agent), 2 parts polydimethylsiloxane (defoamer), 8 parts quinacridone violet (waterborne color paste), and 12 parts deionized water.

[0096] Compared to Example 3, no water-based ink adhesive was added.

[0097] The preparation method is the same as in Example 3 (the step of adding the adhesive for water-based ink is omitted).

[0098] The components and contents of each embodiment are shown in Table 2:

[0099] Table 2. Components and Contents of Examples

[0100] weight ratio test group Polyacrylate nanospheres Waterborne polyurethane resin Wetting and leveling agents Defoamer Water-based ink adhesion promoter Water-based pigments Example 1 10 50 0.5 1 0.5 2 Example 2 10 55 1.5 1.5 1.5 6 Example 3 10 60 3 2 2 8 Comparative Example 1 0 60 3 2 2 8 Comparative Example 2 30 60 3 2 2 8 Comparative Example 3 10 30 3 2 2 8 Comparative Example 4 10 60 0 2 2 8 Comparative Example 5 10 60 3 0 2 8 Comparative Example 6 10 60 3 2 0 8

[0101] Performance testing

[0102] 1. Detection of particle size distribution and thermal decomposition temperature of polyacrylate nanospheres

[0103] (1) Particle size of polyacrylate nanospheres

[0104] This experiment uses dynamic light scattering (DLS). An appropriate amount of sample is diluted with deionized water and ultrasonically dispersed for 5 min to ensure uniform dispersion. 1 mL of the dispersion is injected into the sample cell to avoid the generation of air bubbles. Test parameters are set, and the test is run. Each sample is measured 3 times, and the particle size range is recorded.

[0105] (2) Thermogravimetric analysis (TGA)

[0106] Accurately weigh 10-15 mg of sample and place it in a crucible; load the crucible into the TGA furnace and set the temperature program; run the test and record the TGA curve and DTG curve; read the thermal decomposition temperature (Td, defined as the temperature corresponding to 5% weight loss) and the residual mass.

[0107] 2. Performance Testing of Water-Based Microsphere Foaming Ink

[0108] (1) Foaming height test: The inks prepared in each example and comparative example were printed on polyester fabric through a 100-mesh screen with a film thickness of 0.3 mm. The film was heated at 140°C for 3 min, and the thickness difference before and after foaming was measured.

[0109] (2) Adhesion test: Test according to GB / T9286 cross-cut adhesion test and record the percentage of peel area.

[0110] (3) Waterproof performance test: room temperature immersion method, record the initial immersion time.

[0111] Performance test results:

[0112] 1. Performance test results of polyacrylate nanospheres:

[0113] For details on the particle size and thermal decomposition temperature of polyacrylate nanospheres, please refer to Table 3.

[0114] Table 3. Particle size and thermal decomposition temperature of polyacrylate nanospheres

[0115] experimental group Particle size / nm Thermal decomposition temperature / °C Preparation Example 1 220-360 198 Preparation Example 2 165-280 205 Preparation Example 3 145-205 215 Preparation of Comparative Example 1 200-450 180 Preparation of Comparative Example 2 200~600 176 Preparation of Comparative Example 3 240-550 196

[0116] The test results show that in Preparation Examples 1, 2, and 3, the higher the methyl methacrylate content, the lower the particle size distribution of the polyacrylate nanospheres, but the higher the thermal decomposition temperature and the higher the thermal stability. When the methyl acrylate content is high, the number of microspheres is small, but the particle size is large.

[0117] The reaction rate of the polymer in Comparative Example 1 (without initiator) was reduced, it could not spontaneously nucleate, the particle size distribution of the formed microspheres was uneven, and the thermal decomposition temperature was also reduced.

[0118] In the preparation of Comparative Example 2 (without crosslinking agent), the polymer chains could not form an effective chemical crosslinking network, resulting in a random powder structure rather than a spherical structure, a significantly widened particle size distribution, and a substantial decrease in thermal stability.

[0119] The particle size range of Comparative Example 3 (without foaming agent) was significantly increased, and the particle size distribution was uneven. In addition to its role as a foaming agent, n-hexane also acts as a solvent in the oil phase of the polyacrylate nanospheres, which helps to disperse the reactants evenly and form uniform nanospheres.

[0120] 2. Performance test results of water-based microsphere foaming ink:

[0121] The performance test results of water-based microsphere foaming ink are shown in Table 4:

[0122] Table 4. Performance test results of water-based microsphere foaming ink

[0123] experimental group Foaming height (mm) Adhesion (peel-off rate) Initial soaking time (s) Example 1 0.75 1% 135 Example 2 0.68 2% 125 Example 3 0.52 3% 110 Comparative Example 1 0.05 18% 80 Comparative Example 2 0.85 2% 105 Comparative Example 3 0.49 20% 124 Comparative Example 4 0.38 8% 115 Comparative Example 5 0.65 3% 125 Comparative Example 6 0.50 15% 105

[0124] The experimental results show that Examples 1-4 all exhibited good foaming height (0.52-0.75 mm) and excellent adhesion (peel rate 1-3%), demonstrating good waterproof performance. With the increase of the proportion of polyacrylate nanospheres (Examples 1, 2, and 3), the foaming height and waterproof performance improved. Example 1, using 10 parts polyacrylate nanospheres and 50 parts polyurethane resin, showed the best overall performance.

[0125] Comparative Example 1 (without polyacrylate nanospheres) showed a foaming height of 0.05 mm and a significant decrease in foaming ability. Polyacrylate nanospheres are the most critical factor in the foaming of water-based microsphere foaming inks.

[0126] Comparative Example 2 (with the amount of polyacrylate nanospheres increased to 30 parts) showed a foaming height of 0.85 mm, enhancing the foaming ability of the water-based microsphere foaming ink and improving the adhesion of water-based pigments. However, excessive use of polyacrylate nanospheres resulted in overly dense pores, which could lead to pore merging. Additionally, the ink was prone to uneven heating, ultimately resulting in uneven pore size distribution and a rough, uneven foamed surface.

[0127] In Comparative Example 3 (where the amount of polyurethane resin binder was reduced to 30 parts), the pigment peeling rate in the water-based microsphere foaming ink was significantly increased, while the adhesion was decreased, indicating that polyurethane resin plays a significant role in improving pigment adhesion.

[0128] Comparative Example 4 (without wetting and leveling agent) showed a slight decrease in foam height (0.38 mm) and an increase in peel rate to 8%, indicating that the wetting and leveling agent helps to achieve uniform ink coating and microsphere dispersion.

[0129] Comparative Example 5 (without defoamer) had no significant effect on foaming height, but the presence of foam led to uneven pigment dispersion and a significant decrease in ink adhesion.

[0130] Comparative Example 6 (without adhesion promoter) showed a significant decrease in adhesion to 15%, verifying the necessity of adhesion promoter for the bonding strength between ink and substrate.

[0131] In summary, the ink composition of the present invention achieves high foaming effect, excellent adhesion and good waterproof performance through the synergistic effect of polyacrylate nanospheres and waterborne polyurethane resin, combined with a reasonable combination of various additives, resulting in clearly visible foamed microspheres.

[0132] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A water-based microsphere foaming ink composition for three-dimensional printing, characterized in that, Includes the following components by weight: 10 parts polyacrylate nanospheres, 50-60 parts waterborne polyurethane resin, 0.5-3 parts wetting and leveling agent, 1-2 parts defoamer, 0.5-2 parts waterborne ink adhesion promoter, 2-8 parts waterborne pigment, and 2-12 parts deionized water.

2. The aqueous microsphere foaming ink composition according to claim 1, characterized in that, The preparation method of the polyacrylate nanospheres is as follows: (1) Preparation of oil phase: Methyl methacrylate, methyl acrylate, azobisisobutyronitrile, 1,4-butanediol dimethacrylate and n-hexane were added to the reaction vessel and stirred to obtain oil phase liquid; (2) Preparation of aqueous phase: Add NaOH to deionized water and dissolve it completely. Transfer the NaOH solution to a three-necked flask, add sodium dodecyl sulfate, and stir thoroughly for 20-30 min. Add MgCl2·6H2O to distilled water and dissolve it completely for later use. Use a peristaltic pump to add the MgCl2·6H2O solution to the three-necked flask and increase the stirring speed to form a relatively stable magnesium hydroxide particle dispersion. Finally, add sodium chloride, sodium nitrite, and anhydrous ethanol to the flask and stir thoroughly to obtain an aqueous phase liquid. (3) Preparation of polyacrylate nanospheres: The prepared oil phase liquid was added to the aqueous phase liquid and emulsified by a homogenizer to fully disperse the oil phase liquid in the aqueous phase liquid. The water bath temperature was heated to 60~70℃ and reacted for 6~12 hours under mechanical stirring at 150-400 rpm to initially obtain a polyacrylate nanosphere suspension. Dilute hydrochloric acid was added dropwise to the polyacrylate nanosphere suspension to adjust the pH to about 3-4. After stirring for a period of time, magnesium hydroxide was removed, and the mixture was washed with water 3-5 times and filtered. After drying, polyacrylate nanospheres were obtained.

3. The method for preparing polyacrylate nanospheres according to claim 2, characterized in that, The weight ratio of methyl methacrylate, methyl acrylate, azobisisobutyronitrile, 1,4-butanediol dimethacrylate and n-hexane in (1) is (20-100):300:(0.3-2):(4-25):(95-125).

4. The method for preparing polyacrylate nanospheres according to claim 2, characterized in that, The weight ratio of NaOH and MgCl2·6H2O in (2) is 1:2-6.

5. The method for preparing polyacrylate nanospheres according to claim 2, characterized in that, The weight ratio of the oil phase liquid to the water phase liquid in (3) is 1:2-8.

6. The aqueous microsphere foaming ink composition according to claim 1, characterized in that, The wetting and leveling agent is any one or a mixture of two of polyether-modified organosilicon and polyether-modified dimethylpolysiloxane.

7. The aqueous microsphere foaming ink composition according to claim 1, characterized in that, The defoamer is any one of polydimethylsiloxane or modified polysiloxane.

8. The aqueous microsphere foaming ink composition according to claim 1, characterized in that, The adhesion promoter for the water-based ink is any one or a mixture of multiple silane coupling agents, titanate coupling agents, and aluminate coupling agents.

9. The aqueous microsphere foaming ink composition according to claim 1, characterized in that, The aqueous colorant is any one of phthalocyanine blue, phthalocyanine green, and quinacridone violet.

10. A method for preparing the aqueous microsphere foaming ink composition according to any one of claims 1-9, characterized in that, Includes the following steps: (1) Preparation of polyurethane linking emulsion: Add waterborne polyurethane resin to a dispersion tank and stir at a speed of 400 rpm. Add liquid additives such as defoamer and wetting agent in sequence and stir for 3-5 min. Add waterborne color paste and mix evenly. (2) Reduce the stirring speed to 200 rpm, slowly add polyacrylate nanospheres into the dispersion tank, keep the system temperature at 25~40℃, stir for 6~8 min, add an appropriate amount of deionized water, filter with a 200 mesh filter to obtain the water-based microsphere foaming ink composition.