A method for preparing a yarn tube paper from a maranta residue

By combining banana taro residue with recycled waste paper pulp and wood pulp short fiber through a composite formula and modification process, the problem of unstable fiber uniformity and strength in the production of yarn tube paper was solved, achieving the effect of effectively reducing costs and improving paper quality.

CN123133218APending Publication Date: 2026-11-20贵州鹏昇(集团)纸业有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611411884.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, when agricultural waste such as crop straw, bagasse, and bamboo shavings are used to replace short fibers from wood pulp to prepare yarn tube paper, there are problems such as poor fiber uniformity, unstable strength, high impurity content, and complex pretreatment processes, resulting in high production costs and an inability to effectively reduce raw material price fluctuations.

Method used

A composite formula combining banana taro residue, recycled waste paper pulp, and wood pulp short fiber is adopted. Through a gentle warm water soaking and rubbing modification process, interfering components such as gum and starch in the banana taro residue are removed. Combined with cationic starch and alkyl ketene dimers as functional additives, a gradient three-dimensional interwoven structure is formed to achieve a high proportion of wood pulp short fiber replacement.

Benefits of technology

It achieves a high proportion (30%~50%) replacement of wood pulp short fiber, reduces raw material costs by 30%~45%, improves the production stability and market competitiveness of yarn tube paper, ensures the uniformity, flatness and strength of paper, and avoids fiber bonding loss and impurity interference.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the technical field of bobbin paper processing, and relates to a preparation method of bobbin paper prepared from canna residue, comprising the following steps: S1, selecting non-molded canna residue, removing impurities, cleaning, drying, crushing, and sieving; soaking in warm water, dehydrating after soaking, rubbing and separating after dehydrating, and obtaining modified canna residue for standby; S2, separately beating waste paper recycled pulp and wood pulp short fibers; adding wood pulp short fibers to the waste paper recycled pulp, and adding the modified canna residue, then uniformly stirring to form a composite fiber slurry; S3, removing impurities from the composite fiber slurry, controlling the impurity content in the composite fiber slurry to be less than or equal to 3%, and adding a functional additive to the composite fiber slurry; S4, feeding the uniformly stirred composite fiber slurry in S3 into a special paper machine for bobbin paper to be formed by being cast; drying the formed paper sheet; S5, performing calendering treatment on the dried paper sheet; and finally obtaining finished bobbin paper. The present application is used to realize the reuse of agricultural waste in the bobbin paper processing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of yarn tube paper processing technology, specifically to a method for preparing yarn tube paper from banana and taro residue. Background Technology

[0002] Yarn tube paper is a specialized industrial paper used in the textile industry, primarily for the preparation of textile yarn tubes, thread tubes, and paper rolls. It requires moderate fiber strength, uniform fiber distribution, low impurities, low ash content, and stable physicochemical properties. Currently, the main raw material for yarn tube paper production in the industry is wood pulp staple fiber. As a scarce forestry resource derivative, wood pulp staple fiber has consistently high prices, and its price fluctuates dramatically due to factors such as forestry policies, market supply and demand, and international trade, directly leading to a continuous increase in the production cost of yarn tube paper.

[0003] To reduce the cost of papermaking raw materials, existing technologies have included research and applications of using agricultural waste such as crop straw, bagasse, and bamboo shavings to replace part of the wood pulp fiber in the preparation of industrial paper. However, existing alternative raw materials generally have drawbacks: First, most agricultural waste fibers are uneven in thickness, have high levels of impurities and cells, and exceed the standards for ash and impurities. Directly replacing short wood pulp fibers will result in poor fiber uniformity, unstable strength, and excessively high impurity content in the yarn tube paper, failing to meet the production standards for high-end yarn tube paper. Second, the addition ratio of existing alternative raw materials is generally low, mostly below 20%, resulting in limited cost reduction and efficiency improvement effects and failing to effectively alleviate the production pressure caused by fluctuations in raw material prices. Third, most agricultural waste pretreatment processes are complex, requiring high-temperature cooking, multiple bleaching, and deep deashing processes, which increase equipment and energy costs, offsetting the cost advantages of raw material substitution and resulting in low industrial application value.

[0004] Taro is a widely cultivated economic crop in Southwest and South my country, with high yields and low planting costs. Taro residue, a byproduct of taro starch processing, is produced in huge quantities annually. Most of this residue is directly discarded or incinerated on-site, resulting in not only a waste of biomass resources but also environmental pollution. Currently, there is no mature process in the industry for using taro residue to replace wood pulp short fibers at a high proportion for large-scale production of high-quality yarn tube paper, nor is there a suitable integrated production method for pretreatment, proportioning, and papermaking. How to efficiently and proportionally utilize taro residue to replace high-cost wood pulp short fibers, while ensuring the quality of yarn tube paper products meets standards, and significantly reduce raw material costs, is a pressing technical challenge in this field. Summary of the Invention

[0005] The present invention aims to provide a method for preparing yarn tube paper from banana and taro residue, so as to realize the reuse of agricultural waste in the yarn tube paper processing.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: a method for preparing yarn tube paper from banana taro residue, comprising the following components according to the composition ratio of 1000 kg of oven-dry yarn tube paper: 100-120 kg of wood pulp short fiber, 30-60 kg of modified banana taro residue, 1.0-3.0 kg of functional additives, with the remainder being recycled waste paper pulp; The preparation according to the group allocation ratio includes the following steps: S1. Select banana taro residue without mold, remove impurities, wash, dry and crush and sieve; soak in 40~50℃ warm water for 30~60 minutes, stirring continuously during the soaking process, dehydrate after soaking, rinse with clean water and dehydrate again, and after dehydration, knead for 10~15 minutes to loosen and dissociate the fibers of banana taro residue to obtain modified banana taro residue for later use. S2, waste paper recycled pulp and wood pulp short fiber are fed into pulping equipment for pulping, and the degree of freeness is controlled at 35~45°SR; according to the composition ratio of 1000kg oven-dry yarn tube mass, wood pulp short fiber is added to waste paper recycled pulp, and modified banana taro residue is added, and then stirred at a uniform speed for 20~30min to form composite fiber pulp. S3, Perform multi-stage screening and centrifugation to remove fine impurities and undissociated pulp from the composite fiber pulp, control the impurity content in the composite fiber pulp to ≤3%, add functional additives to the composite fiber pulp, and then stir evenly; S4, the composite fiber slurry that was mixed evenly in S3 is fed into a special papermaking machine for tube paper to form the paper. The papermaking speed and wire pressure are stabilized to ensure uniform paper sheet formation. The formed paper sheet is dried in a multi-stage gradient to gradually remove moisture and control the wet basis moisture content of the finished product to ≤7.5%. S5. The dried paper is calendered to flatten the paper surface and ensure uniform thickness. Finally, after winding, slitting, and inspection, the finished yarn tube paper is obtained.

[0007] Preferably, as an improvement, when soaking the banana taro residue in warm water in step S1, the solid-liquid ratio is 1:4~6; and the kneading speed is 150~200 r / min.

[0008] Preferably, as an improvement, each 1000 kg of oven-dry yarn tube paper contains 100 kg of wood pulp short fiber and 50 kg of modified banana taro residue.

[0009] Preferably, as an improvement, the functional additives include a starch enhancer and a waterproofing agent, wherein the mass ratio of the starch enhancer and the waterproofing agent is 2 to 10:1, the starch enhancer is a modified starch enhancer selected from one or more of cationic starch, amphoteric starch, and oxidized starch; and the waterproofing agent is an alkyl ketene dimer.

[0010] The advantages of this invention compared to the prior art are: 1. This invention employs a composite formula combining recycled waste paper pulp matrix, wood pulp short fiber reinforcement, and banana leaf residue functional modification, achieving a high-proportion replacement of expensive wood pulp short fiber with banana leaf residue (30%–50%). Both banana leaf residue and recycled waste paper pulp are low-cost, renewable solid waste resources with stable supply and minimal price fluctuations. This effectively avoids production cost fluctuations caused by changes in wood pulp prices, reducing overall raw material costs by 30%–45%, and significantly enhancing the production stability and market competitiveness of yarn tube paper manufacturers.

[0011] 2. Recycled pulp from waste paper suffers from defects such as fiber aging, high rigidity, and poor interlacing bonding. Further compounding with agricultural short fiber waste further damages the pulp's interlacing network, resulting in loose paper, reduced strength, and a dull paper surface, making it impossible to produce high-quality yarn tube paper. The industry generally avoids this compounding system. This invention uses a gentle warm water impurity removal and mild sizing modification process to precisely remove interfering components such as gums, starch, and sugars from banana root residue that affect fiber bonding, while retaining the excellent flexibility of the original short fibers. Modified banana root residue fine fibers precisely fill the fiber pores formed by the interlacing of recycled pulp and wood pulp short fibers, creating a gradient three-dimensional interlacing structure with "coarse fiber skeleton support, medium fiber strength enhancement, and fine fiber dense filling." This effectively compensates for the weak fiber bonding of waste paper pulp while avoiding the flocculation defects of banana root residue fibers. The finished paper exhibits uniform light yellow fiber bundles, with significantly better flatness, density, and uniformity than conventional waste paper pulp composite yarn tube paper.

[0012] 3. Banana taro residue contains residual starch and anionic impurities. Adding alkyl ketone dimers alone results in easy hydrolysis and poor retention. Cationic starch, on the one hand, compensates for the loss of fiber bonding force caused by the substitution of short fibers and improves the ring crush strength of paper. On the other hand, it can act as a protective colloid for AKD, inhibiting premature hydrolysis of AKD and improving the retention and sizing efficiency of waterproofing agents in banana taro residue pulp. Under the condition of high-proportion substitution of short fibers, excellent paper strength and moisture resistance can be obtained at the same time. Detailed Implementation

[0013] The following detailed description illustrates the specific implementation method: Example 1: A method for preparing yarn tube paper from banana taro residue, comprising the following components based on the mass ratio of 1000 kg of oven-dry yarn tube paper: 100.0 kg of wood pulp short fiber, 30.0 kg of modified banana taro residue, 1.0 kg of functional additives, with the remainder being recycled waste paper pulp.

[0014] The preparation according to the group allocation ratio includes the following steps: S1. Select mold-free banana taro residue, remove impurities, wash, dry, crush and pass through a 40-mesh sieve; soak in 40℃ warm water for 60 minutes with a solid-liquid ratio of 1:4, stirring continuously during the soaking process; dehydrate after soaking, then rinse with clean water and dehydrate again; after dehydration, knead at 150r / min for 10 minutes to loosen and dissociate the banana taro residue fibers, and obtain modified banana taro residue for later use.

[0015] S2, waste paper recycled pulp and wood pulp short fiber are fed into pulping equipment for pulping, and the degree of pulping is controlled at 35°SR; according to the composition ratio of 1000kg oven-dry yarn tube mass, wood pulp short fiber is added to waste paper recycled pulp, and modified banana taro residue is added, and then stirred at a uniform speed for 20 minutes to form composite fiber pulp.

[0016] S3. Perform multi-stage screening and centrifugation to remove fine impurities and undissociated pulp from the composite fiber pulp, controlling the impurity content in the composite fiber pulp to ≤3%. Add functional additives to the composite fiber pulp, and control the pH of the composite fiber pulp at 7.5. The functional additives are a starch reinforcing agent and a waterproofing agent with a mass ratio of 2:1. The starch reinforcing agent is cationic starch, and the waterproofing agent is an alkyl ketene dimer. Then stir evenly.

[0017] S4. The composite fiber slurry that has been mixed evenly in S3 is fed into a special papermaking machine for yarn tube paper to form the paper. The papermaking speed and wire pressure are stabilized to ensure uniform paper sheet formation. The formed paper sheet is dried in a multi-stage gradient to gradually remove moisture and control the wet basis moisture content of the finished product to ≤7.5%.

[0018] S5. The dried paper is calendered to flatten the paper surface and ensure uniform thickness. Finally, after winding, slitting, and inspection, the finished yarn tube paper is obtained.

[0019] Example 2 A method for preparing yarn tube paper from banana taro residue, comprising the following components based on the mass ratio of 1000 kg of oven-dry yarn tube paper: 120.0 kg of wood pulp short fiber, 60.0 kg of modified banana taro residue, 3.0 kg of functional additives, with the remainder being recycled waste paper pulp.

[0020] The preparation according to the group allocation ratio includes the following steps: S1. Select mold-free banana taro residue, remove impurities, wash, dry, crush and pass through a 40-mesh sieve; soak in 50℃ warm water for 30 minutes with a solid-liquid ratio of 1:6, stirring continuously during the soaking process; dehydrate after soaking, then rinse with clean water and dehydrate again; after dehydration, knead at 200r / min for 15 minutes to loosen and dissociate the banana taro residue fibers, and obtain modified banana taro residue for later use.

[0021] S2, waste paper recycled pulp and wood pulp short fiber are fed into pulping equipment for pulping, and the degree of pulping is controlled at 45°SR; according to the composition ratio of 1000kg oven-dry yarn tube mass, wood pulp short fiber is added to waste paper recycled pulp, and modified banana taro residue is added, and then stirred at a uniform speed for 30 minutes to form composite fiber pulp.

[0022] S3. Perform multi-stage screening and centrifugation to remove fine impurities and undissociated pulp from the composite fiber pulp, controlling the impurity content in the composite fiber pulp to ≤3%. Add functional additives to the composite fiber pulp, and control the pH of the composite fiber pulp at 7.5. The functional additives are starch reinforcing agent and waterproofing agent in a mass ratio of 10:1. The starch reinforcing agent is oxidized starch, and the waterproofing agent is an alkyl ketene dimer. Then stir evenly.

[0023] S4. The composite fiber slurry that has been mixed evenly in S3 is fed into a special papermaking machine for yarn tube paper to form the paper. The papermaking speed and wire pressure are stabilized to ensure uniform paper sheet formation. The formed paper sheet is dried in a multi-stage gradient to gradually remove moisture and control the wet basis moisture content of the finished product to ≤7.5%.

[0024] S5. The dried paper is calendered to flatten the paper surface and ensure uniform thickness. Finally, after winding, slitting, and inspection, the finished yarn tube paper is obtained.

[0025] Example 3 A method for preparing yarn tube paper from banana taro residue, comprising the following components based on the mass ratio of 1000 kg of oven-dry yarn tube paper: 110.0 kg of wood pulp short fiber, 40.0 kg of modified banana taro residue, 2.0 kg of functional additives, with the remainder being recycled waste paper pulp.

[0026] The preparation according to the group allocation ratio includes the following steps: S1. Select mold-free banana taro residue, remove impurities, wash, dry, crush and pass through a 40-mesh sieve; soak in 45℃ warm water for 50 minutes with a solid-liquid ratio of 1:5, stirring continuously during the soaking process; dehydrate after soaking, then rinse with clean water and dehydrate again; after dehydration, knead at 180r / min for 13 minutes to loosen and dissociate the banana taro residue fibers, and obtain modified banana taro residue for later use.

[0027] S2, waste paper recycled pulp and wood pulp short fiber are fed into pulping equipment for pulping, and the degree of pulping is controlled at 40°SR; according to the composition ratio of 1000kg oven-dry yarn tube mass, wood pulp short fiber is added to waste paper recycled pulp, and modified banana taro residue is added, and then stirred at a uniform speed for 25 minutes to form composite fiber pulp.

[0028] S3. Perform multi-stage screening and centrifugation to remove fine impurities and undissociated pulp from the composite fiber pulp, controlling the impurity content in the composite fiber pulp to ≤3%. Add functional additives to the composite fiber pulp, and control the pH of the composite fiber pulp at 7.5. The functional additives are a starch reinforcing agent and a waterproofing agent with a mass ratio of 4:1. The starch reinforcing agent is amphoteric starch, and the waterproofing agent is an alkyl ketene dimer. Then stir evenly.

[0029] S4. The composite fiber slurry that has been mixed evenly in S3 is fed into a special papermaking machine for yarn tube paper to form the paper. The papermaking speed and wire pressure are stabilized to ensure uniform paper sheet formation. The formed paper sheet is dried in a multi-stage gradient to gradually remove moisture and control the wet basis moisture content of the finished product to ≤7.5%.

[0030] S5. The dried paper is calendered to flatten the paper surface and ensure uniform thickness. Finally, after winding, slitting, and inspection, the finished yarn tube paper is obtained.

[0031] Comparative experiment To verify the technical effects of the modified banana taro residue pretreatment process and the synergistic effect of starch enhancer and alkyl ketene dimer described in this invention, the following comparative examples and embodiments were set up for performance comparison. Unless otherwise specified, the raw material ratio, beating degree, papermaking process and drying conditions of each comparative example are consistent with those of Example 3, and the basis weight of the finished paper is 180 g / m².

[0032] Comparative Example 1: No banana and taro residue was added, the amount of short wood pulp fiber was 150 kg, the remainder was recycled paper pulp, and the functional additives were the same as in Example 3.

[0033] Comparative Example 2: The banana and taro residue was not subjected to the warm water soaking and kneading modification process described in this invention. It was simply chopped and directly added to the slurry. The remaining proportions and processes were the same as in Example 1.

[0034] Comparative Example 3: No starch reinforcing agent was added to the slurry, only an alkyl ketene dimer waterproofing agent of the same mass as in Example 1 was added, and the remaining proportions and processes were the same as in Example 1.

[0035] Comparative Example 4: The amount of banana and taro residue added was 80 kg (exceeding the upper limit of this invention), wood pulp short fiber was 100 kg, and the rest was the same as in Example 1, to verify the effect of high addition amount on paper performance.

[0036] Table 1 Comparison of paper-forming performance between the examples and comparative examples.

[0037] As shown in Table 1: 1. The ring crush index, bursting index, and transverse tear strength of Examples 1 to 3 are not lower than those of Comparative Example 1 (i.e., the conventional formula with no banana taro residue and 150 kg of wood pulp short fiber). This shows that under the condition that banana taro residue replaces 30 to 60 kg of wood pulp short fiber, the paper strength is still maintained at the same level and is not deteriorated due to the addition of agricultural short fiber.

[0038] 2. Comparative Example 2, compared to Example 1, used the same amount of banana taro residue but was not soaked in warm water or subjected to kneading modification; its ring crush index increased from 7.5 N. m / g decreased to 5.4N The sizing degree decreased from 1.3 mm to 0.4 mm, and the ash content increased from 7.2% to 14.2%, indicating that if the gum, starch, sugar and anionic impurities in the banana taro residue are not removed, they will significantly damage the fiber binding and interfere with sizing. The mild modification process described in this invention is the key to high-proportion utilization of banana taro residue.

[0039] 3. Compared with Example 1, Comparative Example 3, by omitting the starch reinforcing agent, decreased the sizing degree from 1.3 mm to 0.6 mm, and the ring crush index from 7.5 N. m / g decreased to 6.1N The m / g result confirms the synergistic effect of cationic starch as a protective colloid for AKD, inhibiting its premature hydrolysis in banana residue slurry and improving its retention rate.

[0040] 4. Comparative Example 4 shows that when the amount of banana taro residue exceeds 60 kg, even with the modification process of the present invention, the ring crush index and sizing degree also show a significant decrease, indicating that the dosage range of 30-60 kg defined in the claims of the present invention is a reasonable range that takes into account both cost reduction and paper performance.

[0041] The above descriptions are merely embodiments of the present invention, and common knowledge such as specific technical solutions and / or characteristics are not described in detail here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the technical solutions of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing yarn tube paper from banana and taro residue, characterized in that, The composition of 1000kg oven-dry paper tubes includes the following components: 100-120kg wood pulp short fiber, 30-60kg modified banana taro residue, 1.0-3.0kg functional additives, and the remainder is recycled waste paper pulp. The preparation according to the group allocation ratio includes the following steps: S1. Select banana taro residue without mold, remove impurities, wash, dry and crush and sieve; soak in 40~50℃ warm water for 30~60 minutes, stirring continuously during the soaking process, dehydrate after soaking, rinse with clean water and dehydrate again, and after dehydration, knead for 10~15 minutes to loosen and dissociate the fibers of banana taro residue to obtain modified banana taro residue for later use. S2, waste paper recycled pulp and wood pulp short fiber are fed into pulping equipment for pulping, and the degree of freeness is controlled at 35~45°SR; according to the composition ratio of 1000kg oven-dry yarn tube mass, wood pulp short fiber is added to waste paper recycled pulp, and modified banana taro residue is added, and then stirred at a uniform speed for 20~30min to form composite fiber pulp. S3, Perform multi-stage screening and centrifugation to remove fine impurities and undissociated pulp from the composite fiber pulp, control the impurity content in the composite fiber pulp to ≤3%, add functional additives to the composite fiber pulp, and then stir evenly; S4, the composite fiber slurry that was mixed evenly in S3 is fed into a special papermaking machine for tube paper to form the paper. The papermaking speed and wire pressure are stabilized to ensure uniform paper sheet formation. The formed paper sheet is dried in a multi-stage gradient to gradually remove moisture and control the wet basis moisture content of the finished product to ≤7.5%. S5. The dried paper is calendered to flatten the paper surface and ensure uniform thickness. Finally, after winding, slitting, and inspection, the finished yarn tube paper is obtained.

2. The method for preparing yarn tube paper from banana and taro residue according to claim 1, characterized in that: In step S1, when soaking the banana and taro residue in warm water, the solid-liquid ratio is 1:4~6; the kneading speed is 150~200 r / min.

3. The method for preparing yarn tube paper from banana and taro residue according to claim 2, characterized in that: In every 1000 kg of oven-dry paper tubes, there are 100 kg of wood pulp short fibers and 50 kg of modified banana taro residue.

4. The method for preparing yarn tube paper from banana and taro residue according to claim 3, characterized in that: The functional additives include starch enhancers and waterproofing agents, with a mass ratio of 2 to 10:

1. The starch enhancer is a modified starch enhancer, selected from one or more of cationic starch, amphoteric starch, and oxidized starch. The waterproofing agent is an alkyl ketene dimer.