A method for consolidating low-dusting tissue paper, low-dusting tissue paper and a scratch-resistant packaging bag

By implementing regionally differentiated water-based consolidation on snowflake paper, the problem of simultaneously controlling the friction dusting on the surface of snowflake paper and the puncture and shedding in the cutting and sewing area has been solved, achieving the characteristics of low shedding, softness and scratch resistance, and full paper-based repulping.

CN123133231APending Publication Date: 2026-11-20SUZHOU MYS ENVIRONMENTAL PROTECTION & TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611288798.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously control frictional powdering in large product contact areas and puncture debris in small cutting and sewing areas on snowflake paper. Furthermore, overall surface strengthening treatment can lead to paper hardening, reduced softness, and decreased processability.

Method used

Differentiated water-based consolidation is implemented on the snowflake paper. The product contact area is consolidated with lower strength to suppress frictional powdering, while the cutting and sewing areas are consolidated with higher strength to improve local bonding strength. Regional differentiated treatment is achieved by adjusting the dry basis unit area treatment amount and penetration depth.

Benefits of technology

With lower material usage, it effectively controls frictional powdering and shedding in the cutting and sewing areas, maintains paper softness and processability, avoids paper caking, is suitable for repulping, and the scratch-resistant packaging bags reduce shedding under transportation vibration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123133231A_ABST
    Figure CN123133231A_ABST
Patent Text Reader

Abstract

The present application relates to paper surface treatment and paper-based protective packaging material technical field, especially to a kind of low-dusting tissue paper's consolidation method, low-dusting tissue paper and scratch-resistant packaging bag, consolidation method includes: providing tissue paper base paper;First aqueous consolidation solution is applied to the product contact area intended to be towards packaged product;Second aqueous consolidation solution is applied to the strip area corresponding to cutting edge, folding edge and sewing path;Drying forms two consolidation zones, and at least one of the processing capacity and penetration depth of second consolidation zone is greater than first consolidation zone;Consolidation solution is aqueous system, consolidation component can form hydrogen bond, ionic bond or physical entanglement with cellulose fiber, and drying does not form independent plastic film.The present application controls two types of dust sources with low material consumption, and gives consideration to low-dusting, soft scratch-resistant and full paper-based repulpability.Solve the problem that tissue paper friction powder and sewing area dust are difficult to be considered, and the whole surface strengthening treatment leads to paper hardening.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of paper surface treatment and paper-based protective packaging materials, and particularly to a method for consolidating low-shedding floss paper, the low-shedding floss paper, and scratch-resistant packaging bags. Background Technology

[0002] Snowflake paper, also known as down-proof paper or down paper, is a specialty paper characterized by low basis weight, high bulk, softness, and porosity. Snowflake paper is soft, lightweight, and has a friendly paper base and touch, making it a suitable alternative to non-woven fabrics for protective packaging bags of digital products.

[0003] However, the surface of the floss paper contains loosely bonded fine fibers, fillers, and processing powders. During transport and vibration, the packaged product repeatedly rubs against the inner surface of the packaging bag, causing these fine fibers, fillers, and processing powders to easily detach from the paper surface, forming powder-based debris that contaminates the surface of the packaged product. Simultaneously, the floss paper is subjected to cutting, puncture, and alternating tensile forces near the cut edges and sewing needle holes, creating another source of localized debris.

[0004] In related technologies, anti-dusting treatments for paper often involve applying starch, cellulose derivatives, microfibrillated cellulose, or polysaccharide hydrocolloids to the entire surface of the paper for sizing or coating. For example, patent application CN110088399A discloses a method for reducing paper dusting tendency by using a dispersion containing microfibrillated cellulose and starch for surface sizing. Patent application CN121871190A discloses a method for impregnating and reinforcing the edge cut surfaces of all-paper-based containers to prevent paper dust from falling off. Paper bag structures in related technologies also employ folded edges, reinforcing strips, or sewn seals.

[0005] If the entire surface of the snowflake paper is uniformly treated to meet the high strength requirements of the seam, it will cause the paper to harden, increase the coefficient of friction, reduce air permeability and softness, and increase the amount of binding material used. If only the snowflake paper is treated with a small amount of the entire surface, the strength near the needle holes and cut edges will still be insufficient, and the problem of flaking at the seam cannot be solved.

[0006] Therefore, how to control frictional powdering in large product contact areas and puncture debris in small cutting and sewing areas on the same sheet of snowflake paper with low material usage, while maintaining paper softness, processability, and repulping capability of the entire paper base, is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0007] The purpose of this invention is to address the shortcomings of existing technologies by providing a method for consolidating low-shedding lint-free paper, low-shedding lint-free paper, and scratch-resistant packaging bags. By applying differentiated water-based consolidation to the product contact area (towards the packaged product) and the strip areas corresponding to predetermined cut edges, predetermined folds, and predetermined sewing paths on the same sheet of lint-free paper, the product contact area is kept soft with a lower treatment intensity to fix loose paper particles, while the strip areas are made more flexible with a higher treatment intensity to improve local bonding strength. This solves the technical problems of simultaneously controlling surface friction dusting and puncture shedding in the cut and sewing areas, and the issue of paper hardening caused by overall surface strengthening treatment. The result is lint-free paper that combines low shedding, softness, scratch resistance, and repulpability of the entire paper base with lower material usage.

[0008] To achieve the above objectives, the present invention provides a method for consolidating low-shedding snowflake paper, comprising the following steps: S1 provides the base paper for the snowflake paper; S2, apply a first aqueous consolidation liquid to a first region of the snowflake paper base paper, the first region being the product contact area of ​​the snowflake paper base paper that is intended to face the packaged product; S3, applying a second aqueous consolidating liquid to a second region of the snow cotton paper base paper, the second region being a strip region corresponding to at least one of a predetermined cutting edge, a predetermined folding edge, and a predetermined sewing path; S4, the snowflake paper base paper processed by steps S2 and S3 is dried so that the first region forms a first consolidation zone and the second region forms a second consolidation zone, to obtain low-shedding snowflake paper. Wherein, the dry basis unit area treatment capacity of the first consolidation zone is M1, and the average penetration depth of the first consolidation zone is D1; ​​the dry basis unit area treatment capacity of the second consolidation zone is M2, and the average penetration depth of the second consolidation zone is D2; M1, M2, D1, and D2 satisfy at least one of the following conditions: M2 > M1; D2 > D1; The first aqueous consolidation solution and the second aqueous consolidation solution may have the same or different compositions. Both the first aqueous consolidation solution and the second aqueous consolidation solution contain water and at least one consolidation component. The consolidation component can form hydrogen bonds, ionic bonds or physical entanglement with cellulose fibers. No independent plastic film is formed during the drying process.

[0009] In step S1 above, the snowflake paper base paper serves as the carrier for the entire consolidation process. The thick, porous paper structure of the snowflake paper base paper forms the basis for subsequent differentiated penetration consolidation. In step S2 above, the first aqueous consolidation solution is applied to the surface layer of the product contact area at a low dosage. The consolidation components connect the loose fine powder and short fibers on the paper surface to the fiber network through hydrogen bonds, ionic bonds, or physical entanglement, thus preserving the paper's porosity. The effect of this step is to suppress frictional dusting with a low material dosage while maintaining the paper's softness and cushioning properties. In step S3 above, the second aqueous consolidation solution is applied concentratedly to the strip areas that will subsequently require cutting, folding, and sewing. This ensures that the dry basis treatment per unit area or penetration depth in this area is higher than in the product contact area. The effect of this step is to improve the local bonding strength near the cut edges and sewing needle holes, suppress the generation of puncture debris, and ensure seam strength. In step S4 above, drying removes moisture, which fixes the consolidation components in the two regions and prevents the formation of independent plastic films. The resulting snowflake paper retains its full paper-based properties and can enter the paper recycling and repulping process.

[0010] The core working principle of this invention is to allocate the consolidation treatment intensity according to the source of dust and the function of the area. Frictional dusting originates from loose particles on the paper surface in large product contact areas, where only a low treatment intensity sufficient to fix the surface dust is needed. Puncture debris originates from small areas of cut edges and sewing paths, requiring higher treatment intensity in strip areas to resist cutting and puncture. By making the dry basis unit area treatment amount M2 of the second consolidation zone greater than that of the dry basis unit area treatment amount M1 of the first consolidation zone, or by making the average penetration depth D2 of the second consolidation zone greater than that of the average penetration depth D1 of the first consolidation zone, two consolidation zones with different treatment intensities are formed on the same sheet of lint paper. This allows for the simultaneous control of two types of dust sources with a lower total material usage and avoids paper caking caused by high-intensity treatment of the entire surface.

[0011] Preferably, both M2 > M1 and D2 > D1 are satisfied, with M2 / M1 being 1.2–5.0 and M1 being 0.15–0.60 g / m³. 2 M2 is 0.75–3.00 g / m³ 2 D1 is 25% to 50% of the thickness of the snowflake paper base paper, and D2 is 70% to 100% of the thickness of the snowflake paper base paper.

[0012] In the above technical solution, when both M2 > M1 and D2 > D1 are true, the strip region has higher strength than the product contact area in both the total amount of consolidation material and the consolidation depth, resulting in a more stable balance between seam strength and paper softness. When M2 / M1 is between 1.2 and 5.0, the strip region can achieve a identifiable strength increase, while the increase in the average material usage across the entire width is limited. M1 is between 0.15 and 0.60 g / m². 2At this time, the surface powder in the product contact area can be effectively fixed and the porosity of the paper hole remains at a high level; M2 is 0.75~3.00 g / m 2 When D2 reaches 70% to 100% of the paper thickness, the fiber bond around the suture needle hole can resist the edge breakage caused by needle puncture.

[0013] Preferably, the consolidating component is selected from at least one of modified starch, cellulose derivatives, microfibrillated cellulose, nanocellulose, alginate, pectin, and guar gum; the cellulose derivative is carboxymethyl cellulose or sodium carboxymethyl cellulose.

[0014] In the above technical solutions, the listed consolidation components are all water-based materials compatible with paper fibers. They can be combined with cellulose fibers through hydrogen bonds, ionic bonds or physical entanglement. After drying, they do not form a continuous thermoplastic film that is difficult to break down, and the repulping performance of the resulting snowflake paper is not substantially affected.

[0015] Preferably, based on the total mass of the first aqueous consolidation solution, the first aqueous consolidation solution contains 0.5% to 3.0% modified starch and 0.05% to 0.5% cellulose derivative, with the remainder being water and additives; in step S3, by increasing the solid content of the second aqueous consolidation solution, increasing the number of coatings of the second aqueous consolidation solution, and extending the penetration time, at least one of M2 > M1 and D2 > D1 is achieved.

[0016] In the above technical solution, the modified starch forms a film after drying and fixes the paper powder, while the cellulose derivative acts as a thickener and bridges the fine powder. Both can form an effective surface consolidation even at low concentrations. Increasing the solid content, increasing the number of coatings, or extending the penetration time can all improve the treatment intensity of the strip area without changing the chemical system of the consolidation solution. The process is simple to implement and compatible with existing surface sizing and coating equipment.

[0017] Preferably, the total solid content of the first aqueous consolidation solution and the second aqueous consolidation solution is independently 0.5% to 6.0%; the drying temperature in step S4 is 40 to 90°C.

[0018] In the above technical solution, when the solid content is in a low concentration range of 0.5% to 6.0%, the penetration depth of the consolidation solution into the paper surface is controllable, preventing the consolidation components from accumulating and forming a film on the paper surface. A drying temperature of 40 to 90°C can remove moisture without causing high-temperature embrittlement of the paper, maintaining good bulk.

[0019] Preferably, after step S4, the method further includes a step of locally compacting the second consolidation zone, wherein the linear pressure of the local compaction is 20 to 80 N / cm, and the roller temperature of the local compaction is 40 to 60°C.

[0020] In the above technical solution, local compaction only acts on the strip where the second consolidation zone is located, increasing the density and surface strength of the seam strip and further improving the tear resistance of the seam. The product contact area is not affected by compaction, and the whole paper does not clump.

[0021] Preferably, the snowflake paper base paper in step S1 is made from bleached sulfate softwood pulp and bleached sulfate hardwood pulp, wherein the bleached sulfate softwood pulp accounts for 60% to 80% by mass and the bleached sulfate hardwood pulp accounts for 20% to 40% by mass; the freeness of the snowflake paper base paper is 28 to 38°SR, the filler content is ≤5%, the wet strength agent content is ≤0.5%, and the basis weight is 80 to 120 g / m³. 2 The thickness is 0.35 to 0.55 mm, and the snowflake paper base paper does not contain fluorescent whitening agents; step S1 also includes pretreatment of the snowflake paper base paper by dust removal and humidity conditioning.

[0022] In the above technical solution, bleached sulfate softwood pulp provides fiber length and strength skeleton, while bleached sulfate hardwood pulp improves paper surface fineness; low beating degree of 28-38°SR maintains paper sheet bulk and softness; filler dosage not exceeding 5% can reduce the source of free dust on the paper surface; wet strength agent dosage not exceeding 0.5% can avoid hindering repulping and disintegration; dust removal and moisture conditioning pretreatment only remove free dust and do not change the bonding state of paper surface fibers.

[0023] A low-shedding lint-free paper of the present invention includes a first consolidation zone and a second consolidation zone. The first consolidation zone is formed in the product contact area of ​​the low-shedding lint-free paper, and the second consolidation zone is formed in a strip area of ​​the low-shedding lint-free paper. The strip area corresponds to at least one of a predetermined cut edge, a predetermined fold edge, and a predetermined stitching path. The dry basis unit area treatment capacity of the first consolidation zone is M1, and the average penetration depth of the first consolidation zone is D1. The dry basis unit area treatment capacity of the second consolidation zone is M2, and the average penetration depth of the second consolidation zone is D2. M1, M2, D1, and D2 satisfy at least one of the following conditions: M2 > M1; D2 > D1. The consolidation components of the first consolidation zone and the consolidation components of the second consolidation zone are each capable of independently forming hydrogen bonds, ionic bonds, or physical entanglements with cellulose fibers. The low-shedding lint-free paper does not contain an independent plastic coating.

[0024] Preferably, the low-shedding snowflake paper simultaneously satisfies M2 > M1 and D2 > D1, with M2 / M1 being 1.2–5.0 and M1 being 0.15–0.60 g / m³. 2 M2 is 0.75–3.00 g / m³ 2D1 is 25%–50% of the thickness of the low-shedding snowflake paper, and D2 is 70%–100% of the thickness of the low-shedding snowflake paper; the binding component is selected from at least one of modified starch, cellulose derivatives, microfibrillated cellulose, nanocellulose, alginate, pectin, and guar gum; the base paper of the low-shedding snowflake paper is made from 60%–80% bleached sulfate softwood pulp and 20%–40% bleached sulfate hardwood pulp, with a freeness of 28–38°SR, filler content ≤5%, and basis weight of 80–120 g / m³. 2 .

[0025] In the above technical solution, the low-shedding snowflake paper remains soft and has low friction and dust loss in the product contact area, and has higher local bonding strength in the strip area. The differentiated structure of the two consolidation zones is quantitatively defined by the dry basis unit area treatment and average penetration depth, and the product structure is clear and detectable.

[0026] The present invention provides a scratch-resistant packaging bag made of the aforementioned low-shedding lint-free paper. The cut edge of the scratch-resistant packaging bag is folded into the non-product contact side of the scratch-resistant packaging bag, and the seam of the scratch-resistant packaging bag passes through the second bonding area.

[0027] In the above technical solution, after the cut edge is folded into the non-product contact side, the debris generated by the cut edge will not come into contact with the packaged product; the sewing thread passes through the reinforced second consolidation zone, the edge of the needle hole is not easy to break, the sewing strength is high, and the packaging bag releases less debris to the packaged product under transportation vibration, forming a scratch-proof protection for the surface of the packaged product.

[0028] Preferably, the cut edge is double-folded toward the non-product contact side; the sewing thread is cellulose-based sewing thread, which is selected from at least one of combed cotton sewing thread, regenerated cellulose filament sewing thread, and paper twist thread; the stitch length is 3-5 mm.

[0029] In the above technical solution, the double fold wraps the cut surface inside the folded edge, further isolating debris; the cellulose-based stitching and the paper base are both cellulose materials, and the stitching area and the paper base are consistent in the repulping and degradation path; when the stitch spacing is 3-5mm, both the needle density and the stitch strength are taken into account.

[0030] Preferably, the scratch-resistant packaging bag has an opening, a folded opening, or a paper-based seal; the scratch-resistant packaging bag is used to contain easily scratched products, including mobile phones, tablets, laptop accessories, headphones, camera equipment, surface decorative parts, precision metal parts, or precision glass parts.

[0031] Compared with related technologies, the present invention has the following advantages: First, the treatment intensity is allocated according to the source of dust. The large-area product contact area is treated with only the lower treatment intensity required to maintain softness, while the small-area strip area is treated with a higher treatment intensity. Compared with the high-intensity treatment of the whole surface, the average amount of binding material used across the whole width is reduced, the whole paper does not clump, and the soft and fluffy characteristics of the snowflake paper are maintained.

[0032] Secondly, the first consolidation zone fixes loose paper particles to suppress frictional dusting, while the second consolidation zone increases the local bonding strength near the suture needle holes and the cut edge to suppress puncture debris. Combined with the structure where the cut edge folds into the non-product contact side, both types of dust sources are controlled simultaneously. The anti-scratch packaging bag provides significantly better protection for the surface of the packaged product than a single treatment method.

[0033] Third, the consolidation components are all water-based materials that can form hydrogen bonds, ionic bonds or physical entanglement with cellulose fibers. The drying process does not form an independent plastic film. The resulting snowflake paper and scratch-resistant packaging bags retain the properties of a full paper base and can enter the paper recycling and repulping path, which is compatible with the degradable design direction. Attached Figure Description

[0034] Fig. 1 This is a process flow diagram of the consolidation method for the low-shedding snowflake paper of the present invention. Fig. 2 This is a schematic diagram of the differentiated consolidation region of the low-shedding snowflake paper of the present invention; Fig. 3 This is a schematic diagram showing the working state of the scratch-resistant packaging bag of the present invention.

[0035] The reference numerals in the figures include: 11. First consolidation zone; 12. Second consolidation zone; 21. Easily scratched products. Detailed Implementation

[0036] refer to Figs. 1 to 3 The present invention will be further described in detail below with reference to specific embodiments and comparative examples. The following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.

[0037] In this specification, "snowflake paper" refers to a special type of paper that is primarily composed of cellulose fibers, has a low basis weight, high bulk, and is soft and porous. The typical basis weight of snowflake paper is 80–120 g / m³. 2 Typical thickness is 0.35–0.55 mm, with a loose thickness of approximately 4.7 cm. 3 / g, air permeability of 500-800 mL / min, both sides are uncoated paper, without plastic coating, short fibers and a small amount of free powder are visible on the paper surface. Dry basis unit area treatment refers to the oven-dry mass of the consolidated component remaining on a unit area of ​​paper after the consolidation solution has dried, which is calculated by converting the solid content of the consolidation solution to the wet coating amount, and the unit is g / m². 2The average penetration depth refers to the proportion of the paper thickness to which the binding component penetrates. The determination method is as follows: when the binding component is mainly starch, an iodine-potassium iodide solution is used for color development; when the binding component is mainly cellulose derivatives, methylene blue is used as a tracer. After sampling, frozen sections are prepared, and the proportion of the colored layer thickness to the paper thickness is measured under an optical microscope. Each group should have at least three parallel samples, and the average value and standard deviation are reported. In this specification, the filler and wet strength agent dosages are based on oven-dry pulp mass.

[0038] In step S2, the first aqueous consolidation liquid can be applied by spraying, roller coating, printing, or spot coating. In step S3, the second aqueous consolidation liquid can be applied by dipping, brushing, or repeated coating 2 to 3 times. Alternatively, the treatment intensity of the second consolidation zone can be higher than that of the first consolidation zone by increasing the solid content of the second aqueous consolidation liquid, extending the penetration time, or locally compacting the second consolidation zone. The drying in step S4 can be carried out using hot air, infrared, or other drying methods suitable for paper materials. One optional drying process is as follows: first, pre-dry at 45±5℃ for 5-8 minutes with a hot air velocity of 1-2 m / s to reduce the moisture content to below 20%; then, perform main drying at 70±5℃ for 3-5 minutes with a hot air velocity of 2-3 m / s and dehumidify to ensure that the relative humidity of the dehumidification environment does not exceed 40% and the moisture content is reduced to 8%-12%; finally, adjust the humidity balance at 23±2℃ and 50±5% relative humidity for no less than 24 hours to ensure that the moisture content before bag making is 6±1%.

[0039] The following commercially available materials can be used as the consolidation components: modified starch such as hydroxypropyl starch, with a gelatinization temperature of 60–70℃ and a 4% paste viscosity of 200–800 mPa·s, which acts as the main consolidation component to form a film and fix the surface powder; sodium carboxymethyl cellulose, with a degree of substitution of 0.80–0.90 and a 2% solution viscosity of 300–800 mPa·s, which acts as a thickener, film-forming agent, and bridger of fine powder; microfibrillated cellulose, with an aqueous dispersion liquid-solid content of 2%–5%, fiber diameter of 20–100 nm, and an aspect ratio greater than 50, which acts as a surface fiber bridger and reinforcement agent; sodium alginate, with a 1% solution viscosity of 200–500 mPa·s, which can crosslink with calcium ions and other polyvalent metal ions to strengthen the second consolidation zone; and guar gum, with a 1% solution viscosity of 3000–5000 mPa·s, which acts as a thickener, water-retaining agent, and synergistic film-forming agent. When scratch-resistant packaging bags are used in food contact scenarios, the pulp raw materials and additives used shall be verified in accordance with GB 4806.8-2022 and GB 9685-2016.

[0040] Cellulose-based sutures are preferred. Suitable cellulose-based sutures include: 100% combed cotton thread, 60S / 3 specification, approximately 0.30 mm diameter, breaking strength not less than 9.8 N, and elongation at break of 6%–9%; regenerated cellulose filament thread, 120D / 2 specification, approximately 0.25 mm diameter, breaking strength not less than 6.0 N, and elongation at break of 12%–18%; and paper twist thread, 100–150 g / km basis weight, and 0.8–1.2 mm diameter. The stitch length should be 3–5 mm, with the final choice of thread and stitch length determined based on the achievement of acceptable tensile and tear strength at the seam.

[0041] Example 1: Preparation of low-shedding floss paper and scratch-resistant packaging bags based on modified starch and sodium carboxymethyl cellulose system This embodiment uses a scratch-resistant packaging bag as an example to illustrate the complete process of a method for consolidating low-shedding lint paper, the low-shedding lint paper, and the scratch-resistant packaging bag according to the present invention.

[0042] Step 1, Base Paper Pretreatment: Provide snowflake paper base paper, which is made of 70% bleached sulfate softwood pulp and 30% bleached sulfate hardwood pulp, with a freeness of 32°SR and a basis weight of 90 g / m³. 2 The thickness is 0.42 mm, the amount of lightweight calcium carbonate filler is 4%, and no wet strength agent or fluorescent whitening agent is added. The base paper of the snowflake paper is dusted and conditioned, and the basis weight, thickness, moisture content, surface roughness, and initial dust loss are recorded. This process removes free dust from the paper surface and stabilizes the moisture content of the base paper, providing consistent base paper conditions for the uniform penetration of the subsequent consolidation solution.

[0043] Step 2, Forming the First Consolidation Zone: Prepare the first aqueous consolidation solution, which, by total mass, contains 2.8% hydroxypropyl starch and 0.2% sodium carboxymethyl cellulose, with the remainder being water and a small amount of defoamer, resulting in a total solids content of 3.0%. Apply the first aqueous consolidation solution to the entire product contact area of ​​the wadding paper base paper facing the packaged product using a roller coating method, with a wet application rate of approximately 14 g / m². 2 The calculated dry basis unit area treatment capacity M1 is approximately 0.4 g / m². 2 In the above steps, the consolidation liquid is applied to the surface layer of the paper at a low amount. Hydroxypropyl starch and sodium carboxymethyl cellulose connect the loose fine powder and short fibers to the fiber network through hydrogen bonds. The effect of this step is to fix the surface powder while retaining the paper pores. It was measured that the average penetration depth D1 of the first consolidation zone is about 35% of the paper thickness, and no significant change was observed in the softness of the paper surface.

[0044] Step 3, Forming the Second Consolidation Zone: Prepare a second aqueous consolidation solution. The second aqueous consolidation solution is in the same chemical system as the first aqueous consolidation solution, with the total solid content increased to 4.5%. Apply the second aqueous consolidation solution twice along the strip areas containing the predetermined cutting edge, predetermined folding edge, and predetermined stitching path, using a repeated spraying method. The total wet application amount is approximately 35 g / m². 2 The equivalent dry basis unit area treatment capacity M2 is approximately 1.6 g / m². 2 The M2 / M1 ratio is approximately 4.0, and the average penetration depth D2 of the second consolidation zone is approximately 85% of the paper thickness. The purpose of this process is to ensure that the strip areas traversed by the cutting, folding, and sewing paths have a higher consolidation strength than the product contact areas, resisting edge breakage caused by subsequent cutting and needle puncture.

[0045] Step 4, Drying and Local Compaction: The snowflake paper after applying the consolidation solution undergoes pre-drying and main drying sequentially. The pre-drying temperature is 45℃ for 6 minutes, and the main drying temperature is 70℃ for 4 minutes. It is then conditioned at 23℃ and 50% relative humidity for 24 hours, resulting in a moisture content of approximately 6%. After drying, the stitching strip in the second consolidation zone is locally compacted at a linear pressure of 50 N / cm and a roller temperature of 50℃. During this process, moisture is removed, and the consolidation components are fixed in both areas without forming an independent plastic coating. Local compaction further increases the density and surface strength of the stitching strip, while the bulk and softness of the product contact area remain unaffected.

[0046] Step 5, bag making: Cut the dried low-shedding snowflake paper according to the predetermined size, fold the cut edge to the non-product contact side of the scratch-resistant packaging bag, sew it with 100% combed cotton yarn sewing thread with a stitch length of 4 mm, and pass the sewing thread through the second fixing zone. Set a folded opening at the bag opening to obtain the scratch-resistant packaging bag.

[0047] The scratch-resistant packaging bag in this embodiment undergoes the complete process described above, such as... Fig. 2 As shown, the product contact area forms a soft first bonding zone 11, and the stitching strip forms a reinforced second bonding zone 12, as... Fig. 3 As shown, the easily scratched product 21 comes into contact with the first consolidation zone 11 after being placed inside the bag. A transport vibration test was conducted on the resulting scratch-resistant packaging bag, and the powder shedding per unit area was measured to be 2.1 mg / m². 2 The average length of the pinhole edge crack is 1.3 mm; the seam tensile strength is 80 N / 50 mm; the seam tear force is 10.2 N; there is one scratch on the product surface; the softness is 44 g; the flexural stiffness is 2.0 mN·m; the surface strength is 2.4 m / s; the coefficient of dynamic friction is 0.46; the air permeability is 640 mL / min; and the average dry basis material content across the entire width is 0.9 g / m². 2 .

[0048] The working principle of the low-shedding lint-free paper consolidation method in Example 1 is as follows: Lint from the lint-free paper originates from two types of areas: large areas in contact with the product experience repeated friction with the packaged product during transport vibrations, resulting in powdering and shedding; small areas, such as cut and sewn strips, generate localized debris due to cutting and needle puncture. In this example, the consolidation strength is allocated according to the function of each area, with the product contact area having a consolidation strength of approximately 0.4 g / m² (M1). 2 The low-volume treatment fixes the surface powder and keeps it soft, with the stitched strips at an M2 of approximately 1.6 g / m. 2 The high throughput and deep penetration of 85% paper thickness enhance local bonding strength. Combined with double-fold concealment of the cut edges and cellulose-based stitching, both types of lint sources are controlled simultaneously on the same sheet of paper, and the average amount of consolidation material used across the entire width is much lower than that of the full-surface high-strength treatment scheme.

[0049] Example 2: Preparation of low-shedding floss paper and scratch-resistant packaging bags based on microfibrillated cellulose and starch system The difference between this embodiment and Embodiment 1 lies in the consolidation system and the throughput level. The first aqueous consolidation solution is an aqueous dispersion of microfibrillated cellulose and oxidized starch. The microfibrillated cellulose fibers have a diameter of 20–100 nm. The total solid content of the first aqueous consolidation solution is 1.5%. It is applied to the product contact area by spraying, with a wet application rate of approximately 10 g / m². 2 The calculated M1 is approximately 0.15 g / m³. 2 D1 is approximately 28% of the paper thickness. The total solids content of the second aqueous consolidation solution is 3.0%, and it is sprayed twice in the strip area, which translates to approximately 0.8 g / m². 2 The M2 / M1 ratio is approximately 5.0, and D2 is approximately 72% of the paper thickness. The remaining base paper, drying, and bag-making conditions are the same as in Example 1. In the above steps, microfibrillated cellulose fixes the paper surface particles through fine fiber bridging, suppressing dusting even with a low application amount; the measured dusting per unit area of ​​the resulting scratch-resistant packaging bag is 3.5 mg / m². 2 The average length of the pinhole edge crack was 1.8 mm, the tensile strength of the seam was 72 N / 50 mm, the number of scratches on the product surface was 2, and the bending stiffness was 1.8 mN·m. Replacing the microfibrillated cellulose in this embodiment with nanocellulose and implementing the same process yielded bags with comparable dust shedding and seam strength.

[0050] Example 3: Preparation of low-shedding floss paper and scratch-resistant packaging bags using an alginate ion crosslinking system The difference between this embodiment and Embodiment 1 lies in the strengthening method of the second consolidation zone. The first aqueous consolidation solution is an aqueous solution of sodium alginate with a total solid content of 2.0%, applied to the product contact area using a local printing method, with an equivalent M1 of approximately 0.5 g / m². 2D1 is approximately 45% of the paper thickness. The second aqueous consolidation solution is an aqueous sodium alginate solution with a total solids content of 6.0%, applied to the strip area by dip coating, with a calculated M2 of approximately 2.5 g / m². 2 The ratio of M2 to M1 is approximately 5.0, and D2 is approximately 95% of the paper thickness. After drying, the strip area is sprayed with a calcium chloride aqueous solution for post-treatment, forming a calcium ion-crosslinked alginate network in the second consolidation zone. In the above steps, the ion-crosslinked network further improves the wet and dry bonding strength of the stitched strip; the powder shedding per unit area of ​​the obtained scratch-resistant packaging bag is measured to be 1.8 mg / m². 2 The average length of the pinhole edge crack was 1.0 mm, the tensile strength at the seam was 88 N / 50 mm, the number of surface scratches was 1, and the bending stiffness was 2.4 mN·m. The effects of calcium salt residue on paper appearance, hygroscopicity, surface cleanliness, and repulping properties were confirmed during implementation.

[0051] Example 4: Preparation of low-shedding floss paper and scratch-resistant packaging bags This embodiment verifies the upper limit of each parameter range. The base paper of the snowflake paper is made from 80% bleached sulfate softwood pulp and 20% bleached sulfate hardwood pulp, with a freeness of 38°SR and a basis weight of 120 g / m³. 2 The thickness is 0.55 mm, the filler content is 5%, and no wet strength agent or fluorescent whitening agent is added. A first aqueous consolidation solution is prepared, containing 3.0% hydroxypropyl starch and 0.5% sodium carboxymethyl cellulose by weight, with a total solids content of 3.5%. It is applied to the product contact area using a roller coating method, with a wet application rate of approximately 17 g / m². 2 The calculated M1 is approximately 0.6 g / m³. 2 D1 is approximately 50% of the paper thickness. The second aqueous consolidation solution is from the same system as the first aqueous consolidation solution, with a total solids content of 6.0%. It is applied along the strip area with a wet application rate of approximately 50 g / m². 2 The equivalent m2 is approximately 3.0 g / m³. 2 The M2 / M1 ratio is approximately 5.0, and D2 is approximately 100% of the paper thickness. The consolidation solution is printed onto the back of the snowflake paper. It is then dried at 90℃ to a moisture content of 8%–12%. After moisture equilibration, the stitching strips are locally compacted with a linear pressure of 80 N / cm and a roller temperature of 60℃. During bag making, the cut edges are double-folded towards the non-product contact side and sewn with paper twist thread at a stitch spacing of 5 mm. The measured powder shedding per unit area of ​​the resulting scratch-resistant packaging bag is 1.5 mg / m². 2The average length of the pinhole edge crack was 0.8 mm, the tensile strength of the seam was 92 N / 50 mm, the number of scratches on the product surface was 1, and the bending stiffness was 2.8 mN·m. In this embodiment, the high upper limit of the treatment volume made the strength of the seam strip reach the highest level among all embodiments, and the bending stiffness increased, but it was still far lower than that of the comparative example 2 with full-surface high strength treatment, and the cushioning and protection of the paper surface was preserved.

[0052] Example 5: Preparation of low-shedding floss paper and scratch-resistant packaging bags This embodiment verifies the lower limit of each parameter range. The base paper of the snowflake paper is made from 60% bleached sulfate softwood pulp and 40% bleached sulfate hardwood pulp, with a freeness of 28°SR and a basis weight of 80 g / m³. 2 The thickness is 0.35 mm, the filler dosage is 5%, the wet strength agent dosage is 0.5%, and no fluorescent whitening agent is added. A first aqueous consolidation solution is prepared, containing 0.5% oxidized starch and 0.05% sodium carboxymethyl cellulose by weight, with a total solid content of 0.55%. It is applied to the product contact area in two coats, with a total wet application rate of approximately 28 g / m². 2 The calculated M1 is approximately 0.15 g / m³. 2 D1 is approximately 25% of the paper thickness. The second aqueous consolidation solution is from the same system as the first aqueous consolidation solution, with a total solids content of 2.5%. It is applied along the strip area with extended penetration time, and the wet application rate is approximately 30 g / m². 2 The equivalent M2 is approximately 0.75 g / m³. 2 The M2 / M1 ratio is approximately 5.0, and D2 is approximately 70% of the paper thickness. The paper is then dried at 40℃, and after moisture equilibration, the sewn strips are locally compacted with a line pressure of 20 N / cm and a roller temperature of 40℃. During bag making, the cut edges are double-folded towards the non-product contact side and sewn with regenerated cellulose filament thread at a stitch spacing of 3 mm. The measured dust shedding per unit area of ​​the resulting scratch-resistant packaging bag is 4.0 mg / m². 2 The average length of the pinhole edge crack was 2.4 mm, the tensile strength of the seam was 58 N / 50 mm, the number of scratches on the product surface was 3, and the bending stiffness was 1.7 mN·m. These results indicate that even when all parameters are taken at their lower limits, the amount of powder shedding from the bag is still significantly lower than that of the unconsolidated Comparative Example 1, and the seam strength is still significantly higher than that of the unreinforced seam area in Comparative Example 3. When the oxidized starch and sodium carboxymethyl cellulose in the first aqueous consolidation solution of this embodiment were replaced with 1.0% pectin and 0.4% guar gum, and the same process was followed, the powder shedding per unit area of ​​the resulting bag was 4.4 mg / m². 2 The tensile strength of the seam is 55 N / 50 mm, which also meets the requirement of low shedding.

[0053] Example 6: Preparation of low-shedding floss paper and scratch-resistant packaging bags This embodiment verifies the implementation effect under low differentiation. The base paper and pretreatment conditions of the snowflake paper are the same as in Example 1. The composition of the first aqueous consolidation solution is the same as in Example 1, with a total solids content of 3.0%, and it is applied to the product contact area by roller coating, with a wet application amount of approximately 20 g / m². 2 The calculated M1 is approximately 0.6 g / m³. 2 D1 is approximately 50% of the paper thickness. The second aqueous consolidation solution is from the same system as the first aqueous consolidation solution and has the same total solids content. It is applied along the strip area with a wet application rate of approximately 25 g / m². 2 The equivalent M2 is approximately 0.75 g / m³. 2 The ratio of M2 to M1 was approximately 1.25, and D2 was approximately 70% of the paper thickness. The paper was then dried according to the drying curve described in Example 1, with localized compaction of the sewn strips at a linear pressure of 30 N / cm and a roller temperature of 45°C. The bag-making conditions were the same as in Example 1. The measured powder shedding per unit area of ​​the resulting scratch-resistant packaging bag was 2.8 mg / m². 2 The average length of the pinhole edge crack was 1.9 mm, the tensile strength of the seam was 68 N / 50 mm, the number of scratches on the product surface was 2, and the bending stiffness was 1.9 mN·m. In this embodiment, the difference in processing volume between the second consolidation zone and the first consolidation zone was small, and the powder shedding control and seam strength of the bag were still better than those of Comparative Example 1 and Comparative Example 3, indicating that the technical effect of the present invention can still be achieved when M2 / M1 is close to 1.2.

[0054] Test Methods: The bags in each embodiment and comparative example were tested under the same conditions. Before the test, the bags were conditioned for at least 24 hours at a temperature of 23±2℃ and a relative humidity of 50±5% according to GB / T 4857.2. A standard simulated polished metal block of equal mass to the actual product was loaded inside the bag, with at least three parallel samples per group. Vibration tests were performed according to GB / T 4857.7-2005. The selected test severity for this project was: vibration frequency 10 Hz, double amplitude 2.0 mm, vertical vibration for 30 min, and vibration for 10 min each in the front-back and left-right directions; alternatively, a vertical random vibration test could be performed according to GB / T 4857.23-2021, with the random vibration spectrum selected and fully recorded according to the actual transportation environment or customer specifications. The method for determining the amount of powder shedding is as follows: A pre-weighed 0.5 μm pore size filter membrane is placed inside the bag to collect the shed material. After the test, the filter membrane is dried at 105±2℃ for 2 h and weighed. The amount of powder shedding per unit area is calculated based on the inner surface area of ​​the bag, and the unit is mg / m². 2Simultaneously, the number of scratches on the product surface is visually counted. The length of pinhole edge cracks is measured microscopically after sewing; the tensile strength of the seam is determined according to GB / T 12914 constant-rate tensile testing; the bending stiffness is determined according to GB / T 22364; the softness is determined according to TAPPI T 498; the surface strength is determined according to GB / T 2679.15; the coefficient of dynamic friction is determined according to GB / T 10006; and the air permeability is determined according to GB / T 458.

[0055] Comparative Example 1 is a packaging bag made of existing frosting paper without any consolidation treatment, with polyester sewing thread used for stitching; Comparative Example 2 is a bag whose entire surface is consolidated with the same treatment strength as the second consolidation zone; Comparative Example 3 is a bag with only the inner surface undergoing low-level consolidation and no reinforcement in the seam area. The base paper, bag dimensions, loading, and test conditions for each comparative example are the same as in the examples. Comparative Example 1 is used to characterize the dust shedding baseline of untreated frosting paper; Comparative Example 2 is used to characterize the effect of full-surface high-strength treatment on softness and material usage; and Comparative Example 3 is used to characterize the insufficient seam strength when only the product contact area is treated. The dust shedding per unit area of ​​Comparative Example 1 was measured to be 25.4 mg / m². 2 The average length of the pinhole edge crack was 7.5 mm, the tensile strength at the seam was 32 N / 50 mm, the flexural stiffness was 1.6 mN·m, and the number of scratches on the product surface was 9; the powder loss per unit area of ​​Comparative Example 2 was 3.2 mg / m². 2 The average length of the pinhole edge crack was 2.1 mm, the tensile strength at the seam was 76 N / 50 mm, the flexural stiffness was 6.2 mN·m, the softness was 85 g, the air permeability was 210 mL / min, and the average dry basis material usage across the entire width was 2.4 g / m². 2 The dust loss per unit area in Comparative Example 3 was 8.7 mg / m². 2 The average length of the pinhole edge crack was 5.4 mm, the tensile strength at the seam was 45 N / 50 mm, the flexural stiffness was 1.9 mN·m, the number of surface scratches was 5, and the average dry basis material content across the entire width was 0.6 g / m². 2 .

[0056] The experimental results show that the powder loss per unit area of ​​the bag in Example 1 was 25.4 mg / m² compared to that in Comparative Example 1. 2 Decreased to 2.1 mg / m³ 2The dust loss was reduced by 91.7%; the tensile strength at the seam increased from 32 N / 50 mm to 80 N / 50 mm, an increase of approximately 150%; the average length of the pinhole edge crack decreased from 7.5 mm to 1.3 mm; while the flexural stiffness only increased from 1.6 mN·m to 2.0 mN·m, an increase of approximately 25%, and the paper surface remained soft. The flexural stiffness of Comparative Example 2 reached 6.2 mN·m, an increase of approximately 288% compared to Comparative Example 1, the paper surface became matted and lost the cushioning and protective properties of the snowflake paper, and the average dry basis material usage across the entire width was 2.7 times that of Example 1; the tensile strength at the seam of Comparative Example 3 was only 45 N / 50 mm, and there was significant dust shedding near the pinholes. The comparison shows that although the high-strength treatment on the entire surface can reduce dust shedding, it leads to matting of the paper surface, and treating only the product contact area results in insufficient seam strength. Only by distributing the consolidation strength according to the functional differences of the area can low dust shedding, high seam strength, and low stiffness increase be achieved simultaneously.

[0057] The environmental assessment method is as follows: Laboratory fragmentation and sieving tests are conducted on the snowflake paper obtained in each embodiment. Fragmentation rate, sieve residue rate, adhesive content, pulp appearance, and pulp strength are recorded to confirm the compatibility of the consolidation system with the paper recycling and repulping pathway. If the product is to be advertised as compostable or biodegradable, additional testing will be conducted according to the applicable standards of the target market. Water-based consolidation materials are not necessarily recyclable or biodegradable; the final conclusion will be based on the standard tests of the target market.

[0058] The above description is only a preferred embodiment of the present invention. For those skilled in the art, there will be changes in the specific implementation and application scope based on the ideas of the present invention. The content of this specification should not be construed as a limitation of the present invention.

Claims

1. A method for consolidating low-shedding snowflake paper, characterized in that, Includes the following steps: S1 provides the base paper for the snowflake paper; S2, apply a first aqueous consolidation liquid to a first region of the snowflake paper base paper, the first region being the product contact area of ​​the snowflake paper base paper that is intended to face the packaged product; S3, applying a second aqueous consolidating liquid to a second region of the snow cotton paper base paper, the second region being a strip region corresponding to at least one of a predetermined cutting edge, a predetermined folding edge, and a predetermined sewing path; S4, the snowflake paper base paper processed by steps S2 and S3 is dried so that the first region forms a first consolidation zone and the second region forms a second consolidation zone, to obtain low-shedding snowflake paper. Wherein, the dry basis unit area treatment capacity of the first consolidation zone is M1, and the average penetration depth of the first consolidation zone is D1; ​​the dry basis unit area treatment capacity of the second consolidation zone is M2, and the average penetration depth of the second consolidation zone is D2. M1, M2, D1, and D2 satisfy at least one of the following conditions: M2 > M1; D2 > D1; The first aqueous consolidation solution and the second aqueous consolidation solution may have the same or different compositions. Both the first aqueous consolidation solution and the second aqueous consolidation solution contain water and at least one consolidation component, which can form hydrogen bonds, ionic bonds or physical entanglement with cellulose fibers. No independent plastic film is formed during the drying process.

2. The consolidation method according to claim 1, characterized in that, Simultaneously satisfying M2 > M1 and D2 > D1, M2 / M1 is 1.2–5.0; M1 is 0.15–0.60 g / m 2 M2 is 0.75–3.00 g / m³ 2 ; D1 is 25% to 50% of the thickness of the snowflake paper base paper, and D2 is 70% to 100% of the thickness of the snowflake paper base paper.

3. The consolidation method according to claim 1 or 2, characterized in that, The consolidating component is selected from at least one of modified starch, cellulose derivatives, microfibrillated cellulose, nanocellulose, alginate, pectin and guar gum; The cellulose derivative is carboxymethyl cellulose or sodium carboxymethyl cellulose.

4. The consolidation method according to claim 3, characterized in that, Based on the total mass of the first aqueous solidification solution, the first aqueous solidification solution contains 0.5% to 3.0% modified starch and 0.05% to 0.5% cellulose derivatives, with the remainder being water and additives; In step S3, at least one of M2 > M1 and D2 > D1 is achieved by increasing the solid content of the second aqueous consolidation liquid, increasing the number of coatings of the second aqueous consolidation liquid, and extending the penetration time.

5. The consolidation method according to claim 1 or 2, characterized in that, The total solids content of the first aqueous consolidation solution and the second aqueous consolidation solution is independently 0.5% to 6.0%; The drying temperature in step S4 is 40–90°C.

6. The consolidation method according to claim 1 or 2, characterized in that, Step S4 is followed by a step of locally compacting the second consolidation zone, wherein the linear pressure of the local compaction is 20 to 80 N / cm and the roller temperature of the local compaction is 40 to 60°C.

7. The consolidation method according to claim 1 or 2, characterized in that, The snowflake paper base paper mentioned in step S1 is made from bleached sulfate softwood pulp and bleached sulfate hardwood pulp, wherein the bleached sulfate softwood pulp accounts for 60% to 80% by mass and the bleached sulfate hardwood pulp accounts for 20% to 40% by mass. The snowflake paper base paper has a freeness of 28–38°SR, a filler content of ≤5%, a wet strength agent content of ≤0.5%, and a basis weight of 80–120 g / m³. 2 The thickness is 0.35–0.55 mm, and the snowflake paper base paper does not contain fluorescent whitening agents; Step S1 also includes pretreatment of the snowflake paper base paper by dust removal and moisture conditioning.

8. A low-shedding snowflake paper, characterized in that, It includes a first consolidation zone and a second consolidation zone, the first consolidation zone being formed in the product contact area of ​​the low-shedding lint paper, and the second consolidation zone being formed in the strip area of ​​the low-shedding lint paper, the strip area corresponding to at least one of a predetermined cut edge, a predetermined fold edge, and a predetermined sewing path; The dry basis unit area treatment capacity of the first consolidation zone is M1, and the average penetration depth of the first consolidation zone is D1; ​​the dry basis unit area treatment capacity of the second consolidation zone is M2, and the average penetration depth of the second consolidation zone is D2. M1, M2, D1, and D2 satisfy at least one of the following conditions: M2 > M1; D2 > D1; The consolidation components in the first consolidation zone and the consolidation components in the second consolidation zone can each independently form hydrogen bonds, ionic bonds, or physical entanglements with cellulose fibers, and the low-shedding snowflake paper does not contain an independent plastic coating.

9. A scratch-resistant packaging bag, characterized in that, The scratch-resistant packaging bag is made of the low-shedding snow cotton paper as described in claim 8, and the cut edge of the scratch-resistant packaging bag is folded into the non-product contact side of the scratch-resistant packaging bag, and the seam of the scratch-resistant packaging bag passes through the second consolidation area.

10. The scratch-resistant packaging bag according to claim 9, characterized in that, The cut edge is double-folded toward the non-product contact side; The suture is a cellulose-based suture, which is selected from at least one of combed cotton yarn sewing thread, regenerated cellulose filament sewing thread, and paper twist thread; The stitch spacing is 3–5 mm.

Citation Information

Patent Citations

  • A process for surface sizing using a jet cooked dispersion comprising microfibrillated cellulose, starch and pigment and / or filler

    CN110088399A

  • Enhanced protection method for edge section of full-paper-based container

    CN121871190A