Sandwiched layup silicone mica plate and preparation method and application thereof

By using a sandwich-layer structure design and combining mica paper of different surface densities with molding and curing, the performance shortcomings of mica board in terms of bending strength and impact toughness are solved, achieving improvements in high strength, stability and production consistency while maintaining insulation performance.

CN123133232APending Publication Date: 2026-11-20GOODE EIS SUZHOU CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611483279.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing mica sheets have performance shortcomings in balancing bending strength and impact toughness, and the interface problems caused by thickness differences affect mechanical stability and mass production consistency.

Method used

A sandwich structure is designed using mica paper with different surface densities. A second composite organosilicon mica board is stacked in the middle of the first composite organosilicon mica board on both sides. The difference in surface density combined with a specific symmetrical arrangement forms a sandwich structure of organosilicon mica board through molding and curing.

Benefits of technology

It improves flexural strength, tensile strength, and dynamic impact strength, reduces the dispersion of mechanical properties, enhances product stability and consistency in mass production, while maintaining continuous high-temperature resistance, dielectric strength, and flame-retardant ceramic insulation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123133232A_ABST
    Figure CN123133232A_ABST
Patent Text Reader

Abstract

The application provides a sandwiched lamination organic silicon mica plate and a preparation method and application thereof. The sandwiched lamination organic silicon mica plate comprises a first composite organic silicon mica plate, a second composite organic silicon mica plate and a first composite organic silicon mica plate which are sequentially stacked; the first composite organic silicon mica plate comprises at least one layer of first organic silicon mica paper, and the second composite organic silicon mica plate comprises at least one layer of second organic silicon mica paper; the first organic silicon mica paper adopts a first mica paper, and the second organic silicon mica paper adopts a second mica paper, and the surface densities of the first mica paper and the second mica paper are different. The sandwiched lamination organic silicon mica plate provided by the application is matched by using mica papers with different surface densities, and the second composite organic silicon mica plate is stacked between the two first composite organic silicon mica plates; the difference in surface density is combined with specific symmetrical arrangement; the sandwiched lamination organic silicon mica plate has bending, tensile and dynamic impact strength, product stability and impact delamination fracture resistance, and batch production consistency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of high temperature resistant insulating composite materials technology, and relates to a sandwich-laid organosilicon mica board, its preparation method and application. Background Technology

[0002] Organosilicon mica sheets are molded from mica paper impregnated with organosilicon resin. They possess high temperature resistance, high insulation, and flame retardant properties, making them a core material for thermal protection in power battery packs and insulation in high-voltage motors. Conventional commercial mica sheets are prepared by continuous stacking and molding of mica paper of a single basis weight (thickness). The industry mainstream classifies them into three types: single low-area-density thin mica paper (≤100g / m³). 2 ) Continuously laminated boards: mica paper is fully impregnated with resin, has strong interlayer bonding, and excellent tensile strength, but low flexural strength and impact toughness; single medium-density mica paper (100g / m²) 2 -180g / m 2 100g / m 2 and 180g / m 2 Continuously laminated boards: Mica paper has increased resin penetration difficulty, is prone to interlayer defects, exhibits large dispersion in mechanical properties, and has lower flexural strength and impact toughness; single high-area-density thick mica paper (≥180g / m²) 2 Continuously laminated boards have a high proportion of mica skeleton, but the paper body has large pores and stacking gaps, making it difficult for silicone resin to fully impregnate. After molding, there are a large number of dry spots and interconnected pores inside, resulting in a significant decrease in flexural strength, tensile strength, and impact toughness, and the material is prone to delamination and brittle fracture. It is evident that the above-mentioned single-thickness mica paper layup has obvious performance shortcomings, generally exhibiting the following defects: First, it is impossible to simultaneously achieve high flexural strength and high impact toughness, presenting a contradiction between strength and toughness; Second, high-basis-weight thick mica paper is difficult to impregnate, resulting in a large number of pores and weak interfaces inside after molding, leading to rapid crack penetration and delamination under stress, resulting in poor mechanical stability; Third, the mechanical data of single-mica paper laminates have large dispersion, and the performance of batch products fluctuates significantly, making them prone to failure and loss of thermal barrier protection under vibration and impact conditions of power batteries; Fourth, if thin and thick mica paper are directly and irregularly mixed and laminated, the high residual thermal stress between the layers due to excessive difference in basis weight makes the interface a naturally weak layer, leading to brittle delamination under stress, which in turn reduces impact performance.

[0003] Therefore, in order to address the above-mentioned defects, existing composite structures employ a mixture of thin and thick layups to improve mechanical properties. However, these are all designed for carbon fiber and glass fiber reinforced resin systems. Currently, there is no technical solution for mica-organosilicon insulating systems that uses mica paper of different areal densities (basis weights) to synergistically improve flexural strength, tensile strength, and impact toughness. Furthermore, mica paper is formed by overlapping inorganic mica flakes, and its porosity and wetting characteristics are completely different from those of fiber fabrics. The layup approach of fiber composite materials cannot be directly applied, and the performance defects of single-thickness mica paper layups cannot be significantly improved.

[0004] Therefore, based on the above-mentioned technical problems, how to provide a composite organosilicon mica board with a layered structure that takes into account bending strength, tensile strength, dynamic impact strength, product stability, and resistance to impact delamination is a technical problem that urgently needs to be solved. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this application aims to provide a sandwich-layered silicone mica board, its preparation method, and its applications. The sandwich-layered silicone mica board provided in this application uses mica papers of different areal densities, with a second composite silicone mica board layered between two first composite silicone mica boards. The difference in areal density, combined with a specific symmetrical arrangement, results in a sandwich-layered silicone mica board that balances bending strength, tensile strength, dynamic impact strength, product stability, and resistance to impact delamination. Furthermore, it exhibits low mechanical property dispersion, improved consistency in mass production, and suitability for industrial-scale mass production, adapting to existing production lines. Moreover, while still employing a silicone-mica substrate system, the sandwich-layered silicone mica board retains its original advantages in insulation and fire resistance, such as continuous high-temperature resistance, dielectric strength, and flame-retardant ceramicization.

[0006] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a sandwich-layered silicone mica board, the sandwich-layered silicone mica board comprising a first composite silicone mica board, a second composite silicone mica board and the first composite silicone mica board stacked sequentially. The first composite organosilicon mica board includes at least one layer of first organosilicon mica paper, and the second composite organosilicon mica board includes at least one layer of second organosilicon mica paper. The areal density of the first mica paper used in the first organosilicon mica paper is different from that of the second mica paper used in the second organosilicon mica paper.

[0007] In some embodiments, the thickness of the sandwich-layered silicone mica board is 0.8mm-1.5mm.

[0008] In some embodiments, the first composite organosilicon mica board includes x layers of first organosilicon mica paper, and the second composite organosilicon mica board includes y layers of second organosilicon mica paper, where x:y is 1:(1.2-3).

[0009] In some embodiments, the difference between the areal density of the first mica paper and the areal density of the second mica paper is 40 g / m³. 2 -60g / m 2 .

[0010] In some embodiments, the areal density of the first mica paper is 80 g / m³. 2 -140g / m 2 .

[0011] In some embodiments, the areal density of the second mica paper is 80 g / m³. 2 -140g / m 2 .

[0012] In some embodiments, the first organosilicon mica paper includes organosilicon resin, and the content of the organosilicon resin is 8wt%-10wt% of the mass of the first mica paper.

[0013] In some embodiments, the second organosilicon mica paper includes organosilicon resin, and the content of the organosilicon resin is 8wt%-10wt% of the mass of the second mica paper.

[0014] Secondly, this application also provides a method for preparing a sandwich-layered organosilicon mica board according to the first aspect, the method comprising the following steps: At least one layer of first organosilicon mica paper is stacked sequentially, and at least one layer of second organosilicon mica paper is stacked on the surface, and at least one layer of first organosilicon mica paper is stacked on the surface again. The resulting overall sandwich structure is molded and cured to obtain a sandwiched organosilicon mica board. The areal density of the first mica paper used in the first organosilicon mica paper is different from that of the second mica paper used in the second organosilicon mica paper.

[0015] In some embodiments, the method for preparing the first organosilicon mica paper includes: coating at least one side surface of the first mica paper with an organosilicon resin solution, and then baking it to obtain the first organosilicon mica paper.

[0016] In some embodiments, the method for preparing the second organosilicon mica paper includes: coating at least one side surface of the second mica paper with an organosilicon resin solution, and then baking it to obtain the second organosilicon mica paper.

[0017] In some embodiments, the molding curing temperature is 220°C-240°C.

[0018] In some embodiments, the pressure of the molding and curing process is 3.0 MPa-4.0 MPa.

[0019] In some embodiments, the heat preservation and pressure holding time for molding curing is 20 min to 50 min.

[0020] In some embodiments, after the molding and curing process is completed, demolding and natural cooling are also included.

[0021] Thirdly, this application also provides an application of a sandwich-laid silicone mica board, wherein the sandwich-laid silicone mica board prepared according to the method described in the first aspect or the preparation method described in the second aspect is applied to a thermal runaway fireproof insulation board, a high-temperature resistant insulation board, or a flame-retardant insulation gasket.

[0022] Compared with the prior art, this application has the following advantages: 1) The sandwich-layered silicone mica board provided in this application uses mica paper with different areal densities, and a second composite silicone mica board is stacked in the middle between the first composite silicone mica boards on both sides. The difference in areal density combined with a specific symmetrical arrangement can: 1) simultaneously improve bending strength and tensile strength, resulting in high bending resistance and high tensile load-bearing capacity; 2) synergistically improve dynamic impact strength, enhancing the fracture resistance under dynamic loads; 3) reduce the dispersion of mechanical properties, improve the consistency of mass production, and adapt to the combined working conditions of vibration, extrusion, and impact of new energy battery packs; In addition, the sandwich-layered silicone mica board provided in this application provides a matching integrated molding process, which can be industrialized for mass production without the need for additional complex equipment, is compatible with existing silicone mica board production lines, and can improve production efficiency.

[0023] 2) The sandwich-layered silicone mica board provided in this application only adjusts the layup structure and still adopts the silicone-mica substrate system. The sandwich-layered silicone mica board can still maintain the original insulation and fireproof advantages of continuous high temperature resistance of 500℃-1000℃, dielectric strength of 15kV / mm-25kV / mm, and flame-retardant ceramicization without sacrificing the basic thermal insulation performance. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the structure of the sandwich-layered silicone mica board provided in Example 1.

[0025] Among them, 1-first composite organosilicon mica board; 2-second composite organosilicon mica board; 11-first organosilicon mica paper; 21-second organosilicon mica paper. Detailed Implementation

[0026] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments. However, the examples below are merely simplified examples of this application and do not represent or limit the scope of protection of this application. The scope of protection of this application shall be determined by the claims.

[0027] In this application, technical features or solutions described using open-ended terms such as "comprising" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond those listed. For example, if A includes a1, a2, and a3, unless otherwise specified, it means that A may consist only of a1, a2, and a3, or it may include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3" and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements."

[0028] In some embodiments, this application provides a sandwich-layered organosilicon mica board, the composite organosilicon mica board comprising a first composite organosilicon mica board, a second composite organosilicon mica board and the first composite organosilicon mica board stacked sequentially; The first composite organosilicon mica board includes at least one layer of first organosilicon mica paper, and the second composite organosilicon mica board includes at least one layer of second organosilicon mica paper. The areal density of the first mica paper used in the first organosilicon mica paper is different from that of the second mica paper used in the second organosilicon mica paper.

[0029] The sandwich-layered silicone mica board provided in this application uses mica paper of different areal densities in combination, with a second composite silicone mica board layered between the first composite silicone mica boards on both sides. The difference in areal density, combined with a specific symmetrical arrangement, results in a sandwich-layered silicone mica board that balances flexural strength, tensile strength, dynamic impact strength, product stability, and resistance to impact delamination. Furthermore, it exhibits low mechanical property dispersion, improved consistency in mass production, and suitability for industrial-scale mass production, making it compatible with existing production lines. In addition, it still uses a silicone-mica substrate system, and the sandwich-layered silicone mica board retains its original advantages in insulation and fire resistance, such as continuous high-temperature resistance, dielectric strength, and flame-retardant ceramicization.

[0030] In some embodiments, the thickness of the sandwich-layered silicone mica plate is 0.8mm-1.5mm, such as 0.8mm, 0.9mm, 1.0mm, 1.1mm, 1.2mm, 1.3mm, 1.4mm or 1.5mm, preferably 0.85mm-1.15mm.

[0031] In some embodiments, the first composite organosilicon mica board includes x layers of first organosilicon mica paper, and the second composite organosilicon mica board includes y layers of second organosilicon mica paper, where x:y is 1:(1.2-3), such as 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.2, 1:2.5, 1:2.8, or 1:3, etc.

[0032] This application limits the layer ratio of the two to 1:(1.2-3) for x:y, which can realize that the sandwich-laid organosilicon mica board takes into account bending strength, tensile strength, dynamic impact strength, product stability and impact delamination fracture resistance. If the layer ratio is less than 1:1.2, the lower proportion of the core layer weakens the synergistic load-bearing effect between the surface and core layers, making the sandwich-laid silicone mica plate prone to local deformation and damage concentration during loading. This results in a decrease in the bending strength, tensile strength, and dynamic impact strength of the sandwich-laid silicone mica plate. If the layer ratio exceeds 1:3, the lower proportion of the surface layer weakens its constraint on core layer deformation and crack propagation. Under bending and impact loads, the smaller surface layer may not be sufficient to effectively disperse local surface damage, and the damage is more likely to propagate to the core layer and the interface between the surface and core layers. Under tensile loads, the damage propagation may also weaken the synergistic load-bearing capacity of each layer, resulting in varying degrees of reduction in the bending strength, tensile strength, and dynamic impact strength of the sandwich-laid silicone mica plate.

[0033] It should be noted that this application does not impose specific requirements or special limitations on the values ​​of x and y. The number of adaptive layers can be selected based on the choice of mica paper with different surface densities (different surface densities correspond to different thickness values) and the thickness of the target required interlayer silicone mica board, as long as x:y is 1:(1.2-3).

[0034] In some embodiments, the difference between the areal density of the first mica paper and the areal density of the second mica paper is 40 g / m³. 2 -60g / m 2 For example, 40g / m 2 45g / m 2 50g / m 2 55g / m 2 Or 60g / m 2 wait.

[0035] It should be noted that the difference between the areal density of the first mica paper and the areal density of the second mica paper in this application can be that the areal density of the first mica paper is greater than that of the second mica paper, exceeding it by 40 g / m². 2 -60g / m 2Alternatively, the areal density of the second mica paper could be greater than that of the first mica paper, by 40 g / m². 2 -60g / m 2 .

[0036] This application achieves a surface density difference of 40 g / m³ between the first and second mica papers. 2 -60g / m 2 To avoid excessive residual thermal stress between heterogeneous layers leading to interfacial debonding failure, a balance must be struck between static flexural strength, tensile strength, and dynamic impact strength. If the difference is too large, the increased differences in thickness, resin impregnation, and compaction behavior between the two mica papers may result in a more uneven interlayer bonding state under the same pressing conditions. This leads to uneven load transfer and localized stress concentration, making cracks more likely to initiate in weak areas and propagate along the interlayer, thus reducing the flexural strength, tensile strength, and dynamic impact strength of the sandwich-layout silicone mica board. Conversely, if the difference is too small, the structure and load-bearing characteristics of the surface and core layers may become similar, weakening the effect of differentiating the surface layer's performance and the core layer's support, and failing to effectively improve flexural strength, tensile strength, and dynamic impact strength.

[0037] In some embodiments, the areal density of the first mica paper is 80 g / m³. 2 -140g / m 2 For example, 80g / m 2 90g / m 2 100g / m 2 110g / m 2 120g / m 2 130g / m 2 Or 140g / m 2 wait.

[0038] In some embodiments, the areal density of the second mica paper is 80 g / m³. 2 -140g / m 2 For example, 80g / m 2 90g / m 2 100g / m 2 110g / m 2 120g / m 2 130g / m 2 Or 140g / m 2 wait.

[0039] This application adjusts the surface density of the first mica paper to 80 g / m³. 2 -140g / m 2 The surface density of the second mica paper is 80 g / m³. 2 -140g / m 2The difference in areal density is 40 g / m². 2 -60g / m 2 This method allows for the creation of sandwich-laid silicone mica boards that balance flexural strength, tensile strength, dynamic impact strength, product stability, and resistance to impact delamination. However, if the areal density of the first or second mica paper is too high, or both are too high, the difficulty of resin penetration and internal gas expulsion may increase. This can easily lead to weak areas such as insufficient local wetting, porosity, or uneven resin distribution, weakening the bonding quality within the mica paper and between layers. Under flexural and tensile loads, these weak areas are prone to stress concentration, promoting crack initiation and propagation, reducing load transfer and synergistic load-bearing capacity between layers. Under impact loads, this can induce local cracking and delamination, causing premature and concentrated damage propagation, limiting the overall load-bearing and energy absorption capacity of the board, and consequently reducing the flexural strength, tensile strength, and dynamic impact strength of the sandwich-laid silicone mica board.

[0040] In some embodiments, the first organosilicon mica paper includes organosilicon resin, and the content of the organosilicon resin is 8wt%-10wt% of the mass of the first mica paper, such as 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%.

[0041] In some embodiments, the second organosilicon mica paper includes organosilicon resin, and the content of the organosilicon resin is 8wt%-10wt% of the mass of the second mica paper, such as 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%.

[0042] In some embodiments, this application also provides a method for preparing the sandwich-layered organosilicon mica board of the above embodiments, the preparation method comprising the following steps: At least one layer of first organosilicon mica paper is stacked sequentially, and at least one layer of second organosilicon mica paper is stacked on the surface, and at least one layer of first organosilicon mica paper is stacked on the surface again. The resulting overall sandwich structure is molded and cured to obtain a sandwiched organosilicon mica board. The areal density of the first mica paper used in the first organosilicon mica paper is different from that of the second mica paper used in the second organosilicon mica paper.

[0043] The preparation process of this application is completely based on the existing process of composite organosilicon mica board, without the need for new equipment or extended molding cycle; only the layup stacking method is adjusted, and conventional organosilicon mica paper (commercial mica paper and organosilicon resin) is still used, without special modifying additives, and the threshold for industrialization is low.

[0044] In some embodiments, the method for preparing the first organosilicon mica paper includes: coating at least one side surface of the first mica paper with an organosilicon resin solution, and then baking it to obtain the first organosilicon mica paper.

[0045] In some embodiments, the method for preparing the second organosilicon mica paper includes: coating at least one side surface of the second mica paper with an organosilicon resin solution, and then baking it to obtain the second organosilicon mica paper.

[0046] In some embodiments, the molding curing temperature is 220℃-240℃, such as 220℃, 225℃, 230℃, 235℃ or 240℃.

[0047] In some embodiments, the molding and curing pressure is 3.0 MPa-4.0 MPa, such as 3.0 MPa, 3.2 MPa, 3.5 MPa, 3.8 MPa or 4.0 MPa.

[0048] In some embodiments, the heat preservation and pressure holding time for molding curing is 20min-50min, such as 20min, 30min, 40min or 50min.

[0049] It should be noted that this application does not impose specific requirements or special limitations on the baking temperature and time. As long as the solvent in the silicone resin solution can be removed and the solvent content is reduced to 0.8%-2%, it is acceptable. Those skilled in the art can make adaptive selections and adjustments according to the actual situation.

[0050] In some embodiments, after the molding and curing process is completed, demolding and natural cooling are also included.

[0051] In some embodiments, this application also provides an application of a sandwich-laid silicone mica board, wherein the sandwich-laid silicone mica board of the above embodiments, or the sandwich-laid silicone mica board prepared by the preparation method described in the above embodiments, is applied to a thermal runaway fireproof insulation board, a high-temperature resistant insulation board, or a flame-retardant insulation gasket.

[0052] This application includes thermal runaway fireproof and heat-insulating partitions for new energy power battery packs, high-temperature resistant insulation boards for high-voltage motor stators, and flame-retardant insulation gaskets for energy storage devices, covering all new energy insulation and heat insulation needs.

[0053] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0054] The methyl silicone resin solution used in the specific implementation method of this application consists of: liquid methyl silicone resin with a solid content of 50wt%, purchased from Jilin Donghu Organosilicon Co., Ltd., model DH-1 (50 parts), toluene solvent (25 parts added), methanol solvent (25 parts added), and phosphoric acid curing agent (0.4 parts added).

[0055] Example 1 This embodiment provides a sandwich-layered silicone mica board. Figure 1 The diagram shows a structural schematic of the sandwich-layered silicone mica board provided in Example 1. As can be seen from the figure, the sandwich-layered silicone mica board consists of 6 layers of first silicone mica paper 11 (forming a first composite silicone mica board 1), 8 layers of second silicone mica paper 21 (forming a second composite silicone mica board 2), and 6 layers of first silicone mica paper 11 (forming a first composite silicone mica board 1) stacked sequentially. The first organosilicon mica paper 11 uses a first mica paper with an areal density of 80 g / m³. 2 The thickness is 0.042 mm, and the content of methyl silicone resin is 9 wt% of the mass of the first mica paper; The second organosilicon mica paper 21 uses a second mica paper with an areal density of 120 g / m³. 2 The thickness is 0.056 mm, and the content of methyl silicone resin is 9 wt% of the mass of the second mica paper.

[0056] That is, in the sandwich-layered silicone mica board of this embodiment, the surface density of the mica paper is controlled to be 80 g / m³. 2 -120g / m 2 -80g / m 2 .

[0057] The preparation method of the above-mentioned sandwich-layered organosilicon mica board includes the following steps: A methyl silicone resin solution was coated on one side of the first mica paper, and then baked in an oven at 100°C for 1 minute to obtain the first organosilicon mica paper. A methyl silicone resin solution was coated on one side of the second mica paper, and then baked in an oven at 100°C for 1 minute to obtain the second organosilicon mica paper. Six layers of first organosilicon mica paper are stacked sequentially, followed by eight layers of second organosilicon mica paper on the surface, and then another six layers of first organosilicon mica paper on the surface. The resulting sandwich structure is placed in a flat vulcanizing machine, which is preheated to 240°C and subjected to a constant pressure of 3.9 MPa for 30 minutes to complete the cross-linking and curing of methyl silicone resin. The board is then removed and allowed to cool naturally at room temperature to obtain the sandwich-laid organosilicon mica board.

[0058] The differences between the sandwich-layered silicone mica panels provided in Examples 2-7, the layered silicone mica panels provided in Comparative Examples 1-3, and the asymmetric layered silicone mica panel provided in Comparative Example 4 and Example 1 are shown in Table 1. The preparation methods of Examples 2-7 and Comparative Examples 1-4 were adaptively adjusted according to the structural changes, while remaining consistent with Example 1. The areal density was 160 g / m³. 2 The mica paper has a thickness of 0.095mm.

[0059] Table 1 The flexural strength, impact strength, and tensile strength of the sandwich-layered silicone mica panels provided in Examples 1-7, the silicone mica panels provided in Comparative Examples 1-3, and the asymmetric silicone mica panel provided in Comparative Example 4 were tested. The specific test methods are as follows: 1) Bending performance: The three-point bending test was conducted according to GB / T1449-2005. A universal testing machine was used to test rectangular specimens at room temperature, with a beam speed of 1.0 mm / min and a fixed support span of 16 mm. Five valid specimens (n=5) were tested for each configuration, and the average value was taken. The bending strength of each specimen was calculated.

[0060] 2) Impact Strength: Impact strength was tested according to ISO 179-1:2010. A pendulum impact testing machine was used to conduct impact tests on unnotched rectangular specimens in a horizontal orientation (i.e., the impact direction is perpendicular to the wide face of the specimen) at room temperature. Impact strength was calculated by dividing the energy absorbed when the specimen fractured by its original cross-sectional area. Five valid specimens (n=5) were tested for each configuration, and the average value was taken to calculate the impact strength of each specimen.

[0061] 3) Tensile properties: Tested according to GB / T1447-2005. A universal testing machine was used to perform tensile tests on dumbbell-shaped specimens at room temperature. An extensometer with a gauge length of 50 mm was used to directly measure axial strain throughout the test. The extensometer was installed at the center of the gauge length of the specimen and remained in this position until the specimen fractured. A preload of 1 N was first applied to eliminate initial relaxation, followed by loading at a constant beam speed of 1.0 mm / min. The testing machine's data acquisition system simultaneously recorded the force and extensometer strain signals. The stress-strain curve was plotted using the strain measured by the extensometer, rather than the beam displacement. Five valid specimens (n=5) were tested for each configuration, and the average value was taken to calculate the tensile strength of each specimen.

[0062] The specific test results are shown in Table 2.

[0063] Table 2 The data shows that: 1) As can be seen from Examples 1 and 2, the sandwich-laid organosilicon mica board provided in this application uses mica paper with different surface densities and a second composite organosilicon mica board is stacked in the middle of the first composite organosilicon mica board on both sides. The difference in surface density combined with a specific symmetrical arrangement results in a sandwich-laid organosilicon mica board that takes into account bending strength, tensile strength, dynamic impact strength, product stability and impact delamination fracture resistance.

[0064] Specifically, by using mica paper of different areal densities for symmetrical sandwich layering, the resulting sandwich-layered organosilicon mica board exhibited a flexural strength of 284.36 MPa-293.21 MPa and an impact strength of 20.48 kJ / m². 2 -20.90kJ / m 2 The tensile strength is 175.86MPa-189.33MPa.

[0065] The sandwich-layered silicone mica board provided in Example 1 possesses high mechanical properties and is suitable for dynamic impact conditions in vehicles and energy storage applications. The surface layer uses 80g / m³... 2 Thin mica paper, with its small thickness, allows for complete impregnation with methyl silicone resin solution. After molding, the surface layer is dense and free of large pores. Under bending loads, the surface layer can withstand maximum tensile and compressive stresses. The dense surface layer significantly increases the critical value for crack initiation, preventing premature cracking of the surface layer of the laminated organosilicon mica board. Under impact loads, the thin mica paper on the surface layer has strong interfacial bonding, which can induce cracks to repeatedly deflect and slide along the interlayer, absorbing a large amount of impact fracture energy. The core layer uses 120g / m³ mica. 2 Mica paper, with 80g / m² on both sides 2 Thin mica paper forms a symmetrical sandwich structure, providing support for the board and promoting load distribution through the synergistic load-bearing of the surface and core layers, which is beneficial to improving bending load-bearing capacity and tensile strength. At the same time, the multi-layer interface may increase energy dissipation during impact by promoting crack deflection, extending crack propagation path and dispersing local damage, thus balancing mechanical strength and impact resistance. In addition, the surface density difference between the surface and core layers of mica paper is 40 g / m³. 2During the curing process, the difference in interlayer thermal shrinkage is small, the residual thermal stress is low, and there are no obvious debonding gaps at the heterogeneous interface. The load can be uniformly transferred between the layers. During impact, the crack repeatedly deflects at the heterogeneous interface and slips and delaminates between the layers, absorbing a large amount of impact energy and significantly optimizing the dynamic impact strength. At the same time, the symmetrical structure of the sandwich-laid silicone mica board ensures that the middle layer is precisely located at the center of the core layer, and there is no bending or warping during pressing and use. It also eliminates the additional interlayer stress caused by asymmetrical layup and further reduces stress concentration. Compared with the composite silicone mica board with single-area density mica paper layup, the mechanical test data error is large and the internal pores and dry spot defects are randomly distributed. The symmetrical sandwich-laid structure of this application introduces multiple uniform interfaces, weakens the stress concentration caused by local micro-defects, and significantly reduces the standard deviation of bending and impact data of batch products, resulting in higher consistency in industrial production.

[0066] The sandwich-layered silicone mica board provided in Example 2 still possesses high mechanical properties and is suitable for dynamic impact conditions in vehicles and energy storage. The surface layer uses 120g / m³ m². 2 Medium mica paper, with a core layer of 80g / m² 2 Thin mica paper, with a layer count of 4-12-4, achieves a flexural strength of 284.36 MPa and an impact strength of 20.48 kJ / m². 2 The tensile strength reached 175.86 MPa. Compared with Example 1, it maintains a similar performance level, indicating that with the corresponding number of layers and areal density configuration, it is also possible to achieve optimal levels of flexural strength, tensile strength, and dynamic impact strength.

[0067] 2) As can be seen from Examples 1-2 and 3, if the thickness of the sandwich-laid silicone mica board is too thick, the internal defects will increase relatively, and the whole board will be more prone to delamination. The interlayer separation weakens the load transfer and cooperative bearing capacity between each layer, making the sandwich-laid silicone mica board more prone to interlayer damage propagation under bending and impact loads, thus leading to a decrease in overall mechanical properties. It is impossible to simultaneously achieve optimal levels of bending strength, tensile strength and dynamic impact strength.

[0068] 3) As can be seen from Examples 1-2 and Examples 4-5, this application limits the layer ratio of the two to 1:(1.2-3) for x:y, which can ensure that the bending strength, tensile strength and dynamic impact strength are all at a better level.

[0069] 4) As can be seen from Examples 1-2 and Examples 6-7, the areal density of the first mica paper in this application is controlled to be 80 g / m³. 2 -140g / m 2 The surface density of the second mica paper is 80 g / m³. 2 -140g / m 2 The difference in areal density is 40 g / m².2 -60g / m 2 It can achieve a good balance of bending strength, tensile strength and dynamic impact strength.

[0070] 5) As can be seen from Comparative Examples 1-3, compared with Examples 1 and 2, the bending strength and dynamic impact strength of the composite organosilicon mica board with single-area density mica paper layup will be significantly reduced under similar total thickness.

[0071] Specifically, the flexural strength of the sandwich-laid silicone mica plate in Example 1 is increased by 12.76%, 40.94%, and 47.02% respectively compared with Comparative Examples 1-3, and the dynamic impact strength is increased by 12.61%, 26.67%, and 49.93% respectively compared with Comparative Examples 1-3. Although the tensile strength is slightly reduced, the degree of reduction is low. Compared with Comparative Examples 1-3, Example 1 can take into account the overall flexural strength, tensile strength, and dynamic impact strength.

[0072] 6) As can be seen from Comparative Example 4, using 80g / m 2 and 120g / m 2 Even with the same total thickness, the asymmetric layup structure of the sandwich-layup silicone mica sheet in Example 1 shows that its flexural strength, dynamic impact strength, and tensile strength are increased by 13.45%, 29.25%, and 31.44%, respectively, compared to Comparative Example 4. This demonstrates that the symmetrical sandwich-layup structure employed in this application offers comprehensive advantages in static load-bearing capacity and impact energy absorption. The use of mica paper with the same areal density on both sides of the silicone mica sheet prevents bending and warping during pressing and use, eliminating the additional interlayer stress caused by the asymmetric layup, thereby further reducing stress concentration and improving flexural strength, tensile strength, and dynamic impact strength.

[0073] In summary, the sandwich-layered silicone mica board provided in this application uses mica paper of different areal densities in combination, with a second composite silicone mica board layered between the first composite silicone mica boards on both sides. The difference in areal density, combined with a specific symmetrical arrangement, results in a sandwich-layered silicone mica board that balances flexural strength, tensile strength, dynamic impact strength, product stability, and resistance to impact delamination. Furthermore, it exhibits low mechanical property dispersion, improved consistency in mass production, and suitability for industrial-scale mass production, making it compatible with existing production lines. Moreover, by still using a silicone-mica substrate system, the sandwich-layered silicone mica board retains its original advantages in insulation and fire resistance, such as continuous high-temperature resistance, dielectric strength, and flame-retardant ceramicization.

[0074] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A sandwich-layered silicone mica board, characterized in that, The sandwich-layered organosilicon mica board includes a first composite organosilicon mica board, a second composite organosilicon mica board, and the first composite organosilicon mica board stacked in sequence. The first composite organosilicon mica board includes at least one layer of first organosilicon mica paper, and the second composite organosilicon mica board includes at least one layer of second organosilicon mica paper. The areal density of the first mica paper used in the first organosilicon mica paper is different from the areal density of the second mica paper used in the second organosilicon mica paper.

2. The sandwich-layered organosilicon mica board according to claim 1, characterized in that, The thickness of the sandwich-layered silicone mica board is 0.8mm-1.5mm.

3. The sandwich-layered organosilicon mica board according to claim 1 or 2, characterized in that, The first composite organosilicon mica board includes x layers of first organosilicon mica paper, and the second composite organosilicon mica board includes y layers of second organosilicon mica paper, where x:y is 1:(1.2-3).

4. The sandwich-layered organosilicon mica board according to any one of claims 1-3, characterized in that, The difference between the areal density of the first mica paper and the areal density of the second mica paper is 40 g / m³. 2 -60g / m 2 .

5. The sandwich-layered silicone mica board according to claim 4, characterized in that, The areal density of the first mica paper is 80 g / m³. 2 -140g / m 2 ; And / or, the areal density of the second mica paper is 80 g / m³. 2 -140g / m 2 .

6. The sandwich-layered organosilicon mica board according to any one of claims 1-5, characterized in that, The first organosilicon mica paper includes organosilicon resin, and the content of the organosilicon resin is 8wt%-10wt% of the mass of the first mica paper. And / or, the second organosilicon mica paper includes organosilicon resin, the content of which is 8wt%-10wt% of the mass of the second mica paper.

7. A method for preparing a sandwich-layered organosilicon mica board according to any one of claims 1-6, characterized in that, The preparation method includes the following steps: At least one layer of first organosilicon mica paper is stacked sequentially, and at least one layer of second organosilicon mica paper is stacked on the surface, and at least one layer of first organosilicon mica paper is stacked on the surface again. The resulting overall sandwich structure is molded and cured to obtain a sandwiched organosilicon mica board. The areal density of the first mica paper used in the first organosilicon mica paper is different from the areal density of the second mica paper used in the second organosilicon mica paper.

8. The preparation method according to claim 7, characterized in that, The preparation method of the first organosilicon mica paper includes: coating at least one side surface of the first mica paper with an organosilicon resin solution, and then baking it to obtain the first organosilicon mica paper; And / or, the method for preparing the second organosilicon mica paper includes: coating at least one side surface of the second mica paper with an organosilicon resin solution, and then baking it to obtain the second organosilicon mica paper.

9. The preparation method according to claim 8, characterized in that, The molding and curing temperature is 220℃-240℃; And / or, the molding and curing pressure is 3.0 MPa-4.0 MPa; And / or, the heat preservation and pressure holding time for the molding and curing is 20 min to 50 min; And / or, after the molding and curing process is complete, the process also includes demolding and natural cooling.

10. An application of a sandwich-layered silicone mica board, characterized in that, The sandwich-layered organosilicon mica board according to any one of claims 1-6, or the sandwich-layered organosilicon mica board prepared by the preparation method according to any one of claims 7-9, is applied to thermal runaway fireproof and heat-insulating partitions, high-temperature resistant insulating boards, or flame-retardant insulating gaskets.