Mildew-proof non-combustible plate

By adding wetting agents and organic mildew inhibitors to the melamine impregnation solution of non-combustible boards, the problem of mold growth in humid environments is solved, achieving a highly effective mildew prevention effect without affecting the appearance, and meeting the standards for mildew prevention and flame retardancy.

CN123133233APending Publication Date: 2026-11-20JIANGSU BODA NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611548405.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing non-combustible boards are prone to mold growth in humid environments, affecting the lifespan of the boards and indoor air quality. Furthermore, the addition of conventional anti-mold agents can affect the appearance of the products.

Method used

Adding a wetting agent and an organic mildew inhibitor to the melamine impregnation solution allows the organic mildew inhibitor to be bound within the melamine-formaldehyde resin network, preventing migration during hot pressing that could affect the appearance.

Benefits of technology

While ensuring the product's appearance, the stability of its anti-mildew performance is improved to meet the ASTM G21-15 anti-mildew grade 0 standard, without affecting the flame retardant and mechanical properties of the board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1791442524058-000001
    Figure REF-OBJ-1791442524058-000001
Patent Text Reader

Abstract

The present application relates to the technical field of building decoration plate, and more particularly to a mildew-proof non-combustible plate prepared by hot-pressing a group embryo; the group embryo comprises surface layer impregnated paper, adhesive layer impregnated paper, cement board, adhesive layer impregnated paper and surface layer impregnated paper arranged in sequence; the surface layer impregnated paper is obtained by impregnating surface layer base paper with triamine impregnating glue solution and then drying and curing; the raw material of the triamine impregnating glue solution comprises non-ionic wetting agent and organic mildew-proof agent. The mildew-proof non-combustible plate provided by the present application introduces non-ionic wetting agent and organic mildew-proof agent at the same time, so that the organic mildew-proof agent molecules are bound in the MF resin network, the mildew-proof performance is improved, and the stability of the mildew-proof effect is improved under the premise of ensuring the appearance of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building decorative panels, and in particular to a mildew-resistant and non-combustible panel. Background Technology

[0002] Non-combustible boards are a core material for modern building fire protection decoration, interior partitions, and ceiling decoration. With their excellent Class A non-combustible properties, high-temperature resistance, and structural stability, they are widely used in public places such as shopping malls, hospitals, office buildings, and underground projects. Currently available non-combustible boards mostly use magnesium-based or silicate inorganic materials as their base material. The base material has a highly porous structure, and these pores easily absorb moisture, dust, and nutrients from microorganisms in the air. In humid environments such as southern regions, kitchens, bathrooms, and damp underground spaces, mold and algae can easily grow, not only damaging the decorative layer of the board and reducing its lifespan, but also fostering harmful microorganisms and affecting indoor air quality and human health.

[0003] Currently, the industry commonly improves the mildew resistance of non-combustible boards by adding mildew inhibitors. Commonly used water-soluble mildew inhibitors include isothiazolinones, quaternary ammonium salts, and inorganic mildew inhibitors. While the addition of these mildew inhibitors can improve the mildew resistance of the boards to some extent, it also affects the appearance of the decorative surface layer, making it difficult to balance mildew resistance with product aesthetics. Summary of the Invention

[0004] To address the problem that existing boards often fail to balance mold resistance and product appearance, this invention provides a mold-resistant and non-flammable board. This board incorporates both a wetting agent and an organic mold inhibitor into the raw materials of the melamine impregnation adhesive. This allows the organic mold inhibitor to be trapped within the melamine-formaldehyde resin network, inhibiting the migration and blooming of the mold inhibitor to the surface during hot pressing, thus solving the problem of existing boards failing to balance mold resistance and product appearance.

[0005] The technical solution adopted by this invention to solve its technical problem is: A mildew-resistant and non-combustible board is prepared by hot pressing of preforms; The preform comprises a surface impregnated paper, an adhesive layer impregnated paper, a cement board, an adhesive layer impregnated paper, and a surface impregnated paper stacked sequentially. The surface impregnated paper is obtained by impregnating the surface base paper with a melamine impregnation solution and then drying and curing it. The raw materials of the melamine impregnation solution, by weight, include the following components: 100 parts of melamine-formaldehyde resin; Hardener 0.1-0.3 parts; Defoamer 0.03-0.1 parts; Penetrating agent 0.1-0.3 parts; Release agent 0.03-0.1 parts; Dust collector 0.1-0.3 parts; 3.0-5.0 parts of nonionic wetting agent; 0.5-1.0 parts of organic antifungal agent.

[0006] Optionally, the nonionic wetting agent is a polyether-based substance.

[0007] Optionally, the polyether is polyethylene glycol.

[0008] Optionally, the curing agent is selected from at least one of A710 and A710-L.

[0009] Optionally, the defoamer is an organosilicon defoamer.

[0010] Optionally, the penetrant is an organosilicon-based penetrant.

[0011] Optionally, the hot pressing process parameters are: hot pressing temperature of 130-150℃ and hot pressing pressure of 70-85 kg / cm². 2 .

[0012] Optionally, the adhesive layer impregnated paper is obtained by impregnating the adhesive layer base paper with a phenolic impregnating adhesive solution and then drying and curing it.

[0013] Optionally, the raw materials of the phenolic impregnation solution, by weight, include the following components: 100 parts of phenolic resin; Solvent 5-15 parts.

[0014] Optionally, the solvent is selected from at least one of water and methanol.

[0015] The beneficial effects of this invention are: The mildew-resistant and non-flammable board provided by this invention introduces both a nonionic wetting agent and an organic mildew inhibitor, which binds the organic mildew inhibitor molecules within the MF resin network. This improves the mildew resistance and enhances the stability of the mildew resistance while maintaining the product's appearance. Detailed Implementation

[0016] The present invention will now be described in further detail. The embodiments described below are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0017] To address the problem of existing boards failing to balance mold resistance and product appearance, this invention provides a mold-resistant and non-combustible board. This board is prepared by hot-pressing a preform. The preform comprises, in sequence, a surface impregnated paper layer, an adhesive impregnated paper layer, a cement board, and the surface impregnated paper layer, forming a symmetrical five-layer composite structure. The surface impregnated paper layers are located on the outermost sides, serving as decorative layers. The adhesive impregnated paper layers are located between the surface impregnated paper and the cement board, providing adhesion and stress buffering. The cement board is located in the center, serving as the non-combustible substrate and bearing the main mechanical load.

[0018] The surface-impregnated paper in this invention is obtained by impregnating a surface base paper with a melamine impregnation solution and then drying and curing it; the raw materials of the melamine impregnation solution include the following components by weight: 100 parts of melamine-formaldehyde resin; Hardener 0.1-0.3 parts; Defoamer 0.03-0.1 parts; Penetrating agent 0.1-0.3 parts; Release agent 0.03-0.1 parts; Dust collector 0.1-0.3 parts; 3.0-5.0 parts of nonionic wetting agent; 0.5-1.0 parts of organic antifungal agent.

[0019] Of the above components, melamine-formaldehyde resin serves as the matrix resin, providing the main adhesive and film-forming properties of the impregnating adhesive. Melamine-formaldehyde resin possesses high crosslinking density and excellent hardness, abrasion resistance, water resistance, and heat resistance. During hot pressing, it further undergoes condensation and curing to form a three-dimensional network structure, firmly encapsulating additives such as mildew inhibitors and wetting agents within the resin network, endowing the decorative surface layer with high strength, high abrasion resistance, and high water resistance. The curing agent catalyzes the condensation and curing reaction of the melamine-formaldehyde resin, lowering the curing temperature and shortening the curing time, ensuring that the resin fully crosslinks to form a dense network during hot pressing. The addition of the curing agent avoids defects such as surface stickiness, poor water resistance, and insufficient strength caused by incomplete resin curing. The defoamer eliminates air bubbles generated during the preparation and impregnation of the melamine impregnating adhesive. If air bubbles are present in the adhesive, white spots, pinholes, and other defects will remain on the paper surface after impregnation, affecting the final appearance consistency of the decorative surface layer. Penetrating agents are used to reduce the surface tension of the melamine impregnation solution and improve its wetting and penetration ability into the base paper fibers. The base paper is a porous cellulose material; good permeability ensures that the adhesive fully penetrates the fibers and distributes evenly, avoiding defects such as incomplete impregnation and uneven surface coating. Release agents improve the release properties of the finished product from the press mold during hot pressing, preventing the finished board from adhering to the press plate and causing surface scratches, damage, or texture distortion. Dust removers inhibit the condensation of volatile components in the adhesive during impregnation and drying, reducing paper surface defects and environmental pollution caused by dust settling. Nonionic wetting agents can form hydrogen bonds with organic mildew inhibitors, thus binding the organic mildew inhibitor molecules within the MF (melamine-formaldehyde) resin network. This effectively inhibits the migration and blooming of organic mildew inhibitors to the board surface during high-temperature hot pressing, avoiding impact on the product's decorative appearance. Simultaneously, it reduces the volatilization loss of organic mildew inhibitors at high temperatures, ensuring efficient retention of the mildew inhibitor within the board, thereby maintaining a stable mildew-proof effect. Without this wetting agent, the organic mildew inhibitor will cause blooming and whitening on the finished product's appearance and a decrease in mildew resistance after wiping due to volatilization and migration during hot pressing. The organic mildew inhibitor is the core functional component of this invention. By selecting an organic mildew inhibitor as the mildew-resistant component, and utilizing its excellent compatibility with melamine-formaldehyde resin, it helps to distribute evenly within the MF resin network. Furthermore, its synergistic effect with the nonionic wetting agent prevents migration and blooming onto the board surface during high-temperature hot pressing, thus improving mildew resistance while maintaining the product's appearance.

[0020] The preferred solid content of the melamine impregnation solution of this invention is 45%-55%, and the pH value is 8.5-9.5.

[0021] The mildew-resistant and non-flammable board provided by this invention introduces both a nonionic wetting agent and an organic mildew inhibitor, which binds the organic mildew inhibitor molecules within the MF resin network. This improves the mildew resistance and enhances the stability of the mildew resistance while maintaining the product's appearance.

[0022] The preferred nonionic wetting agent of this invention is a polyether-based substance.

[0023] When the nonionic wetting agent is a polyether, its mechanism of action is as follows: its long-chain polyether structure forms hydrogen bonds with the organic mildew inhibitor, binding the organic mildew inhibitor molecules inside the MF (melamine formaldehyde) resin network. This effectively inhibits the migration and blooming of the organic mildew inhibitor to the board surface during high-temperature hot pressing, avoiding affecting the decorative appearance of the product. At the same time, it reduces the volatilization loss of the organic mildew inhibitor at high temperatures, ensuring that the mildew inhibitor remains efficiently in the board, thereby maintaining a stable mildew-proof effect.

[0024] Specifically, the preferred polyether material in this invention is polyethylene glycol.

[0025] When the nonionic wetting agent is polyethylene glycol, its mechanism of action is as follows: the polyethylene glycol molecular chain contains a large number of ether bonds and terminal hydroxyl groups. The ether oxygen and hydroxyl groups are hydrophilic groups, and the hydrocarbon chains have weak lipophilic properties. The molecules are directionally adsorbed at the solid-liquid interface, reducing the surface tension of the aqueous solution and the solid-liquid interfacial tension, replacing the air film on the solid surface, making it easier for the liquid to spread and penetrate on the substrate surface, thus achieving wetting. At the same time, it is adsorbed on the particle surface to form a hydration layer, which helps to disperse, reduces particle agglomeration, and binds the organic antifungal agent molecules inside the MF (melamine formaldehyde) resin network.

[0026] Furthermore, the present invention preferably uses polyethylene glycol PEG400 / 600 (such as PEG400, PEG600, or mixtures thereof) to further improve its compatibility with melamine-formaldehyde resin while maintaining good hydrogen bond binding. Specifically, PEG400-600 has suitable molecular weight and chain length, and the hydrogen bond strength formed with organic fungicides is moderate, which can effectively inhibit the migration and blooming of organic fungicides without affecting their fungicidal activity release due to excessive binding.

[0027] These polyethers have excellent hydrogen bond donor or acceptor capabilities, can form similar hydrogen bond binding effects with organic fungicides, and have good compatibility with MF resin systems.

[0028] Currently, when the amount of conventional mildew inhibitors used in non-combustible boards in the industry is too low, the finished product's mildew resistance level cannot reach the highest level 0 standard. Increasing the addition ratio can improve the mildew resistance effect, but it can easily cause the appearance of the decorative paper to deteriorate, affecting the decorative effect of the board surface. In addition, most mildew inhibitors have poor temperature resistance and are prone to decomposition and failure during the hot pressing process of the board, resulting in insufficient mildew resistance stability. Based on this, the present invention preferably uses IW-PS as an organic mildew inhibitor. IW-PS has comprehensive advantages such as good temperature resistance, low addition amount, long-lasting mildew resistance, and good compatibility with inorganic substrates. Moreover, its urethane groups can form hydrogen bonds with nonionic wetting agents, thereby forming a hydrogen bond binding effect between IW-PS and nonionic wetting agents, binding IW-PS inside the MF resin network, inhibiting the migration of blooms to the surface during hot pressing and reducing the loss of IW-PS due to high-temperature volatilization. A low addition amount can stably achieve the ASTM G21-15 (2021) mildew resistance level 0 standard without affecting the flame retardant performance, mechanical properties, and decorative appearance of the board. Furthermore, IW-PS anti-mold agent has excellent temperature resistance and compatibility. It does not decompose or become ineffective during the entire process of board forming and curing. It is evenly dispersed on the board surface, achieving long-lasting anti-mold protection. The anti-mold service life is synchronized with the service life of the board.

[0029] Excellent anti-mildew performance can be achieved with low addition amount. Therefore, the addition of IW-PS anti-mildew agent will not affect the basic performance of inorganic non-combustible board. The finished board still maintains the Class A non-combustible characteristics. At the same time, it has excellent bending strength, water resistance and aging resistance, which solves the contradiction of traditional anti-mildew boards that are "anti-mildew but not fireproof, fireproof but not anti-mildew".

[0030] The present invention preferably uses a curing agent selected from at least one of A710 and A710-L to effectively promote resin crosslinking and ensure the hardness, abrasion resistance and water resistance of the decorative surface layer.

[0031] The present invention preferably uses an organosilicon defoamer, and more preferably selects at least one of TEGO Foamex 810 and BYK-024 to effectively eliminate bubbles generated during the preparation and impregnation of the melamine impregnation solution, avoid white spots, pinholes and other appearance defects in the impregnated paper, and improve the appearance consistency of the finished decorative surface layer.

[0032] The present invention preferably uses an organosilicon-based penetrant as the penetrant, and more preferably selects at least one of TEGO Wet 260 and AT-910 to effectively reduce the surface tension of the melamine impregnation solution, improve the wetting and penetration ability of the base paper fibers, ensure that the solution fully penetrates into the fiber and is evenly distributed, and avoid defects such as incomplete impregnation and uneven surface coating.

[0033] The preferred release agent of this invention is selected from at least one of TAG Release 606 and ACMOS 1124B, so as to effectively improve the release property between the finished product and the press template during hot pressing, and prevent the finished product sheet from adhering to the press plate, causing surface scratches, damage or texture distortion.

[0034] The dust removal agent of this invention is preferably selected from at least one of A306 and A888-L, so as to effectively inhibit the condensation of volatile components during impregnation and drying to form particulate dust, reduce paper surface defects and environmental pollution caused by dust settling, and improve the consistency of finished product appearance.

[0035] The preferred hot-pressing process parameters for this invention are: hot-pressing temperature of 130-150℃ and hot-pressing pressure of 70-85 kg / cm². 2 To ensure optimal performance, the following parameters must be applied: Low temperature results in incomplete curing of the melamine-formaldehyde resin, leading to insufficient surface hardness and water resistance; excessive temperature exacerbates the volatilization and thermal decomposition loss of IW-PS, affecting its anti-mildew durability; and excessive pressure leads to insufficient interlayer bonding, blistering, and delamination; while excessive pressure causes excessive compression of the substrate, reducing the board's toughness. Within this range, the MF resin is fully cured, the anti-mildew agent is firmly coated, and the overall performance of the board achieves an optimal balance.

[0036] The present invention preferably uses adhesive layer impregnated paper, which is obtained by impregnating adhesive layer base paper with phenolic resin impregnation solution and then drying and curing it. The phenolic resin adhesive layer prepared by this method has excellent water resistance, heat resistance and toughness, and has good adhesion to both the surface impregnated paper and cement board impregnated with melamine resin impregnation solution. It can form a multi-layer composite structure of surface decorative layer-adhesive layer-cement board substrate during hot pressing, which takes into account the hardness and wear resistance of the decorative surface layer and the toughness and adhesion of the adhesive layer.

[0037] Specifically, the raw materials of the phenolic impregnation solution preferably include the following components by weight: 100 parts of phenolic resin; Solvent 5-15 parts.

[0038] This formula is simple, efficient, and easy to prepare. Phenolic resin, as the main resin of the adhesive layer, can be further cured and cross-linked during the hot pressing process to form a strong adhesive layer. The addition of solvent can effectively adjust the viscosity and solid content of the adhesive, allowing the adhesive to fully wet the base paper of the adhesive layer, ensuring the uniformity and bonding strength of the adhesive layer.

[0039] The solvent of this invention is preferably selected from at least one of water and methanol. These solvents have good solubility and controllable volatility for phenolic resins, and can be easily removed during the impregnation and drying process without leaving residues in the adhesive layer, thus avoiding affecting the adhesive strength and water resistance of the adhesive layer.

[0040] The mildew-resistant and non-combustible board provided by this invention meets both the GB 8624 Class A non-combustible standard and the ASTM G21-15 (2021) mildew-resistant Class 0 standard. The board has excellent mechanical properties and weather resistance, and the preparation process is simple, making it suitable for large-scale industrial production.

[0041] The mildew-resistant and non-combustible board provided by this invention can be prepared according to the following method: S1: Prepare the melamine impregnation solution according to the formula; S2: Impregnate the surface base paper with a melamine impregnation solution and then dry and cure it to obtain surface impregnated paper; Specifically, in this step, the surface base paper is impregnated with a melamine impregnation solution, preferably with the amount of sizing controlled at 90%-150%. After impregnation, it is sent to an oven and dried at 80-135℃ until the volatile content is 6.0%-9.0%, and then cooled for later use. S3: Prepare the phenolic impregnation solution according to the formula; S4: The adhesive layer base paper is impregnated with phenolic impregnation solution and then dried and cured to obtain adhesive layer impregnated paper; Preferably, the impregnation amount in this step is controlled at 120%-140%. After impregnation, the product is sent to an oven and dried at 110-130℃ until the volatile content is 7.0%-8.0%. It is then cooled and stored for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is hot-pressed to obtain a mildew-proof and non-flammable board.

[0042] The mildew-proof and non-combustible board provided by this invention has a simple and controllable preparation process, requires no additional special equipment, has moderate raw material costs, is suitable for large-scale industrial mass production, and is compatible with various humid and high fire protection requirements in building scenarios.

[0043] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below.

[0044] Unless otherwise specified, the curing agent in all embodiments and comparative examples of this invention is A710, the defoamer is TEGO Foamex 810, the penetrant is TEGO Wet 260, the release agent is TAG Release 606, the dust remover is A306, the nonionic wetting agent is PEG400, the organic mildew inhibitor is IW-PS, and the solvent is water.

[0045] Example 1

[0046] This embodiment provides a method for preparing a mildew-resistant and non-combustible board, including the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.0 part of organic mildew inhibitor, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0047] Example 2

[0048] This embodiment provides a method for preparing a mildew-resistant and non-combustible board, including the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 0.5 parts of organic mildew inhibitor, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0049] Example 3

[0050] This embodiment provides a method for preparing a mildew-resistant and non-combustible board, including the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 3.0 parts of nonionic wetting agent and 1.0 part of organic mildew inhibitor, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0051] Example 4

[0052] This embodiment provides a method for preparing a mildew-resistant and non-combustible board, including the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 5.0 parts of nonionic wetting agent and 1.0 part of organic mildew inhibitor, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0053] Each comparative example of the present invention is compared with Example 1.

[0054] Comparative Example 1 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 1.0 part of organic mildew inhibitor, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0055] Comparative Example 2 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 0.5 parts of copper borate, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0056] Comparative Example 3 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.0 part of copper borate, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0057] Comparative Example 4 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.5 parts of copper borate, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0058] Comparative Example 5 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 2.0 parts of copper borate, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0059] Comparative Example 6 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 0.5 parts of nano silver, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0060] Comparative Example 7 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.0 part of nano silver, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0061] Comparative Example 8 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.5 parts of nano silver, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0062] Comparative Example 9 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 2.0 parts of nano silver, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0063] Comparative Example 10 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 0.5 parts of nano zinc oxide, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0064] Comparative Example 11 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.0 parts of nano zinc oxide, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0065] Comparative Example 12 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 1.5 parts of nano zinc oxide, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0; S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0066] Comparative Example 13 This comparative example provides a method for preparing a mildew-resistant and non-combustible board, comprising the following steps: S1: According to the weight percentage, add 100 parts of melamine-formaldehyde resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 0.2 parts of penetrant, 0.05 parts of defoamer, 0.2 parts of dust remover, 0.05 parts of release agent and 0.2 parts of curing agent in sequence, stir for 10 minutes to mix evenly, then add 4.0 parts of nonionic wetting agent and 2.0 parts of nano zinc oxide, stir for 10 minutes, filter to remove impurities, and obtain melamine impregnation solution. Control the solid content of melamine impregnation solution to be 50% and the pH value to be 9.0. S2: The quantitative amount is 100g / m 2 The surface base paper is impregnated with melamine impregnation solution, the amount of sizing is controlled at 120%, and dried at 120℃ until the volatile content is about 7.5% to obtain surface impregnated paper, which is then cooled for later use. S3: Add 100 parts by weight of phenolic resin to the mixing tank and stir for 15 minutes to make it flow evenly; add 10 parts by weight of solvent, stir for 10 minutes, mix evenly, and obtain phenolic impregnation solution. S4: The quantitative amount is 180g / m 2 The adhesive layer base paper is impregnated with phenolic resin, the impregnation amount is controlled at 50%, and dried until the volatile content is about 7.0% to obtain adhesive layer impregnated paper, which is then cooled for later use. S5: Assemble the surface impregnated paper + adhesive layer impregnated paper + cement board + adhesive layer impregnated paper + surface impregnated paper. S6: The preform is fed into a hot press at 140℃ and 78 kg / cm². 2 Under the given conditions, the board is hot-pressed for 60 minutes, held under pressure and cooled to below 80°C. The pressure is then released, the board is removed, and left to stand for 24 hours to eliminate internal stress, resulting in a mildew-resistant and non-combustible board.

[0067] The properties of the plates prepared in the above embodiments and comparative examples were tested using the following methods: 1. Anti-mildew performance: According to ASTM G21-15 (2021) test, after 28 days of constant temperature and humidity incubation, no mold growth is observed on the surface and inside of the board, which is rated as anti-mildew level 0; 2. Flame retardant performance: According to GB 8624-2012 test, there is no open flame, no smoldering, and no dripping, meeting the Class A non-combustible standard; 3. Appearance: Visual inspection.

[0068] The test results are shown in Table 1: Table 1

[0069] This invention uses an inorganic non-combustible substrate as its core, combined with a specialized high-efficiency anti-mildew system, and employs a low-dosage IP-WS additive. This allows the boards to consistently meet the ASTM G21-15 (2021) mildew resistance level 0 standard while satisfying Class A non-combustible performance, without any degradation in mechanical properties, water resistance, or weather resistance. The preparation process of this invention is simple, the raw materials are highly compatible, and the resulting boards possess excellent fire resistance, non-combustibility, high-efficiency mildew resistance, and aging resistance, making them suitable for building decoration construction in humid environments and public fire-fighting areas, with broad application prospects.

[0070] The difference between Comparative Example 1 and Example 1 is that no nonionic wetting agent was added. Due to the large solid-liquid interfacial tension, the liquid could not fully wet the surface of the board, resulting in poor leveling of the coating layer. Furthermore, the organic anti-mildew agent molecules could not be bound inside the MF (melamine formaldehyde) resin network, resulting in spots on the surface and a decline in appearance quality.

[0071] The difference between Comparative Example 2 and Example 1 is that 0.5 parts by weight of copper borate was used instead of 1.0 parts by weight of organic antifungal agent in Example 1. Due to insufficient addition of antifungal agent, the antifungal effect was poor, and the antifungal level could only reach level 2.

[0072] The difference between Comparative Example 3 and Example 1 is that 1.0 part by weight of copper borate was used instead of 1.0 part by weight of organic antifungal agent in Example 1. Due to insufficient addition of antifungal agent, the antifungal effect was still poor, and the antifungal level could only reach level 2.

[0073] The difference between Comparative Examples 4 and 5 and Example 1 is that 1.5 parts by weight and 2.0 parts by weight of copper borate were used to replace 1.0 parts by weight of organic antifungal agent in Example 1, respectively. The antifungal level was 1, which still did not reach 0. At the same time, although a nonionic wetting agent was added to the system, the nonionic wetting agent could not form hydrogen bonds with copper sulfate. The high amount of added copper borate caused the appearance of the board to turn white, the cross-linking was insufficient, the water resistance was poor, and it was easy to effloresce and crack when exposed to moisture.

[0074] Comparative Examples 6-9 served as the nano-silver control group. The difference from Example 1 was that 0.5, 1.0, 1.5, and 2.0 parts by weight of nano-silver replaced the 1.0 part by weight of organic antifungal agent in Example 1, respectively. At each addition ratio, the antifungal grade of the boards was 2-3, with mold coverage of 10%-30%, failing to reach the 0-grade standard. When the addition amount was ≥1.5%, the boards showed efflorescence. Comparative Examples 10-13 were the nano zinc oxide control group. The difference from Example 1 was that 0.5, 1.0, 1.5 and 2.0 parts by weight of nano zinc oxide replaced 1.0 part by weight of the organic antifungal agent in Example 1, respectively. The antifungal effect was extremely poor under all gradient additions of the antifungal agent, with an antifungal level of 3 or above. It could only slightly inhibit surface mold, while a large amount of mold grew inside the substrate, and it would affect the appearance of the board by causing precipitation and whitening.

[0075] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A mildew-resistant and non-combustible board, characterized in that, It is prepared by hot pressing of preforms; The preform comprises a surface impregnated paper, an adhesive layer impregnated paper, a cement board, an adhesive layer impregnated paper, and a surface impregnated paper stacked sequentially. The surface impregnated paper is obtained by impregnating the surface base paper with a melamine impregnation solution and then drying and curing it. The raw materials of the melamine impregnation solution, by weight, include the following components: 100 parts of melamine-formaldehyde resin; Hardener 0.1-0.3 parts; Defoamer 0.03-0.1 parts; Penetrating agent 0.1-0.3 parts; Release agent 0.03-0.1 parts; Dust collector 0.1-0.3 parts; 3.0-5.0 parts of nonionic wetting agent; 0.5-1.0 parts of organic antifungal agent.

2. The mildew-resistant and non-flammable board as described in claim 1, characterized in that, The nonionic wetting agent is a polyether-based substance.

3. The mildew-resistant and non-flammable board as described in claim 2, characterized in that, The polyether substance is polyethylene glycol.

4. The mildew-resistant and non-flammable board as described in claim 1, characterized in that, The curing agent is selected from at least one of A710 and A710-L.

5. The mildew-resistant and non-combustible board as described in claim 1, characterized in that, The defoamer is an organosilicon defoamer.

6. The mildew-resistant and non-flammable board as described in claim 1, characterized in that, The penetrant is an organosilicon-based penetrant.

7. The mildew-resistant and non-combustible board as described in claim 1, characterized in that, The hot pressing process parameters are as follows: hot pressing temperature is 130-150℃, and hot pressing pressure is 70-85 kg / cm². 2 .

8. The mildew-resistant and non-combustible board as described in any one of claims 1-7, characterized in that, The adhesive layer impregnated paper is obtained by impregnating the adhesive layer base paper with phenolic resin and then drying and curing it.

9. The mildew-resistant and non-flammable board as described in claim 8, characterized in that, The raw materials of the phenolic impregnation solution, by weight, include the following components: 100 parts of phenolic resin; Solvent 5-15 parts.

10. The mildew-resistant and non-flammable board as described in claim 9, characterized in that, The solvent is selected from at least one of water and methanol.