Floating structure monomer post-cast strip and its maintenance method
By using steel connectors and strain sensors to monitor stress in the post-cast strip and dynamically adjusting the preload of the locking bolts, the problems of corrosion and stress relaxation in the post-cast strip in the marine environment are solved, thus improving the reliability and durability of the structural connection.
Patent Information
- Application Number
- CN202611198506.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-05-21
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, post-cast strips in marine environments suffer from insufficient reliability of structural connection nodes due to screw corrosion and stress relaxation, affecting the overall strength and long-term durability of the structure.
The design employs pre-embedded steel connectors and external bolts, combined with strain sensors to monitor stress signals in real time. Stress relaxation compensation is calculated through stress extreme value difference analysis, and the preload of the locking bolts is dynamically adjusted. The curing time is optimized by combining temperature and humidity data.
It effectively protects steel from corrosion, improves the reliability of connection nodes, ensures the long-term strength and durability of the structure, and optimizes the maintenance period.
Smart Images

Figure CN123133262A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to structural engineering, and more specifically, to a post-cast strip for a floating structural unit and a method for its maintenance. Background Technology
[0002] In marine engineering and large bridge construction, prefabricated floating structure units combining fiber-reinforced polymer (FRP) and ultra-high performance concrete (UHPC) are used (such as...). Figure 1 As shown in the diagram, this is a development trend. Such structures are typically assembled from prefabricated components (including prefabricated slabs and beams made of FRP-UHPC) using post-cast connection methods such as wet bonding. During assembly, post-cast strips are formed between prefabricated beams and between prefabricated beams and external supports formed by connecting prefabricated slabs. Structural connections are achieved by casting UHPC into these post-cast strips. To facilitate the construction of these post-cast strips, traditional methods typically involve pre-embedding bolts in the prefabricated components on both sides of the strip to facilitate subsequent steel plate installation. However, these pre-embedded bolts not only protrude from the surface of the prefabricated components, but they are also susceptible to corrosion and damage during long-term use in marine environments, thus affecting the structural integrity and even the reliability of the connection.
[0003] Furthermore, in existing technologies, after the aforementioned post-cast strip connection is completed, during the curing process, UHPC and adhesives will experience shrinkage and stress relaxation. The resulting minute deformation may cause stress shifts (reduction in preload) between the beam end and the precast slab, leading to stress relaxation in the connection area and potentially a gradual decrease in the joint preload. If this stress relaxation is not monitored and compensated for, long-term use may result in microcracks or loosening of the structural connection joints, affecting the overall strength and long-term durability of the structure. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to address the shortcomings of the prior art by providing a post-cast strip for a floating structural unit and its maintenance method. This invention solves the technical problem in the prior art where stress relaxation during the maintenance process of the post-cast strip leads to a decrease in the preload of the joint and insufficient long-term reliability. It realizes dynamic monitoring and active compensation of the stress of the structural connection joint, thereby improving the connection strength and long-term reliability of the structural joint.
[0005] The present invention discloses a post-cast strip for a floating structural unit, comprising a strip body disposed between two precast components, wherein a strain sensor is installed in the strip body, and multiple steel connectors are pre-embedded in the precast components on both sides of the strip body, and post-cast holes are provided between the steel connectors and the outer surfaces of the precast components. Supporting steel plates are provided on the outer side of the strip body, and the supporting steel plates are connected to the steel connectors by locking bolts.
[0006] Preferably, it further includes a seal, which consists of a sealing section screwed into a steel connector and a filling section that fills and seals the post-gating hole.
[0007] A method for curing the post-cast strip of the aforementioned floating structural unit, the method comprising:
[0008] After the prefabricated components are overlapped and formed into a belt, the supporting steel plate is installed on the outside of the belt.
[0009] A strain sensor is built into the belt, then UHPC is cast into the belt, and the floating structure unit is cured.
[0010] During the maintenance process, the stress signal output by the strain sensor is collected in real time. Based on the stress signal, stress extreme value difference analysis is performed to determine whether the UHPC cast in the belt exhibits stress relaxation. If so, the stress trend value is calculated, and the stress relaxation compensation amount is calculated in combination with the initial reference stress value. The stress relaxation compensation amount is then applied to the locking bolt.
[0011] After the UHPC cast in the belt has cured to the target strength, the steel plate support is removed.
[0012] Preferably, the stress extremum difference analysis specifically includes:
[0013] Stress peak and stress valley values are extracted from all stress signals collected during the set sampling period. The maximum stress change is calculated based on the difference between the stress peak and stress valley values. If the absolute value of the maximum stress change is greater than the preset maximum stress change threshold, it is determined that the UHPC cast in the belt has experienced stress relaxation.
[0014] Preferably, the stress trend value is calculated by using exponential smoothing based on the forgetting factor, with the real-time stress signal at the current moment and the stress estimate at the previous moment as parameters.
[0015] Preferably, the formula for calculating the stress relaxation compensation amount is:
[0016] ,
[0017] In the formula, Δcomp(t) is the adjustment amount of the bolt compensation preload to be applied at the current moment; β is the compensation gain coefficient; S1 represents the stress trend value; S0 represents the initial reference stress value.
[0018] Preferably, during the curing process of the floating structure unit, the temperature and humidity data of the environment in which the floating structure unit is located are detected, and the comprehensive curing rate attenuation factor is calculated using the temperature and humidity data. The comprehensive curing rate attenuation factor is combined with the preset target curing degree threshold of the UHPC poured at the post-pouring strip to calculate the predicted curing time value. After the predicted curing time value is compensated by a positive time amount, it is determined that the UHPC poured at the post-pouring strip has been cured to the target strength.
[0019] Preferably, the formula for calculating the predicted maintenance time is:
[0020] ,
[0021] In the formula, The target curing threshold for the UHPC poured at the pre-set post-pouring strip; The comprehensive curing rate attenuation factor corresponds to the i-th sampling time ti; The time interval between two samplings; This is a predicted maintenance time.
[0022] Preferably, the positive time compensation is 10%-20% of the predicted maintenance time.
[0023] Beneficial effects
[0024] The advantages of this invention are:
[0025] 1. The present invention adopts a design that combines pre-embedded steel connectors with external bolts and post-pouring holes. This design not only satisfies the need for fixing and installing steel plates, but also provides a reasonable hiding position for the steel connectors. After the post-pouring strip is poured and cured, the steel connectors can be protected by sealing the post-pouring holes. This avoids the problem of exposed steel at the connection of precast components, which could lead to corrosion and affect the reliability of the connection.
[0026] 2. By adding strain sensors to the post-cast strip and using stress extreme value difference analysis, significant stress relaxation events are identified from the acquired raw signals. Once stress relaxation is determined to have occurred, the stress relaxation compensation amount is calculated. Finally, this compensation amount is converted into an adjustment action for the preload of the locking bolts, realizing active and closed-loop compensation for the preload of the joint. This solves the stress relaxation problem caused by material properties during the curing process of the post-cast strip and can significantly improve the reliability of the joint.
[0027] 3. By combining temperature and humidity data with the preset target curing threshold of UHPC poured at the post-pouring strip, the predicted curing time can be calculated to predict the remaining curing time required to reach the target strength. This can better adapt to the changing climate conditions on site and avoid the problems of strength defects caused by insufficient curing or delays caused by over-curing. Attached Figure Description
[0028] Figure 1 A schematic diagram of the existing floating structure unit's three-dimensional structure;
[0029] Figure 2 This is a three-dimensional structural diagram of the post-cast strip of the present invention.
[0030] Figure 3 This is a schematic cross-sectional view of the post-cast strip structure of the present invention.
[0031] Among them: 1-precast slab, 2-precast beam, 3-post-cast strip, 4-steel connector, 5-post-cast hole, 6-support steel plate, 7-locking bolt, 8-sealant, 9-FRP reinforcement structure. Detailed Implementation
[0032] The present invention will be further described below with reference to embodiments, but this does not constitute any limitation on the present invention. Any limited modifications made by any person within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0033] See Figures 1-2 Floating structural units can be applied to the construction and installation of prefabricated marine engineering structures such as offshore platforms, floating bridges, and offshore wind power foundations. Their specific structure typically consists of an outer support member composed of several prefabricated slabs 1 connected together, and an inner support member set within the outer support member. The inner support member is composed of several prefabricated beams 2 connected together. To achieve the connection between the inner and outer support members, post-cast strips 3 are provided between the beam ends of the prefabricated beams 2 and between the beam ends and the outer support members. The post-cast strips 3 typically contain FRP (fiberglass reinforced plastic) reinforcement structures 9. During connection, the overlapping areas of the FRP reinforcement structures 9 are overlapped using a wet bonding method, and then UHPC (ultra-high-performance concrete) is poured onto the post-cast strips 3.
[0034] Furthermore, to facilitate the successful casting of UHPC within the post-cast strip 3, the traditional method involves pre-embedding bolts in the precast components on both sides of the post-cast strip 3 to facilitate subsequent steel plate installation. However, these pre-embedded bolts not only protrude from the surface of the precast components, but are also susceptible to corrosion and damage during long-term use in a marine environment, thus affecting the structural integrity and even the reliability of the connection. Figure 3As shown, for this purpose, multiple steel connectors 4 are pre-embedded in the precast components on both sides of the post-cast strip 3 of the floating structural unit proposed in this invention, and post-cast holes 5 are provided between the steel connectors 4 and the outer surface of the precast components. Supporting steel plates 6 are provided on the outer side of the post-cast strip 3, and the supporting steel plates 6 are connected to the steel connectors 4 by locking bolts 7. After the post-cast strip 3 is poured, the locking bolts 7 and the supporting steel plates 6 can be removed. Since the steel connectors 4 are built into the precast components, only the post-cast holes 5 need to be sealed to protect the internal steel, thereby avoiding the problem of exposed steel at the connection point of the precast components causing corrosion and affecting the connection reliability.
[0035] Furthermore, in order to digitize the data during the curing process of the post-cast strip, this embodiment installs a strain sensor in the strip body 3, which is used to collect stress data of the post-cast strip during the curing process, providing data support for the adjustment of the connectors during the subsequent curing process.
[0036] In one embodiment, the aforementioned post-cast strip further includes a sealing element 8. This sealing element 8 consists of a sealing section screwed into the steel connector 4 and a filling section that fills and seals the post-cast hole 5. The sealing section can be made of seawater-resistant plastic; the filling section can be cast using UHPC, or a UHPC-cast filling section can be used with an adhesive to fill the post-cast hole 5. This design effectively isolates the corrosive environment, extends the service life of the connection joint, and avoids the problem of clogging the threaded holes in the steel connector 4 caused by casting UHPC into the post-cast hole 5. That is, in subsequent maintenance, if the post-cast strip 3 needs to be recast, the filling section and sealing section can be removed sequentially, and the steel connector 4 can be used again to install the supporting steel plate 6.
[0037] After the precast slab 1 and precast beam 2 of the precast assembled floating structure are spliced together to form the post-cast strip 3, a supporting steel plate 6 can be added to form a casting mold, and then UHPC is cast in the post-cast strip 3. After the post-cast strip is cast and cured to a certain strength, the steel plate can be removed. However, during this curing process, UHPC and adhesive will shrink and experience stress relaxation. The resulting slight deformation may cause stress shift (reduction of preload) between the beam end and the precast slab. If the displacement or stress is not compensated, the reliability of the joint connection will be affected. Therefore, this invention proposes the following curing method for the post-cast strip:
[0038] During the curing process, stress signals output by strain sensors are collected in real time. Based on the stress signals, stress extreme value difference analysis is performed to determine whether stress relaxation occurs in the UHPC poured in the post-pouring strip 3. If so, the stress trend value is calculated, and the stress relaxation compensation amount is calculated in combination with the initial reference stress value. The stress relaxation compensation amount is then applied to the locking bolts 7. This curing process continues until the UHPC poured in the post-pouring strip 3 has cured to the target strength, after which the steel plate 6 support is removed.
[0039] In an embodiment of the present invention, by collecting stress signals in the post-cast strip 3 region in real time during the curing process, stress relaxation caused by UHPC shrinkage and creep can be detected; through stress extreme value difference analysis, significant stress relaxation events can be identified from the collected original signals; once stress relaxation is determined to occur, the stress relaxation compensation amount is calculated; finally, the compensation amount is converted into the pre-tightening force adjustment action of the locking bolt 7 to achieve compensation for the pre-tightening force of the node, thereby solving the stress relaxation problem caused by material characteristics during the curing process of the post-cast strip and significantly improving the reliability of the node.
[0040] Regarding the stress extreme value difference analysis based on stress signals mentioned above, this analysis specifically involves: extracting the stress peak and stress trough values from all stress signals collected within a set sampling period; calculating the maximum stress change based on the difference between the stress peak and stress trough values; if the absolute value of the maximum stress change is greater than the preset maximum stress change threshold, then the UHPC poured in the post-pouring strip 3 is determined to have experienced stress relaxation. In the early stages of curing, if the UHPC experiences significant volume shrinkage or stress relaxation, its internal stress will fluctuate considerably (decline) in a short period. By comparing the difference between the stress peak and trough values within an initial time period, this abnormal stress release phenomenon can be quickly and effectively identified, providing a trigger condition for subsequent trend analysis and compensation calculations. As a specific implementation method, the set sampling period can be one hour after the start of curing, and the preset maximum stress change threshold can be experimentally calibrated based on the material properties of the UHPC and the preload of the connection design.
[0041] Regarding the aforementioned stress trend value, its calculation method is as follows: exponential smoothing based on a forgetting factor is used, with the current real-time stress signal and the previous stress estimate as parameters. The specific calculation formula can be expressed as:
[0042] .
[0043] in This represents the stress trend value at the current time t. This is the real-time stress signal acquired at the current time t. Let be the stress estimate at the previous time t-1 (i.e., the trend value at the previous time), and α be the smoothing coefficient (i.e., the forgetting factor). The value of α can range from 0.1 to 0.3.
[0044] Based on the stress trend value calculated above, and combined with the initial reference stress value, the stress relaxation compensation amount is calculated. The formula for calculating the stress relaxation compensation amount is as follows:
[0045] .
[0046] In the formula, Δcomp(t) is the adjustment amount of the bolt compensation preload to be applied at the current moment; β is the compensation gain coefficient; and S0 is the initial reference stress value. From this calculation formula, it can be seen that when... When the value is below S0, Δcomp(t) is negative, indicating that the bolt preload needs to be reduced to compensate for stress loss; conversely, it needs to be increased.
[0047] Besides stress monitoring, the duration of curing is also a crucial factor affecting the reliability of joints. In the curing method of this invention, after curing begins, temperature and humidity data of the environment surrounding the floating structure are monitored. These data are used to calculate a comprehensive curing rate attenuation factor. This factor is then combined with a preset target curing degree threshold for the UHPC poured at the post-cast strip to calculate a predicted curing time. After a positive time compensation is applied to the predicted curing time, it is determined that the UHPC poured at the post-cast strip has been cured to the target strength. In other words, by monitoring temperature and humidity in real time and calculating the comprehensive curing rate attenuation factor, the curing process can be dynamically assessed relative to standard conditions to determine whether the current environment accelerates or decelerates the process. By accumulating the impact of the comprehensive curing rate attenuation factor and comparing it with the target curing degree threshold, the remaining curing time required to reach the target strength can be predicted. This method better adapts to varying on-site climatic conditions, avoiding strength defects due to insufficient curing or project delays caused by over-curing.
[0048] In this embodiment, the curing time prediction is calculated by combining the comprehensive curing rate attenuation factor with the target curing degree threshold, as mentioned above. The formula for calculating the predicted curing time is as follows:
[0049] .
[0050] In the formula, The target curing threshold for the UHPC poured at the pre-set post-pouring strip; Let be the comprehensive curing rate attenuation factor corresponding to the i-th sampling time ti, where
[0051] .
[0052] In the formula, a and b are the empirical weighting coefficients for temperature and humidity, respectively, and their values are typically 0.1 ≤ a ≤ 0.50 and 0.05 ≤ b ≤ 0.3. t : Ambient temperature at current time t. T0: Base curing temperature, e.g., 20°C. Ht: Ambient relative humidity at current time t. H0: Base curing relative humidity, e.g., 50%. The time interval between two samplings; This is a predicted maintenance time.
[0053] In practical applications, since theoretical prediction models may contain certain errors, this invention proposes to compensate the predicted curing time with a positive time factor, which is 10%-20% of the predicted curing time. This additional 10%-20% curing time ensures that the UHPC strength has a higher probability of fully reaching and exceeding the design target strength, thereby guaranteeing the final quality of the structural connection nodes. Simultaneously, it optimizes the curing period while ensuring structural safety, avoiding unnecessary excessive extension.
[0054] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the structure of the present invention, and these will not affect the effectiveness of the implementation of the present invention or the practicality of the patent.
Claims
1. A post-cast strip for a floating structural unit, characterized in that, The belt (3) is set between two precast components. A strain sensor is installed in the belt (3). Multiple steel connectors (4) are pre-embedded in the precast components on both sides of the belt (3). A post-casting hole (5) is provided between the steel connector (4) and the outer surface of the precast component. A support steel plate (6) is provided on the outer side of the belt (3). The support steel plate (6) is connected to the steel connector (4) by a locking bolt (7).
2. The post-cast strip of a floating structural unit according to claim 1, characterized in that, It also includes a seal (8), which consists of a sealing section screwed into a steel connector (4) and a filling section that fills and seals the post-gating hole (5).
3. A method for curing the post-cast strip of a floating structural unit as described in any one of claims 1-2, characterized in that, The method is as follows: After the prefabricated components are assembled and the belt (3) is formed, the supporting steel plate (6) is installed on the outside of the belt (3). A strain sensor is built into the belt (3), and then UHPC is cast into the belt (3) and the floating structure unit is cured. During the maintenance process, the stress signal output by the strain sensor is collected in real time. Based on the stress signal, stress extreme value difference analysis is performed to determine whether the UHPC poured in the belt (3) has stress relaxation. If so, the stress trend value is calculated, and the stress relaxation compensation amount is calculated in combination with the initial reference stress value. The stress relaxation compensation amount is then applied to the locking bolt (7). After the UHPC poured into the belt (3) has been cured to the target strength, the steel plate (6) support is removed.
4. The maintenance method according to claim 3, characterized in that, The stress extremum difference analysis specifically refers to: Stress peak and stress valley values are extracted from all stress signals collected from the set sampling period. The maximum stress change is calculated based on the difference between the stress peak and stress valley values. If the absolute value of the maximum stress change is greater than the preset maximum stress change threshold, it is determined that the UHPC cast in the belt (3) is under stress relaxation.
5. The maintenance method according to claim 3, characterized in that, The stress trend value is calculated by using exponential smoothing based on the forgetting factor, with the real-time stress signal at the current moment and the stress estimate at the previous moment as parameters.
6. The maintenance method according to claim 3, characterized in that, The formula for calculating the stress relaxation compensation amount is: , In the formula, Δcomp(t) is the adjustment amount of the bolt compensation preload to be applied at the current moment; β is the compensation gain coefficient; This represents the stress trend value; S0 is the initial reference stress value.
7. The maintenance method according to claim 3, characterized in that, During the curing process of the floating structure unit, the temperature and humidity data of the environment in which the floating structure unit is located are detected. The comprehensive curing rate attenuation factor is calculated using the temperature and humidity data. The comprehensive curing rate attenuation factor is combined with the preset target curing degree threshold of the UHPC poured at the post-pouring strip to calculate the predicted curing time value. After the predicted curing time value is compensated by a positive time amount, it is determined that the UHPC poured at the post-pouring strip has been cured to the target strength.
8. The maintenance method according to claim 7, characterized in that, The formula for calculating the predicted maintenance time is as follows: , In the formula, The target curing threshold for the UHPC poured at the pre-set post-pouring strip; The comprehensive curing rate attenuation factor corresponding to the i-th sampling time ti; The time interval between two samplings; This is a predicted maintenance time.
9. The maintenance method according to claim 7, characterized in that, The positive time compensation is 10%-20% of the predicted maintenance time.