Self-lubricating bearing and manufacturing process thereof

By employing a gradient three-dimensional interconnected pore structure and a composite self-lubricating layer in the self-lubricating bearing, the problems of insufficient interfacial bonding strength and uneven lubrication performance are solved, achieving high-strength bonding and long-lasting lubrication, making it suitable for heavy-load conditions.

CN123134151APending Publication Date: 2026-11-20JIAXING WUZHOU BEARING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611311158.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing self-lubricating bearings suffer from problems such as insufficient interfacial bonding strength, uneven lubricant distribution, limited lubricant reserves, and difficulty in balancing mechanical strength and lubrication performance. In particular, under heavy load or impact conditions, coating peeling and material cracking are prone to occur.

Method used

The design employs a metal matrix and a composite self-lubricating layer. The metal matrix has a gradient three-dimensional interconnected pore structure. The transition layer is formed by metal powder with a particle size smaller than that of the matrix pores, creating a metallurgical bond. The self-lubricating functional layer includes a polymer matrix, a solid lubricant, and a reinforcing phase. The micro-pit structure increases the contact area and mechanical locking effect, forming a dual enhancement mechanism of chemical bonding and mechanical locking.

Benefits of technology

It achieves a high-strength bond between the self-lubricating functional layer and the metal substrate, improving the bearing's load-bearing capacity and the durability of its lubrication performance. It is suitable for heavy-duty applications, extends service life, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123134151A_ABST
    Figure CN123134151A_ABST
Patent Text Reader

Abstract

The application discloses a kind of self-lubricating bearings and manufacturing process thereof, belong to bearing technical field.The self-lubricating bearing includes metal matrix and composite self-lubricating layer, metal matrix is powder metallurgy forming body, its inside has the gradient three-dimensional interconnected porosity structure of surface porosity higher than heart porosity;Composite self-lubricating layer includes transition layer and self-lubricating functional layer sequentially arranged from inside to outside, the transition layer is made of metal powder with smaller particle size than the average pore diameter of the metal matrix, by sintering diffusion into the surface porosity of the metal matrix, and form metallurgical bonding with the metal matrix.Its manufacturing process includes powder mixing, pressing, pre-sintering, transition layer preparation, self-lubricating functional layer composite, solidification forming and finishing machining and other steps.The application realizes high-strength metallurgical bonding of self-lubricating functional layer and metal matrix through transition layer design, solves the problem of easy peeling of traditional self-lubricating coating;The gradient three-dimensional interconnected porosity structure of metal matrix can store lubricating oil, realize the synergistic effect of solid lubrication and oil-containing lubrication.The bearing of the application has high bearing capacity, excellent self-lubricating performance and long service life, and the manufacturing process is simple and reliable, suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of bearing technology, and in particular to a self-lubricating bearing and its manufacturing process. Background Technology

[0002] Bearings are key components in mechanical transmission systems and are widely used in various rotating equipment and reciprocating motion mechanisms. Traditional bearings require regular lubrication and maintenance using lubricating oil or grease during operation, which not only increases maintenance costs but also makes it difficult for conventional lubricating oils to evaporate, decompose, or fail under special operating conditions such as high temperature and high vacuum, thus failing to meet usage requirements.

[0003] Self-lubricating bearings achieve low-friction operation without the need for external lubricants by introducing solid lubricants (such as graphite, molybdenum disulfide, and polytetrafluoroethylene) into the bearing housing or friction surfaces. Existing self-lubricating bearings mainly suffer from the following technical problems: First, the interfacial bonding strength is insufficient. In traditional coated self-lubricating bearings, the self-lubricating coating and the metal substrate are heterogeneous interfaces with limited bonding strength. Under heavy load or impact conditions, the coating is prone to peeling off, leading to bearing failure.

[0004] Secondly, the lubricant distribution is uneven. In existing powder metallurgy self-lubricating bearings, it is difficult to control the uniformity of the distribution of solid lubricant in the matrix, resulting in significant differences in lubrication performance in different areas of the bearing.

[0005] Third, the lubricant supply is limited. As the lubricant in embedded self-lubricating bearings is gradually consumed over time, the bearing friction coefficient increases significantly, thus limiting its service life.

[0006] Fourth, it is difficult to balance mechanical strength and lubrication performance. The lubricant content in powder metallurgy self-lubricating bearings is limited by the process; excessively high content will significantly reduce the mechanical strength of the bearing, and material cracking or collapse is likely to occur in actual use.

[0007] In recent years, researchers have proposed the concept of gradient self-lubricating bearings, such as using a three-layer structure design (pressure-bearing layer, transition layer, and lubrication layer) to improve overall performance, or optimizing interfacial bonding through the porosity difference of gradient copper powder layers. However, the transition layer of existing gradient self-lubricating bearings mostly uses a simple mixture of pressure-bearing and lubrication layer materials, failing to achieve deep integration of metal powder with the matrix pores; their pore structure is mostly a single porosity distribution, without considering the gradient porosity design between the surface and the core. Therefore, the improvement in interfacial bonding strength and load-bearing capacity remains limited. Summary of the Invention

[0008] The purpose of this invention is to provide a self-lubricating bearing and its manufacturing process, which can achieve a high-strength metallurgical bond between the self-lubricating functional layer and the metal substrate, improve the bearing's load-bearing capacity and the durability of its self-lubricating performance, and has a simple structure and is easy to manufacture, thereby solving the problems mentioned in the background art.

[0009] To achieve the above objectives, the present invention provides the following technical solution: A self-lubricating bearing includes a metal substrate and a composite self-lubricating layer, wherein the composite self-lubricating layer is disposed on the friction working surface of the metal substrate; The metal matrix is ​​a powder metallurgy shaped body, which has a gradient three-dimensional interconnected pore structure with a surface porosity higher than the core porosity. The composite self-lubricating layer includes a transition layer and a self-lubricating functional layer arranged sequentially from the inside to the outside. The transition layer is composed of metal powder, the particle size of which is smaller than the average pore diameter of the metal matrix. The transition layer is embedded in the surface pores of the metal matrix and forms a metallurgical bond with the metal matrix. The self-lubricating functional layer covers the transition layer and has a thickness of 0.5 to 5.0 mm.

[0010] By adopting the above technical solution, the transition layer metal powder, because its particle size is smaller than the average pore diameter of the matrix, can fully diffuse into the pores of the matrix surface during sintering, forming a dual-reinforced structure of three-dimensional mechanical interlocking and metallurgical bonding. This achieves a high-strength bond between the self-lubricating functional layer and the metal matrix, solving the problem of easy peeling of traditional self-lubricating coatings. The gradient three-dimensional interconnected pore structure of the metal matrix gives the surface a higher porosity, providing sufficient embedding space for the transition layer, while also storing lubricating oil to achieve a synergistic effect of solid lubrication and oil-containing lubrication.

[0011] As a further aspect of the present invention: the metal matrix is ​​formed by pressing and sintering iron-based powder or copper-based powder, with a surface porosity of 15% to 35% and a core porosity of 5% to 20%, and the surface porosity is higher than the core porosity.

[0012] By adopting the above technical solution, the higher porosity of the surface layer provides more anchor points and a larger specific surface area for the diffusion and infiltration of the transition layer metal powder, significantly improving the interfacial bonding strength; the lower porosity of the core ensures that the matrix has sufficient mechanical strength. This gradient pore structure of "sparse on the outside and dense on the inside" achieves synergistic optimization of lubrication performance and mechanical strength.

[0013] As a further aspect of the present invention: the self-lubricating functional layer comprises a polymer matrix material, a solid lubricant, and a reinforcing phase; The solid lubricant is selected from one or more of graphite, molybdenum disulfide, polytetrafluoroethylene, and hexagonal boron nitride; The reinforcing phase is selected from one or more of silicon carbide whiskers, alumina particles, and carbon fibers.

[0014] By adopting the above technical solution, the solid lubricant provides self-lubricating performance with a low coefficient of friction, the reinforcing phase effectively improves the wear resistance and compressive strength of the composite self-lubricating layer, and the bridging and toughening effect of silicon carbide whiskers and carbon fibers can inhibit the crack propagation of the self-lubricating functional layer.

[0015] As a further aspect of the present invention: in the self-lubricating functional layer, the polymer matrix material has a mass percentage content of 50% to 80%, the solid lubricant has a mass percentage content of 10% to 35%, and the reinforcing phase has a mass percentage content of 5% to 15%.

[0016] By adopting the above technical solution, the reasonable component ratio ensures that the self-lubricating functional layer has both good lubrication performance and sufficient mechanical strength.

[0017] As a further aspect of the present invention: the polymer matrix material is selected from one or more of polytetrafluoroethylene, polyimide, and polyetheretherketone.

[0018] By adopting the above technical solution, the polymer material has excellent heat resistance, mechanical properties and chemical stability, and is suitable as a matrix for self-lubricating functional layers.

[0019] As a further aspect of the present invention: the transition layer is composed of metal powder of the same type or homology as the metal matrix, the particle size of which is smaller than the average pore diameter of the metal matrix, and diffuses into the surface pores of the metal matrix through sintering.

[0020] By adopting the above technical solution, the particle size of the transition layer metal powder is smaller than the average pore diameter of the matrix, which ensures that the powder particles can fully enter the pores during the sintering process and form a three-dimensional interlocking structure in the shape of "anchors"; the same or homogeneous metal powder ensures good metallurgical compatibility between the transition layer and the matrix.

[0021] As a further aspect of the present invention: a plurality of micro-pits are provided on the friction working surface of the metal substrate, the depth of the micro-pits being 0.1 to 1.0 mm, and the composite self-lubricating layer filling the micro-pits and covering the friction working surface.

[0022] By adopting the above technical solution, the micro-dimple structure increases the contact area and mechanical locking effect between the self-lubricating functional layer and the metal substrate, and forms a dual enhancement mechanism of "chemical bonding + mechanical locking" with the metallurgical bonding of the transition layer, which further improves the interfacial bonding strength.

[0023] This invention also provides a manufacturing process for a self-lubricating bearing, comprising the following steps: Step 1, Powder Mixing: Mix metal powder, pore-forming agent, and lubricant evenly in a certain proportion. The pore-forming agent is ammonium bicarbonate or urea, and the amount of pore-forming agent added is 5% to 20% of the mass of the metal powder. Step 2, pressing: The mixed powder obtained in Step 1 is filled into the bearing mold and pressed into shape under a pressure of 300-800 MPa to obtain the bearing blank; Step 3, pre-sintering: The bearing blank obtained in step 2 is pre-sintered under a protective atmosphere at a sintering temperature of 800-1100℃ and a holding time of 30-180 minutes to obtain a porous metal matrix with a gradient three-dimensional interconnected pores with a surface porosity higher than the core porosity. Step 4, Transition layer preparation: A metal powder slurry is coated onto the friction working surface of the porous metal substrate. The particle size of the metal powder in the slurry is smaller than the average pore diameter of the porous metal substrate. Secondary sintering is carried out under a protective atmosphere at a temperature of 900–1200°C and a holding time of 20–120 minutes, allowing the metal powder to diffuse into the surface pores of the porous metal substrate to form a transition layer. Step 5, self-lubricating functional layer composite: The self-lubricating functional layer composite material is applied onto the transition layer, wherein the self-lubricating functional layer composite material comprises a polymer matrix material, a solid lubricant, and a reinforcing phase; Step 6, Curing and Molding: The product obtained in Step 5 is heated and cured at a temperature of 250-400℃ for 30-180 minutes to ensure a tight bond between the self-lubricating functional layer and the transition layer. Step 7, finishing: Machining is performed according to the final size requirements of the bearing to achieve the required dimensional accuracy and surface roughness.

[0024] By adopting the above technical solution, the manufacturing process is based on powder metallurgy technology, with a simple process flow, and is suitable for mass production. Through the coordinated control of the type and amount of pore-forming agent, as well as the pre-sintering temperature and time, the one-step forming of the gradient pore structure is realized. The composite of the transition layer and the self-lubricating functional layer is completed in one process flow, without the need for additional bonding equipment, thus reducing manufacturing costs.

[0025] As a further aspect of the present invention: in step one, the metal powder is iron powder or copper powder, the pore-forming agent is ammonium bicarbonate or urea, and the amount of pore-forming agent added is 5% to 20% of the mass of the metal powder.

[0026] By employing the above technical solution, ammonium bicarbonate or urea decomposes and volatilizes during the pre-sintering process. Because its decomposition temperature matches the sintering temperature window of copper / iron-based powders, a uniformly distributed gradient three-dimensional interconnected pore structure can be formed in the matrix. When the amount of pore-forming agent added is less than 5%, the porosity is insufficient; when it is greater than 20%, the matrix strength decreases significantly.

[0027] As a further aspect of the present invention: the protective atmosphere in step three is nitrogen, argon, or a mixture of hydrogen and nitrogen.

[0028] By adopting the above technical solution, a protective atmosphere is used to prevent the metal powder from oxidizing during high-temperature sintering, thus ensuring the sintering quality.

[0029] As a further aspect of the present invention: the metal powder in the metal powder slurry of step four has the same composition as the metal powder in step one.

[0030] By adopting the above technical solution, metal powders with the same composition ensure the metallurgical compatibility and bonding strength between the transition layer and the metal substrate.

[0031] As a further aspect of the present invention, the heating and curing in step six is ​​carried out in a vacuum environment or under a protective atmosphere.

[0032] By adopting the above technical solutions, a vacuum or protective atmosphere environment is used to prevent the polymer matrix material from oxidizing and degrading during the high-temperature curing process.

[0033] As a further aspect of the present invention, after step seven, an immersion step is also included: the finished bearing is immersed in lubricating oil and kept under vacuum for 10 to 60 minutes, so that the lubricating oil penetrates into the pores of the metal substrate.

[0034] By adopting the above technical solution, vacuum impregnation allows the lubricating oil to fully fill the three-dimensional interconnected pores of the metal matrix, achieving the oil-containing self-lubricating function and further extending the service life of the bearing.

[0035] Compared with the prior art, the beneficial effects of the present invention are: This invention limits the particle size of the transition layer metal powder to be smaller than the average pore diameter of the metal matrix, allowing the metal powder to fully diffuse into the surface pores of the porous metal matrix during sintering. This forms a dual-reinforcement structure of three-dimensional mechanical interlocking and metallurgical bonding, completely solving the problem of insufficient bonding strength and easy delamination and peeling caused by the heterogeneous interface between traditional self-lubricating coatings and the matrix.

[0036] This invention utilizes ammonium bicarbonate or urea as pore-forming agents, and precisely controls the addition amount (5%–20%), pre-sintering temperature (800–1100℃), and time (30–180 minutes) to form a gradient three-dimensional interconnected pore structure in a metal matrix, where the surface porosity (15%–35%) is higher than the core porosity (5%–20%). The higher surface porosity provides ample embedding space and anchor points for the transition layer, while the lower core porosity ensures the load-bearing capacity of the matrix, achieving synergistic optimization of lubrication performance and mechanical strength.

[0037] In the self-lubricating functional layer of the present invention, the solid lubricant is uniformly distributed, and the gradient three-dimensional interconnected pore structure of the metal matrix can store lubricating oil, realizing the synergistic effect of solid lubrication and oil-containing lubrication. Even after the solid lubricant is partially consumed, the lubricating oil stored in the pores can still provide continuous lubrication, significantly extending the service life of the bearing.

[0038] The self-lubricating functional layer of the present invention adopts a three-phase composite system of "polymer matrix material + solid lubricant + reinforcing phase". The introduction of the reinforcing phase (silicon carbide whiskers, alumina particles, carbon fibers) not only improves the compressive strength and wear resistance of the composite self-lubricating layer, but also inhibits the crack propagation of the self-lubricating functional layer through the bridging and toughening effect of whiskers / fibers.

[0039] This invention, through the synergistic design of micro-pit structure and metallurgical combination of transition layer, forms a dual interface enhancement mechanism of "chemical bonding + mechanical locking", which significantly improves the interface peeling strength.

[0040] The metal matrix formed by powder metallurgy in this invention has high mechanical strength, while the reinforcing phase in the self-lubricating functional layer effectively improves the wear resistance and compressive strength of the composite self-lubricating layer, making the bearing suitable for heavy-load conditions.

[0041] The manufacturing process of this invention is based on powder metallurgy technology, with a simple process flow that is suitable for mass production. The composite of the transition layer and the self-lubricating functional layer is completed in one process flow, without the need for additional bonding or coating equipment, thus reducing manufacturing costs.

[0042] Other features and advantages of the present invention will be disclosed in detail in the following detailed description and accompanying drawings. Attached Figure Description

[0043] Figure 1 This is a schematic diagram of an overall structure in one embodiment of the present invention; Figure 2 This is a partially enlarged schematic diagram of the bonding between the surface pores of the metal substrate and the transition layer in an embodiment of the present invention.

[0044] The figures are labeled as follows: 1. Metal substrate; 2. Transition layer; 3. Self-lubricating functional layer; 4. Pores; 5. Micro-pits. Detailed Implementation

[0045] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0046] See Figure 1-2 As shown, a self-lubricating bearing and its manufacturing process are disclosed. The self-lubricating bearing includes a metal substrate 1 and a composite self-lubricating layer, which is disposed on the friction working surface of the metal substrate 1.

[0047] In this embodiment, the metal substrate 1 is a powder metallurgy formed body, which has a gradient three-dimensional interconnected pore structure 4 with a surface porosity higher than the core porosity. The metal substrate 1 is formed by pressing and sintering iron-based powder or copper-based powder, with a surface porosity of 15% to 35% and a core porosity of 5% to 20%.

[0048] In this embodiment, the composite self-lubricating layer includes a transition layer 2 and a self-lubricating functional layer 3 arranged sequentially from the inside out. The transition layer 2 is composed of metal powder, the particle size of which is smaller than the average pore diameter 4 of the metal substrate 1. The transition layer 2 is embedded in the surface pores 4 of the metal substrate 1, forming a metallurgical bond with the metal substrate 1. The transition layer 2 is composed of metal powder of the same type or homology as the metal substrate 1, and diffuses into the surface pores 4 of the metal substrate 1 through sintering.

[0049] In this embodiment, the self-lubricating functional layer 3 covers the transition layer 2, and its thickness is 0.5–5.0 mm. The self-lubricating functional layer 3 comprises a polymer matrix material, a solid lubricant, and a reinforcing phase. The polymer matrix material is selected from one or more of polytetrafluoroethylene, polyimide, and polyetheretherketone. The solid lubricant is selected from one or more of graphite, molybdenum disulfide, polytetrafluoroethylene, and hexagonal boron nitride. The reinforcing phase is selected from one or more of silicon carbide whiskers, alumina particles, and carbon fibers.

[0050] In this embodiment, in the self-lubricating functional layer 3, the mass percentage of the polymer matrix material is 50% to 80%, the mass percentage of the solid lubricant is 10% to 35%, and the mass percentage of the reinforcing phase is 5% to 15%.

[0051] In this embodiment, multiple micro-pits 5 are provided on the friction working surface of the metal substrate 1. The depth of the micro-pits 5 is 0.1-1.0 mm. The composite self-lubricating layer fills the micro-pits 5 and covers the friction working surface. The micro-pit 5 structure increases the contact area and mechanical locking effect between the self-lubricating functional layer 3 and the metal substrate 1. It forms a dual enhancement mechanism of "chemical bonding + mechanical locking" with the metallurgical bonding of the transition layer 2, further improving the interfacial bonding strength.

[0052] In this embodiment, the manufacturing process of the self-lubricating bearing includes the following steps: Step 1, Powder Mixing: Mix the metal powder, pore-forming agent, and lubricant evenly according to the specified proportions. The metal powder is iron powder or copper powder, and the pore-forming agent is ammonium bicarbonate or urea. The amount of pore-forming agent added is 5% to 20% of the mass of the metal powder.

[0053] Step 2, pressing: The mixed powder obtained in Step 1 is filled into the bearing mold and pressed into shape under a pressure of 300-800 MPa to obtain the bearing blank.

[0054] Step 3, Pre-sintering: The bearing blank obtained in Step 2 is pre-sintered under a protective atmosphere at a sintering temperature of 800–1100℃ and a holding time of 30–180 minutes to obtain a porous metal matrix 1 with a gradient three-dimensional interconnected pores 4 where the surface porosity is higher than the core porosity. The protective atmosphere is nitrogen, argon, or a hydrogen-nitrogen mixture.

[0055] Step four, preparation of transition layer 2: A metal powder slurry is coated onto the friction working surface of the porous metal substrate 1. The particle size of the metal powder in the slurry is smaller than the average pore diameter 4 of the porous metal substrate 1. A secondary sintering process is performed under a protective atmosphere at a temperature of 900–1200°C for 20–120 minutes, allowing the metal powder to diffuse into the surface pores 4 of the porous metal substrate 1, forming transition layer 2. The metal powder in the slurry has the same composition as the metal powder in step one.

[0056] Step 5, self-lubricating functional layer 3 composite: The self-lubricating functional layer 3 composite material is applied on the transition layer 2. The self-lubricating functional layer 3 composite material includes a polymer matrix material, a solid lubricant and a reinforcing phase.

[0057] Step Six, Curing and Molding: The product obtained in Step Five is heated and cured at a temperature of 250–400℃ for 30–180 minutes to ensure a tight bond between the self-lubricating functional layer 3 and the transition layer 2. Heating and curing are performed in a vacuum environment or under a protective atmosphere.

[0058] Step 7, finishing: Machining is performed according to the final size requirements of the bearing to achieve the required dimensional accuracy and surface roughness.

[0059] Step 8, Immersion: Immerse the finished bearing in lubricating oil and maintain it under vacuum for 10 to 60 minutes to allow the lubricating oil to penetrate into the pores 4 of the metal substrate 1.

[0060] In this embodiment, it can be understood that the self-lubricating bearing obtained by the above manufacturing process has high load-bearing capacity, excellent self-lubricating performance and long service life.

[0061] This invention provides a self-lubricating bearing and its manufacturing process, which can achieve a high-strength metallurgical bond between the self-lubricating functional layer 3 and the metal substrate 1, thereby improving the bearing's load-bearing capacity and the durability of its self-lubricating performance, resulting in high reliability.

[0062] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

[0063] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A self-lubricating bearing, characterized in that, It includes a metal substrate (1) and a composite self-lubricating layer, wherein the composite self-lubricating layer is disposed on the friction working surface of the metal substrate (1); The metal matrix (1) is a powder metallurgy molded body, which has a gradient three-dimensional interconnected pore (4) structure with a surface porosity higher than the core porosity. The composite self-lubricating layer includes a transition layer (2) and a self-lubricating functional layer (3) arranged sequentially from the inside to the outside. The transition layer (2) is composed of metal powder, the particle size of which is smaller than the average pore diameter of the metal matrix (1). The transition layer (2) is embedded in the surface pores (4) of the metal matrix (1) and forms a metallurgical bond with the metal matrix (1). The self-lubricating functional layer (3) covers the transition layer (2).

2. The self-lubricating bearing according to claim 1, characterized in that, The thickness of the self-lubricating functional layer (3) is 0.5 to 5.0 mm; the self-lubricating functional layer (3) comprises a polymer matrix material, a solid lubricant and a reinforcing phase; The solid lubricant is selected from one or more of graphite, molybdenum disulfide, polytetrafluoroethylene, and hexagonal boron nitride; The reinforcing phase is selected from one or more of silicon carbide whiskers, alumina particles, and carbon fibers.

3. The self-lubricating bearing according to claim 2, characterized in that, In the self-lubricating functional layer (3), the polymer matrix material has a mass percentage of 50% to 80%, the solid lubricant has a mass percentage of 10% to 35%, and the reinforcing phase has a mass percentage of 5% to 15%.

4. The self-lubricating bearing according to claim 2, characterized in that, The polymer matrix material is selected from one or more of polytetrafluoroethylene, polyimide, and polyetheretherketone.

5. The self-lubricating bearing according to claim 1, characterized in that, The metal matrix (1) is formed by pressing and sintering iron-based powder or copper-based powder, with a surface porosity of 15% to 35% and a core porosity of 5% to 20%, and the surface porosity is higher than the core porosity.

6. The self-lubricating bearing according to claim 1, characterized in that, The metal substrate (1) has a plurality of micro-pits (5) on its friction working surface. The depth of the micro-pits (5) is 0.1 to 1.0 mm. The composite self-lubricating layer fills the micro-pits (5) and covers the friction working surface.

7. A manufacturing process for a self-lubricating bearing as described in any one of claims 1 to 6, characterized in that, Includes the following steps: Step 1, Powder Mixing: Mix metal powder, pore-forming agent, and lubricant evenly in a certain proportion. The pore-forming agent is ammonium bicarbonate or urea, and the amount of pore-forming agent added is 5% to 20% of the mass of the metal powder. Step 2, pressing: The mixed powder obtained in Step 1 is filled into the bearing mold and pressed into shape to obtain the bearing blank; Step 3, pre-sintering: The bearing blank obtained in step 2 is pre-sintered in a protective atmosphere at a sintering temperature of 800-1100℃ and a holding time of 30-180 minutes to obtain a porous metal matrix (1) with a gradient three-dimensional interconnected pore structure (4) where the surface porosity is higher than the core porosity. Step 4, preparation of transition layer (2): Metal powder slurry is coated on the friction working surface of the porous metal substrate (1). The particle size of the metal powder in the metal powder slurry is smaller than the average pore diameter of the porous metal substrate (1). Secondary sintering is carried out under a protective atmosphere. The sintering temperature is 900-1200℃ and the holding time is 20-120 minutes, so that the metal powder diffuses into the surface pores (4) of the porous metal substrate (1) to form transition layer (2). Step 5, self-lubricating functional layer (3) composite: apply the self-lubricating functional layer (3) composite material onto the transition layer (2), wherein the self-lubricating functional layer (3) composite material comprises a polymer matrix material, a solid lubricant and a reinforcing phase; Step 6, Curing and Molding: The product obtained in Step 5 is heated and cured at a temperature of 250-400℃ for 30-180 minutes to ensure that the self-lubricating functional layer (3) and the transition layer (2) are tightly bonded. Step 7, Finishing: Machining is performed according to the final dimensional requirements of the bearing.

8. The manufacturing process according to claim 7, characterized in that, In step one, the metal powder is iron powder or copper powder; in step two, the pressing pressure is 300-800 MPa; in step three, the protective atmosphere is nitrogen, argon, or a hydrogen-nitrogen mixture; in step four, the metal powder in the metal powder slurry has the same composition as the metal powder in step one; in step six, the heating and curing is carried out in a vacuum environment or under a protective atmosphere.

9. The manufacturing process according to claim 7, characterized in that, The process following step seven includes an immersion step: immersing the finished bearing in lubricating oil and maintaining it under vacuum for 10 to 60 minutes.