A low-rigidity high-durability rubber bushing and a manufacturing method thereof

By using a split shell, open slot, embedded insert, and double-layer rubber integrated vulcanization structure, the problem of excessive stiffness of rubber bushings under external loads is solved, and differentiated stiffness design in different directions is achieved, improving the vibration reduction performance and durability of rubber bushings.

CN123134178APending Publication Date: 2026-11-20DONGFENG COMML VEHICLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611527026.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing rubber bushings tend to quickly enter a high-stiffness state under external loads, resulting in a large overall stiffness value and poor vibration damping performance, especially under low-frequency large-displacement vibrations. It is difficult to achieve differentiated stiffness design in different directions to improve comfort and durability.

Method used

It adopts a split shell, opening groove, embedded insert and double-layer rubber integrated vulcanization structure. By setting different stiffness parameters in different directions, combined with the pretreatment of dissimilar metals and the base coating plus top coating bonding system, and adopting a segmented temperature-controlled injection vulcanization process, it avoids over-vulcanization cracking of thin-walled rubber and releases residual vulcanization stress.

Benefits of technology

It achieves differentiated stiffness in different directions, providing both low-stiffness vibration reduction and high support and durability, thus improving the overall vehicle comfort and durability, and exhibiting excellent bonding strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123134178A_ABST
    Figure CN123134178A_ABST
Patent Text Reader

Abstract

The application provides a low-rigidity high-durability rubber bushing and a manufacturing method thereof, which comprises an inner cylinder, a plurality of outer shells arranged on the outer side of the inner cylinder, an injection body arranged between the outer shells and the inner cylinder, a plurality of inserts arranged in the injection body, and open grooves arranged between the outer shells. The bushing has different rigidity parameters in different directions through the split outer shell, the open groove, the embedded insert and the integrated vulcanization structure of the double-layer rubber, can provide low rigidity in the torsion or the circumference, and can provide high support and durability through the insert and the limiting structure, thereby solving the problems that the existing bushing is easily rapidly in the high-rigidity state under the action of the external load, the overall rigidity value is large, the damping performance is poor, and the problem is more obvious under the low-frequency large-displacement vibration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of automotive bushings, and in particular to a low-stiffness, high-durability rubber bushing and its manufacturing method. Background Technology

[0002] Rubber bushings are commonly used elastic connecting elements in vehicle suspensions, chassis, powertrains, and industrial vibration damping equipment. They achieve load bearing, vibration isolation, buffering, and displacement compensation through the elastic deformation of rubber.

[0003] In existing technologies, a common type of rubber spring or rubber bushing employs a circular cross-section sleeve structure, where rubber is filled within the entire circular cavity between the inner and outer cylinders, utilizing the compression, shearing, and torsional deformation of the rubber to provide stiffness. This type of structure is relatively simple to manufacture and can meet vibration reduction requirements under general working conditions. However, due to the approximately symmetrical geometric characteristics of the circular cross-section in all directions, its axial, radial, and torsional stiffness are often interrelated, making it difficult to design different stiffness parameters for different directions.

[0004] For complex stress conditions such as those in commercial vehicle suspensions, it is generally desirable for bushings to have lower stiffness in one direction to improve comfort and vibration isolation, while having higher stiffness in another direction to ensure handling stability and durability. Existing circular cross-section structures cannot achieve both simultaneously. Furthermore, when the rubber fills the entire circular bushing, the deformation space of the rubber is small, and it tends to quickly enter a high-stiffness state under external loads, resulting in a large overall stiffness value and poor vibration damping performance, especially under low-frequency, large-displacement vibrations.

[0005] To address the aforementioned issues, this solution achieves different stiffness values ​​in the longitudinal and vertical directions. The longitudinal stiffness can reach an ultra-low stiffness of 300 N / mm, exhibiting non-linear variable stiffness characteristics. When the vehicle is traveling on a good road surface, the vibration amplitude is small, and the rubber bushing exhibits low stiffness characteristics. However, when the vehicle is traveling on a poor road surface, the vibration amplitude is large, causing the inner and outer rubber bushings to deform and come into contact, increasing the bushing stiffness and effectively dampening large vibrations, thus improving overall vehicle comfort.

[0006] Therefore, there is a need for a rubber bushing that can have differentiated stiffness in different directions, while also ensuring adhesive strength and long-term durability, as well as a method for its preparation. Summary of the Invention

[0007] The main objective of this invention is to provide a low-stiffness, high-durability rubber bushing and its manufacturing method, which solves the problem that existing bushings tend to quickly enter a high-stiffness state under external loads, resulting in a large overall stiffness value, poor vibration damping performance, and more pronounced issues under low-frequency, large-displacement vibrations.

[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a low-rigidity, high-durability rubber bushing, including an inner cylinder, a plurality of outer shells on the outer side of the inner cylinder, an injection molded body between the outer shells and the inner cylinder, and a plurality of inserts inside the injection molded body; There are openings between the outer shells.

[0009] In the preferred embodiment, the inner cylinder is also provided with a through inner hole, and the inner hole is provided with multiple keyways.

[0010] In the preferred embodiment, the outer shell includes half piece one and half piece two, which are semi-circular. Half piece one includes an arc-shaped side and a flat side, and half piece one and half piece two have the same structure.

[0011] In the preferred embodiment, half piece one and half piece two are symmetrically arranged on both sides of the inner cylinder, and the opening slot is arranged between the planar sides of half piece one and half piece two. The outer side of half piece one is also provided with shell ribs, and shell grooves are formed between the shell ribs. One side of half piece one is also provided with shell protrusion.

[0012] In the preferred embodiment, half piece one and half piece two can swing between 0-10 degrees. When the swing angle is greater than 10 degrees, half piece one and half piece two abut against each other on their planar sides.

[0013] In the preferred embodiment, one side of the injection molded body is provided with a boss one, and the other side is provided with a boss two, and the injection molded body covers the outside of the insert. Boss one and boss two are respectively located at both ends of the outer shell.

[0014] In the preferred embodiment, the injection molded body is further provided with an inner cylinder, and a side plate is provided on the outside of the inner cylinder. A connecting body is provided between the side plate and the inner cylinder, and the connecting body has a certain degree of elasticity. The insert is encased in the connector, the inner cylinder is connected to the inner cylinder, the side plate is connected to the outer shell, and the injection molded body is also provided with multiple heat dissipation grooves. The outer side of the inner cylinder is also provided with multiple reinforcing elements.

[0015] In the preferred embodiment, one side of the insert has an arc-shaped surface, and a through hole is provided on the arc-shaped surface, through which the injection molded body penetrates; The curved surface faces the inner cylinder.

[0016] The above-mentioned method for manufacturing a low-stiffness, high-durability rubber bushing includes: S1: The steel inner cylinder is successively treated with alkaline washing and degreasing, shot blasting and rust removal and phosphating, and the aluminum alloy inserts and split outer shell are successively treated with degreasing, sandblasting and roughening and passivation. S2: Spray a primer onto the surface of the metal parts and dry it. Then spray an elastic adhesive onto the insert, the outer circle of the inner cylinder and the inner circle of the outer shell to form a composite adhesive layer. S3: The mold is pre-assembled with inner cylinder and insert in layers, and the split outer shell is placed in the two side cavities with reserved opening slots to enable the multi-layer structure to be closed and positioned synchronously. S4: Segmented temperature-controlled injection vulcanization is adopted. First, low-temperature plasticization and filling are carried out, and then high temperature and high pressure are used to cross-link and bond the rubber, avoiding over-vulcanization cracking of hollow thin-walled rubber. S5: After vulcanization, cool and demold, remove the semi-finished product, and keep the split shell to naturally form an opening groove to release some of the vulcanization stress; S6: Trim and clean the burrs from the rolled-up rubber ventilation and heat dissipation grooves, pre-press the outer shell to a round state and maintain pressure to offset residual vulcanization stress and improve durability; S7: Ultrasonic scanning is used to inspect the interface between the insert, injection molded body and metal. After confirming that there are no delamination bubbles, the product is transferred to finished product inspection.

[0017] In the preferred embodiment, in step S1, the surface roughness of the insert is Ra25~35μm; In step S2, all metal parts are sprayed with a rubber-metal general primer with a dry film thickness of 5-15μm, and dried at 80℃ for 3-5 minutes to keep the adhesive surface completely dry. The insert is coated with elastic adhesive on both the top and bottom sides, the inner cylinder outer circle, and the two halves of the outer shell. In step S3, the opening groove has a break gap of 3-4 mm; In step S4, the injection pressure and injection speed are divided into four stages: injection, plasticizing, holding pressure, and vulcanization. In step S6, the pre-compressed shell is held in a rounded state for 4-5 minutes.

[0018] This invention provides a low-stiffness, high-durability rubber bushing and its manufacturing method, which has the following beneficial effects: 1. The present invention uses a split shell, an open groove, an embedded insert and a double-layer rubber integrated vulcanization structure to enable the bushing to have different stiffness parameters in different directions. It can provide low stiffness in torsion or circumferential direction, and can also provide high support and durability through insert and limiting structure. 2. The rubber deformation space is reasonable to avoid excessive overall stiffness. Differentiated pretreatment of dissimilar metals and the bonding system of primer and topcoat improve the bonding strength. Segmented temperature-controlled injection vulcanization avoids over-vulcanization cracking of thin-walled rubber. Pre-compression releases residual vulcanization stress. Combined with heat dissipation grooves, it improves long-term durability. It has excellent comprehensive vibration reduction and durability performance. Attached Figure Description

[0019] The present invention will be further described below with reference to the accompanying drawings and embodiments: Figure 1 This is an isometric view of the bushing of the present invention; Figure 2 This is an axonometric view of the bushing of the present invention from another direction; Figure 3This is an axial side view of the housing of the present invention; Figure 4 This is a front view of the bushing of the present invention; Figure 5 This is a schematic diagram of half of the housing of the present invention; Figure 6 This is an axial side view of the injection molded body of the present invention; Figure 7 This is a cross-sectional schematic diagram of the bushing of the present invention; Figure 8 This is a schematic diagram of the installation of the bushing of the present invention; Figure 9 This is a graph showing the X-axis stiffness of the bushing of the present invention; Figure 10 This is a diagram showing the Z-axis stiffness curve of the bushing of this invention; In the diagram: Inner cylinder 1; Inner hole 101; Keyway 102; Outer shell 2; Half piece 1 201; Half piece 2 202; Shell rib 203; Shell groove 204; Shell protrusion 205; Arc side 206; Flat side 207; Injection molded body 3; Connector 301; Reinforcing body 302; Heat dissipation groove 303; Boss 1 304; Boss 2 305; Inner cylinder body 306; Side plate body 307; Insert plate 4; Arc surface 401; Through hole 402; Opening slot 5. Detailed Implementation

[0020] Example 1 like Figure 1-10 As shown, a low-rigidity, high-durability rubber bushing includes an inner cylinder 1, a plurality of outer shells 2 on the outside of the inner cylinder 1, an injection molded body 3 between the outer shells 2 and the inner cylinder 1, and a plurality of inserts 4 inside the injection molded body 3. An opening slot 5 is provided between the outer shells 2.

[0021] In the preferred embodiment, the inner cylinder 1 is further provided with a through inner hole 101, and the inner hole 101 is provided with multiple keyways 102.

[0022] In the preferred embodiment, the outer shell 2 includes a first half piece 201 and a second half piece 202, which are semi-circular. The first half piece 201 includes an arc-shaped side 206 and a flat side 207. The first half piece 201 and the second half piece 202 have the same structure.

[0023] In the preferred embodiment, half piece 1 201 and half piece 202 are symmetrically arranged on both sides of the inner cylinder 1, and the opening slot 5 is arranged between the planar sides 207 of half piece 1 201 and half piece 202. The outer side of half piece 201 is also provided with shell stiffener 203, a shell groove 204 is formed in front of the shell stiffener 203, and a shell protrusion 205 is also provided on one side of half piece 201.

[0024] In the preferred embodiment, half piece 1 201 and half piece 202 can swing between 0-10 degrees. When the swing angle is greater than 10 degrees, half piece 1 201 and half piece 202 abut against each other on their planar sides.

[0025] In the preferred embodiment, one side of the injection molded body 3 is provided with a boss 304 and the other side is provided with a boss 305, and the injection molded body 3 covers the outside of the insert 4. Boss 1 304 and Boss 2 305 are respectively located at both ends of the outer shell 2.

[0026] In the preferred embodiment, the injection molded body 3 is further provided with an inner cylinder 306, and a side plate 307 is provided on the outside of the inner cylinder 306. A connecting body 301 is provided between the side plate 307 and the inner cylinder 306, and the connecting body 301 has a certain elasticity. The insert 4 is encased in the connector 301, the inner cylinder 306 is connected to the inner cylinder 1, the side plate 307 is connected to the outer shell 2, and the injection molded body 3 is also provided with multiple heat dissipation slots 303. The outer side of the inner cylinder 306 is also provided with multiple reinforcing bodies 302, which are used to improve the bending strength of the inner cylinder 306.

[0027] In the preferred embodiment, one side of the insert 4 is provided with an arc-shaped surface 401, and a through hole 402 is provided on the arc-shaped surface 401, through which the injection molded body 3 penetrates the through hole 402. The curved surface 401 faces the inner cylinder 1.

[0028] The above-mentioned method for manufacturing a low-stiffness, high-durability rubber bushing includes: S1: The steel inner cylinder 1 is successively subjected to alkaline washing and degreasing, shot blasting and rust removal and phosphating treatment, and the aluminum alloy insert 4 and the split outer shell 2 are successively subjected to degreasing, sandblasting roughening and passivation treatment. S2: Spray a primer onto the surface of the metal parts and dry it. Then spray an elastic adhesive onto the insert 4, the outer circle of the inner cylinder 1 and the inner circle of the outer shell 2 to form a composite adhesive layer. S3: The mold is pre-assembled with inner cylinder 1 and insert 4 in layers, and the split outer shell 2 is placed in the two side cavities and reserved with a disconnected opening slot 5, so that the multi-layer structure can be closed and positioned synchronously. S4: Segmented temperature-controlled injection vulcanization is adopted. First, low-temperature plasticization and filling are carried out, and then high temperature and high pressure are used to cross-link and bond the rubber, avoiding over-vulcanization cracking of hollow thin-walled rubber. S5: After vulcanization, cool and demold, remove the semi-finished product, and keep the split outer shell 2 to naturally form the opening groove 5 to release some of the vulcanization stress; S6: Trim and clean the 303 burrs of the rolled rubber ventilation and heat dissipation grooves, pre-press the outer shell 2 to a round state and maintain pressure to offset residual stress from vulcanization and improve durability; S7: Use ultrasonic scanning to inspect the interface between insert 4, injection body 3 and metal. After confirming that there are no delamination bubbles, proceed to finished product inspection.

[0029] In the preferred embodiment, in step S1, the surface roughness of insert 4 is Ra25~35μm; In step S2, all metal parts are sprayed with a rubber-metal general primer with a dry film thickness of 5-15μm, and dried at 80℃ for 3-5 minutes to keep the adhesive surface completely dry. Insert 4 is coated with elastic adhesive on both the upper and lower sides, inner cylinder 1 is coated on the outer circle, and two halves of the outer shell 2 are coated with elastic adhesive on two separate sprays. In step S3, the opening groove has a 53-4 mm break gap; In step S4, the injection pressure and injection speed are divided into four stages: injection, plasticizing, holding pressure, and vulcanization. In step S6, the pre-pressurized outer shell 2 is held under pressure for 4-5 minutes until it reaches a fully round state.

[0030] Example 2 Further explanation in conjunction with Example 1, such as Figure 1-10 The structure shown is a low-stiffness, high-durability rubber bushing. The bushing includes an inner cylinder 1, which is a metal tube, preferably made of 20# steel pipe. The inner cylinder 1 has an inner hole 101 that runs through it along its axis, and the inner hole 101 is used to pass through shaft-like parts.

[0031] The inner hole 101 has multiple keyways 102 on its wall. The multiple keyways 102 can be evenly or non-uniformly distributed along the circumference and are used to mate with the key on the shaft to achieve circumferential positioning and torque transmission.

[0032] The inner cylinder 1 has multiple outer shells 2 on its outer side. In this embodiment, the outer shell 2 adopts a two-piece structure, namely, half-piece one 201 and half-piece two 202. Half-piece one 201 and half-piece two 202 are both semi-circular. Half-piece one 201 includes an arc-shaped side 206 and a flat side 207. Half-piece one 201 and half-piece two 202 have the same structure and are symmetrically arranged on both sides of the inner cylinder 1.

[0033] An opening groove 5 is provided between half-piece 201 and half-piece 202, and the opening groove 5 is arranged between the planar sides 207 of half-piece 201 and half-piece 202. The opening groove 5 prevents the two halves of the shell from directly contacting each other in the initial state, thereby providing space for rubber deformation and shell swing.

[0034] Preferably, the opening groove 5 has a width of 4mm in its natural state, allowing half piece one 201 and half piece two 202 to swing between 0-10 degrees; when the swing angle is greater than 10 degrees, the planar sides 207 of half piece one 201 and half piece two 202 abut against each other, forming a mechanical limit to prevent excessive deformation of the rubber.

[0035] The outer side of the half-piece 201 is also provided with shell stiffeners 203, and shell grooves 204 are formed between the shell stiffeners 203. The shell grooves 204 can reduce weight and increase heat dissipation area. One side of the half-piece 201 is also provided with a shell protrusion 205, which can be used for positioning with the mold or for mating with adjacent parts.

[0036] The outer casing 2 is preferably made of cast aluminum material, such as aluminum alloy, to reduce weight and facilitate molding.

[0037] An injection-molded body 3 is provided between the outer shell 2 and the inner cylinder 1. The injection-molded body 3 is a rubber elastomer formed by injection vulcanization of natural rubber, including an inner rubber layer and / or an outer rubber layer.

[0038] The injection molded body 3 has multiple inserts 4 inside, preferably aluminum alloy inserts, such as Al6061, and they are arranged symmetrically in the upper and lower parts. One side of the insert 4 has an arc-shaped surface 401 facing the inner cylinder 1. The arc-shaped surface 401 has a through hole 402. During the vulcanization process, the injection molded body 3 penetrates the through hole 402, thereby firmly covering and mechanically locking the insert 4.

[0039] One side of the injection-molded body 3 has a first boss 304, and the other side has a second boss 305. The first boss 304 and the second boss 305 are respectively located at both ends of the outer shell 2 for axial limiting, assembly positioning, or providing additional elastic deformation area. The injection-molded body 3 also has an inner cylinder 306 inside, and a side plate 307 is provided on the outer side of the inner cylinder 306. A connecting body 301 is provided between the side plate 307 and the inner cylinder 306. The connecting body 301 has a certain degree of elasticity.

[0040] The insert 4 is encased in the connector 301, the inner cylinder 306 is connected to the inner cylinder 1, and the side plate 307 is connected to the outer shell 2. Thus, the inner cylinder 1, the injection-molded body 3, the insert 4, and the outer shell 2 form a multi-layered composite structure. In this embodiment, the bushing is an integral five-layer vulcanized structure consisting of a metal inner cylinder, an inner rubber layer, symmetrical upper and lower aluminum alloy inserts, an outer rubber layer, and a two-half cast aluminum outer cylinder.

[0041] Because the outer shell 2 is divided into half-piece 201 and half-piece 202, with an opening groove 5 between them, the bushing has low stiffness in the circumferential or torsional direction; while the insert 4 provides reinforcing support in the vertical direction, giving it higher stiffness in that direction. Therefore, the bushing has different stiffness parameters in different directions, which can balance low stiffness vibration reduction and high durability load-bearing capacity.

[0042] Example 3 To further illustrate with Example 2, a method for preparing the aforementioned low-stiffness, high-durability rubber bushing is provided. This method features specific process optimizations for double-layer rubber, embedded inserts, and disconnectable outer cylinders, comprising a total of six steps.

[0043] The first step is process 1, which involves pretreatment of metal parts by type. For the inner metal cylinder 1, such as a 20# steel pipe, ultrasonic alkaline washing and degreasing, shot blasting with φ0.8mm alloy steel shot to remove rust, and phosphating are performed sequentially to form a phosphating adsorption film on the surface of the steel part, thereby improving its adhesion to rubber.

[0044] For the aluminum alloy insert 4, such as Al6061, and the two halves of the cast aluminum outer cylinder 2, ultrasonic degreasing, 80-mesh alumina sandblasting roughening, and chromate passivation are performed sequentially. After sandblasting roughening, the surface roughness Ra is controlled at 25~35μm to increase the mechanical interlocking area; Chromate passivation improves the chemical stability of aluminum surfaces and prevents electrochemical corrosion and debonding. This process differentiates surface treatments for steel and aluminum substrates, using appropriate abrasives to increase surface roughness for different materials and employing different chemical surface treatments to enhance the adhesion stability of the material surfaces.

[0045] The next step is process 2, which involves precise layering of a two-component specialized adhesive. In the primer stage, a universal rubber-metal primer is sprayed onto all metal parts, with a dry film thickness controlled at 5-15 μm. This is then dried at 80℃ for 3-5 minutes to ensure the adhesive surface is completely dry. In the topcoat stage, elastic adhesive is sprayed twice onto the upper and lower surfaces of the insert 4, the outer circumference of the inner cylinder 1, and the inner circumference of the two halves of the outer shell 2.

[0046] This two-layer composite system of primer and topcoat is suitable for bonding natural rubber NR to dissimilar metals such as aluminum alloy and carbon steel, which can improve the bonding strength and improve the resistance to environmental aging.

[0047] Next, process 3 is carried out, namely the molding of metal inserts and the hot vulcanization of rubber and metal. The mold adopts a layered positioning pre-installed vulcanization mold with built-in positioning grooves.

[0048] The lower mold is pre-installed with a metal inner cylinder 1, which is covered by an inner rubber layer. Two symmetrical aluminum alloy inserts 4 are embedded in the upper and lower slots and precisely positioned. The outer rubber blank wraps around the outside of the inserts 4. The two halves of the cast aluminum outer cylinder 2 are placed in the left and right cavities of the mold, with a 4mm gap reserved for separation. During vulcanization, the injection pressure and injection speed are used to perform vulcanization in four stages: injection, plasticizing, holding pressure, and vulcanization.

[0049] As an example, the injection section temperature can be 90±5℃, the pressure can be 100~120±10kg / cm², and the time can be 10~20s; the plasticizing section temperature can be 80±5℃, the pressure can be 80~100kg / cm², and the time can be 20~40s, so that the rubber material flows slowly to fill the cavity and prevents air bubbles in the hollow section. The temperature of the pressure holding section can be 150±5℃, the pressure can be 180±10kg / cm², and the time can be 2~3min; the temperature of the vulcanization section can be 150±5℃, the pressure can be 180±10kg / cm², and the vulcanization time can be 10min, so that the rubber is completely cross-linked and the metal and rubber interfaces undergo chemical reaction and bonding.

[0050] It should be noted that the above parameters for the injection section and the holding pressure section are exemplary parameters for natural rubber injection vulcanization, and those skilled in the art can adjust them appropriately according to the rubber compound formulation, product size and mold structure.

[0051] This vulcanization process can simultaneously position the inner cylinder 1, two insert plates 4, and the two split outer cylinders 2, enabling multi-layer structure production in a single mold closing operation, improving production efficiency and ensuring product dimensional stability. An annular ventilation overflow groove is provided on the mold parting surface to match the finished product's flanged heat dissipation groove. After vulcanization, the mold is cooled, demolded, and opened, allowing the bushing semi-finished product to be removed as a single piece, with the two outer cylinders 2 maintaining a natural 4mm gap.

[0052] Then, proceed to step 4, which involves secondary trimming of the flanged rubber grooves. Use scissors or pliers to clean the burrs around the ventilation and heat dissipation grooves of the flanged rubber, ensuring that the groove width is uniform and unobstructed, to ensure sufficient heat dissipation during subsequent use. Next, proceed to step 5, which involves pre-compression assembly simulation.

[0053] Specialized tooling is used to pre-compress the disassembled outer cylinder 2 to a fully spherical state and hold the pressure for 5 minutes to counteract residual vulcanization stress, ensuring product dimensional stability and improving the overall vehicle durability. Finally, process 6, non-destructive testing of the bonding, is performed. Ultrasonic scanning is used to inspect the interface between the insert 4, the inner and outer rubber, and the metal skeleton. After confirming the absence of delamination and bubble defects, the product proceeds to finished product testing.

[0054] The core difference of this process lies in the simultaneous vulcanization of double-layer rubber, embedded aluminum alloy inserts, and split cast aluminum outer cylinder, forming multiple composite interfaces in one step; it is compatible with natural commercial vehicle rubber and also compatible with both carbon steel and aluminum alloy. The segmented temperature-controlled injection vulcanization process ensures stable and controllable process parameters, preventing over-vulcanization cracking of the hollow thin-walled rubber. Post-treatment increases pre-compression to release vulcanization stress, significantly improving the rubber's durability.

[0055] Example 4 To further illustrate with Example 3, destructive tests were conducted on the aforementioned bushing to verify the adhesion, stiffness, and fatigue properties of the insert to the rubber. First, an axial pull-out bond destructive test was performed to verify the bond strength between the insert 4 and the rubber. The test standard referenced ASTM D429 Method A and the national standard GB / T11211-2009. A universal testing machine was used to apply a uniform tensile test at 25 mm / min until the rubber tore or the interface separated.

[0056] The test results show that the failure fracture surfaces were all tearing of the rubber body, with no delamination at the interface of the aluminum alloy insert 4 and the metal cylinder. The adhesive adhesion rate on the metal surface was 100%, and the bonding strength was ≥4MPa, which is higher than the standard of ≥3.5MPa for traditional integral bushings (see attached figure). Secondly, a large displacement stiffness destructive fatigue test in the X-axis was conducted to verify the nonlinear variable stiffness durability. The test fixture used an MTS biaxial dynamic test bench, with reciprocating loading of ±8mm in the X-axis, a frequency of 2Hz, and 2 million consecutive cycles.

[0057] The comparison sample was a traditional closed-type hollow bushing, which developed a through-crack in the rubber after 1.6 million cycles; the bushing of the present invention showed no through-tears after 2 million cycles, only slight elastic deformation at the hollowed-out rounded corners, and the insert 4 effectively dispersed the stress, as shown in the attached figure. Third, a ±10° axial torsional destructive test was conducted to verify the low torsional stiffness structure.

[0058] The rubber was continuously twisted to an extreme angle of 15°, with the rounded corners of the hollowed-out section contacting the limit, and no tearing occurred. The control sample without inserts showed root cracking at 11°, as shown in the bushing torsion cross-section diagram. Fourth, a high and low temperature alternating durability destructive test was conducted to verify the durability improvement effect of the heat sink.

[0059] After cycling and continuous vibration at -40℃ to 120℃ for 1000 hours, the following results were observed: the flanged ventilation grooves provided sufficient heat dissipation, and the rubber did not undergo thermal aging or powdering; the traditional bushings without heat dissipation grooves showed surface hardening and cracking.

[0060] The above tests demonstrate that the bushing of the present invention exhibits excellent performance in terms of adhesive strength, nonlinear variable stiffness, torsional low stiffness, fatigue durability, and high and low temperature durability.

[0061] The above embodiments are merely preferred technical solutions of the present invention and should not be considered as limitations on the present invention. The scope of protection of the present invention should be limited to the technical solutions described in the claims, including equivalent substitutions of the technical features described in the claims. That is, equivalent substitutions and improvements within this scope are also within the scope of protection of the present invention.

Claims

1. A low-stiffness, high-durability rubber bushing, characterized in that: It includes an inner cylinder (1), a plurality of outer shells (2) are provided on the outside of the inner cylinder (1), an injection molded body (3) is provided between the outer shell (2) and the inner cylinder (1), and a plurality of inserts (4) are provided inside the injection molded body (3). An opening groove (5) is provided between the outer shell (2).

2. The low-stiffness, high-durability rubber bushing according to claim 1, characterized in that: The inner cylinder (1) is also provided with a through inner hole (101), and multiple keyways (102) are provided in the inner hole (101).

3. The low-stiffness, high-durability rubber bushing according to claim 1, characterized in that: The outer shell (2) includes half piece one (201) and half piece two (202), half piece one (201) and half piece two (202) are semi-circular, half piece one (201) includes an arc side (206) and a flat side (207), and half piece one (201) and half piece two (202) have the same structure.

4. The low-stiffness, high-durability rubber bushing according to claim 3, characterized in that: Half piece one (201) and half piece two (202) are symmetrically arranged on both sides of the inner cylinder (1), and the opening slot (5) is arranged between the planar side (207) of half piece one (201) and half piece two (202); The outer side of half piece 1 (201) is also provided with shell stiffeners (203), and shell grooves (204) are formed between the shell stiffeners (203). One side of half piece 1 (201) is also provided with shell protrusions (205).

5. The low-stiffness, high-durability rubber bushing according to claim 1, characterized in that: Half piece one (201) and half piece two (202) can swing between 0-10 degrees. When the swing angle is greater than 10 degrees, half piece one (201) and half piece two (202) abut against each other on the plane side.

6. The low-stiffness, high-durability rubber bushing according to claim 1, characterized in that: One side of the injection body (3) is provided with a boss (304) and the other side is provided with a boss (305). The injection body (3) covers the outside of the insert (4). Boss 1 (304) and Boss 2 (305) are respectively located at both ends of the outer shell (2).

7. The low-stiffness, high-durability rubber bushing according to claim 6, characterized in that: The injection body (3) is further provided with an inner cylinder (306) inside, and a side plate (307) is provided on the outside of the inner cylinder (306). A connecting body (301) is provided between the side plate (307) and the inner cylinder (306). The connecting body (301) has a certain elasticity. The insert (4) is encased in the connector (301), the inner cylinder (306) is connected to the inner cylinder (1), the side plate (307) is connected to the outer shell (2), and the injection molded body (3) is also provided with multiple heat dissipation grooves (303). The outer side of the inner cylinder (306) is also provided with multiple reinforcing bodies (302).

8. The low-stiffness, high-durability rubber bushing according to claim 1, characterized in that: The insert (4) has an arc-shaped surface (401) on one side, and a through hole (402) is provided on the arc-shaped surface (401), through which the injection body (3) penetrates the through hole (402). The curved surface (401) faces the inner cylinder (1).

9. A method for manufacturing a low-stiffness, high-durability rubber bushing according to any one of claims 1-8, characterized in that: The method includes: S1: The steel inner cylinder (1) is successively degreased by alkaline washing, shot blasted to remove rust and phosphated, and the aluminum alloy insert (4) and the split outer shell (2) are successively degreased, roughened by sandblasting and passivated. S2: Spray primer on the surface of metal parts and dry it, then spray elastic adhesive on the outer circle of insert (4), inner cylinder (1) and outer circle of outer shell (2) to form a composite adhesive layer; S3: The mold is pre-assembled with inner cylinder (1) and insert (4) in layers, and the split outer shell (2) is placed in the two side cavities and reserved with a disconnected opening slot (5) so that the multi-layer structure can be closed and positioned synchronously. S4: Segmented temperature-controlled injection vulcanization is adopted. First, low-temperature plasticization and filling are carried out, and then high temperature and high pressure are used to cross-link and bond the rubber, avoiding over-vulcanization cracking of hollow thin-walled rubber. S5: After vulcanization, cool and demold, take out the semi-finished product, and keep the split shell (2) to naturally form the opening groove (5) to release some of the vulcanization stress; S6: Trim and clean the burrs of the flanged rubber ventilation and heat dissipation groove (303), pre-press the outer shell (2) to a round state and maintain pressure to offset residual stress of vulcanization and improve durability; S7: Use ultrasonic scanning to inspect the interface between the insert (4), the injection body (3) and the metal. After confirming that there are no layered bubbles, proceed to the finished product inspection.

10. A low-stiffness, high-durability rubber bushing according to claim 9, characterized in that: step In S1, the surface roughness of the insert (4) is Ra25~35μm; In step S2, all metal parts are sprayed with a rubber-metal general primer with a dry film thickness of 5-15μm, and dried at 80℃ for 3-5 minutes to keep the adhesive surface completely dry. Insert (4) upper and lower double sides, inner cylinder (1) outer circle, two halves of outer shell (2) secondary spraying of elastic adhesive; In step S3, the opening groove (5) has a break gap of 3-4 mm; In step S4, the injection pressure and injection speed are divided into four stages: injection, plasticizing, holding pressure, and vulcanization. In step S6, the pre-pressurized outer shell (2) is held under pressure for 4-5 minutes until it reaches a fully round state.