Tile ceramic armor with deflection mechanism

By introducing asymmetric geometry and deflection interfaces into ceramic composite armor, continuous deflection of the projectile is achieved, solving the problem of insufficient resistance of traditional ceramic composite armor against multiple attacks and high-energy armor-piercing projectiles, and improving protection performance and energy dissipation efficiency.

CN123134818APending Publication Date: 2026-11-20NINGBO UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611191470.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional ceramic composite armor is insufficient in resisting multiple hits and controlling interface failure when facing new high-energy armor-piercing projectiles and high-speed fragments. The unchanged attitude of the projectile during penetration leads to premature failure of the overall structure and low energy absorption efficiency.

Method used

The modular ceramic armor with an asymmetric geometry induces the projectile to deflect twice in succession by setting first and second deflection interfaces on the ceramic protective unit, thereby reconstructing the penetration trajectory and causing attitude instability, increasing the contact area between the projectile and the ceramic and the energy dissipation.

Benefits of technology

It significantly improves the ability to withstand multiple hits and the protective performance, extends the penetration path of the projectile, enhances the energy dissipation efficiency, reduces the penetration capability of the projectile, and improves the stability and impact resistance of the overall structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123134818A_ABST
    Figure CN123134818A_ABST
Patent Text Reader

Abstract

The application provides a tile ceramic armor with a deflection mechanism, which comprises a back plate and a ceramic protection layer fixed on the upper surface of the back plate, the ceramic protection layer comprises a plurality of ceramic protection units arranged in sequence in a first direction, and two adjacent ceramic protection units are mutually adhered and fixed; the ceramic protection unit comprises a plurality of ceramic blocks arranged in sequence in a second direction, the second direction is perpendicular to the first direction, and two adjacent ceramic blocks are mutually adhered and fixed; the ceramic block is provided with a deflection structure, the deflection structure comprises a first deflection interface and a second deflection interface, a projectile can sequentially contact the first deflection interface and the second deflection interface in the penetration process, and the projectile is induced to continuously deflect twice, thereby realizing penetration trajectory reconstruction and attitude instability; meanwhile, stress wave reflection and crack blocking effects are generated at the plurality of joint interfaces, the volume of the ceramic material participating in energy absorption by crushing is increased, and the synergistic energy absorption effect of the back plate is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of armor protection, and in particular to a modular ceramic armor with a deflection mechanism. Background Technology

[0002] The modern armor protection field is facing severe challenges from new high-energy armor-piercing projectiles, high-speed fragmentation, and multi-functional warheads. Traditional homogeneous armor, due to its excessive surface density, can no longer meet the dual requirements of modern armored vehicles for lightweight design and high mobility. Against this backdrop, ceramic composite armor, with its high hardness, high melting point, and low density properties, has become the most widely used protective structure. Under high-speed impact loads, ceramic materials can induce severe passivation, deformation, and even fragmentation in high-hardness projectiles, significantly reducing their penetration capability. However, traditional ceramic composite armor, limited by the inherent defects of ceramic materials such as high brittleness and low fracture toughness, still suffers from significant deficiencies in its resistance to multiple strikes and interface failure control. For example, the widely used composite ballistic plates embedded with hexagonal ceramic pieces, while able to resist projectile penetration to a certain extent and exhibiting localized damage, do not change the projectile's trajectory during penetration due to the geometric symmetry of the hexagonal splicing structure. When the projectile penetrates the symmetrical ceramic structure, symmetrical damage occurs. After penetrating the ceramic layer, the projectile often retains a certain sharp angle. This residual sharp angle will drastically aggravate the local damage of the backplate during subsequent penetration, causing the overall structure to fail prematurely, significantly reducing the energy absorption efficiency, and ultimately causing the projectile to completely penetrate the entire protective structure.

[0003] Chinese invention patent CN105865267A discloses a composite bulletproof plate embedded with irregularly shaped ceramic pieces. These ceramic pieces have a hexagonal structure, and the ceramic plates are seamlessly joined by edge protrusions and grooves in a metal plate. However, existing research indicates that while the hexagonal ceramic pieces can resist high-speed impacts and exhibit localized damage, the projectile's attitude remains unchanged. Due to the random nature of the impact, the projectile may exhibit a sharp angle upon impact with the ceramic plate. This sharp angle exacerbates the damage to the backplate during penetration, leading to premature structural failure, reduced energy absorption efficiency, and ultimately, the projectile penetrating the entire ceramic protective structure. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a modular ceramic armor with a deflection mechanism that employs an asymmetric geometric structure and triggers two distinct deflection mechanisms in a continuous time sequence of projectile penetration, thereby improving deflection protection performance and resistance to multiple attacks.

[0005] This invention provides a modular ceramic armor with a deflection mechanism, comprising a backplate 1 and a ceramic protective layer fixed to the upper surface of the backplate 1. The ceramic protective layer includes a plurality of ceramic protective units 20 arranged sequentially in a first direction, with adjacent ceramic protective units 20 bonded and fixed to each other. Each ceramic protective unit 20 includes a plurality of ceramic blocks 2 arranged sequentially in a second direction, the second direction being perpendicular to the first direction, with adjacent ceramic blocks 2 bonded and fixed to each other. The ceramic blocks 2 are provided with a deflection structure, which includes a first deflection interface and a second deflection interface. During penetration, the projectile can sequentially contact the first deflection interface and the second deflection interface, inducing the projectile to deflect twice consecutively, thereby achieving penetration trajectory reconstruction and attitude instability.

[0006] Furthermore, the first deflection interface and the second deflection interface have the same deflection direction but different deflection angles.

[0007] Furthermore, the first deflection interface and the second deflection interface are arranged symmetrically or asymmetrically with respect to the central axis of the ceramic block 2.

[0008] Furthermore, the top surface of the ceramic block 2 has a first inclined surface and serves as the first deflection interface, and at least one side wall of the ceramic block 2 has a second inclined surface and serves as the second deflection interface.

[0009] Furthermore, the ceramic block 2 has a first mounting surface 201 that can be attached and fixed to the back plate 1. The front end of the first mounting surface 210 is provided with a second mounting surface 202 that can be attached and fixed to the front ceramic block 2. The rear end of the first mounting surface 201 is provided with a third mounting surface 205 that can be attached and fixed to the rear ceramic block 2. The second mounting surface 202 and the third mounting surface 205 are both inclined surfaces and parallel to each other. The second mounting surface 202 and the third mounting surface 205 are connected by a first connecting surface 203 and a second connecting surface 204 in sequence. The first connecting surface 203 is an inclined surface and has a different inclination angle from the second mounting surface 202.

[0010] Furthermore, the second connecting surface 204 is a plane parallel to the first mounting surface 201 or an inclined surface with a different inclination direction than the first connecting surface 203.

[0011] Furthermore, the ceramic block 2 is formed by cutting off the obtuse angle along the line connecting the midpoints of the two adjacent obtuse-angled sides at the top of the rhombus or parallelogram.

[0012] Furthermore, the ceramic block 2 is formed by cutting off the obtuse angle along the line connecting the midpoints of the two adjacent obtuse angle sides at the top of the rhombus or parallelogram, and cutting off the acute angle along the line connecting the midpoints of the two adjacent acute angle sides at the top.

[0013] Furthermore, the acute angle of the rhombus or parallelogram is 30°-60°.

[0014] Furthermore, the ceramic protective layer is fixedly connected to the back plate by a first adhesive layer 101, and two adjacent ceramic blocks 2 are fixedly connected by a second adhesive layer 102, and the thickness of the first adhesive layer 101 is greater than the thickness of the second adhesive layer 102.

[0015] The modular ceramic armor of this invention with a deflection mechanism has the following advantages: 1. A deflection penetration mechanism is proposed to achieve two consecutive deflections of the projectile, thereby increasing the degree of attitude instability. By generating an asymmetric stress field on the inclined contact surface during the impact of the projectile, the projectile is forced to undergo lateral displacement and deflection, increasing the contact area between the projectile and the ceramic. More kinetic energy is consumed by multi-angle fragmentation. Compared with the traditional hexagonal structure, the rhomboid truncated configuration can more effectively change the trajectory of the projectile and prevent the projectile from penetrating with a sharp angle. 2. Significantly increases the actual penetration path length of the projectile, increases the volume of ceramic material participating in fragmentation and energy absorption, and forms a stepped energy dissipation mechanism. The front ceramic layer causes the projectile to break up and lose mass, the rear layer uses the deflection effect to further decelerate, and finally the back plate absorbs the residual kinetic energy, realizing the gradual decay of energy. 3. The irregular splicing structure forms a multi-interface crack blocking network, which improves the ability to resist multiple hits, increases the contact area between the projectile and the back plate, reduces local stress concentration, and local damage only affects a single ceramic block rather than the whole, which significantly improves the ability to resist multiple hits. In addition, the staggered bonding design of the front and rear units enhances the stability of the overall structure. 4. By designing the cross-sectional angle, the deflection of the projectile can be controlled, which promotes the tumbling, fragmentation and mass loss of the projectile and improves the energy dissipation efficiency. Its active defense mechanism is superior to the passive resistance of traditional homogeneous armor, causing the projectile to continuously lose its attitude during the penetration process and reducing the penetration efficiency. 5. The modular splicing design is compatible with existing ceramic molding and bonding processes. The standardized production of diamond-shaped blocks facilitates quality control. The edge bonding parts are fixed into a whole by adhesive, taking into account both structural strength and manufacturability. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the structure of the modular ceramic armor with deflection mechanism of the present invention; Figure 2 This is a side view of the modular ceramic armor with a deflection mechanism of the present invention; Figure 3 for Figure 2 Enlarged view of section A in the middle; Figure 4 This is a cross-sectional view of the ceramic blocks of the modular ceramic armor with a deflection mechanism of the present invention. Figure 5 This is a schematic diagram of the structure of the modular ceramic armor with deflection mechanism of the present invention; Figure 6 This is a schematic diagram of the modular ceramic armor with a deflection mechanism of the present invention from another angle. Figure 7 This is a schematic diagram of the penetration deflection path of the modular ceramic armor with a deflection mechanism of the present invention. Figure 8 This is a schematic diagram of the structure of a second embodiment of the modular ceramic armor with a deflection mechanism of the present invention; Figure 9 This is a side view of a second embodiment of the modular ceramic armor with a deflection mechanism of the present invention; Figure 10 for Figure 9 Enlarged view of section B in the middle; Figure 11 This is a cross-sectional view of a ceramic block in Embodiment 2 of the modular ceramic armor with a deflection mechanism of the present invention. Figure 12 This is a schematic diagram of the structure of a second embodiment of the modular ceramic armor with a deflection mechanism of the present invention; Figure 13 This is a schematic diagram of another angle of the second embodiment of the modular ceramic armor with deflection mechanism of the present invention; Figure 14 This is a schematic diagram of the penetration deflection path of a second embodiment of the modular ceramic armor with a deflection mechanism of the present invention; Figure 15 This is a schematic diagram of the penetration simulation targeting the traditional hexagonal structure; Figure 16 This is a schematic diagram of penetration simulation according to Embodiment 1 of the present invention; Figure 17 This is a schematic diagram of the penetration simulation of Embodiment 2 of the present invention; Figure 18 The numerical simulation diagram shows the impact process. Figure 19 This is a comparison chart of the impact velocity and backplate displacement results. Detailed Implementation

[0017] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.

[0018] See Figure 1-14This invention provides a modular ceramic armor with a deflection mechanism, comprising a back plate 1 and a ceramic protective layer fixed to the upper surface of the back plate 1. The ceramic protective layer includes a plurality of ceramic protective units 20 arranged sequentially in a first direction, with adjacent ceramic protective units 20 being bonded and fixed to each other. Each ceramic protective unit 20 includes a plurality of ceramic blocks 2 arranged sequentially in a second direction, which is perpendicular to the first direction. The first direction can be defined as the X-axis direction or the front-back direction, and the second direction can be defined as the Y-axis direction (left-right direction). Adjacent ceramic blocks 2 are bonded and fixed to each other by an adhesive.

[0019] In this application, a deflection structure is provided on the ceramic block 2. The deflection structure includes a first deflection interface and a second deflection interface. During the penetration process, the projectile can sequentially contact the first deflection interface and the second deflection interface, and induce the projectile to deflect twice in succession, thereby realizing the reconstruction of the penetration trajectory and attitude instability.

[0020] This application uses structural design to cause the projectile to be subjected to uneven forces during penetration, inducing it to deflect and yaw. This is an effective way to improve the efficiency of armor protection. By constructing an irregular ceramic structure, the projectile will generate a significant deflection angle during penetration, thus attenuating the projectile's kinetic energy.

[0021] By setting a first deflection interface and a second deflection interface on a single ceramic block, a two-step reconstruction of the projectile's penetration trajectory is achieved. When the projectile contacts the two deflection interfaces in sequence, it will be subjected to two asymmetric forces, generating a continuous deflection torque. The projectile's angle of impact itself can induce the projectile to deflect due to asymmetric resistance. This application actively creates this path under penetration conditions through its structure. The two deflections fundamentally change the projectile's motion direction and attitude. When the projectile's attitude and trajectory change significantly, its penetration path will be lengthened, energy loss will be aggravated, and its penetration capability will be greatly weakened, thus improving its protective performance.

[0022] During use, when the penetrator impacts the ceramic protective layer perpendicularly, it first contacts the first inclined interface. Due to the interface's inclination angle, the penetration load is decomposed into normal and tangential components. Under the action of an asymmetric compressive stress field, the projectile undergoes its first deflection. As the penetration depth increases, the projectile continues to contact the second inclined interface, which generates a new asymmetric stress field, causing the projectile to deflect again on top of the first deflection, resulting in a second attitude change. Because the two deflection processes occur consecutively, the projectile's penetration trajectory changes from a straight line to a broken line, causing the projectile to continuously overturn, tumble, and break apart. Simultaneously, the epoxy resin layer at the interface dissipates impact energy and causes stress waves to be reflected and transmitted at the interface, thereby weakening the crack propagation capability. The spliced ​​network formed by multiple irregularly shaped ceramic blocks further hinders crack propagation, achieving local damage limitation and protection against multiple impacts.

[0023] In this application, the first deflection interface and the second deflection interface have the same deflection direction but different deflection angles. The two deflection interfaces have the same direction, and the projectile is subjected to the same deflection torque when passing through them in sequence. The cumulative effect of the two deflection angles makes the final deflection amplitude much greater than that of a single deflection interface, effectively disrupting the stable penetration attitude of the projectile. The first deflection interface achieves a smooth initial deflection, preventing the projectile from breaking uncontrollably due to excessive deflection. The second deflection interface further expands the deflection amplitude, forming a double deflection and increasing the deflection angle. Furthermore, the multiple asymmetric forces extend the deflection path of the projectile, increase the interaction time and contact area with the ceramic layer, significantly improve the energy dissipation efficiency, thereby weakening the penetration capability of the projectile and improving the protective performance.

[0024] In this embodiment, the first deflection interface and the second deflection interface are symmetrically or asymmetrically arranged with respect to the central axis of the ceramic block 2. Preferably, an asymmetrical structure is adopted.

[0025] The top surface of the ceramic block 2 in this application has a first inclined surface, which serves as a first deflection interface, and at least one side wall of the ceramic block 2 has a second inclined surface, which serves as a second deflection interface.

[0026] In this embodiment, the ceramic block 2 has a first mounting surface 201 that can be attached and fixed to the back plate 1. A second mounting surface 202 is provided at the front end of the first mounting surface 201, which can be attached and fixed to the front end of the ceramic block 2. A third mounting surface 205 is provided at the rear end of the first mounting surface 201, which can be attached and fixed to the rear end of the ceramic block 2. Both the second mounting surface 202 and the third mounting surface 205 are inclined surfaces and parallel to each other. A first connecting surface 203 and a second connecting surface 204 are sequentially connected between the second mounting surface 202 and the third mounting surface 205. Specifically, the second mounting surface 202 is connected to the first connecting surface 203. The first connecting surface 203 is connected to the second connecting surface 204, and the second connecting surface 204 is connected to the third mounting surface 205. The first connecting surface 203 is an inclined surface, which has the same tilt (deflection) direction as the second mounting surface 202, but with a different tilt (deflection) angle. The first mounting surface 201 is attached and fixed to the back plate 1 to ensure that the ceramic block is stably mounted on the back plate. The second mounting surface 202 and the third mounting surface 205 are inclined surfaces and parallel to each other, so that adjacent ceramic blocks can be attached to each other through the inclined surfaces to achieve a tight and seamless splicing, effectively transferring and dispersing the impact load. The inclined surfaces of the above mounting surface and the first connecting surface can cause the projectile to deflect.

[0027] In this embodiment, the second connecting surface 204 is a plane parallel to the first mounting surface 201 (see [reference]). Figure 4 ( ), or an inclined plane. When it is an inclined plane, the inclination direction of the inclined plane is different from that of the first connecting surface 203. See [reference] Figure 11 .

[0028] In this embodiment, the ceramic block 2 can adopt different irregular ceramic structures; Example 1, see Figures 1-6 The ceramic block 2 is formed by cutting off the obtuse angle along the line connecting the midpoints of the two adjacent obtuse angle sides at the top of the rhombus or parallelogram. That is, the obtuse angle is cut off by the line connecting the midpoints of the two obtuse angle sides at the top of the rhombus or parallelogram (not a rectangle) to form the irregular structure of the ceramic block in Embodiment 1. The above cutting is used to describe the shape of the ceramic block 2, rather than physical cutting and processing.

[0029] See Figure 4 The cross-section is rhomboid, with sides ab, bc, cd, and da. The plane containing side ab serves as the first mounting surface 201, the plane containing side ad serves as the second mounting surface 202, and the plane containing side bc serves as the third mounting surface 205. ∠adc is an obtuse angle, and ∠bcd is an acute angle. The obtuse angle adc is cut off along the line connecting the midpoint of side ad and the midpoint of side cd, thus creating the first connecting surface 203, which is an inclined surface. The cross-section of the ceramic block is rhomboid or parallelogram, which has an asymmetrical edge angle layout. Based on this, the obtuse angle is cut off along the line connecting the midpoints of the two sides of the top obtuse angle, so that the top of the ceramic block forms a first connecting surface 203 with a specific inclined surface. This changes the symmetrical force-bearing mode of the traditional hexagonal or rectangular ceramic block. When the projectile penetrates, the asymmetrical inclined surface structure causes the projectile to be subjected to uneven lateral force, actively inducing its deflection.

[0030] Example 2, see Figures 8-13 In this embodiment, the ceramic block 2 is formed by cutting off the obtuse angle along the line connecting the midpoints of the two adjacent obtuse angle sides at the top of the rhombus or parallelogram, and cutting off the acute angle along the line connecting the midpoints of the two adjacent acute angle sides at the top. That is, the obtuse angle is cut off by connecting the midpoints of the two sides of the obtuse angle at the top of the rhombus or parallelogram (not a rectangle), and at the same time, the obtuse angle is cut off by connecting the midpoints of the two sides of the acute angle at the top of the top, forming the irregular structure of the ceramic block in Embodiment 2. The above cutting is used to describe the shape composition of the ceramic block 2, rather than physical cutting and processing.

[0031] See Figure 11The cross-section is rhomboid, with sides ab, bc, cd, and da. The plane containing side ab serves as the first mounting surface 201, the plane containing side ad serves as the second mounting surface 202, and the plane containing side bc serves as the third mounting surface 205. ∠adc is an obtuse angle, and ∠bcd is an acute angle. The obtuse angle adc is cut off along the line connecting the midpoint of side ad and the midpoint of side cd, thus creating the first connecting surface 203. Simultaneously, the acute angle bcd is cut off along the line connecting the midpoint of side dc and the midpoint of side bc, thus forming the second connecting surface 204. Both the first connecting surface 203 and the second connecting surface 204 are inclined planes with opposite inclination directions, forming a apex structure between the first and second connecting surfaces. When the projectile penetrates, the asymmetrical inclined plane structure subjectes the projectile to uneven lateral forces, actively inducing its deflection.

[0032] In this embodiment, the acute angle α of the rhombus or parallelogram is 30°~60°. This angle range can effectively induce the projectile to deflect in a controllable manner, increase the contact area, and improve the kinetic energy dissipation efficiency. Furthermore, the acute angle of the rhombus or parallelogram is 30°~50°, preferably 45°, which achieves the best balance between deflection effect and structural stability, avoiding fragility due to too small an angle or insufficient deflection of the projectile due to too large an angle.

[0033] A first adhesive layer 101 is used to fix the ceramic protective layer and the back plate together, and a second adhesive layer 102 is used to fix two adjacent ceramic blocks 2 together. This ensures a high-strength bond between the ceramic protective layer and the back plate, prevents delamination failure during impact, and stabilizes the interface bonding. In this embodiment, the thickness of the first adhesive layer 101 is greater than the thickness of the second adhesive layer 102. In this embodiment, the thickness of the first adhesive layer 101 is 0.5mm-1.0mm, preferably 0.6mm. This allows for a stable fixed connection between the two layers and can also absorb some of the impact energy, reducing the instantaneous stress of the ceramic protective layer.

[0034] In this embodiment, the ceramic protective layer includes multiple ceramic protective units 20. The second adhesive layer includes a second adhesive layer I disposed between two adjacent ceramic protective units and a second adhesive layer II disposed between two adjacent ceramic blocks 2 within the same ceramic protective unit. The ceramic blocks are arranged in a matrix structure. Two adjacent ceramic blocks 2 at the front and back are bonded and fixedly connected by the second adhesive layer I, and two adjacent ceramic blocks 2 on the left and right are bonded and fixedly connected by the second adhesive layer II, ensuring that each ceramic block 2 is tightly fixed and connected, thereby improving the overall impact resistance. In this embodiment, the thickness of the second adhesive layer I and the second adhesive layer II is 0.2mm-0.5mm, preferably 0.3mm, which balances the bonding strength and the compactness of the structure.

[0035] In this embodiment, the adhesive layer (agent) is aerospace-grade epoxy resin. This type of adhesive has relatively high bonding strength and good mechanical properties. When applied to the bonding between ceramics and ceramics, or between ceramics and metals, it can improve the overall elastic resistance to a certain extent. In order to ensure the stability of the overall bonding, the adhesive is filled and compacted in all the gaps in the overall structure.

[0036] In this embodiment, the back plate 1 is made of materials such as metal, PE, and aramid; the ceramic block is made of high-hardness ceramics such as boron carbide, alumina, silicon carbide, and silicon nitride; and a composite armor is formed by combining high tensile strength materials such as aluminum alloy, steel, or ultra-high molecular weight polyethylene (UHMWPE) with the ceramic panel to compensate for the shortcomings of poor plasticity and low fracture toughness of ceramics.

[0037] When the penetrator impacts the irregularly shaped ceramic panel vertically, the stress wave is reflected and unloaded at the interface due to the influence of the low-impedance medium interface. This induces the projectile to become unloaded and unstable, causing the penetrator to deviate from its vertical trajectory. The first deflection interface induces the projectile to deflect initially, and the second deflection interface further expands the projectile's yaw angle, achieving two consecutive deflections. This causes the projectile to become continuously unstable and prolongs its actual penetration path. At the same time, because the interfaces of the rhomboid splicing blocks are inclined to the panel, this overlapping splicing method of inclined interfaces generates stress wave reflection and crack blocking effects at multiple splicing interfaces during crack propagation. This increases the volume of ceramic material participating in crushing and energy absorption, and enhances the energy absorption capacity of the back plate.

[0038] To gain a more intuitive understanding of the anti-penetration effect of this application, simulations were performed on existing ceramic armor and the ceramic armor of this application.

[0039] The simulation tool used was ANASY / LS-DYNA finite element simulation software.

[0040] Simulation 1: For existing hexagonal ceramic structures: See Figure 15 The impact simulation of a flat-nosed projectile on a ceramic composite armor constructed from traditional hexagonal blocks was conducted using ANASY / LS-DYNA finite element simulation software. The selected flat-nosed projectile (Type 6) had a diameter of 10.8 mm and a length of 52 mm, and was made of T12A steel. The hexagonal blocks had a side length of 16.65 mm and a height of 12 mm. The backplate was made of 6061 aluminum alloy with dimensions of 200 mm * 200 mm * 5 mm. The composite armor was constructed by bonding the blocks together and bonding the ceramic protective layer to the backplate. For mesh generation, the bullet mesh element size was approximately 1.1 mm, while the ceramic protective layer and backplate mesh element size were 0.8 mm. The mesh was fined in the middle contact area of ​​the aluminum alloy backplate. By adding keywords to set erosion contact, the following results were obtained: Figure 15The diagram shows a simulation of the penetration of a hexagonal ballistic ceramic composite armor.

[0041] Simulation 2: Ceramic block structure according to Embodiment 1 of this application: See Figure 16 The impact simulation of this structure using ANASY / LS-DYNA finite element simulation software was conducted. The selected flat-nosed projectile 6 had a diameter of 10.8 mm and a length of 52 mm, and was made of T12A steel. The ceramic block had an angle of 45°, a side length of 17 mm, and a portion of the ceramic was cut off along the centerline of the long diagonal of the parallelogram. The height was 12 mm and the width was 28 mm, which is the ceramic block structure in Example 1. The backplate was made of 6061 aluminum alloy with dimensions of 200 mm * 200 mm * 5 mm. For mesh generation, the bullet mesh element size was approximately 0.4 mm, while the mesh element size for the ceramic protective layer and the backplate was 0.5 mm. The mesh was also refined in the middle contact area of ​​the aluminum alloy backplate, and erosion contact was set by adding keywords. The simulation yielded the following results: Figure 16 The diagram shows a simulation of the penetration of ceramic composite armor.

[0042] Simulation 2: Ceramic block structure according to Embodiment 2 of this application: See Figure 17 The impact simulation of this structure using ANASY / LS-DYNA finite element simulation software was conducted. The selected flat-nosed projectile 6 had a diameter of 10.8 mm and a length of 52 mm, and was made of T12A steel. The ceramic block had an angle of 45°, a side length of 17 mm, and was partially cut along the line connecting the midpoints of the left and right sides of the parallelogram, with a height of 12 mm and a width of 28 mm, which is the ceramic block structure in Example 2. The back plate was made of 6061 aluminum alloy with dimensions of 200 mm * 200 mm * 5 mm. For mesh generation, the bullet mesh element size was approximately 0.4 mm, and the mesh element size of the ceramic protective layer and the back plate was 0.5 mm. The mesh was also refined in the middle contact area of ​​the aluminum alloy back plate, and the erosion contact was set by adding keywords. The results were as follows: Figure 17 The diagram shows a simulation of the penetration of ceramic composite armor.

[0043] Figures 15-17 The simulation results for the three structures are shown in the comparison diagram. As can be seen from the damage cloud map, the entire process can be divided into the following four stages: Hexagonal structure: 1. At T=50 μs ( Figure 15 a) When the projectile begins to contact the ceramic layer, a strong compression wave is generated at the contact interface and propagates to the inside of the projectile and the back of the ceramic respectively. At this time, the projectile has not yet shown obvious erosion or damage. The compression wave propagates symmetrically in the hexagonal ceramic structure. 2. At T=100 μs ( Figure 15b) The projectile continues to penetrate and propel the ceramic forward, forming a distinct ceramic fragmentation cone. At the same time, the back plate bulges and deforms under stress. 3. At T=200 μs ( Figure 15 c) The projectile body continuously penetrates the ceramic layer, and the projectile exhibits obvious penetration during the penetration process; 4. At T=300 μs ( Figure 15 d) The remaining kinetic energy of the projectile is further absorbed by the backplate, and the penetration process tends to end. Throughout the entire process, the projectile does not deflect. The ceramic block structure of Embodiment 1 and the ceramic block structure of Embodiment 2 of this application: 1. In the initial stage of penetration (T=50 μs), the projectile comes into contact with the ceramic, and a strong compression wave is generated at the contact point and propagates bidirectionally into the ceramic and the projectile. The damage cloud map shows that the stress wave is transmitted asymmetrically, and the projectile is rapidly destroyed at the same time. 2. During the penetration development stage (T=100 μs), the ceramic on one side warps due to asymmetric stress. The angle of the rhomboid truncated structure guides the change in the stress wave path, causing non-uniform damage between the ceramic and the projectile. The first deflection interface induces initial deflection of the projectile, and the second deflection interface further expands the projectile's yaw angle, achieving two consecutive deflections, causing continuous attitude instability of the projectile and extending the actual penetration path. As penetration continues, the projectile pushes the ceramic cone forward, the backplate undergoes plastic bending deformation, and the projectile deflects. This process prolongs the projectile-target contact time and enhances the retention effect. 3. At T=200 μs, the projectile continues to interact with the ceramic, and the projectile undergoes further erosion. 4. By the late stage of penetration (T=300 μs), the projectile penetrates the ceramic layer at a certain angle.

[0044] Figure 18 The relationship between ceramic energy absorption and impact velocity shows that the energy absorption of ceramics in all three structures increases monotonically with increasing impact velocity, which is consistent with the strain rate sensitivity of ceramic materials. However, the ceramic blocks in Embodiments 1 and 2 of this application exhibit a higher level of energy absorption, and the slope of their growth curves is more significant, indicating that the ceramic layer in the rhomboid truncated composite armor is more fully broken and utilized, which is consistent with the ceramic breakage situation in the experiment.

[0045] Figure 19The curve showing the relationship between backplate displacement and time reveals information from the perspective of overall structural response and protective aftereffects. This curve illustrates the lateral deformation (back convexity) process of the armor backplate under impact load. As can be seen from the figure, all curves undergo a rapid displacement increase, reach a peak value, and then stabilize. In this dynamic response, the peak and stable values ​​of the backplate displacement curve corresponding to the rhomboid truncated structure at different impact velocities are systematically lower than those of the hexagonal structure under the same conditions. This strongly demonstrates that the rhomboid truncated composite armor can dissipate more impact energy in the ceramic layer when subjected to impact, thus transferring less residual energy to the backplate and effectively suppressing the overall deformation of the backplate. A comparison of projectile velocity and backplate displacement data shows that the ceramic block structure of this application has better ballistic performance than the traditional hexagonal structure.

[0046] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A modular ceramic armor with a deflection mechanism, characterized in that: The system includes a backplate and a ceramic protective layer fixed to the upper surface of the backplate. The ceramic protective layer includes multiple ceramic protective units arranged sequentially in a first direction, with adjacent ceramic protective units bonded and fixed to each other. Each ceramic protective unit includes multiple ceramic blocks arranged sequentially in a second direction, which is perpendicular to the first direction, with adjacent ceramic blocks bonded and fixed to each other. The ceramic blocks are provided with a deflection structure, which includes a first deflection interface and a second deflection interface. During penetration, the projectile can sequentially contact the first deflection interface and the second deflection interface, inducing the projectile to deflect twice consecutively, thereby achieving penetration trajectory reconstruction and attitude instability.

2. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The first deflection interface and the second deflection interface have the same deflection direction but different deflection angles.

3. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The first deflection interface and the second deflection interface are arranged symmetrically or asymmetrically with respect to the central axis of the ceramic block.

4. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The top surface of the ceramic block has a first inclined surface and serves as the first deflection interface, and at least one side wall of the ceramic block has a second inclined surface and serves as the second deflection interface.

5. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The ceramic block has a first mounting surface that can be attached and fixed to the back plate. The front end of the first mounting surface is provided with a second mounting surface that can be attached and fixed to the front ceramic block. The rear end of the first mounting surface is provided with a third mounting surface that can be attached and fixed to the rear ceramic block. The second mounting surface and the third mounting surface are both inclined surfaces and parallel to each other. The second mounting surface and the third mounting surface are connected by a first connecting surface and a second connecting surface in sequence. The first connecting surface is an inclined surface and has a different inclination angle from the second mounting surface.

6. The modular ceramic armor with a deflection mechanism as described in claim 5, characterized in that: The second connecting surface is a plane parallel to the first mounting surface or an inclined surface with a different inclination direction than the first connecting surface.

7. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The ceramic block is formed by cutting off the obtuse angle along the line connecting the midpoints of the two adjacent obtuse-angled sides at the top of the rhombus or parallelogram.

8. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The ceramic block is formed by cutting off the obtuse angle along the line connecting the midpoints of the two adjacent obtuse angle sides at the top of the rhombus or parallelogram, and cutting off the acute angle along the line connecting the midpoints of the two adjacent acute angle sides at the top.

9. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The acute angle of the rhombus or parallelogram is 30°-60°.

10. The modular ceramic armor with a deflection mechanism as described in claim 1, characterized in that: The ceramic protective layer is fixedly connected to the back plate by a first adhesive layer, and two adjacent ceramic blocks are fixedly connected by a second adhesive layer, wherein the thickness of the first adhesive layer is greater than the thickness of the second adhesive layer.

Citation Information