Multilayer gradient structure lightweight high-strength composite explosion-proof container and preparation method thereof
The explosion-proof container designed with a multi-layer gradient structure solves the problems of wave impedance matching and low energy absorption efficiency of composite explosion-proof containers, achieving a lightweight, multi-stage energy absorption and high-efficiency protection effect without secondary damage, and is suitable for rapid response and field emergency scenarios.
Patent Information
- Application Number
- CN202611216452.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-20
AI Technical Summary
Existing composite explosion-proof containers lack scientific wave impedance matching design, are prone to delamination between layers, and have low energy absorption efficiency due to the single material composite material, resulting in insufficient protection against explosive impacts and the risk of secondary injury.
The device employs a multi-layered gradient structure design, including an impact-resistant inner liner, an energy dissipation sandwich layer, and a high-strength confinement outer shell layer. These layers are composed of a polyurea/carbon nanotube composite layer, a three-dimensional woven aramid fiber-reinforced aluminum-based foam metal layer, and a carbon fiber-reinforced epoxy resin base layer, respectively. Through orthogonal staggered layering and graphene modification, a gradient shell with wave impedance matching is formed. Dynamic monitoring is achieved by combining a pressure relief explosion-proof valve and an FBG fiber optic grating sensor.
It achieves extreme lightweighting, significantly improves mobile deployment capabilities, boasts excellent multi-stage energy absorption efficiency, eliminates the risk of secondary damage, exhibits robust comprehensive mechanical properties, and demonstrates significantly superior impact resistance compared to traditional steel and single-material composite containers.
Smart Images

Figure CN123134841A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of explosion-proof containers made of composite materials, specifically to explosion-proof containers made of multi-layered gradient structure lightweight high-strength composite materials and their preparation methods. Background Technology
[0002] With the normalization of global counter-terrorism operations, the increasing complexity of the international security situation, and the continuous improvement of modern industrial standards for the storage and transportation of hazardous chemicals, the demand for high-grade, high-reliability explosion-proof containers in both military and civilian markets continues to experience explosive growth. The core function of explosion-proof containers is to completely contain the ultra-high-pressure shock wave, instantaneous high-temperature flame, and ultra-high-speed irregular fragments generated by the fragmentation of the explosive casing in the event of an unexpected internal explosion. Statistical analysis shows that the flight speed of conventional explosion fragments can reach 800m / s-1200m / s, thereby maximizing the protection of surrounding personnel, facilities, and the environment.
[0003] Currently, most explosion-proof containers used in domestic and international markets and actual operations are still manufactured using high-strength alloy steel or explosion-proof armor steel through multi-layer rolling and welding. The density of these metal materials is approximately 7.8 × 10³ kg / m³, and the tensile strength of steel explosion-proof containers under standard operating conditions is approximately 490 MPa. Although these metal explosion-proof containers possess a certain degree of blast resistance and protection against low-to-medium yield explosions, they exhibit the following irreconcilable and significant drawbacks in practical engineering applications and rapid emergency response: The equipment is extremely heavy: a single steel explosion-proof container with the same protective equivalent (1.5kg TNT) can weigh up to 52.0kg, making it extremely inflexible in terms of transportation, deployment, vehicle mounting, and on-site manual delivery. It simply cannot meet the modern usage requirements of portable, unpowered, and rapid emergency response operations.
[0004] The risk of secondary injury is significant: Metal materials exhibit a certain tendency towards brittle fracture under heavy-load explosions and overload impacts. Multiple simulated explosion tests show that when the explosive yield exceeds the design limit, the rupture of a steel container will produce an average of more than 14 high-speed metal fragments. Once the container shell breaks and shatters, it easily generates a large number of uncontrolled metal fragments with extremely high speeds and sharp edges. These fragments, flying in all directions, can cause severe secondary damage and create even more uncontrollable indirect harm.
[0005] To achieve weight reduction, some existing research has begun to explore the use of fiber-reinforced composite materials to fabricate explosion-proof containers. However, most existing composite explosion-proof containers suffer from design limitations, generally employing a single material, a single layup direction, or a simple hybrid homogeneous structure. Measured data shows that the energy absorption density per unit volume of a typical single-carbon fiber explosion-proof container is only 18.4 J / cm³. When faced with the combined dynamic forces of the "instantaneous ultra-high pressure shock wave" and "high-speed sharp fragments" unique to sudden explosions, it exhibits insurmountable destructive limitations: on the one hand, due to the lack of scientific impedance matching design, the shock wave is reflected and superimposed within the material, leading to large-area delamination, peeling, and tearing between the layers of heterogeneous composite materials; on the other hand, the lack of a macroscopic energy absorption mechanism in a single material results in low energy absorption efficiency, making local wall thickness easily penetrated by irregular high-speed sharp fragments. In a 1.5 kg TNT equivalent test, a typical carbon fiber container exhibits overall disintegration. Summary of the Invention
[0006] This invention provides a multi-layered gradient structure lightweight high-strength composite explosion-proof container and its preparation method, aiming to solve the problems of existing composite explosion-proof containers lacking scientific wave impedance matching design, easy delamination between layers, and low energy absorption efficiency of single-material composite materials.
[0007] The technical solution provided by this invention is as follows: This invention provides a multi-layered gradient structure lightweight high-strength composite explosion-proof container, comprising an impact-resistant inner liner, an energy dissipation sandwich layer, and a high-strength confinement outer shell layer stacked sequentially from the inside out. The impact-resistant inner liner is a polyurea / carbon nanotube composite modified layer, made of polyurea resin, amino-terminated polyether, multi-walled carbon nanotubes and silane coupling agent; The energy dissipation sandwich layer is a three-dimensional braided aramid fiber reinforced aluminum-based foam metal composite layer. The volume fraction of aramid fiber in the three-dimensional braided aramid fiber reinforced aluminum-based foam metal composite layer is 15%-25%, the porosity of aluminum-based foam metal is 75%-85%, and the aluminum-based foam metal is filled inside the spatial grid formed by the aramid fiber. The high-strength confinement outer shell layer is a carbon fiber reinforced epoxy resin matrix composite material layer. The carbon fibers in the carbon fiber reinforced epoxy resin matrix composite material layer are wound on the outer surface of the energy dissipation sandwich layer in an orthogonal staggered layup pattern of [0° / 45° / 90° / -45°].
[0008] Optionally, the impact-resistant liner layer contains the following raw materials in parts by weight: 80-100 parts polyurea resin, 20-30 parts amino-terminated polyether, 1.5-3.5 parts multi-walled carbon nanotubes, and 0.5-1.2 parts silane coupling agent.
[0009] Optionally, graphene microsheets are added to the epoxy resin matrix of the high-strength confining outer shell layer, and the amount of graphene microsheets added is 1wt%-2wt% of the total resin mass.
[0010] Optionally, the opening of the explosion-proof container is equipped with a pressure relief explosion-proof valve, which includes a metal valve body and a brittle pressure relief plate with a preset fracture groove.
[0011] Optionally, an FBG fiber grating sensor is disposed inside the energy dissipation sandwich layer; A connecting seat is fixedly connected to the outer side of the high-strength constraint outer shell layer. A mounting ring is detachably connected to the connecting seat, and a protective cover is fixedly connected to the mounting ring. A micro motor and a start-stop controller are fixedly connected to the mounting ring. The micro motor and the FBG fiber grating sensor are both electrically connected to the start-stop controller. Optionally, the output end of the micro motor is connected to a rotating block, the inner top wall of the protective cover is connected to a rubber elastic band, the bottom end of the rubber elastic band is connected to a round block, the round block is coated with a magnetic coating, the protective cover is provided with a plug hole, a warning rod is movably inserted into the plug hole, and the bottom end of the warning rod is fixedly connected to the round block.
[0012] The present invention also provides a method for preparing an explosion-proof container made of lightweight, high-strength composite material with a multi-layered gradient structure, comprising the following steps: Polyurea resin, amino-terminated polyether, multi-walled carbon nanotubes and silane coupling agent are mixed and stirred, and after ultrasonic dispersion, they are applied to a metal core mold by vacuum-assisted molding or high-pressure spraying. After curing, the impact-resistant inner lining layer is obtained. Using a liner-lined core mold as a skeleton, an aramid fiber skeleton is woven in a multi-axis CNC three-dimensional braiding machine. The aluminum-based foam metal is then filled into the fiber mesh through vacuum-assisted pressure impregnation. After cooling, the outer surface is flattened to obtain the energy dissipation sandwich layer. Carbon fibers are wound onto the outer surface of the energy dissipation sandwich layer in an orthogonal staggered layup manner, and then cured in an autoclave to obtain the high-strength confinement outer shell layer. Remove the core mold, process the container opening and flange, assemble the pressure relief explosion-proof valve, and after airtightness testing, obtain the multi-layer gradient structure lightweight high-strength composite explosion-proof container.
[0013] Optionally, the polyurea resin, amino-terminated polyether, multi-walled carbon nanotubes, and silane coupling agent are formulated in the following weight ratios: 80-100 parts polyurea resin, 20-30 parts amino-terminated polyether, 1.5-3.5 parts multi-walled carbon nanotubes, and 0.5-1.2 parts silane coupling agent; the mixing and stirring speed is 800-1200 rpm, and the stirring time is 20-30 min; the ultrasonic dispersion treatment uses a frequency of 40 kHz-60 kHz, and the dispersion time is 40-50 min.
[0014] Optionally, the volume fraction of the aramid fiber is 15%-25%; the porosity of the aluminum-based foam metal is 75%-85%; and the external air pressure during vacuum-assisted pressure impregnation is 1.5MPa-3.0MPa.
[0015] Optionally, the dynamic tension of the carbon fiber winding is 40N-60N; the autoclave curing process is as follows: the temperature is increased to 80℃ at 1.5℃ / min and held at 80℃ for 1 hour, then increased to 130℃ and pressure of 0.6MPa is applied and held at 130℃ for 3 hours, and then cooled to below 50℃ before being removed from the autoclave.
[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. Extremely lightweight design, significantly enhanced mobility and deployment capabilities: Compared to traditional armored steel explosion-proof containers with equivalent blast resistance and blast capacity (1.5kg TNT), this invention, through the extensive use of high-performance long fibers, lightweight foam metals, and modified polymer materials, reduces the overall structural weight by more than 60%, with a measured weight reduction of 64.4%. The 18.5kg weight allows for single-person transport and rapid deployment, resulting in a revolutionary leap in equipment portability, rapid on-site deployment without power, and vehicle-mounted emergency load mobility. This makes it highly suitable for rapid response special police operations and individual soldier emergency response in the field.
[0017] 2. Superior Multi-Stage Energy Absorption Efficiency and Excellent Wave Impedance Matching: Through a unique "flexible-tough-rigid" wave impedance stepped gradient shell wall thickness design, the ultra-high pressure shock wave from the explosion undergoes continuous interface reflection, scattering, and waveform attenuation as it penetrates different interlayer media. Energy testing systems have shown that the overall dynamic energy conversion and absorption efficiency of the explosion is more than 40% higher than that of traditional steel structures and 130% higher than that of ordinary single carbon fiber containers. The multi-stage heterogeneous materials ensure high-efficiency dissipation of the shock wave's dynamic energy, effectively dispersing the impact load and protecting the overall structure from collapse.
[0018] 3. Eliminating the risk of secondary injury, with comprehensive safety protection: Since the outer shell does not contain large pieces of brittle, heavy metal, the explosion-proof container of this invention, when faced with extreme overload damage exceeding its limits, exhibits failure modes including large-strain tearing of the flexible matrix, tensile fracture of continuous fiber bundles, and localized powdery crushing of the aluminum-based foam metal. In a 1.5kg TNT equivalent ultimate explosion test, this product produces absolutely no high-energy, sharp-spraying secondary high-velocity metal fragments throughout the entire destruction process; the number of fragments is zero, completely avoiding the potential for secondary indirect injury to innocent personnel and key facilities.
[0019] 4. Robust comprehensive mechanical properties, perfectly combining penetration resistance and instability prevention: This invention achieves an overall tensile strength of up to 820 MPa by introducing a multi-walled carbon nanotube micronetwork into the flexible inner liner, using a three-dimensional integrated braiding technique in the core layer, and employing graphene modification and scientifically optimized orthogonal layup design in the outer shell layer. This significantly surpasses the 490 MPa of steel containers and the 610 MPa of ordinary carbon fiber containers. Its tensile strength, impact dynamic toughness, resistance to high-speed sharp fragment penetration, and macroscopic instability resistance are all significantly superior to traditional single-material and simple hybrid composite materials. The interlaminar shear bonding force is extremely high, and after fatigue cycle testing (1000 impact cycles), the structure shows no delamination or cracking, demonstrating excellent structural stability and fatigue life. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of the overall structure of the explosion-proof container made of lightweight, high-strength composite material with a multi-layer gradient structure according to the present invention. Figure 2 This is a schematic diagram of the pressure relief explosion-proof valve in this invention; Figure 3 This is a three-dimensional schematic diagram of the protective cover assembly structure in this invention; Figure 4 This is a schematic diagram of the mounting ring structure in this invention; Figure 5 This is a schematic diagram showing the connection relationship between the warning bar and the rotating block in this invention; Figure 6 This is a schematic diagram of the internal structure of the protective cover in this invention; Figure 7 This is a schematic diagram showing the state of the warning bar after it has been moved upwards in this invention; Figure 8 This is a flowchart of the preparation method of the present invention.
[0021] Explanation of reference numerals in the figure: 1-Impact-resistant inner lining; 2-Energy dissipation sandwich layer; 3-High-strength confinement outer shell layer; 4-Pressure relief explosion-proof valve; 41-Metal valve body; 42-Brittle pressure relief plate; 5-Connecting seat; 6-Mounting ring; 7-Protective cover; 8-Micro motor; 9-Rotating block; 10-Rubber elastic band; 11-Circular block; 12-Magnetic coating; 13-Insertion hole; 14-Warning rod. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the embodiments described below are only some, not all, of the embodiments of the present invention. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in conjunction with the accompanying drawings is intended merely to illustrate selected embodiments of the invention and is not intended to limit the scope of protection claimed by the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0023] Example 1 like Figure 1 As shown, this embodiment provides a multi-layered gradient structure lightweight high-strength composite explosion-proof container, including an impact-resistant inner liner 1, an energy dissipation sandwich layer 2, and a high-strength confinement outer shell layer 3, which are tightly stacked from the inside to the outside.
[0024] The impact-resistant inner liner 1 is a polyurea / carbon nanotube composite modified flexible layer. As the first protective barrier directly facing the internal explosion source, it is used to bear the dynamic high strain rate load of the instantaneous explosion shock wave and prevent high-energy explosion fragments from penetrating the container wall.
[0025] The energy dissipation sandwich layer 2 is a three-dimensional woven aramid fiber reinforced aluminum-based foam metal composite layer, which serves as the middle core energy-absorbing layer structure. It is used to fully absorb and dissipate the shear and impact energy generated by the explosion through macroscopic and microscopic progressive plastic collapse.
[0026] The high-strength constraint outer shell layer 3 is a carbon fiber reinforced epoxy resin matrix composite material layer, which serves as the outermost rigid support and is used to form a high-rigidity overall centripetal constraint for the entire container under the high-pressure expansion state of an explosion.
[0027] The impact-resistant inner lining layer 1 is prepared from the following specific weight parts of raw materials through scientific formulation and composite modification: 80-100 parts of polyurea resin, 20-30 parts of amino-terminated polyether, 1.5-3.5 parts of multi-walled carbon nanotubes, and 0.5-1.2 parts of silane coupling agent.
[0028] In the energy dissipation sandwich layer 2, the volume fraction of three-dimensional braided aramid fiber is strictly controlled at 15%-25%, the micro porosity of aluminum-based foam metal is controlled at 75%-85%, and the spatial grid formed by the three-dimensional braided aramid fiber is completely filled with interconnected or closed-cell aluminum-based foam metal.
[0029] In this embodiment, the polyurea resin is preferably 90 parts, the amino-terminated polyether is preferably 25 parts, the multi-walled carbon nanotube is preferably 2.5 parts, and the silane coupling agent is preferably 0.8 parts; the volume fraction of the three-dimensional braided aramid fiber is 20%, and the microporosity of the aluminum-based foam metal is controlled at 80%.
[0030] In the high-strength confinement outer shell layer 3, the carbon fibers used as reinforcement are precisely wound on the outer surface of the energy dissipation sandwich layer 2 in a quasi-unidirectional layup pattern of [0° / 45° / 90° / -45°]n orthogonal interlacing. Graphene microsheets, accounting for 1wt%-2wt% of the total resin mass, are uniformly added to the epoxy resin matrix as a micro-reinforcing phase, preferably 1.5wt% of graphene microsheets. Wherein, [0° / 45° / 90° / -45°]n represents the carbon fiber layup cyclic arrangement. The 0°, 45°, 90°, and -45° angles within the parentheses form a basic layup unit, corresponding to four fiber layup angles: along the component axis, at 45° to the axis, perpendicular to the component axis, and at -45° to the axis. These angles respectively bear the functions of axial tension and compression, shear and torsion resistance, circumferential force, and balancing shear coupling. The four layers together form a quasi-isotropic layup structure with balanced in-plane mechanical properties. The subscript n outside the parentheses indicates the number of times the four-layer unit is repeatedly laid and wound. Different values of n correspond to different total layup layers. For example, n=1 means that the carbon fiber layup cycles once according to the four fiber layup angles: along the component axis, at 45° to the axis, perpendicular to the component axis, and at -45° to the axis. n=2 means that the carbon fiber layup cycles twice according to the four fiber layup angles: along the component axis, at 45° to the axis, perpendicular to the component axis, and at -45° to the axis. This layup sequence is adapted to the precision winding molding process on the outer surface of the component. The 0° and 90° fibers are orthogonally distributed, and the ±45° fibers are interlaced, which eliminates the anisotropy of unidirectional carbon fiber materials, ensuring uniform stress performance in the axial, circumferential, and shear dimensions. Combined with an internal energy dissipation sandwich layer, it comprehensively improves the overall structural load-bearing capacity, impact resistance, and energy absorption. In this embodiment, n=4 indicates that the carbon fiber layup is cyclically repeated four times at four different fiber angles: along the component's axial direction, at 45° to the axial direction, perpendicular to the component's axial direction, and at -45° to the axial direction.
[0031] like Figure 2As shown, the opening of the explosion-proof container is specially equipped with a mechanical pressure relief explosion-proof valve 4. The pressure relief explosion-proof valve 4 specifically includes a metal valve body 41 and a brittle pressure relief plate 42 with a preset fracture groove. When the instantaneous gas pressure inside the explosion-proof container exceeds the preset safety threshold due to an explosion, the pressure relief plate 42 will instantly undergo local shear fracture along the preset fracture groove, thereby achieving safe diversion and pressure relief. The pressure relief valve has a preset opening pressure of 180MPa and can automatically achieve directional tearing pressure relief when the instantaneous deflagration pressure of the gas inside the container exceeds the design safety index, further significantly improving the overall system safety of the equipment.
[0032] The impact-resistant inner liner layer 1, as the innermost flexible protective layer, is made of a polyurea / carbon nanotube composite modified flexible material, with a finished thickness controlled between 3mm and 5mm, preferably 4mm. Its core mechanism lies in two aspects: firstly, it cleverly utilizes the strong nonlinear viscoelastic deformation characteristics unique to polyurea elastomers when facing dynamic high-strain-rate impact loads, enabling it to adaptively absorb and weaken the peak energy of the initial shock wave during large deformations; secondly, the microscopically uniformly dispersed multi-walled carbon nanotubes within the polyurea can exert microscopic nanotube pull-out, crack bridging, and deflection effects when the matrix is penetrated by localized high-energy sharp fragments, effectively inhibiting the macroscopic crack propagation and tearing of the polymer matrix and preventing high-speed fragments from penetrating and breaking through the layer structure. Experimental measurements show that this layer can effectively resist the penetration of simulated fragments at a velocity of 900m / s.
[0033] The energy dissipation sandwich layer 2, serving as the intermediate tough energy-absorbing layer, has a thickness of 15mm-25mm, preferably 20mm. It employs a three-dimensional integrated woven aramid fiber combined with an aluminum-based foam metal composite structure. This creates a unique dual-synergistic and highly efficient energy absorption and dissipation mechanism of "grid constraint + skeleton collapse" at both the macroscopic and microscopic levels. When residual shock waves and energy from the inner liner are transmitted to this layer, the three-dimensional woven aramid fiber spatial grid exerts a strong flexible tensile constraint, while the aluminum-based foam metal filling the grid undergoes large-area progressive plastic collapse, pore wall crushing, and buckling deformation under impact load. Through the long-stroke plastic plateau effect of the material, the dynamic kinetic energy of the explosion is efficiently converted into the material's own plastic deformation energy, fully dissipating the explosion energy. The energy dissipation sandwich layer 2 is the main energy-absorbing structure of this container.
[0034] The high-strength confinement outer shell layer 3, as the outermost rigid confinement layer, is made of carbon fiber reinforced epoxy resin matrix composite material with a specific orthogonal staggered layup pattern. This layer mainly relies on the ultra-high axial and circumferential mechanical tensile support performance of the high-modulus, high-strength continuous carbon fibers to provide strong rigid external confinement to the overall container shell structure that is rapidly expanding due to the internal explosion, resisting overall bending and instability.
[0035] Example 2 like Figure 3-7 As shown, a connecting seat 5 is fixedly connected to the outer side of the high-strength constraint outer shell layer 3, and a mounting ring 6 is detachably connected to the outer side of the connecting seat 5. A protective cover 7 is fixedly connected to the top of the mounting ring 6.
[0036] An FBG fiber optic grating sensor is installed inside the energy dissipation sandwich layer 2. A micro motor 8 and a start / stop controller are fixedly connected to the top of the mounting ring 6. A rotating block 9, which can be made of metal, is fixedly connected to the output end of the micro motor 8. A pair of rubber elastic bands 10 are fixedly connected to the inner top wall of the protective cover 7. The bottom ends of the pair of rubber elastic bands 10 are fixedly connected to the same circular block 11, which can be made of metal. The side of the circular block 11 away from the rubber elastic bands 10 is coated with a magnetic coating 12 that magnetically connects with the circular block 11. An insertion hole 13 is provided on the protective cover 7. A warning rod 14 is movably inserted into the insertion hole 13, and the bottom end of the warning rod 14 is fixedly connected to the circular block 11. In the initial state, the rubber elastic bands 10 are in a stretched state.
[0037] During use, when the FBG fiber optic sensor inside the energy dissipation sandwich layer 2 detects that the explosion-proof energy absorption capacity of the energy dissipation sandwich layer 2 is exhausted, the start / stop controller will activate the micro motor 8, causing its output end to drive the rotating block 9 to rotate, thereby separating the rotating block 9 from the magnetic coating 12. After the magnetic attraction between the rotating block 9 and the magnetic coating 12 is removed, the elastic tension of the rubber elastic band 10 will cause the round block 11 to move the warning rod 14 upward, thereby causing the top of the warning rod 14 to protrude from the insertion hole 13, thus reminding personnel to promptly inspect or replace the energy dissipation sandwich layer 2 to ensure the normal use of the explosion-proof container.
[0038] like Figure 8 As shown, this invention provides a method for preparing a multi-layered gradient structure lightweight high-strength composite explosion-proof container. This method is used to prepare the aforementioned multi-layered gradient structure lightweight high-strength composite explosion-proof container, and includes the following steps: S1: Impact-resistant inner lining layer 1 preformed The impact-resistant inner liner 1 is prefabricated by mixing polyurea resin and amino-terminated polyether in a vacuum mixer, treating the multi-walled carbon nanotube slurry with an ultrasonic dispersion device, and then uniformly coating the composite material onto a metal core mold through a vacuum-assisted molding or high-pressure spraying system. After constant temperature curing, a high-precision inner liner is obtained.
[0039] The specific process parameters are as follows: Raw material ratio: 90 parts polyurea resin, 25 parts amino-terminated polyether, 2.5 parts multi-walled carbon nanotubes, and 0.8 parts silane coupling agent.
[0040] Mixing parameters: Vacuum stirring at 1000 rpm for 20 min, uniformity deviation <2%; Dispersion parameters: 50 kHz ultrasonic oscillation for 45 min, agglomeration rate <3%; Molding parameters: VARI or high-pressure spraying, curing at 55℃ for 24 h, thickness 35 mm, error ≤ ±0.2 mm.
[0041] S2: Energy dissipation sandwich layer 2 composite molding The energy dissipation sandwich layer 2 uses a core mold with an inner liner as a skeleton. The aramid fiber skeleton is woven in a conformal manner on a multi-axis CNC three-dimensional braiding machine. After being installed in a pressure-resistant mold, the aluminum-based foam metal is filled with fiber mesh through vacuum-assisted pressure impregnation. After cooling, the outer surface is precisely leveled by a high-precision CNC grinding machine to obtain the finished sandwich layer.
[0042] The specific process parameters are as follows: the volume fraction of aramid fiber is 20%, the porosity of aluminum-based foam metal is 80% (detected by gas adsorption method), the external air-filling reverse mechanical pressure is 1.5MPa-3.0MPa, preferably 2.5MPa, and a vacuum-assisted pressure impregnation process is adopted; the thickness of the sandwich layer is 15mm-25mm, preferably 20mm, and the flatness error of the outer surface is <0.3mm.
[0043] S3: High-strength confined outer shell layer 3-winding curing The high-strength confinement outer shell layer 3 is made by combining graphene-modified epoxy resin with carbon fiber, using a multi-axis CNC winding machine to precisely wind it onto the outer surface of the sandwich layer according to an orthogonal staggered layup trajectory, and then completing the overall curing through a program-controlled stepped heating, pressurization and slow cooling process in an autoclave, thus obtaining a high-strength outer shell structure.
[0044] The specific process parameters are as follows: the amount of graphene microplates added is 1wt%-2wt% of the total resin mass, preferably 1.5wt%, and the batch deviation of resin viscosity is <5%; the dynamic tension of carbon fiber winding is 40N-60N, preferably 50N, with fluctuation ≤±1N; the layup method is [0° / 45° / 90° / -45°]n, where n is preferably 4, and an orthogonal staggered method is adopted.
[0045] The autoclave curing process is as follows: the temperature is increased to 80℃ at 1.5℃ / min and held for 1 hour, then increased to 130℃ and pressure of 0.6MPa is applied and held for 3 hours, and then the temperature is slowly cooled to below 50℃ before being removed from the autoclave.
[0046] S4: Post-processing and accessory assembly In the post-processing stage, the internal core mold is removed first, and the container opening and flange are precisely cut and tapped using a five-axis machining center. Then, a mechanical pressure relief explosion-proof valve 4 is installed by pre-embedded titanium alloy threaded rings. Finally, the finished product is delivered after passing the airtightness test.
[0047] The specific process parameters are as follows: the dimensional accuracy of the machined parts is IT7, the pressure relief valve assembly uses a high-strength titanium alloy threaded ring, the airtightness test pressure is 0.2MPa, the pressure holding time is 10min, and there must be no leakage.
[0048] Comparative Example Based on the multi-layer gradient structure lightweight high-strength composite explosion-proof container prepared in Example 2 (Example), this comparative example uses a traditional high-strength steel explosion-proof container (Comparative Example 1) and a common single carbon fiber reinforced composite explosion-proof container (Comparative Example 2) as two sets of comparative reference samples.
[0049] All three sets of samples had a uniform design volume of 0.12 m³, an opening diameter of 280 mm, and a theoretical protective equivalent of 1.5 kg TNT. Under the premise of strictly maintaining complete consistency in the internal effective volume, opening size, and theoretical protective design equivalent of the three sets of samples, macroscopic mechanical property tests were conducted using a universal testing machine. The samples were then transported to a special blasting test site for high-specification live-fire tests of the 1.5 kg TNT military explosive equivalent, including dynamic target firing safety tests. The blasting environment was an open-air site at normal temperature and pressure, and the initial simulated fragment velocity was uniformly set to 950 m / s.
[0050] The specific test and experiment comparison data are shown in Tables 1 and 2: Table 1 Comparison of Core Physical and Mechanical Properties
[0051] Table 2 Explosion-resistant safety test of 1.5kg TNT equivalent
[0052] Based on the real-world test results obtained under rigorous engineering and live-fire testing environments, the embodiments of this invention demonstrate overwhelming and significant advantages in key core technical indicators such as extreme lightweight level, macroscopic static mechanical strength, microscopic and macroscopic energy absorption density, and live-fire blast protection safety and reliability. Under the same blast-proof conditions, the product comprehensively surpasses the two control samples in four core indicators: weight, mechanical strength, energy absorption capacity, and blast-proof safety. Its comprehensive technical performance not only far exceeds that of traditional heavy steel blast-proof containers but also significantly surpasses that of ordinary single-material composite material blast-proof containers, fully meeting and complying with the national requirements for the safe use of high-level special blast-proof, bomb disposal, and core military equipment. Furthermore, the entire manufacturing process parameters are controllable, and the product consistency is good, making it suitable for large-scale mass production and market promotion.
[0053] Specifically, the multi-layer gradient composite explosion-proof container provided by this invention has the following performance advantages: 1. Extremely lightweight design, significantly enhanced mobility and deployment capabilities: Compared to traditional armored steel explosion-proof containers with equivalent blast resistance and blast capacity (1.5kg TNT), this invention, through the extensive use of high-performance long fibers, lightweight foam metals, and modified polymer materials, reduces the overall structural weight by more than 60%, with a measured weight reduction of 64.4%. The 18.5kg weight allows for single-person transport and rapid deployment, resulting in a revolutionary leap in equipment portability, rapid on-site deployment without power, and vehicle-mounted emergency load mobility. This makes it highly suitable for rapid response special police operations and individual soldier emergency response in the field.
[0054] 2. Superior Multi-Stage Energy Absorption Efficiency and Excellent Wave Impedance Matching: Through a unique "flexible-tough-rigid" wave impedance stepped gradient shell wall thickness design, the ultra-high pressure shock wave from the explosion undergoes continuous interface reflection, scattering, and waveform attenuation as it penetrates different interlayer media. Energy testing systems have shown that the overall dynamic energy conversion and absorption efficiency of the explosion is more than 40% higher than that of traditional steel structures and 130% higher than that of ordinary single carbon fiber containers. The multi-stage heterogeneous materials ensure high-efficiency dissipation of the shock wave's dynamic energy, effectively dispersing the impact load and protecting the overall structure from collapse.
[0055] 3. Eliminating the risk of secondary injury, with comprehensive safety protection: Since the outer shell does not contain large pieces of brittle, heavy metal, the explosion-proof container of this invention, when faced with extreme overload damage exceeding its limits, exhibits failure modes including large-strain tearing of the flexible matrix, tensile fracture of continuous fiber bundles, and localized powdery crushing of the aluminum-based foam metal. In a 1.5kg TNT equivalent ultimate explosion test, this product produces absolutely no high-energy, sharp-spraying secondary high-velocity metal fragments throughout the entire destruction process; the number of fragments is zero, completely avoiding the potential for secondary indirect injury to innocent personnel and key facilities.
[0056] 4. Robust comprehensive mechanical properties, perfectly combining penetration resistance and instability prevention: This invention achieves an overall tensile strength of up to 820 MPa by introducing a multi-walled carbon nanotube micronetwork into the flexible inner liner, using a three-dimensional integrated braiding technique in the core layer, and employing graphene modification and scientifically optimized orthogonal layup design in the outer shell layer. This significantly surpasses the 490 MPa of steel containers and the 610 MPa of ordinary carbon fiber containers. Its tensile strength, impact dynamic toughness, resistance to high-speed sharp fragment penetration, and macroscopic instability resistance are all significantly superior to traditional single-material and simple hybrid composite materials. The interlaminar shear bonding force is extremely high, and after fatigue cycle testing (1000 impact cycles), the structure shows no delamination or cracking, demonstrating excellent structural stability and fatigue life.
[0057] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claims. The scope of protection of the present invention is defined by the appended claims and their equivalents. The above descriptions are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions within the technical scope disclosed in the present invention should be covered within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A multi-layered gradient structure lightweight high-strength composite explosion-proof container, characterized in that: It includes an impact-resistant inner lining layer (1), an energy dissipation sandwich layer (2), and a high-strength confinement outer shell layer (3) stacked sequentially from the inside out. The impact-resistant inner liner (1) is a polyurea / carbon nanotube composite modified layer, made of polyurea resin, amino-terminated polyether, multi-walled carbon nanotubes and silane coupling agent; The energy dissipation sandwich layer (2) is a three-dimensional braided aramid fiber reinforced aluminum-based foam metal composite layer. The volume fraction of aramid fiber in the three-dimensional braided aramid fiber reinforced aluminum-based foam metal composite layer is 15%-25%, the porosity of aluminum-based foam metal is 75%-85%, and the aluminum-based foam metal is filled inside the spatial grid formed by the aramid fiber. The high-strength confinement outer shell layer (3) is a carbon fiber reinforced epoxy resin matrix composite material layer. The carbon fibers in the carbon fiber reinforced epoxy resin matrix composite material layer are wound on the outer surface of the energy dissipation sandwich layer (2) in an orthogonal staggered layup manner of [0° / 45° / 90° / -45°].
2. The explosion-proof container of a multi-layered gradient structure lightweight high-strength composite material according to claim 1, characterized in that: The impact-resistant inner lining (1) contains the following raw materials in the following weight proportions: 80-100 parts of polyurea resin, 20-30 parts of amino-terminated polyether, 1.5-3.5 parts of multi-walled carbon nanotubes, and 0.5-1.2 parts of silane coupling agent.
3. The explosion-proof container of multi-layer gradient structure lightweight high-strength composite material according to claim 1, characterized in that: The epoxy resin matrix of the high-strength confinement outer shell layer (3) contains graphene microsheets, and the amount of graphene microsheets added is 1wt%-2wt% of the total resin mass.
4. The explosion-proof container of a multi-layered gradient structure lightweight high-strength composite material according to claim 1, characterized in that: The explosion-proof container is equipped with a pressure relief explosion-proof valve (4) at its opening. The pressure relief explosion-proof valve (4) includes a metal valve body (41) and a brittle pressure relief plate (42) with a preset fracture groove.
5. The explosion-proof container of a multi-layered gradient structure lightweight high-strength composite material according to any one of claims 1-4, characterized in that: An FBG fiber grating sensor is provided inside the energy dissipation sandwich layer (2); A connecting seat (5) is fixedly connected to the outside of the high-strength constraint outer shell layer (3), and a mounting ring (6) is detachably connected to the connecting seat (5). A protective cover (7) is fixedly connected to the mounting ring (6). A micro motor (8) and a start-stop controller are fixedly connected to the mounting ring (6). The micro motor (8) and the FBG fiber optic grating sensor are both electrically connected to the start-stop controller.
6. The explosion-proof container of a multi-layered gradient structure lightweight high-strength composite material according to claim 5, characterized in that: The output end of the micro motor (8) is connected to a rotating block (9), the inner top wall of the protective cover (7) is connected to a rubber elastic band (10), the bottom end of the rubber elastic band (10) is connected to a round block (11), the round block (11) is coated with a magnetic coating (12), the protective cover (7) is provided with a plug hole (13), a warning rod (14) is movably inserted into the plug hole (13), and the bottom end of the warning rod (14) is fixedly connected to the round block (11).
7. A method for preparing a multi-layered gradient structure lightweight high-strength composite explosion-proof container as described in any one of claims 1-6, characterized in that, Includes the following steps: Polyurea resin, amino-terminated polyether, multi-walled carbon nanotubes and silane coupling agent are mixed and stirred, and after ultrasonic dispersion treatment, they are applied to a metal core mold by vacuum-assisted molding or high-pressure spraying. After curing, the impact-resistant inner lining layer (1) is obtained. Using a liner-lined core mold as a skeleton, an aramid fiber skeleton is woven in a multi-axis CNC three-dimensional braiding machine. The aluminum-based foam metal is filled into the fiber mesh through vacuum-assisted pressure impregnation. After cooling, the outer surface is flattened to obtain the energy dissipation sandwich layer (2). Carbon fibers are wound onto the outer surface of the energy dissipation sandwich layer (2) in an orthogonal staggered layup manner and cured in a hot autoclave to obtain the high-strength confinement outer shell layer (3). Remove the core mold, process the container opening and flange, assemble the pressure relief explosion-proof valve (4), and after air tightness test, obtain the multi-layer gradient structure lightweight high-strength composite explosion-proof container.
8. The preparation method according to claim 7, characterized in that: The polyurea resin, amino-terminated polyether, multi-walled carbon nanotubes, and silane coupling agent are formulated in the following weight ratios: 80-100 parts polyurea resin, 20-30 parts amino-terminated polyether, 1.5-3.5 parts multi-walled carbon nanotubes, and 0.5-1.2 parts silane coupling agent. The mixing and stirring speed is 800-1200 rpm, and the stirring time is 20-30 min. The ultrasonic dispersion treatment uses a frequency of 40 kHz-60 kHz and a dispersion time of 40-50 min.
9. The preparation method according to claim 7, characterized in that: The volume fraction of the aramid fiber is 15%-25%; the porosity of the aluminum-based foam metal is 75%-85%; and the external air pressure during vacuum-assisted pressure impregnation is 1.5MPa-3.0MPa.
10. The preparation method according to claim 7, characterized in that: The dynamic tension of the carbon fiber winding is 40N-60N; the autoclave curing process is as follows: the temperature is increased to 80℃ at 1.5℃ / min and held at 80℃ for 1 hour, then increased to 130℃ and pressure of 0.6MPa is applied and held at 130℃ for 3 hours, and then cooled to below 50℃ before being removed from the autoclave.