A flexible pressure sensor structure and a method of manufacturing the same
By optimizing the layered packaging structure and conductive network design of the flexible pressure sensor, the problems of substrate and electrode failure, low resistance strain coefficient and insufficient cycle stability during the stretching process of the sensor were solved, and flexible detection with high sensitivity and durability was achieved.
Patent Information
- Application Number
- CN202611233667.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-20
AI Technical Summary
Existing flexible pressure sensors suffer from problems such as substrate and electrode failure during stretching, low resistance strain coefficient of conductive sensitive layer, insufficient device cyclic stability, and difficulty in adapting to complex curved surfaces and large deformation detection conditions.
Using PDMS film as the top and bottom electrode substrate, a serpentine conductive network is printed, and an adhesive cavity layer made of acrylic pressure-sensitive tape is used. This is combined with a porous elastic PU foam and a conductive network of composite carbon nanotubes and conductive carbon black, through optimized layered encapsulation structure and micropore design.
It significantly improves the elongation, resistance strain coefficient and cyclic stability of the sensor, with an elongation exceeding 100%, a resistance strain coefficient exceeding 50%, and a signal offset of less than 10% after 1000 cyclic stretching cycles, meeting the needs of complex curved surfaces and large deformation detection.
Smart Images

Figure CN123135271A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flexible piezoresistive sensor technology, and in particular to a flexible pressure sensor structure and its fabrication method. Background Technology
[0002] Currently, flexible pressure sensors are mainly classified into three types: piezoresistive, capacitive, and piezoelectric. Piezoresistive sensors use graphene or carbon nanotube composite elastic polymers as the sensitive layer, relying on deformation to change the resistance of the conductive path. They are simple in structure, easy to fabricate on a large scale, and have the widest application. Capacitive sensors rely on the thinning of the elastic dielectric layer under pressure to change the capacitance of the plates, resulting in stable dynamic response. Piezoelectric sensors use piezoelectric films such as polyvinylidene fluoride (PVDF), making them particularly suitable for dynamic impact force detection. To improve sensitivity in low-pressure areas, microstructures such as micro pyramids and porous foams are commonly designed. The substrate materials are often elastomers such as polydimethylsiloxane (PDMS), thermoplastic polyurethane (TPU), and silicone, achieving surface-fitting adhesion. These sensors are widely used in cutting-edge fields such as wearable health monitoring, robotic tactile sensing, and human-computer intelligent interaction.
[0003] However, existing flexible pressure sensors still have the following problems: First, the problem of tensile failure of substrates and electrodes is prominent. Most devices use rigid or semi-rigid materials such as polyethylene terephthalate (PET) as substrates, which are inherently not tensile and can withstand tensile strain of less than 5%. At the same time, interdigitated electrodes are mostly made of conductive silver paste, which is brittle and is very easy to generate microcracks or even complete circuit breaks during stretching or bending, leading to permanent circuit failure.
[0004] Second, the compressive deformation capacity is poor and the strain coefficient (GF) is low. The compressive deformation range of traditional piezoresistive structures is extremely narrow, the elastic recovery capacity is poor, and the resistance strain coefficient (GF, calculated by formula: GF=ΔR / (R*ε), where ΔR is the change in resistance, R is the initial resistance, and ε is the compressive deformation) is generally low, less than 10. Even with optimization of the microstructure, it is difficult to exceed 50, making it impossible to accurately identify weak deformation signals.
[0005] Third, sensitivity and pressure range are inherently mutually exclusive. High-sensitivity sensors usually do not have a very high detection upper limit, and the linear range usually does not exceed 20% of the full range.
[0006] Fourth, there is insufficient hysteresis and cyclic stability. Under repeated loading, the hysteresis error is about 15% to 35%, and the signal drift reaches ±20% after more than 10,000 cycles. In addition, arraying has problems such as crosstalk of linear wires, difficulty in mass production of small laboratory samples (defect rate >50%), and difficulty in synchronizing various test conditions such as pressure, temperature, and tension. Summary of the Invention
[0007] Therefore, the technical problem to be solved by the present invention is to overcome the problems of substrate and electrode failure during stretching, low resistance strain coefficient of conductive sensitive layer, insufficient device cycle stability, and difficulty in adapting to complex curved surfaces and large deformation detection conditions in the prior art.
[0008] To address the aforementioned technical problems, this invention provides a flexible pressure sensor structure, comprising: Top electrode substrate layer; A bottom electrode substrate layer is disposed opposite to the top electrode substrate layer, and both the top electrode substrate layer and the bottom electrode substrate layer are made of PDMS thin film; A first serpentine conductive network is disposed on the side of the top electrode substrate layer facing the bottom electrode substrate layer; The second serpentine conductive network is disposed on the side of the bottom electrode substrate layer facing the top electrode substrate layer. One of the first serpentine conductive network and the second serpentine conductive network is arranged along the warp direction, and the other is arranged along the weft direction. An upper bonding cavity layer is disposed on the inner side of the top electrode substrate layer; The lower adhesive cavity layer is disposed inside the bottom electrode substrate layer. The upper adhesive cavity layer and the lower adhesive cavity layer each have a cavity region corresponding to the conductive layer in the middle, so that the upper adhesive cavity layer, the lower adhesive cavity layer, and the upper adhesive cavity layer together define an accommodating space. A conductive layer is disposed within the receiving space and is in contact with the first serpentine conductive network and the second serpentine conductive network.
[0009] In one embodiment of the present invention, the first serpentine conductive network includes a plurality of serpentine conductive silver wires spaced apart along the meridian direction, and the second serpentine conductive network includes a plurality of serpentine conductive silver wires spaced apart along the parallel direction.
[0010] In one embodiment of the present invention, the width of each of the serpentine conductive silver wires is 0.4 to 0.6 mm, the spacing between adjacent serpentine conductive silver wires is 0.4 to 0.6 mm, the wave height and wavelength of the serpentine conductive silver wires are both 3 mm to 4 mm, the bending radius is 1.0 to 1.5 mm, and the period of each serpentine conductive silver wire is 6 to 10.
[0011] In one embodiment of the present invention, both the upper adhesive cavity layer and the lower adhesive cavity layer are made of acrylic pressure-sensitive tape, and the 180° peel strength of the acrylic pressure-sensitive tape is 20-30 N / cm, and the elongation at break is 100%-180%.
[0012] In one embodiment of the present invention, the conductive layer comprises a porous elastic polyurethane matrix and multi-walled carbon nanotubes and conductive carbon black dispersed in the porous elastic polyurethane matrix.
[0013] In one embodiment of the present invention, the thickness of the upper adhesive cavity layer and the lower adhesive cavity layer are both 20 μm to 200 μm; the thickness of the conductive layer is 20 μm to 200 μm; and the thickness of the top electrode substrate layer and the bottom electrode substrate layer are both 100 μm.
[0014] This invention also provides a method for fabricating a flexible pressure sensor structure, comprising: A PDMS film is provided to form a top electrode substrate and a bottom electrode substrate. A first serpentine conductive network and a second serpentine conductive network are respectively printed on one surface of the top electrode substrate and the bottom electrode substrate using a screen printing process, and then dried and cured. Thermoplastic polyurethane powder, multi-walled carbon nanotubes and conductive carbon black are mixed and added to dimethyl sulfoxide solvent. After stirring and dispersing, a conductive slurry precursor is obtained. The conductive slurry precursor is filled into a mold and a porous foamed conductive layer is prepared by freeze-drying. We provide acrylic pressure-sensitive tapes, which are prepared by die-cutting to create an upper adhesive cavity layer and a lower adhesive cavity layer with a cavity area in the middle. Place the bottom electrode substrate with the second serpentine conductive network facing upwards, place the conductive layer on the side of the bottom electrode substrate with the second serpentine conductive network, and attach the lower surface of the lower adhesive cavity layer to the upper surface of the bottom electrode substrate, so that the lower adhesive cavity layer surrounds the bottom of the conductive layer and is bonded and sealed to the bottom electrode substrate. The lower surface of the upper adhesive cavity layer is attached to the upper surface of the lower adhesive cavity layer, so that the upper adhesive cavity layer is bonded and sealed to the lower adhesive cavity layer around the top of the conductive layer. Place the top electrode substrate layer with the first serpentine conductive network facing down and attach it to the upper surface of the upper adhesive cavity layer to bond and seal the top electrode substrate layer with the upper adhesive cavity layer. The superimposed structure is then subjected to pressure and left to stand to complete the interlayer bonding.
[0015] In one embodiment of the present invention, the drying and curing process is carried out at 60°C to 80°C.
[0016] In one embodiment of the present invention, the thermoplastic polyurethane powder, the multi-walled carbon nanotubes and the conductive carbon black are mechanically stirred for 2 h and ultrasonically dispersed for 30 min; the stacked structure is uniformly pressurized and held for 15 min, and then left to stand at room temperature for more than 24 h.
[0017] In one embodiment of the present invention, the multi-walled carbon nanotubes and the conductive carbon black constitute conductive carbon powder, wherein the conductive carbon powder is composed of multi-walled carbon nanotubes with a mass ratio of 10% to 30% and conductive carbon black with a mass ratio of 70% to 90%, the sum of the mass ratios of the thermoplastic polyurethane powder and the conductive carbon powder is 100%, the mass ratio of the thermoplastic polyurethane powder is 80% to 95%, and the mass ratio of the conductive carbon powder is 5% to 20%. The thermoplastic polyurethane powder has a particle size of 100 nm to 10 μm; the multi-walled carbon nanotubes have a diameter of 2 nm to 100 nm; and the conductive carbon black is at least one of acetylene black, Ketjen black, and pigment black.
[0018] The technical solution of the present invention has the following advantages over the prior art: The flexible pressure sensor structure and its fabrication method described in this invention effectively overcome the defects of traditional products, such as weak tensile properties, low strain coefficient, and poor cyclic stability, by optimizing the layered packaging structure, conductive material ratio, and micropore design, resulting in significant comprehensive performance advantages.
[0019] This invention uses PDMS thin film as the top and bottom electrode substrates. A curved, serpentine conductive network is printed on the PDMS, and upper and lower bonding cavity layers are made of acrylic pressure-sensitive tape. The top and bottom electrode substrates are connected and sealed by the bonding layers and the conductive layer to ensure sealing during stretching. The intermediate conductive layer is prepared using a soft template removal method to obtain a porous, elastic thermoplastic polyurethane matrix. Specifically, 1% carbon nanotubes and 3% conductive carbon black are added during the preparation of the conductive layer. Multiple rounds of experimental testing show that the flexible pressure sensor prepared by this invention has a tensile strength >100%, a resistance strain coefficient >50, and a signal offset <10% after 1000 cycles of stretching.
[0020] This invention uses porous elastic PU foam as a conductive substrate, and combines it with 1-3% carbon nanotubes and 3-20% conductive carbon black to construct a composite conductive network, which can stably achieve a high resistance strain coefficient greater than 50, significantly improving the sensitivity and accuracy of deformation detection. Combined with upper and lower PDMS thin film encapsulation layers and an acrylic pressure-sensitive adhesive bonding cavity layer structure, along with a serpentine cross-conductive network design, the sensor's tensile strength can reach over 100%, meeting the requirements of flexible detection conditions involving complex curved surfaces and large deformations.
[0021] The structure of this invention can effectively buffer deformation stress, prevent the conductive network from breaking and shifting, and significantly improve the durability of the device. Testing showed that after 1000 cycles of cyclic stretching, the signal offset was less than 10%, solving the performance degradation problem in durability tests of traditional rigid sensors. Attached Figure Description
[0022] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings.
[0023] Figure 1 This is an exploded view of the flexible pressure sensor structure of the present invention.
[0024] Figure 2 This is an electron microscope image showing the microstructure of the conductive layer 7 prepared in Example 1.
[0025] Figure 3 This is the curve showing the relationship between the resistance change rate and pressure of the flexible pressure sensor structure in Example 1.
[0026] Explanation of reference numerals on the accompanying drawings: 1. Top electrode substrate layer; 2. Bottom electrode substrate layer; 3. First serpentine conductive network; 4. Second serpentine conductive network; 5. Upper bonding cavity layer; 6. Lower bonding cavity layer; 7. Conductive layer. Detailed Implementation
[0027] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.
[0028] In this invention, when directions (up, down, left, right, front, and back) are described, it is only for the purpose of describing the technical solution of this invention, and does not indicate or imply that the technical features referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, it should not be construed as a limitation of this invention.
[0029] In this invention, "several" means one or more, "multiple" means two or more, "greater than," "less than," "exceeding," etc., are understood to exclude the stated number; "above," "below," "within," etc., are understood to include the stated number. In the description of this invention, the terms "first" and "second" are used only to distinguish technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.
[0030] In this invention, unless otherwise explicitly defined, the terms "setting," "installing," and "connecting" should be interpreted broadly. For example, they can refer to a direct connection or an indirect connection through an intermediate medium; a fixed connection, a detachable connection, or an integrally formed connection; a mechanical connection, an electrical connection, or a connection capable of mutual communication; or the internal connection of two components or the interaction between two components. Those skilled in the art can reasonably determine the specific meaning of the above terms in this invention based on the specific content of the technical solution.
[0031] Reference Figure 1 As shown, a flexible pressure sensor structure includes: Top electrode substrate layer 1; The bottom electrode substrate layer 2 is disposed opposite to the top electrode substrate layer 1, and both the top electrode substrate layer 1 and the bottom electrode substrate layer 2 are made of PDMS thin film; The first serpentine conductive network 3 is disposed on the side of the top electrode substrate layer 1 facing the bottom electrode substrate layer 2; The second serpentine conductive network 4 is disposed on the side of the bottom electrode substrate layer 2 facing the top electrode substrate layer 1. One of the first serpentine conductive network 3 and the second serpentine conductive network 4 is arranged along the warp direction, and the other is arranged along the weft direction. The upper bonding cavity layer 5 is disposed on the inner side of the top electrode substrate layer 1; The lower adhesive cavity layer 6 is disposed inside the bottom electrode substrate layer 2. The upper adhesive cavity layer 5 and the lower adhesive cavity layer 6 each have a cavity region corresponding to the conductive layer 7 in the middle, so that the upper adhesive cavity layer 5, the lower adhesive cavity layer 6, and the upper adhesive cavity layer 5 and the lower adhesive cavity layer 6 together define an accommodating space. A conductive layer 7 is disposed within the receiving space and contacts the first serpentine conductive network 3 and the second serpentine conductive network 4. The cavity regions in the middle of the upper adhesive cavity layer 5 and the lower adhesive cavity layer 6 are located on the outer periphery of the corresponding first serpentine conductive network 3 and second serpentine conductive network 4.
[0032] Specifically, the first serpentine conductive network 3 includes multiple serpentine conductive silver wires arranged at intervals along the meridian direction, each leading to a junction port. The second serpentine conductive network 4 includes multiple serpentine conductive silver wires arranged at intervals along the parallel direction, each leading to a junction port.
[0033] Specifically, the width of each of the serpentine conductive silver wires is 0.4 to 0.6 mm, the spacing between adjacent serpentine conductive silver wires is 0.4 to 0.6 mm, the wave height and wavelength of each serpentine conductive silver wire are both 3 mm to 4 mm, the bending radius is 1.0 to 1.5 mm, and the period of each serpentine conductive silver wire is 6 to 10.
[0034] Specifically, both the upper adhesive cavity layer 5 and the lower adhesive cavity layer 6 are made of acrylic pressure-sensitive tape with a 180° peel strength of 20-30 N / cm and an elongation at break of 100%-180%. The adapter has a maximum tensile strain of 120%, and the adhesive structure can remain stable within this deformation range. It also has partial deformation recovery capability after unloading.
[0035] Specifically, the conductive layer 7 includes a porous elastic polyurethane matrix and multi-walled carbon nanotubes and conductive carbon black dispersed in the porous elastic polyurethane matrix.
[0036] Specifically, the thickness of the upper adhesive cavity layer 5 and the lower adhesive cavity layer 6 is 20 μm to 200 μm; the thickness of the conductive layer 7 is 20 μm to 200 μm; and the thickness of the top electrode substrate layer 1 and the bottom electrode substrate layer 2 is 100 μm.
[0037] With the above structure, the top electrode substrate layer 1 and the bottom electrode substrate layer 2 are made of stretchable polydimethylsiloxane elastic film. The first serpentine conductive network 3 and the second serpentine conductive network 4 can buffer stress by bending and unfolding during the stretching process, thereby reducing the risk of cracking and open circuit of the conductive line. The conductive layer 7 is made of porous elastic polyurethane matrix and compounded with multi-walled carbon nanotubes and conductive carbon black to form a composite conductive network. Under the action of external force, it produces obvious changes in the conductive path, thereby improving the resistance strain coefficient and the sensitivity of small deformation detection. The upper bonding cavity layer 5 and the lower bonding cavity layer 6 can limit, buffer and seal the conductive layer 7, reducing the influence of interlayer misalignment and water vapor and dust on the device performance.
[0038] The above-mentioned method for fabricating a flexible pressure sensor structure includes: A PDMS film is provided to form a top electrode substrate 1 and a bottom electrode substrate 2. A first serpentine conductive network 3 and a second serpentine conductive network 4 are respectively printed on one surface of the top electrode substrate 1 and the bottom electrode substrate 2 by screen printing process, and then dried and cured. Thermoplastic polyurethane powder, multi-walled carbon nanotubes and conductive carbon black are mixed and added to dimethyl sulfoxide solvent. After stirring and dispersing, a conductive slurry precursor is obtained. The conductive slurry precursor is filled into a mold and a porous foamed conductive layer 7 is prepared by freeze-drying. An acrylic pressure-sensitive tape is provided, and an upper adhesive cavity layer 5 and a lower adhesive cavity layer 6 with a cavity area in the middle are prepared by a die-cutting process. Place the bottom electrode substrate 2 with the second serpentine conductive network 4 facing upwards, place the conductive layer 7 on the side of the bottom electrode substrate 2 with the second serpentine conductive network 4, and attach the lower surface of the lower adhesive cavity layer 6 to the upper surface of the bottom electrode substrate 2, so that the lower adhesive cavity layer 6 surrounds the bottom of the conductive layer 7 and is bonded and sealed to the bottom electrode substrate 2. The lower surface of the upper adhesive cavity layer 5 is attached to the upper surface of the lower adhesive cavity layer 6, so that the upper adhesive cavity layer 5 is bonded and sealed to the lower adhesive cavity layer 6 around the top of the conductive layer 7. The top electrode substrate 1 with the first serpentine conductive network 3 is placed face down and attached to the upper surface of the upper adhesive cavity layer 5, so that the top electrode substrate 1 and the upper adhesive cavity layer 5 are bonded and sealed. The superimposed structure is then subjected to pressure and left to stand to complete the interlayer bonding.
[0039] Specifically, the drying and curing process is carried out at 60 ℃ to 80 ℃.
[0040] Specifically, the thermoplastic polyurethane powder, the multi-walled carbon nanotubes, and the conductive carbon black are mechanically stirred for 2 hours and ultrasonically dispersed for 30 minutes; the stacked structure is uniformly pressurized and held for 15 minutes, and then left to stand at room temperature for more than 24 hours.
[0041] Specifically, the multi-walled carbon nanotubes and the conductive carbon black constitute conductive carbon powder, which is composed of 10% to 30% multi-walled carbon nanotubes and 70% to 90% conductive carbon black by mass. The sum of the mass percentages of the thermoplastic polyurethane powder and the conductive carbon powder is 100%, with the thermoplastic polyurethane powder accounting for 80% to 95% by mass and the conductive carbon powder accounting for 5% to 20% by mass. The thermoplastic polyurethane powder has a particle size of 100 nm to 10 μm; the multi-walled carbon nanotubes have a diameter of 2 nm to 100 nm; and the conductive carbon black is at least one of acetylene black, Ketjen black, and pigment black.
[0042] Example 1 Step 1: Prepare the top electrode substrate layer 1 and the bottom electrode substrate layer 2. A polydimethylsiloxane elastic film with a thickness of 100 μm and an external dimension of 50 mm × 50 mm is selected as the substrate material. The polydimethylsiloxane elastic film has good tensile strength, flexibility and interfacial adhesion.
[0043] Conductive silver paste lines were printed onto the surfaces of two polydimethylsiloxane elastic films using screen printing to form a first serpentine conductive network 3 arranged along the warp direction and a second serpentine conductive network 4 arranged along the weft direction. Each serpentine conductive silver line has a width of 0.5 mm, a spacing of 0.5 mm between adjacent lines, a wave height and wavelength of 4 mm, a bending radius of 1.2 mm, and a cycle of 8 lines. After printing, the polydimethylsiloxane elastic films were cured in a 60 ℃ constant temperature oven for 30 min to ensure a firm bond between the conductive silver lines and the films, thus obtaining the top electrode substrate layer 1 and the bottom electrode substrate layer 2.
[0044] Step 2: Prepare the conductive paste and fabricate the conductive layer 7. Weigh thermoplastic polyurethane powder, multi-walled carbon nanotubes, and acetylene black according to a mass ratio of 85:3:12. The thermoplastic polyurethane powder has a particle size of 1 μm, the multi-walled carbon nanotubes have a diameter of 20 nm, and acetylene black is used as the conductive carbon black filler.
[0045] The thermoplastic polyurethane powder, multi-walled carbon nanotubes, and acetylene black were added to dimethyl sulfoxide solvent, mechanically stirred for 2 h, and ultrasonically dispersed for 30 min to uniformly disperse the multi-walled carbon nanotubes and acetylene black in the thermoplastic polyurethane system, thereby obtaining a conductive paste precursor with a solid content of 15%.
[0046] A soft template removal method was used to fill the cavity of a pre-set soft template with the conductive slurry precursor, ensuring full filling and a smooth surface. The filled soft template was then placed in a freeze-drying apparatus and freeze-dried under vacuum and low temperature conditions to completely remove dimethyl sulfoxide and the soft template, resulting in a porous foamed conductive layer 7 with a thickness of 100 μm and dimensions of 50 mm × 50 mm. (Refer to...) Figure 2 As shown, the conductive layer 7 has continuously distributed micron-sized pores inside, with multi-walled carbon nanotubes and acetylene black attached and dispersed on the pore walls of the thermoplastic polyurethane. The pores are used to improve the compressibility, stretchability and deformation recovery ability of the conductive layer 7.
[0047] Step 3: Device Layer Assembly and Sealing. A 60 μm thick acrylic pressure-sensitive tape is selected and die-cut to form the upper adhesive cavity layer 5 and the lower adhesive cavity layer 6. The bottom electrode substrate layer 2, the lower adhesive cavity layer 6, the conductive layer 7, the upper adhesive cavity layer 5, and the top electrode substrate layer 1 are stacked sequentially from bottom to top. During stacking, the second serpentine conductive network 4 faces upwards, the first serpentine conductive network 3 faces downwards, and the conductive layer 7 is positioned within the cavity regions of the upper adhesive cavity layer 5 and the lower adhesive cavity layer 6.
[0048] After lamination, pressure is uniformly applied to the device under normal temperature and pressure and held for 15 minutes. Then, it is left to stand at room temperature for more than 24 hours to allow the acrylic pressure-sensitive adhesive to fully bond. The upper bonding cavity layer 5 and the lower bonding cavity layer 6 form a sealing structure around the edge of the conductive layer 7 to isolate external moisture and dust and limit the relative displacement between layers.
[0049] Step 4: Performance Testing. The tensile properties, resistance strain coefficient, and cyclic stability of the fabricated flexible pressure sensor structure are tested. The resistance strain coefficient is calculated using the following formula: ; In the formula, The resistance strain coefficient, This represents the change in resistance before and after loading. The initial resistance of the device. The strain is the strain generated during the loading process; in tensile performance testing, the strain is tensile strain, and in compressive performance testing, the strain is compressive strain.
[0050] Test results show that the ultimate tensile strength of the flexible pressure sensor structure fabricated in this embodiment is 120%, and the resistance strain coefficient is 65. After 1000 cycles of tensile testing, the output signal offset of the device is 8%, and all performance characteristics remain stable. (Refer to...) Figure 3 As shown, as the pressure increases, the absolute value of the resistance change rate increases rapidly in the low-pressure region and then gradually stabilizes, indicating that the conductive layer 7 has a significant resistance response in the low-pressure region and maintains continuous output under higher pressure.
[0051] Example 2 The overall preparation process, equipment, and operating environment of this embodiment are the same as those of Example 1, with only the conductive powder ratio, slurry solid composition, and thermoplastic polyurethane powder parameters being adjusted.
[0052] The conductive carbon powder is composed of multi-walled carbon nanotubes and conductive carbon black, wherein multi-walled carbon nanotubes account for 10% of the mass of the conductive carbon powder, and conductive carbon black accounts for 90% of the mass of the conductive carbon powder; the sum of the mass ratios of thermoplastic polyurethane powder and conductive carbon powder is 100%, with conductive carbon powder accounting for 10% and thermoplastic polyurethane powder accounting for 90%. The particle size of the thermoplastic polyurethane powder is 500 nm. The remaining electrode substrate preparation, slurry dispersion, freeze-drying, soft template removal, and layer assembly and sealing processes are all performed according to Example 1.
[0053] Performance test results show that the ultimate tensile strength of the flexible pressure sensor structure prepared in this embodiment is 110%, and the resistance strain coefficient is 55. After completing 1000 cycles of tensile testing, the output signal offset is 9%, and the device has good tensile stability and sensing consistency.
[0054] Finally, it should be noted that the above specific embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A flexible pressure sensor structure, characterized in that, include: Top electrode substrate (1); The bottom electrode substrate (2) is disposed opposite to the top electrode substrate (1), and both the top electrode substrate (1) and the bottom electrode substrate (2) are made of PDMS thin film; A first serpentine conductive network (3) is disposed on the side of the top electrode substrate layer (1) facing the bottom electrode substrate layer (2); The second serpentine conductive network (4) is disposed on the side of the bottom electrode substrate layer (2) facing the top electrode substrate layer (1). One of the first serpentine conductive network (3) and the second serpentine conductive network (4) is arranged along the meridian direction, and the other is arranged along the parallel direction. An upper bonding cavity layer (5) is disposed on the inner side of the top electrode substrate layer (1); The lower bonding cavity layer (6) is disposed inside the bottom electrode substrate layer (2). The upper bonding cavity layer (5) and the lower bonding cavity layer (6) are both provided with cavity regions corresponding to the conductive layer (7) in the middle, so that the upper bonding cavity layer (5), the lower bonding cavity layer (6), and the upper bonding cavity layer (5) and the lower bonding cavity layer (6) together define the accommodating space. A conductive layer (7) is disposed within the accommodating space and contacts the first serpentine conductive network (3) and the second serpentine conductive network (4).
2. The flexible pressure sensor structure according to claim 1, characterized in that, The first serpentine conductive network (3) includes multiple serpentine conductive silver wires arranged at intervals along the meridian direction, and the second serpentine conductive network (4) includes multiple serpentine conductive silver wires arranged at intervals along the parallel direction.
3. The flexible pressure sensor structure according to claim 2, characterized in that, The width of each of the serpentine conductive silver wires is 0.4 to 0.6 mm, the spacing between adjacent serpentine conductive silver wires is 0.4 to 0.6 mm, the wave height and wavelength of each serpentine conductive silver wire are 3 mm to 4 mm, the bending radius is 1.0 to 1.5 mm, and the period of each serpentine conductive silver wire is 6 to 10.
4. The flexible pressure sensor structure according to claim 1, characterized in that, Both the upper adhesive cavity layer (5) and the lower adhesive cavity layer (6) are made of acrylic pressure-sensitive tape. The 180° peel strength of the acrylic pressure-sensitive tape is 20-30 N / cm, and the elongation at break is 100%-180%.
5. The flexible pressure sensor structure according to claim 1, characterized in that, The conductive layer (7) includes a porous elastic polyurethane matrix and multi-walled carbon nanotubes and conductive carbon black dispersed in the porous elastic polyurethane matrix.
6. The flexible pressure sensor structure according to claim 1, characterized in that, The thickness of the upper bonding cavity layer (5) and the lower bonding cavity layer (6) is 20 μm to 200 μm; the thickness of the conductive layer (7) is 20 μm to 200 μm; the thickness of the top electrode substrate layer (1) and the bottom electrode substrate layer (2) is 100 μm.
7. A method for fabricating a flexible pressure sensor structure, characterized in that, include: A PDMS film is provided to form a top electrode substrate (1) and a bottom electrode substrate (2). A first serpentine conductive network (3) and a second serpentine conductive network (4) are respectively printed on one surface of the top electrode substrate (1) and the bottom electrode substrate (2) by screen printing process, and then dried and cured. Thermoplastic polyurethane powder, multi-walled carbon nanotubes and conductive carbon black are mixed and added to dimethyl sulfoxide solvent. After stirring and dispersing, a conductive slurry precursor is obtained. The conductive slurry precursor is filled into a mold and a porous foamed conductive layer is prepared by freeze drying process. (7) An acrylic pressure-sensitive tape is provided, and an upper adhesive cavity layer (5) and a lower adhesive cavity layer (6) with a cavity area in the middle are prepared by a die-cutting process. Place the bottom electrode substrate (2) with the side having the second serpentine conductive network (4) facing upwards, place the conductive layer (7) on the side of the bottom electrode substrate (2) with the second serpentine conductive network (4), and attach the lower surface of the lower adhesive cavity layer (6) to the upper surface of the bottom electrode substrate (2), so that the lower adhesive cavity layer (6) surrounds the bottom of the conductive layer (7) and is bonded and sealed to the bottom electrode substrate (2). The lower surface of the upper adhesive cavity layer (5) is attached to the upper surface of the lower adhesive cavity layer (6) so that the upper adhesive cavity layer (5) is bonded and sealed to the lower adhesive cavity layer (6) around the top of the conductive layer (7). Place the top electrode substrate layer (1) with the first serpentine conductive network (3) facing down and attach it to the upper surface of the upper adhesive cavity layer (5) so that the top electrode substrate layer (1) and the upper adhesive cavity layer (5) are bonded and sealed. The superimposed structure is then subjected to pressure and left to stand to complete the interlayer bonding.
8. The method for fabricating a flexible pressure sensor structure according to claim 7, characterized in that, During drying and curing, the temperature should be between 60 ℃ and 80 ℃.
9. The method for fabricating a flexible pressure sensor structure according to claim 7, characterized in that, The thermoplastic polyurethane powder, the multi-walled carbon nanotubes, and the conductive carbon black were mechanically stirred for 2 h and ultrasonically dispersed for 30 min. The stacked structure was uniformly pressurized and held for 15 min, and then allowed to stand at room temperature for more than 24 h.
10. The method for fabricating a flexible pressure sensor structure according to claim 7, characterized in that, The multi-walled carbon nanotubes and the conductive carbon black constitute conductive carbon powder. The conductive carbon powder is composed of 10% to 30% multi-walled carbon nanotubes and 70% to 90% conductive carbon black by mass. The sum of the mass percentages of the thermoplastic polyurethane powder and the conductive carbon powder is 100%, with the thermoplastic polyurethane powder accounting for 80% to 95% by mass and the conductive carbon powder accounting for 5% to 20% by mass. The thermoplastic polyurethane powder has a particle size of 100 nm to 10 μm; the multi-walled carbon nanotubes have a diameter of 2 nm to 100 nm; and the conductive carbon black is at least one of acetylene black, Ketjen black, and pigment black.