Method for detecting copper and zinc content in high-nickel ternary precursor
By employing a stepwise elution technique using chelated resin microcolumns, the problems of matrix inhibition and zinc loss in the detection of copper and zinc in high-nickel ternary precursors have been solved, achieving efficient and accurate determination of copper and zinc content, which is suitable for the detection of high-nickel ternary precursors.
Patent Information
- Application Number
- CN202611303132.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies for detecting copper and zinc in high-nickel ternary precursors suffer from matrix inhibition effects and zinc loss, resulting in inaccurate detection results and cumbersome operation, making it difficult to meet the accurate detection requirements for trace copper and zinc in high-nickel ternary precursors.
The high-nickel ternary precursor material was fully adsorbed using a chelating resin microcolumn, and then eluted stepwise with eluents of different acidities. Zinc- and copper-containing eluent fractions were collected separately, and the contents of copper and zinc were determined using ICPOES.
It effectively avoids matrix inhibition effects and zinc loss, improves the accuracy and efficiency of detection, significantly reduces the detection limit, and meets the needs for accurate detection of trace copper and zinc in high-nickel ternary precursors.
Smart Images

Figure SMS_7 
Figure SMS_8 
Figure SMS_9
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery cathode material detection technology, and more specifically, to a method for detecting the copper and zinc content in a high-nickel ternary precursor. Background Technology
[0002] High-nickel ternary precursors (NCM / NCA) are key precursors for lithium-ion battery cathode materials. Copper (Cu) and zinc (Zn) are critical trace impurities in the finished product, typically requiring control at the ppm level (e.g., ≤10-50 ppm). Excessive content can lead to micro-short circuits and capacity decay in the battery. Therefore, accurate determination of copper and zinc content is crucial for product quality control. However, after digestion of high-nickel ternary precursors, Ni... 2+ Concentrations can reach thousands to tens of thousands of mg / L. High concentrations of nickel, cobalt, and manganese matrices can cause severe spectral and non-spectral interference in ICP-OES analysis, leading to inaccurate copper and zinc detection results. Therefore, copper and zinc need to be separated and enriched before determination. Currently, the mainstream detection method is the ammonia precipitation-co-precipitation separation and enrichment method. Its principle is: in an ammonia buffer system, Ni... 2+ Co 2+ Mn 2+ It forms a soluble ammonia complex that remains in solution, while Cu 2+ Zn 2+ Then with the added Fe 3+ Or La 3+ Co-precipitation occurs as hydroxides, thus separating copper and zinc from the high-nickel matrix. The precipitate is then dissolved and analyzed by ICP-OES. However, this method still has significant limitations: when nickel concentrations are extremely high, a large amount of nickel-ammonia complexes are easily encapsulated or adsorbed into the precipitate, resulting in a small amount of nickel remaining in the test solution. This creates a matrix inhibition effect on copper and zinc determination, affecting accuracy. Furthermore, zinc partially forms [Zn(NH3)4] in ammoniacal media. 2+ Ammonium complex ions remain in the supernatant, causing zinc loss during the co-precipitation process, resulting in lower measurement results. In addition, the method involves multiple steps such as precipitation, centrifugation, washing, and resolution, which is time-consuming and introduces a high risk of contamination and loss, making it difficult to meet the needs of accurate and efficient determination of trace copper and zinc in high-nickel ternary precursors.
[0003] In view of this, the present invention is proposed. Summary of the Invention
[0004] The purpose of this invention is to provide a method for detecting the copper and zinc content in a high-nickel ternary precursor. This method involves selectively separating copper and zinc elements from a high-nickel matrix in a quantitative solution to obtain a dilute acid solution rich in copper and zinc, followed by ICP-based detection. OES assay completely eliminates matrix inhibition.
[0005] This invention is implemented as follows: This invention provides a method for detecting the copper and zinc content in a high-nickel ternary precursor, comprising the following steps: The high-nickel ternary precursor material was digested and diluted to a final volume to obtain a sample solution, which was then subjected to full adsorption through a chelating resin microcolumn. The chelating resin was eluted stepwise using eluents with different acidities, and zinc-containing and copper-containing eluent fractions were collected separately. ICP was performed on the zinc-containing and copper-containing eluent fractions, respectively. OES determination, and calculation of the copper and zinc content in the precursor material based on the test results.
[0006] In an optional embodiment, the digestion solution used is a nitric acid solution with a concentration of 5.0-7.0 mol / L, the digestion temperature is 200-300℃, and the digestion time is 10-30 min.
[0007] In an optional embodiment, the high-nickel ternary precursor material is nickel cobalt manganese hydroxide or nickel cobalt aluminum hydroxide.
[0008] In an optional embodiment, the sample solution is adjusted to pH 6.0 after being brought to volume; the flow rate of the sample solution through the chelating resin microcolumn is 1.0-2.0 mL / min.
[0009] In an optional embodiment, the chelating resin microcolumn is further rinsed with a buffer solution at pH 6.0 after the full adsorption.
[0010] In an optional embodiment, the chelating resin is Chelex-100 chelating resin.
[0011] In an optional embodiment, the eluent flows through the chelating resin microcolumn at a rate of 1.0-2.0 mL / min.
[0012] In an optional implementation, the stepwise elution includes the following steps: First elution step: Elute with nitric acid solution with pH 3.4-3.6, and discard the eluent; Second elution step: Elution is performed using a nitric acid solution with a pH of 2.2-2.4, and the zinc-containing eluent fraction is collected; Third elution step: Elute with nitric acid solution with pH 1.6-1.8, and discard the eluent; Fourth elution step: Elution was performed using a 2.0 mol / L nitric acid solution, and the copper-containing eluent fraction was collected.
[0013] In an optional implementation, the ICP OES determination includes: shaking the elution fractions separately, filtering, and using the filtrate as the test solution; preparing a blank solution with the same matrix as the test solution; and performing ICP-based analysis. OES technology is used to determine the concentrations of copper and zinc ions in the test solution and the blank solution; the content of copper and zinc in the precursor material is then calculated.
[0014] In an optional embodiment, the oscillation time is 2-4 hours; the filter membrane used for filtration is a 0.22 μm or 0.45 μm aqueous filter membrane.
[0015] The present invention has the following beneficial effects: This invention utilizes chelating resin microcolumns for selective adsorption and stepwise elution of copper and zinc, effectively avoiding the matrix inhibition effect of residual nickel on ICP-OES detection in the ammonia precipitation method and the risk of zinc loss due to the formation of ammonium complex ions in the ammoniatic medium. The spiked recoveries of copper and zinc can reach over 95%. Furthermore, a single pretreatment is sufficient to obtain zinc- and copper-containing eluted fractions after matrix removal, eliminating the need for repeated dilution or multiple pretreatments, making the operation simple and efficient. In addition, this invention effectively eliminates spectral and non-spectral interferences from high-nickel matrices, significantly reducing the detection limit and meeting the requirements for accurate detection of trace copper and zinc in high-nickel ternary precursors. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0017] To address the technical problems of poor detection limits and inaccurate results caused by the easy co-precipitation of nickel leading to matrix inhibition and the easy formation of ammonium complex ions by zinc in existing ammonia precipitation methods, the inventors utilized the differences in the affinity of chelating resins for metal ions at specific pH levels. By using elution solutions with different acidities, ppm-level copper and zinc were selectively separated from g / L-level high-nickel matrices, followed by ICP-OES determination. This completely eliminated matrix interference, avoided the loss of copper and zinc, effectively reduced the detection limit, and significantly improved detection accuracy.
[0018] This invention provides a method for detecting the copper and zinc content in a high-nickel ternary precursor, comprising the following steps: S1. Digest and dilute the high-nickel ternary precursor material to obtain a sample solution, and then perform full adsorption of the sample solution through a chelating resin microcolumn. S2. The chelating resin is eluted stepwise using eluents with different acidities, and the zinc-containing eluent fraction and the copper-containing eluent fraction are collected separately. S3. Perform ICP on the zinc-containing eluent and the copper-containing eluent, respectively. OES determination, and calculation of the copper and zinc content in the precursor material based on the test results.
[0019] In some preferred embodiments, the digestion solution used is a nitric acid solution with a concentration of 5.0-7.0 mol / L, such as 5.0 mol / L, 5.5 mol / L, 6.0 mol / L, 6.5 mol / L, or 7.0 mol / L, preferably a 6.0 mol / L dilute nitric acid solution; the digestion temperature is 200-300℃, such as 200℃, 220℃, 240℃, 260℃, 280℃, or 300℃, preferably 240℃; the digestion time is 10-30 min, such as 10 min, 15 min, 20 min, 25 min, or 30 min.
[0020] This application reveals that the affinity of chelating resins for metal ions under dilute nitric acid conditions follows the order Cu². + >Ni² + >Zn² + Co² + >Mn² + As a non-coordinate anion, nitrate ions do not form stable complexes with metal ions, which is conducive to the complete release of metal ions from the active sites of the resin, ensuring elution efficiency and recovery rate. At the same time, the nitric acid system introduces less matrix interference in ICP-OES detection, and nitric acid is the most commonly used acid medium in ICP-OES analysis. The elution fraction can be directly injected for determination without additional conversion medium, making the operation simpler.
[0021] Furthermore, in some embodiments of this application, the detection method is mainly applicable to undoped high-nickel ternary precursors, such as nickel-cobalt-manganese hydroxide or nickel-cobalt-aluminum hydroxide. The matrix composition of the high-nickel ternary precursor is clear, and the affinity sequence of the chelating resin for Ni, Co, and Mn / Al is clear. The stepwise separation of copper and zinc from the matrix can be achieved by controlling the acidity of the eluent.
[0022] In some preferred embodiments, in step S1, the sample solution is adjusted to pH 6.0 after being brought to volume, and then passed through the chelating resin microcolumn at a flow rate of 1.0~2.0 mL / min for total adsorption. pH 6.0 is the optimal pH range for the chelating resin to adsorb transition metal ions; under these conditions, Cu²⁺ in the solution… + Zn² + Ni² + Co²+ Mn² + All of them can be quantitatively adsorbed by the chelating resin microcolumn, ensuring that the target elements copper and zinc, as well as the matrix elements nickel, cobalt, and manganese, are completely retained on the resin, laying the foundation for subsequent stepwise elution and separation.
[0023] Preferably, the chelating resin is Chelex-100 chelating resin. It should be noted that the pretreatment method of the Chelex-100 resin is as follows: the resin is rinsed sequentially with 2.0 mol / L nitric acid solution and deionized water, and then equilibrated with a pH 6.0 buffer solution for later use.
[0024] In some preferred embodiments, the flow rate of the eluent through the chelating resin microcolumn is 1.0-2.0 mL / min, preferably 1.0 mL / min. Controlling the eluent flow rate within the above range ensures sufficient contact between the eluent and the active sites of the resin, allowing for complete desorption of the target element, while avoiding excessively slow flow rates that would lead to prolonged analysis time, thus balancing separation efficiency and separation effect.
[0025] Specifically, the stepwise elution described in this application includes the following steps: First elution step: Use a nitric acid solution with a pH of 3.4-3.6 (nitric acid concentration approximately 3.16 × 10⁻⁶). -4 Elution was performed using a solution of mol / L, and the effluent was discarded. This step mainly removes the Co²⁺ co-adsorbed on the resin. + and Mn² + Removed by elution from chelating resin, while Cu² + Zn² + and Ni² + It remains on the resin, thus achieving the initial separation of the Co / Mn matrix from the target element.
[0026] The second elution step: Use a nitric acid solution with a pH of 2.2-2.4 (nitric acid concentration approximately 5.01 × 10⁻⁶). - Elution was performed using a solution of 3 mol / L, and the zinc-containing eluent fraction was collected. Under these acidity conditions, Zn²⁺ + The binding force with chelating resin is weak, so it is preferentially eluted, while Cu² + and Ni² + It remains on the resin, thus achieving the separation of zinc from copper and residual nickel.
[0027] The third elution step: Use a nitric acid solution with a pH of 1.6-1.8 (acid concentration approximately 2.00 × 10⁻⁶). - Elution was performed using Ni² mol / L, and the eluent was discarded. This step utilizes Ni² + The property of quantitative elution from the resin under low pH conditions allows for the removal of Ni² adsorbed on the resin. +Peeling and removal, while Cu² + It has a strong binding force with the resin and remains on the resin even at this acidity, thus completely eliminating the interference of the high-nickel matrix on subsequent copper determination.
[0028] Fourth elution step: Elution was performed using a 2.0 mol / L nitric acid solution (corresponding to a pH of approximately -0.3), and the copper-containing eluent fraction was collected. Under higher acidity, Cu²⁺… + The fraction is completely eluted from the resin, and the distillate is collected to obtain a pure copper-rich dilute acid solution.
[0029] It should be noted that the eluent volume in each elution step is calculated based on the bed volume (BV) of the chelating resin microcolumn. The formula for calculating the bed volume is as follows: BV (mL) = π × r 2 × h, Where r is the inner diameter radius of the microcolumn (cm) and h is the height of the resin-filled bed inside the column (cm).
[0030] In this invention, since the chelation exchange reaction rate between metal ions and the functional groups of the chelating resin is relatively slow, sufficient liquid phase volume and resin bed contact time are required to ensure that the exchange reaction tends to be complete. At the same time, increasing the amount of eluent is also beneficial to fully wash out the interfering matrix components that are physically adsorbed or non-specifically bound in the column, and to completely replace the target metal ions from the active sites of the resin into the collection phase. Therefore, the amount of eluent is not less than 10 times the column volume (≥10 BV).
[0031] In practical applications, the dosage can be appropriately increased based on 10 times the column volume, depending on the packing compactness, particle size distribution, and chelating affinity of different batches of resin. This ensures that residual interfering ions on the column are completely removed or the target analyte is completely eluted. The elution endpoint is determined by the absence of target ions in the receiving solution or by the residual interfering ions being below the set threshold.
[0032] Preferably, the amount of eluent used in each elution step can be adjusted according to the column volume of the chelating resin microcolumn to ensure complete elution or removal of each metal ion. For example, when using a chelating resin microcolumn with a column volume of 1.5-2.0 mL, the amount of eluent used in the first elution step is 30 mL, in the second elution step is 40 mL, in the third elution step is 30 mL, and in the fourth elution step is 30 mL.
[0033] In some preferred embodiments, the zinc-containing and copper-containing elution fractions collected in step S2 are shaken separately to ensure thorough mixing, then filtered through a filter membrane, and the filtrate is used as the test solution. Simultaneously, a blank solution with the same matrix as the test solution is prepared to eliminate background interference introduced by reagents and glassware. ICP is then used separately. OES technology was used to determine the concentrations of copper and zinc ions in the test solution and the blank solution, recording the emission spectral intensity of each element. The concentrations of copper and zinc in the test solution were calculated using the standard curve method or the standard addition method. Finally, based on the sample mass, final volume, and dilution factor, the copper and zinc content in the high-nickel ternary precursor material was calculated.
[0034] The copper and zinc content in the high-nickel ternary precursor material is calculated using the following formula:
[0035] Where C is the content of the element to be tested in the sample, in μg / g; c is the mass concentration of the element to be tested in the test solution obtained from the standard curve, in μg / mL; c0 is the mass concentration of the element to be tested in the blank solution, in μg / mL; V is the final volume of the test solution, in mL; f is the dilution factor; and m is the sample mass, in g.
[0036] Preferably, the shaking time is 2-4 h to ensure that the eluted fraction is fully homogenized; the filter membrane used for filtration is a 0.22 μm or 0.45 μm aqueous filter membrane to remove any small particles that may be present in the solution, prevent clogging of the ICP-OES nebulizer, and ensure the stability of the sample introduction system and the accuracy of the measurement results.
[0037] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0038] Example 1 Static Adsorption Test (1) Preparation of simulated sample solution Preparation of simulated high-nickel ternary precursor matrix solution: using Ni² + Co² + Mn² + The matrix is composed of Ni (500 mg / L), Co (50 mg / L), and Mn (50 mg / L); Cu²⁺ is added to it. + and Zn² + The target trace elements were all at a concentration of 1.0 mg / L. The pH of the solution was adjusted to 6.0 using dilute nitric acid or ammonia.
[0039] (2) Test methods Weigh 0.5 g of the pretreated Chelex-100 chelating resin into five conical flasks, and add 50 mL of the simulated sample solution (containing a mixture of Cu, Zn, Ni, Co, and Mn metal ions) to each flask. Adjust the pH of each flask to a different value using dilute nitric acid (flask A: pH 6.0; flask B: pH 3.5; flask C: pH 2.3; flask D: pH 1.7; flask E: 2.0 mol / L nitric acid). Shake at 25°C for 2-4 hours to ensure sufficient contact between the resin and the solution, reaching adsorption / desorption equilibrium. After oscillation, the solution was filtered, and the residual concentrations of Cu, Zn, Ni, Co, and Mn in the filtrate were determined using an inductively coupled plasma optical emission spectrometer (ICP-OES, model: Thermo iCAP Pro X). The instrument operating conditions were as follows: RF power 1150 W, auxiliary gas flow rate 0.5 L / min, nebulizing gas flow rate 0.5 L / min, cooling gas flow rate 12 L / min, analytical pump speed 50 r / min, horizontal observation, Cu detection wavelength 324.754 nm, Zn detection wavelength 206.2 nm (the detection wavelengths of Ni, Co, and Mn were set according to the instrument's recommended conditions). The adsorption or desorption behavior of each metal ion on the resin under different pH conditions was evaluated by calculating the residual rate or desorption rate of each element in the solution, as shown in Table 1.
[0040] Table 1. Detection results of concentration of each element
[0041] Table 1 shows that the residual concentrations of all elements in the filtrate of bottle A (pH 6.0) are extremely low, and the adsorption rates of Cu, Zn, Ni, Co, and Mn are all greater than 95%, indicating that under this pH condition, Chelex-100 resin has excellent adsorption capacity for the above five metal ions and can achieve quantitative total adsorption. In bottle B (pH 3.5), the concentrations of Co and Mn in the filtrate are significantly increased, and the desorption rates are both greater than 80%, while the residual concentrations of Cu, Zn, and Ni are still very low, indicating that under this acidity, Co²⁺… + and Mn² + Selectively eluted, while Cu² + Zn² + and Ni² + The Zn concentration in the filtrate of bottle C (pH 2.3) increased significantly, with a desorption rate greater than 75%, while the residual concentrations of Cu and Ni remained very low, indicating that Zn²⁺ remained on the resin. + Selectively eluted, while Cu² + and Ni² + The Ni concentration in the filtrate of bottle D (pH 1.7) increased sharply, with a desorption rate greater than 80%, while the residual Cu concentration remained at 0.0 mg / L, indicating that Ni²⁺ remained on the resin.+ It was quantitatively eluted, while Cu² + The Cu concentration in the filtrate of bottle E (2.0 mol / L nitric acid) increased significantly, with a desorption rate greater than 95%, indicating that Cu²⁺ remained on the resin. + They were completely eluted. This demonstrates that different metal ions exhibit drastically different adsorption / desorption behaviors under different pH conditions, fully proving that the affinity of Chelex-100 resin for different metal ions can be precisely controlled by acidity.
[0042] The above results indicate that Chelex-100 chelating resin has a strong effect on Cu²⁺ chelation in nitric acid systems. + Zn² + Ni² + Co² + Mn² + The affinity order is Cu² + >Ni² + >Zn² + Co² + >Mn² + Based on this affinity difference, selective stepwise elution of various metal ions can be achieved by precisely controlling the acidity (pH value) of the eluent: removing the Co / Mn matrix at pH 3.5, selectively collecting Zn at pH 2.3, stripping a large amount of Ni matrix at pH 1.7, and finally completely recovering Cu with 2.0 mol / L nitric acid, thus proving the feasibility and technical reliability of the stepwise elution scheme described in this application.
[0043] Example 2: Accuracy and Precision Comparison Test (1) Sample preparation Approximately 0.2 g of each of the 8-series and 9-series high-nickel ternary precursor samples were accurately weighed and placed in a digestion vessel. 15 mL of a 1:1 volume ratio of dilute nitric acid (approximately 6 mol / L) was added, and the mixture was heated at 240°C on a hot plate until completely dissolved. After cooling to room temperature, the solution was diluted to a 200 mL volumetric flask with 2% nitric acid solution to obtain the sample digest. The digest was divided into two groups, A and B. Group A was analyzed using the chelation resin separation-ICP-OES method described in this application, while Group B was analyzed using the ammonia precipitation-coprecipitation separation-ICP-OES method.
[0044] (2) Spiked recovery test Digested samples from groups A and B were used to prepare three parallel samples: a background group (no standard solution added), a low-concentration spiked group (Cu and Zn spiked at 0.5 mg / L each), and a high-concentration spiked group (Cu and Zn spiked at 1.0 mg / L each). Three replicates were prepared for each spike level. Group A samples were subjected to adsorption and stepwise elution using a chelating resin microcolumn, followed by ICP-OES determination of copper and zinc concentrations. Group B samples were enriched by ammonia coprecipitation, and then ICP-OES determination of copper and zinc concentrations was performed. The recoveries and relative standard deviations (RSDs) were calculated based on the results at each spike level to evaluate the accuracy and precision of the two methods. The results are shown in Table 2.
[0045] Table 2. Results of spiked recovery determination for resin method and ammonia precipitation method
[0046] Statistical analysis was performed on the recoveries of the two methods at various spiking levels, and the average recovery, standard deviation (SD), and relative standard deviation (RSD) were calculated. The results are shown in Table 3.
[0047] Table 3. Statistical comparison of recovery rates between resin method and ammonia precipitation method
[0048] Table 3 shows that the resin method achieved an average recovery rate of 97.76% for copper and 98.98% for zinc; while the ammonia precipitation method achieved an average recovery rate of only 88.38% for copper and only 90.37% for zinc. The average recoveries of copper and zinc by the resin method are significantly higher than those by the ammonia precipitation method, indicating that the method described in this application has higher accuracy. Regarding precision, the RSDs for copper and zinc determination by the resin method are 1.82% and 1.70%, respectively, both lower than the 2.08% and 1.91% of the ammonia precipitation method, indicating that the precision of the resin method is also superior to that of the ammonia precipitation method. Therefore, the chelation resin separation-ICP-OES method described in this application demonstrates significantly higher spiked recoveries and lower relative standard deviations than the existing ammonia precipitation method in the detection of copper and zinc content in high-nickel ternary precursors, proving that this method is superior to the traditional ammonia precipitation-coprecipitation separation method in both accuracy and precision, and can meet the requirements for accurate detection of trace copper and zinc in high-nickel ternary precursors.
[0049] Example 3 Verification of interference elimination effect on high-nickel substrate (1) Sample preparation Take approximately 0.2 g of an actual sample of a 9-series or 8-series high-nickel ternary precursor (e.g., Ni0.8Co0.1Mn0.1(OH)2), weigh it accurately, and place it in a digestion container. Add 15 mL of a 1:1 volume ratio of dilute nitric acid (approximately 6 mol / L), and heat on a hot plate at 240°C until completely dissolved. After cooling to room temperature, dilute to a 200 mL volumetric flask with 2% nitric acid solution to obtain the sample digest. Add Cu and Zn standard solutions to the digest to ensure that the theoretical spiking value is 1.00 mg / L for both.
[0050] (2) Experimental grouping The above-mentioned spiked sample digests were divided into four groups, with three parallel samples in each group. Each group underwent ICP-OES analysis after different pretreatment methods. Group ① is the direct dilution test group: the sample digestion solution is directly diluted with 2% nitric acid and then injected for measurement without any matrix separation treatment, which is used to verify the degree of physical interference of the high nickel matrix on the measurement of copper and zinc.
[0051] Group ② is the matrix matching test group: When preparing the standard curve, a mixed matrix solution of Ni, Co and Mn with a concentration equivalent to that of the sample digestion solution is added to match the standard curve with the sample matrix before injection and measurement. This is used to verify whether the matrix matching method can effectively correct spectral interference and differences in atomization efficiency.
[0052] Group ③ is the chelating resin separation group: using the method described in this application, the sample digest was subjected to total adsorption through a Chelex-100 chelating resin microcolumn, and then eluted stepwise according to the steps of removing Co / Mn at pH 3.5, collecting Zn at pH 2.3, removing Ni at pH 1.7, and collecting Cu with 2.0 mol / L nitric acid. After collecting the zinc- and copper-containing eluted fractions, ICP-OES analysis was performed to verify the elimination effect of the chelating resin method on matrix interference.
[0053] Group ④ is the ammonia coprecipitation separation group: the traditional ammonia precipitation-coprecipitation separation method was used for pretreatment, and the precipitate was dissolved and then subjected to ICP-OES determination to compare and evaluate the advantages of the method in this application compared with the traditional method. The results are shown in Table 4.
[0054] Table 4. Effects of different pretreatment methods on the determination of copper and zinc in high-nickel matrices
[0055] Table 4 shows that in Group ①, the direct dilution method, the measured values of copper and zinc were 0.65 mg / L and 0.73 mg / L, respectively, with relative errors of -35% and -27%, indicating that the high-nickel matrix has a significant negative interference (matrix inhibition effect) on the ICP-OES determination of copper and zinc, and the conventional dilution method cannot effectively eliminate this interference. In Group ②, the matrix matching method, although the measurement results were improved by adding Ni, Co, and Mn matrices to the standard curve for correction (the relative errors of copper and zinc decreased to -12% and -18%, respectively), the results were still significantly low due to the difference in physical atomization efficiency caused by the high-salt matrix and the memory effect of the injection system, which could not meet the accuracy requirements of trace analysis. In the fourth group of ammonia coprecipitation separation methods, the measured values of copper and zinc were 0.89 mg / L and 0.91 mg / L, respectively, with relative errors of -11% and -9%. Although this was an improvement over the direct dilution method, the recovery rate was only about 89%~91%. This is presumably due to residual nickel being encapsulated and coprecipitated under the high-nickel matrix, leading to matrix inhibition, and zinc being lost due to the formation of ammonium complex ions in the ammonia medium. In the third group of chelating resin separation methods, the measured values of copper and zinc were 0.98 mg / L and 0.99 mg / L, respectively, with relative errors of -2% and -1%. The spiked recoveries reached 98% and 99%, respectively, with RSDs of 2.33% and 1.33%, respectively. This indicates that after separation by gradient elution with chelating resin, the spectral and non-spectral interferences of the high-nickel matrix were completely eliminated, and the measured results were in high agreement with the theoretical spiked values.
[0056] The above results indicate that the high concentrations of Ni, Co, and Mn in the high-nickel ternary precursor matrix have a significant matrix inhibition effect on the determination of copper and zinc by ICP-OES. Conventional direct dilution methods and matrix matching methods cannot effectively eliminate this interference. The chelating resin separation method described in this application selectively separates and enriches copper and zinc from the high-nickel matrix, completely eliminating matrix interference. The spiked recovery rate reaches 98%~99%, which is significantly better than the direct dilution method (65%~73% recovery rate), the matrix matching method (82%~88% recovery rate), and the traditional ammonia precipitation method (89%~91% recovery rate). This demonstrates that this method has excellent anti-interference ability and accuracy in the detection of trace copper and zinc in high-nickel matrices.
[0057] Based on the results of the static adsorption test and comparative verification test, it can be concluded that Chelex-100 chelating resin has a good effect on Cu²⁺ in a nitric acid system. + Ni² + Zn² + Co² + Mn² + The affinity order is Cu² + >Ni² + >Zn² + Co² + >Mn²+ By precisely controlling the acidity of the eluent for segmented adsorption and elution, selective separation of copper and zinc from high-concentration Ni, Co, and Mn matrices can be achieved. Spiking recovery tests showed that the chelating resin method achieved average recoveries of 97.76% and 98.98% for copper and zinc, respectively, with relative standard deviations (RSDs) of less than 2%, significantly superior to the traditional ammonia co-precipitation method (average recoveries of 88.38% and 90.37% for copper and zinc, respectively, with RSDs > 2%). Validation tests to eliminate interference from the high-nickel matrix further confirmed that high-concentration Ni, Co, and Mn matrices have a significant matrix inhibition effect on the determination of copper and zinc in ICP-OES. Conventional direct dilution and matrix matching methods could not effectively correct for this effect. However, after separation with the chelating resin, the measured values of copper and zinc highly matched the theoretical spiked values, with relative errors of only -2% and -1%, respectively. The above results demonstrate that the chelation resin separation-ICP-OES method described in this application can completely eliminate spectral and non-spectral interferences from high-nickel matrices, significantly improving the accuracy and precision of trace copper and zinc determination. It is a reliable pretreatment and analytical method suitable for confirmatory detection of trace copper and zinc in high-nickel ternary precursors (including 8-series and 9-series).
[0058] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for detecting the copper and zinc content in a high-nickel ternary precursor, characterized in that, Includes the following steps: The high-nickel ternary precursor material was digested and diluted to a final volume to obtain a sample solution, which was then subjected to full adsorption through a chelating resin microcolumn. The chelating resin was eluted stepwise using eluents with different acidities, and zinc-containing and copper-containing eluent fractions were collected separately. ICP was performed on the zinc-containing and copper-containing eluent fractions, respectively. OES determination, and calculation of the copper and zinc content in the precursor material based on the test results.
2. The detection method according to claim 1, characterized in that, The digestion solution used is a nitric acid solution with a concentration of 5.0-7.0 mol / L, the digestion temperature is 200-300℃, and the digestion time is 10-30 min.
3. The detection method according to claim 1, characterized in that, The high-nickel ternary precursor material is nickel cobalt manganese hydroxide or nickel cobalt aluminum hydroxide.
4. The detection method according to claim 1, characterized in that, The sample solution was adjusted to pH 6.0 after being brought to volume; the flow rate of the sample solution through the chelating resin microcolumn was 1.0-2.0 mL / min.
5. The detection method according to claim 1, characterized in that, The process after total adsorption also includes rinsing the chelating resin microcolumn with a buffer solution at pH 6.
0.
6. The detection method according to claim 1, characterized in that, The chelating resin is Chelex-100 chelating resin.
7. The detection method according to claim 1, characterized in that, The eluent flows through the chelating resin microcolumn at a rate of 1.0-2.0 mL / min.
8. The detection method according to claim 1, characterized in that, The stepwise elution includes the following steps: First elution step: Elute with nitric acid solution with pH 3.4-3.6, and discard the eluent; Second elution step: Elution is performed using a nitric acid solution with a pH of 2.2-2.4, and the zinc-containing eluent fraction is collected; Third elution step: Elute with nitric acid solution with pH 1.6-1.8, and discard the eluent; Fourth elution step: Elution was performed using a 2.0 mol / L nitric acid solution, and the copper-containing eluent fraction was collected.
9. The detection method according to claim 1, characterized in that, The ICP OES determination includes: shaking the elution fractions separately, filtering, and using the filtrate as the test solution; preparing a blank solution with the same matrix as the test solution; and performing ICP-based analysis. OES technology is used to determine the concentrations of copper and zinc ions in the test solution and the blank solution; the content of copper and zinc in the precursor material is then calculated.
10. The detection method according to claim 9, characterized in that, The oscillation time is 2-4 hours; the filter membrane used for filtration is a 0.22 μm or 0.45 μm aqueous filter membrane.