A quantitative grading evaluation method for rigid-flexible composite pavement interlayer bonding quality

By conducting oblique shear tests under multiple temperature conditions, an exponential decay model of oblique shear strength-temperature was established and combined with failure modes. The analytic hierarchy process (AHP) was used to calculate the comprehensive score of interlayer bond quality, which solved the problem of multi-dimensional quantitative grading in existing technologies. This enabled multi-dimensional comprehensive evaluation of interlayer bond quality and guidance for engineering improvement.

CN123135597APending Publication Date: 2026-11-20HUBEI ROAD & BRIDGE GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611562343.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, the quality evaluation of interlayer bonding in rigid-flexible composite pavements cannot be carried out through multi-dimensional comprehensive quantitative grading, which makes it impossible to effectively guide engineering improvement and quality grading control.

Method used

By conducting oblique shear tests under multiple temperature conditions, an exponential decay model of oblique shear strength versus temperature was established. Combining failure modes and normalized scores, the analytic hierarchy process (AHP) was used to calculate the comprehensive score of interlayer bond quality, including the normalized score of oblique shear strength, the normalized score of temperature sensitivity, and the normalized score of failure modes.

Benefits of technology

It enables a multi-dimensional comprehensive quantitative grading evaluation of interlayer bond quality, and provides a quantitative characterization of the rate of decay of interlayer bond strength with increasing temperature and the causes of failure, guiding engineering improvement and material selection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123135597A_ABST
    Figure CN123135597A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of pavement engineering, and particularly discloses a quantitative grading evaluation method for the interlayer bonding quality of rigid-flexible composite pavement, which comprises the following steps: roughening treatment is performed on a rigid base plate, bonding material is brushed, an asphalt surface layer is formed, and an oblique shear test piece is cut; oblique shear tests are carried out under multiple temperature conditions, the oblique shear strength values under different temperatures are measured, the oblique shear strength value under the lowest temperature is normalized according to a preset reference value to obtain an interlayer oblique shear strength normalized score, and the fracture surface position is recorded; an exponential decay model of the oblique shear strength-temperature is established according to the oblique shear strength values under different temperatures, a temperature decay rate constant is obtained by fitting, and a temperature sensitivity normalized score is calculated; the failure mode and the normalized score of the failure mode are determined according to the fracture surface position; three normalized scores are taken as evaluation indexes, the weight coefficients are determined by using an analytic hierarchy process, and a comprehensive score is calculated; the quality grade is divided according to a preset comprehensive score interval, and multi-dimensional comprehensive quantitative grading evaluation is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of pavement engineering technology, specifically to a quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement. Background Technology

[0002] Rigid-flexible composite pavements are a mainstream structural form in road engineering, mainly including combinations of cement concrete base courses and asphalt surface courses, combinations of UHPC and SMA wearing course courses, and asphalt overlays on old cement pavements. In this type of structure, the rigid base course provides load-bearing capacity, while the flexible surface course provides driving functionality. The two form a collaborative working system through an adhesive layer, and the quality of the interlayer bonding directly determines the service life and safety of the pavement.

[0003] In the prior art, the quality evaluation of interlayer bonding usually adopts the oblique shear test to determine the interlayer shear strength, and compares the measured strength value with the specification limit or the failure strength of the mixture itself to determine whether the interlayer bonding is qualified.

[0004] However, this single mechanical index of shear strength can only reflect whether the interlayer bond meets the strength requirements. It cannot reveal the cause of failure, the temperature decay law and the overall quality level. It is difficult to make a multi-dimensional comprehensive quantitative grade evaluation of the interlayer bond quality, thus failing to effectively guide engineering improvement and quality grade control. Summary of the Invention

[0005] To address the technical problems in the prior art, this invention provides a quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement, aiming to solve the problem that the evaluation results in the prior art cannot provide a multi-dimensional comprehensive quantitative grading and evaluation of the interlayer bonding quality.

[0006] The technical solution of the present invention is as follows: A quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement includes the following steps: The surface of the rigid base test plate is roughened, an adhesive material is applied, an asphalt mixture surface layer is formed on the adhesive material to form a composite plate, and oblique shear test specimens are cut from the composite plate. The oblique shear specimen is placed on a universal testing machine and oblique shear tests are carried out under multiple temperature conditions. The oblique shear strength value at each temperature is measured. The oblique shear strength value measured at the lowest temperature among the multiple temperature conditions is normalized according to the preset oblique shear strength benchmark value to obtain the normalized score of interlaminar oblique shear strength, and the fracture surface position is recorded. Based on the measured shear strength values ​​at various temperatures, an exponential decay model of shear strength-temperature is established, and the temperature decay rate constant is obtained by fitting. The temperature sensitivity normalization score is calculated based on the temperature decay rate constant. Based on the recorded fracture surface location, the failure mode is determined, and according to the preset correspondence between failure modes and normalized scores, the failure mode normalized score corresponding to the failure mode is determined. The normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode were used as evaluation indicators. The weight coefficients of each evaluation indicator were determined by the analytic hierarchy process (AHP). The comprehensive score of interlaminar bond quality was calculated based on the normalized scores of each evaluation indicator and the weight coefficients. Based on the preset range of comprehensive scores, the interlayer bonding quality is classified into different grades.

[0007] Optionally, the step of normalizing the shear strength value measured at the lowest temperature among the plurality of temperature conditions according to a preset shear strength benchmark value to obtain a normalized score for interlayer shear strength specifically includes: Divide the shear strength value measured at the lowest temperature by the preset shear strength benchmark value to obtain the strength ratio. Multiply the strength ratio by 100 to obtain the normalized score of the interlaminar shear strength; When the strength ratio is greater than 1, the normalized score of the interlaminar shear strength is 100.

[0008] Optionally, the step of establishing an exponential decay model of oblique shear strength versus temperature based on the measured oblique shear strength values ​​at various temperatures specifically includes: The shear strength measured at each temperature is used as the fitting data. The lowest temperature among all temperature points is used as the reference temperature. The shear strength at the reference temperature is used as the reference value of the model. The shear strength decreases exponentially with increasing temperature as the fitting form. An exponential decay model with the temperature decay rate constant as the undetermined parameter is constructed. Using the reference temperature as the fitting reference point, the oblique shear strength values ​​measured at each temperature point are substituted into the exponential decay model, and the least squares method is used for fitting to obtain the exponential decay model of oblique shear strength-temperature and the temperature decay rate constant.

[0009] Optionally, the calculation of the temperature sensitivity normalization score based on the temperature decay rate constant specifically includes: The product of the temperature decay rate constant and the difference between the preset upper temperature limit and the reference temperature is used as the exponential decay factor, where the reference temperature is the lowest temperature among all temperature conditions. The exponential decay factor is negatively represented as the exponential term, and the exponential function value is calculated. The exponential function value is then multiplied by 100 to obtain the normalized score of temperature sensitivity.

[0010] Optionally, the failure mode specifically includes: The failure modes include internal fracture modes of the bonding layer, internal fracture modes of the asphalt mixture, and interface fracture modes of the rigid base layer. When the fracture surface is located inside the adhesive layer, it is diagnosed as an internal fracture mode of the adhesive layer; When the fracture surface is located inside the asphalt mixture, it is diagnosed as an internal fracture mode of the asphalt mixture. When the fracture surface is located at the interface of a rigid base layer, it is diagnosed as a rigid base layer interface fracture mode.

[0011] Optionally, the evaluation index is based on the normalized score of interlaminar shear strength, the normalized score of temperature sensitivity, and the normalized score of failure mode. The weighting coefficients of each evaluation index are determined using the analytic hierarchy process (AHP), specifically including: A hierarchical structure model is constructed, with interlaminar bonding quality as the target layer of the hierarchical structure model, and the normalized score of interlaminar shear strength, the normalized score of temperature sensitivity, and the normalized score of failure mode as the evaluation indicators of the criterion layer of the hierarchical structure model. The Saaty scaling method is used to compare the relative importance of each evaluation index in the criterion layer pairwise, and a judgment matrix is ​​constructed. The judgment matrix is ​​normalized, and the weight coefficients of each evaluation index are calculated based on the normalized judgment matrix.

[0012] Optionally, the step of calculating the comprehensive score of interlayer bonding quality based on each evaluation index and the weighting coefficient specifically includes: The normalized scores of the interlaminar shear strength, temperature sensitivity, and failure mode are multiplied by their respective weighting coefficients to obtain the weighted scores for each evaluation index. The weighted scores of each evaluation indicator are summed to obtain the comprehensive score of interlayer bonding quality.

[0013] This invention also provides a quantitative grading and evaluation system for the interlayer bonding quality of rigid-flexible composite pavement, comprising: The specimen preparation module is used to prepare oblique shear specimens; The oblique shear test module is used to conduct oblique shear tests, measure the oblique shear strength value at various temperatures, normalize the oblique shear strength value measured at the lowest temperature among multiple temperature conditions according to the preset oblique shear strength benchmark value, obtain the normalized score of interlaminar oblique shear strength, and record the fracture surface location. The temperature sensitivity calculation module is used to establish an exponential decay model of shear strength-temperature, and fit it to obtain the temperature decay rate constant. Based on the temperature decay rate constant, the normalized score of temperature sensitivity is calculated. The failure mode diagnosis module is used to determine the failure mode based on the location of the fracture surface, and to determine the failure mode normalization score corresponding to the failure mode according to the preset correspondence between failure modes and normalization scores. The comprehensive scoring module is used to evaluate the interlaminar bond quality by using the normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode as evaluation indicators, and employing the analytic hierarchy process (AHP) to determine the weight coefficients of each evaluation indicator. The grading and determination module is used to classify the interlayer bonding quality level according to the preset comprehensive score range.

[0014] The present invention also provides an electronic device, including a processor and a memory, wherein the memory stores a computer program, and the processor executes the computer program to implement the above-described quantitative grading evaluation method for the interlayer bonding quality of rigid-flexible composite pavement.

[0015] The present invention also provides a non-transitory computer-readable storage medium storing a computer program, which, when executed by a processor, implements the above-described quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement.

[0016] Compared with existing technologies, the quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement provided by this invention has the following beneficial effects: (1) By placing the oblique shear specimen under multiple temperature conditions for oblique shear test, normalizing the oblique shear strength value, establishing an exponential decay model of oblique shear strength-temperature, determining the failure mode and its normalized score, and then using the three normalized scores as evaluation indicators, the analytic hierarchy process is used to calculate the comprehensive score of interlayer bonding quality and classify the grades, so that the evaluation of interlayer bonding quality is transformed from a single strength judgment to a multi-dimensional comprehensive quantitative graded evaluation that covers strength level, temperature decay law and failure cause.

[0017] (2) By normalizing the shear strength value measured at the lowest temperature among multiple temperature conditions according to the preset shear strength benchmark value, the normalized score of interlayer shear strength is obtained, so that the shear strength values ​​of different material systems and different structural combinations have a unified comparison benchmark, which provides a data basis for subsequent weighted synthesis with temperature sensitivity normalized score and failure mode normalized score.

[0018] (3) By establishing an exponential decay model of shear strength-temperature and fitting it to obtain the temperature decay rate constant, it is possible to quantitatively characterize the rate of decay of interlayer bond strength with increasing temperature, providing a quantitative basis for material selection and bonding system design under high temperature conditions.

[0019] (4) By determining the failure mode based on the location of the fracture surface and obtaining the normalized score of the failure mode according to the pre-set correspondence between the failure mode and the normalized score, the evaluation results not only include strength information, but also information on weak links in interlayer bond failure, providing a basis for determining the direction of engineering improvement. Attached Figure Description

[0020] Figure 1 This is a flowchart illustrating the steps of a quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to the present invention. Figure 2 This is a system structure diagram of a quantitative grading evaluation system for the interlayer bonding quality of rigid-flexible composite pavement according to the present invention. Figure 3 This is a schematic diagram of the structure of an electronic device according to the present invention; Figure 4 This is a schematic diagram of the bonding of rigid base plate after different roughening treatments in an embodiment of the present invention. Detailed Implementation

[0021] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0022] Please see Figure 1 This invention provides a quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement, comprising the following steps: S10: Roughen the surface of the rigid base plate, apply adhesive material, form an asphalt mixture surface layer on the adhesive material to form a composite plate, and cut oblique shear specimens from the composite plate.

[0023] In application, the rigid base test plate can be a cement concrete slab, a UHPC slab, an RPC slab, or a base test specimen obtained by core sampling at the engineering site. In this embodiment, a UHPC slab is preferred because: UHPC has extremely high compressive strength and excellent durability. When used as a rigid base, the quality of interlayer bonding has a more significant impact on the overall structural service performance; the surface of UHPC is dense and smooth, and the bonding interface between it and the asphalt surface layer is more likely to become a weak point. Therefore, using a UHPC slab as a rigid base test plate can more rigorously test the discrimination and reliability of the evaluation method of this invention.

[0024] The roughening treatment can be achieved by shot blasting, sandblasting, or grooving; in this embodiment, shot blasting is preferred, and the texture depth after shot blasting is controlled at 0.7mm. The reason for using shot blasting is that it can uniformly remove the laitance layer on the surface of the UHPC board, forming a uniform rough surface, and the shot blasting depth is controllable and the construction efficiency is high. The reason for controlling the texture depth at 0.7mm is that if the texture depth is too small, such as below 0.3mm, the surface roughness is insufficient, and the mechanical interlocking effect between the adhesive material and the substrate is limited; if the texture depth is too large, the local shot blasting depth is uneven, which can easily lead to stress concentration at the interface; a texture depth of 0.7mm can ensure the interface roughness while avoiding excessive local depth, providing a good adhesion foundation for the adhesive material.

[0025] The asphalt mixture surface layer can be SMA, AC, or PA; in this embodiment, SMA-13 ​​is preferred because: SMA (asphalt mastic aggregate mixture) has a dense skeleton structure, high coarse aggregate content, and large asphalt content. Its interlayer bonding quality with the rigid base layer has the most significant impact on the pavement service performance, making it the most typical flexible surface layer form in rigid-flexible composite pavements; the binder of the asphalt mixture surface layer can be high-viscosity, high-elasticity modified asphalt or SBS modified asphalt; in this embodiment, high-viscosity, high-elasticity modified asphalt is preferred because: high-viscosity, high-elasticity modified asphalt has excellent viscosity toughness and elastic recovery ability, and can form a stronger interfacial bond with the binder material, thereby more fully verifying the evaluation effect of the evaluation method of this invention in a high-quality binder system; the asphalt-aggregate ratio of the asphalt mixture surface layer can be determined by the Marshall test, and 6.1% is used in this embodiment because: this asphalt-aggregate ratio is the optimal asphalt-aggregate ratio determined by the Marshall test, which can provide sufficient asphalt film thickness while ensuring the high-temperature stability of the mixture, so that a reasonable matching relationship is formed between the internal strength of the asphalt mixture and the interlayer bonding strength.

[0026] Specifically, an adhesive material is applied to the roughened surface of the rigid base test panel. This adhesive material can be a combination of a two-stage reactive epoxy resin adhesive, epoxy asphalt, or a high-viscosity emulsified asphalt primer layer and a high-viscosity, high-elasticity modified asphalt stress-absorbing layer. In this embodiment, a two-stage reactive epoxy resin adhesive is preferred, with a coating amount of 0.7g. The reason for using a two-stage reactive epoxy resin adhesive is that it has the characteristics of initial micro-curing and subsequent secondary curing under heat. This allows it to soften under heat during asphalt mixture paving and, after compaction, exert excellent bonding properties. Its bonding strength is higher than that of ordinary SBS modified asphalt and epoxy asphalt, thus more fully verifying the evaluation effect of the present invention's evaluation method in high-strength bonding systems. The coating amount is 0.7. The reason is that when the coating amount is too low, the adhesive material cannot evenly cover the roughened substrate surface, and some areas may have missed areas; when the coating amount is too high, the excess adhesive material forms a rich layer between layers, which may become a weak point; 0.7 The amount of coating ensures that the adhesive material evenly covers the substrate surface and forms a reasonable adhesive layer thickness.

[0027] Subsequently, an SMA-13 ​​asphalt mixture surface layer was formed on the bonding material using a roller mill method, resulting in a composite slab consisting of a rigid base course test slab, a bonding material layer, and an asphalt mixture surface layer. The formed composite slab was then cut into 100mm × 100mm × 100mm oblique shear specimens with an oblique shear angle of [missing information]. The preferred bevel angle is... The reason is that when a vehicle brakes suddenly on the road, the horizontal force coefficient is at its maximum, approximately 1, meaning the horizontal stress is equal to the vertical stress. Force decomposition shows that the angle between the horizontal force and the resultant force is... ,use The oblique shear specimen can simulate the interlayer shear stress state of the pavement under the most unfavorable conditions; the oblique shear angle is controlled at... Within a certain range, to ensure uniform stress on the shear surface, facilitate clamping by the fixture, and maximize the shear stress components.

[0028] S20: Place the oblique shear specimen on a universal testing machine and conduct oblique shear tests under multiple temperature conditions. Measure the oblique shear strength value at each temperature. Normalize the oblique shear strength value measured at the lowest temperature among the multiple temperature conditions according to a preset oblique shear strength benchmark value to obtain the normalized score of interlaminar oblique shear strength, and record the fracture surface location.

[0029] In some embodiments, the shear strength value measured at the lowest temperature among the plurality of temperature conditions is normalized according to a preset shear strength benchmark value to obtain an interlayer shear strength normalization score. Specifically, this includes: dividing the shear strength value measured at the lowest temperature by the preset shear strength benchmark value to obtain a strength ratio; multiplying the strength ratio by 100 to obtain the interlayer shear strength normalization score; and when the strength ratio is greater than 1, the interlayer shear strength normalization score is set to 100.

[0030] In application, The multiple temperature conditions include at least three temperature points: 25℃, 40℃, and 60℃; 25℃ is the standard temperature for asphalt-related performance tests in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG 3410—2025), serving as a normal temperature benchmark; 40℃ represents the road surface temperature under high summer temperatures; 60℃ represents the road surface temperature under extreme high temperature conditions; the loading rate for the oblique shear test under each temperature condition is 50. This ensures that only temperature is a single variable.

[0031] The interlayer shear strength is calculated using the following formula: ; In the formula: Interlaminar shear strength ( ); The maximum destructive load recorded by the universal testing machine ( A is the shear area of ​​the specimen (); ),for Square cross-section oblique shear specimen, .

[0032] The lowest temperature among the multiple temperature conditions is 25℃. The shear strength value measured at 25℃ is divided by the preset shear strength benchmark value to obtain the strength ratio. In this embodiment, the preset shear strength benchmark value is 1.8MPa.

[0033] The logic for determining this benchmark value is as follows: Statistical analysis is performed on interlayer oblique shear test data covering different bonding systems: combinations of second-order reactive epoxy resin adhesives, epoxy asphalt adhesives, high-viscosity emulsified asphalt primers and high-viscosity, high-elasticity modified asphalt stress-absorbing layers; and different interface treatment methods: shot blasting, aggregate interlocking, and grooving. Figure 4 As shown in Table 1, the oblique shear strength data under 25℃ conditions are as follows: Table 1: Statistical table of oblique shear strength of different bonding systems and interface treatments at 25℃ The data in Table 1 above are derived from the measured results of interlayer oblique shear tests at 25°C for the three bonding systems and three interface treatment methods combined in this embodiment. The methods are: second-order reactive epoxy resin (shot blasting 0.3mm, 0.5mm, 0.7mm), second-order reactive epoxy resin (crushed stone interlocking, grooved, untreated), epoxy asphalt (shot blasting 0.3mm, 0.5mm, 0.7mm), epoxy asphalt (crushed stone interlocking, grooved, untreated), and high-viscosity emulsified asphalt + high-viscosity high-elasticity stress-absorbing layer (shot blasting 0.3mm, 0.5mm, 0.7mm). A total of 19 sets of oblique shear strength data were collected, including 18 sets of data for high-viscosity emulsified asphalt + high-viscosity high-elasticity stress-absorbing layer (crushed stone interlocking, grooved, untreated) and 1 set of data for second-stage reactive epoxy resin (SBS modified asphalt binder SMA, untreated). Among them, the 2.30 MPa corresponding to "second-stage reactive epoxy resin (crushed stone interlocking)" and the 1.27 MPa corresponding to "second-stage reactive epoxy resin (SBS modified asphalt binder SMA, untreated)" in Table 1 indicate that the fracture surface is located inside the SMA-13 ​​mixture rather than the bonding interface, and the actual bonding strength is greater than the test results.

[0034] Sort the 19 sets of data in Table 1 above according to their shear strength values ​​from smallest to largest, and calculate the shear strength value corresponding to each percentile. The percentile is calculated as follows: after sorting the data from smallest to largest, calculate the position index. ,in For the total number of data ( ), Percentile; if If it is an integer, then the first... percentile is the The data and the first The average of the data; if If the number is not an integer, round it up and take the corresponding index as the first integer. percentile.

[0035] The above 19 sets of data were sorted in ascending order of oblique shear strength value, and the results are shown in Table 2: Table 2: Ranking of Oblique Shear Strength Data under 25℃ Condition Based on the above sorting results, the shear strength value corresponding to each percentile was calculated, and the results are shown in Table 3: Table 3: Percentile Statistics of Oblique Shear Strength Data under 25℃ Condition Table 3 shows that the 75th percentile corresponds to a shear strength of 1.69 MPa. Considering the high requirements for interlayer bonding quality in engineering practice, and taking into account the discriminative power of the evaluation results, it is rounded down to 1.8 MPa and used as the preset benchmark value for shear strength. The physical meaning of this benchmark value is: when the measured shear strength reaches 1.8 MPa, it indicates that the room-temperature shear performance of this interlayer bonding system is better than that of more than 75% of the test samples, reaching an excellent level. The reason for choosing the 75th percentile as the benchmark value is that, in the percentage scoring system, the 75th percentile corresponds to the lower limit of the "good" level, that is, the level corresponding to 75 points, which is consistent with the positioning of the "boundary point of excellent performance". This benchmark value is a recommended value, and in practical applications, it can be adjusted according to the climate and traffic conditions of the specific project location.

[0036] Taking the measured data of the second-order reactive epoxy resin adhesive (shot blasted, texture depth 0.5 mm) in this embodiment as an example, the oblique shear strength at 25℃ is 1.73 MPa, and the strength ratio is... Normalized score of interlayer shear strength When the strength ratio is greater than 1, that is, the measured strength is higher than the benchmark value, the normalized score of the interlayer shear strength is taken as 100.

[0037] Meanwhile, the location of the fracture surface after the oblique shear test was observed and recorded to provide a basis for subsequent failure mode diagnosis; the location of the fracture surface includes three situations: inside the bonding layer, inside the asphalt mixture, and at the interface of the rigid base layer.

[0038] S30: Based on the measured shear strength values ​​at various temperatures, establish an exponential decay model of shear strength-temperature, and obtain the temperature decay rate constant by fitting it. Calculate the temperature sensitivity normalization score based on the temperature decay rate constant.

[0039] In some embodiments, based on the measured shear strength values ​​at various temperatures, an exponential decay model of shear strength versus temperature is established, specifically including: Using the shear strength measured at each temperature as fitting data, the lowest temperature among all temperature points is taken as the reference temperature, and the shear strength at the reference temperature is taken as the model reference value. An exponential decay model is constructed with the shear strength decreasing exponentially with increasing temperature as the fitting form, and the temperature decay rate constant is taken as the parameter to be determined. Using the reference temperature as the fitting reference point, the shear strength values ​​measured at each temperature point are substituted into the exponential decay model, and the least squares method is used for fitting to obtain the exponential decay model of shear strength-temperature and the temperature decay rate constant.

[0040] In application, the oblique shear strength values ​​measured under various temperature conditions are first used as fitting data. In this embodiment, oblique shear tests were conducted on the second-order reactive epoxy resin adhesive under different interface treatments at 25℃, 40℃, and 60℃. The measured results are shown in Table 4.

[0041] Table 4: Measured data of oblique shear strength of second-order reactive epoxy resin adhesives at different temperatures (unit: MPa) In Table 4, "shot blasting 0.3", "shot blasting 0.5", and "shot blasting 0.7" refer to the structural depth after shot blasting treatment being 0.3 mm, 0.5 mm, and 0.7 mm, respectively.

[0042] Plotting the data in Table 4 above with temperature as the x-axis and shear strength as the y-axis, we can observe that the shear strength exhibits a non-linear decay trend with increasing temperature, and the higher the temperature, the faster the decay rate.

[0043] This invention uses an exponential function as the fitting form, that is, it uses the exponential decay of the shear strength with increasing temperature as the fitting form, and constructs an exponential decay model with the temperature decay rate constant as the undetermined parameter.

[0044] The basis for using an exponential function as the fitting form is as follows: Based on the time-temperature equivalence principle, asphalt-based adhesives are viscoelastic materials, and their mechanical properties exhibit a non-linear, exponential decay law with increasing temperature. From the perspective of molecular motion, increased temperature intensifies the movement of asphalt molecular chain segments and weakens intermolecular forces, macroscopically manifesting as a decrease in strength; this process conforms to the basic form of the Arrhenius equation, that is, the reaction rate constant has an exponential relationship with temperature.

[0045] Plotting the measured data in Table 4 with temperature as the x-axis and shear strength as the y-axis, the shear strength shows a non-linear decay trend with increasing temperature, and the higher the temperature, the faster the decay rate; the curve shape of the exponential function is consistent with the distribution trend of the measured data.

[0046] Meanwhile, previous studies have shown that interlaminar pull-out strength, interlaminar shear strength, and temperature all satisfy a single exponential function relationship, with a goodness of fit of [missing information]. It can reach over 0.970.

[0047] The general form of an exponential function is: When applying it to the relationship between shear strength and temperature, let , , , The exponential decay model of the shear strength versus temperature is obtained as follows: ; In the formula: For temperature (°C) oblique shear strength ( ); Reference temperature The shear strength below ( ); The temperature decay rate constant ( This reflects the rate at which interlayer bond strength decreases with increasing temperature; The lowest temperature among all temperature conditions is used as the reference temperature; in this example, it is 25°C. The physical meaning of this model is: the shear strength decreases exponentially with increasing temperature, and the temperature decay rate constant is... The larger the value, the faster the shear strength decreases with increasing temperature.

[0048] From a mathematical perspective, the three data points are precisely enough to determine the exponential function. Two unknown parameters in ( and Therefore, the three-point fitting is mathematically well-posed; when there are more data points than unknown parameters, the least squares method can be used to optimize the fitting and further improve the model accuracy.

[0049] Then, using the reference temperature as the fitting reference point, the oblique shear strength values ​​measured at each temperature point are substituted into the exponential decay model, and the least squares method is used for fitting to obtain the exponential decay model of oblique shear strength-temperature and the temperature decay rate constant.

[0050] Using the measured data from the "Shot blasting 0.5" column in Table 4 as the fitted data: the oblique shear strength at 25℃ is 1.73MPa, at 40℃ it is 0.59MPa, and at 60℃ it is 0.17MPa; substituting these three sets of data into the exponential decay model: when hour, The shear strength at 25℃ is determined from the measured values ​​in Table 4. ; Will Substituting the data from 40℃ and 60℃ into the model, the temperature decay rate constant k is solved using the least squares method to minimize the sum of squared residuals between the measured and calculated values ​​of the shear strength at each temperature point: ; In the formula: Number of temperature points ( =3); For the first Temperature points The measured oblique shear strength value; For the first Temperature points The following is the shear strength value calculated by the model.

[0051] Solving using the least squares method yields the following results. The goodness of fit of the fitting result Calculate using the following formula: ; In the formula: For the first The oblique shear strength value measured at each temperature point; For the first The oblique shear strength values ​​calculated by the model at each temperature point; This represents the average of the measured oblique shear strength values ​​at all temperature points. ; Number of temperature points ( =3).

[0052] In the above formula, The sum of squared residuals reflects the deviation between the model-calculated values ​​and the measured values. The total sum of squares reflects the degree of dispersion of the measured values ​​themselves; The closer the value is to 1, the better the model fits the measured data.

[0053] Calculated using the above formula, we obtain... =0.97, indicating that the exponential function can well describe the variation of shear strength with temperature.

[0054] The data in the other columns of Table 4 (shot blasting 0.3, shot blasting 0.7, crushed stone interlocking, grooving, and no treatment) are listed together as comparative data to facilitate understanding of the impact of different interface treatments on temperature sensitivity. The different temperature decay rate constants corresponding to different interface treatments indicate that the interface treatment method has a significant impact on the temperature sensitivity of interlayer bonding.

[0055] In some embodiments, the temperature sensitivity normalization score is calculated based on the temperature decay rate constant, specifically including: The product of the temperature decay rate constant and the difference between the preset upper temperature limit and the reference temperature is used as the exponential decay factor, where the reference temperature is the lowest temperature among all temperature conditions. The exponential decay factor is then negatively represented as the exponential term, and the exponential function value is calculated. The exponential function value is then multiplied by 100 to obtain the normalized score of the temperature sensitivity.

[0056] In application, firstly, the exponential decay factor is calculated; the exponential decay factor is the temperature decay rate constant. With the preset upper temperature limit and reference temperature The product of the differences, i.e. Among them, the upper limit of temperature Take 60℃ as the reference temperature. The lowest temperature among all temperature conditions is selected; in this embodiment, it is 25°C.

[0057] The reason for choosing 60℃ is that 60℃ is the standard temperature for high-temperature performance testing of asphalt mixtures in the "Technical Specification for Construction of Highway Asphalt Pavement" (JTG F40-2004), which is consistent with the definition of extreme high-temperature conditions in this method; using 60℃ as the upper limit of temperature can reflect the ability of interlayer bonding to maintain its performance at the upper limit of the service temperature range.

[0058] Secondly, the negative value of the exponential decay factor is used as the exponential term to calculate the exponential function value; the exponential function value The physical meaning is: temperature from the reference temperature Increase to the upper temperature limit At that time, the exponential decay model of shear strength-temperature is used. It can be seen that the retention rate of oblique shear strength is .

[0059] Then, the exponential function value is multiplied by 100 to obtain the normalized score of the temperature sensitivity. That is:

[0060] ; In the formula: Temperature sensitivity normalized score; The constant is the temperature decay rate constant; The preset upper temperature limit is set to 60℃; The lowest temperature among all temperature conditions is taken as the reference temperature, which is 25°C in this embodiment.

[0061] The data obtained by fitting the measured data in the "0.5 shot blasting" column of Table 4 For example, the exponential decay factor is Take its negative value and use it as the exponent term to calculate the exponential function value. Multiplying the value of the exponential function by 100 yields... This indicates that under extreme high-temperature conditions of 60°C, the shear strength retention rate of this bonding system is approximately 33.8%.

[0062] S40: Based on the recorded fracture surface location, determine the failure mode, and according to the preset correspondence between failure modes and normalized scores, determine the failure mode normalized score corresponding to the failure mode.

[0063] In some embodiments, the failure mode specifically includes: The failure modes include internal fracture mode of the bonding layer, internal fracture mode of the asphalt mixture, and fracture mode of the rigid base layer interface. When the fracture surface is located inside the bonding layer, it is diagnosed as internal fracture mode of the bonding layer; when the fracture surface is located inside the asphalt mixture, it is diagnosed as internal fracture mode of the asphalt mixture; when the fracture surface is located at the rigid base layer interface, it is diagnosed as fracture mode of the rigid base layer interface.

[0064] In application, based on the location of the fracture surface after the oblique shear test, the failure mode is diagnosed into the following three categories: Internal fracture mode of the adhesive layer: The fracture surface is located inside the adhesive layer, indicating that the interlayer bond strength is lower than the strength of the adhesive material itself, and the adhesive material formulation needs to be optimized or the coating process needs to be improved; the normalized failure mode score corresponding to this failure mode is preset to 65 points.

[0065] Internal fracture mode of asphalt mixture: The fracture surface is located inside the asphalt mixture, indicating that the interlayer bond strength is higher than the strength of the asphalt mixture itself. This is the optimal failure mode, and no further improvement in bond strength is required. The normalized score for this failure mode is preset to 100 points.

[0066] Rigid substrate interface fracture mode: The fracture surface is located at the rigid substrate interface, indicating that the interlayer bond strength is lower than the rigid substrate interface bond strength, requiring improvement of the surface roughening treatment quality of the rigid substrate or removal of interface contaminants. The normalized failure mode score corresponding to this failure mode is preset to 50 points.

[0067] The design logic for the above score difference is as follows: The basis for assigning a full score of 100 points to the internal fracture mode of asphalt mixture is that this mode is the optimal failure mode, the interlayer bond strength is higher than the strength of the asphalt mixture itself, indicating that there are no weak links in the interlayer bond quality, and no engineering improvement is required. Therefore, it is assigned a full score of 100 points in the percentage scoring system.

[0068] The basis for assigning a score of 65 to the internal fracture mode of the adhesive layer is as follows: This mode is a material-level problem, requiring optimization of the adhesive material formulation or improvement of the coating application process; the difficulty of improvement is moderate. A score below 100 reflects the gap between this mode and the optimal mode; it falls within the 60-75 range of the percentage scoring system, indicating relatively low difficulty in improvement; a score of 70 or 80 would not be sufficiently distinguishable from the optimal mode; and a score of 60 or below would not be sufficiently distinguishable from the fracture mode at the rigid substrate interface.

[0069] The basis for assigning 50 points to the rigid substrate interface fracture mode is as follows: This mode involves the quality of the substrate surface treatment, requiring large-area re-treatment such as shot blasting and sandblasting, which is costly and difficult to improve; a score below 65 points reflects that its improvement difficulty is higher than that of the fracture mode inside the adhesive layer; at the same time, a score below 60 points reflects its severity; a score of 40 or 30 points would have too significant a lowering effect on the overall score; a score of 55 points would not be sufficiently distinguishable from a score of 65 points.

[0070] The above three scores are determined based on the engineering improvement difficulty corresponding to each failure mode: the lower the improvement difficulty, the higher the failure mode normalization score; the higher the improvement difficulty, the lower the failure mode normalization score; the failure mode normalization scores corresponding to the three failure modes satisfy the following: internal fracture mode of asphalt mixture (100 points) > internal fracture mode of bonding layer (65 points) > interface fracture mode of rigid base course (50 points); the spacing between the three scores is designed as follows: point, The first gap is larger than the second gap, which reflects that the gap between the optimal mode and the mode that needs improvement is greater than the gap between the two modes that need improvement, consistent with the difference in engineering improvement difficulty among the three modes.

[0071] In cases where fracture surfaces occur at multiple locations simultaneously, if the area of ​​a certain interface exceeds 70%, the main failure mode is determined based on that interface; if no interface has an area exceeding 70%, it is determined to be a mixed failure mode. When comprehensively scoring, the scores of each failure mode are calculated by weighting the area proportions, or the lowest score is taken according to the conservative principle.

[0072] Taking the measured data of the second-order reactive epoxy resin binder (shot blasted, texture depth 0.5mm) in this embodiment as an example, the fracture surface is located inside the SMA mixture, and according to the above diagnostic criteria, it is determined to be an internal fracture mode of asphalt mixture, with a failure mode normalized score. Get 100 points.

[0073] S50: Using the normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode as evaluation indicators, the weight coefficients of each evaluation indicator are determined by the analytic hierarchy process (AHP), and the comprehensive score of interlaminar bond quality is calculated based on the normalized scores of each evaluation indicator and the weight coefficients.

[0074] In some embodiments, the normalized score of interlaminar shear strength, the normalized score of temperature sensitivity, and the normalized score of failure mode are used as evaluation indicators. The weight coefficients of each evaluation indicator are determined using the analytic hierarchy process (AHP), specifically including: A hierarchical model is constructed, with interlaminar bonding quality as the target layer. The normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode are used as evaluation indicators for the criterion layer of the hierarchical model. The relative importance of each evaluation indicator in the criterion layer is compared pairwise using the Saaty scaling method to construct a judgment matrix. The judgment matrix is ​​normalized, and the weight coefficients of each evaluation indicator are calculated based on the normalized judgment matrix.

[0075] In application, firstly, a hierarchical model is constructed. This model uses interlaminar bond quality as the target layer and the normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode as evaluation indicators for the criterion layer. The normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode reflect interlaminar bond quality from different dimensions: the normalized score reflects room-temperature shear resistance, the normalized score reflects the causes of failure and the difficulty of improvement, and the normalized score reflects the ability to maintain performance at high temperatures.

[0076] Secondly, the Saaty scaling method is used to compare the relative importance of each evaluation indicator in the criterion layer pairwise, constructing a judgment matrix. In this embodiment, 15 road engineering experts with senior professional titles were invited to compare the importance of the indicators pairwise according to the Saaty 1-9 scaling method, constructing the following judgment matrix A:

[0077] ; The meaning of this judgment matrix is ​​as follows: the normalized score of interlaminar shear strength is slightly more important than the normalized score of failure mode (scale 2); the normalized score of interlaminar shear strength is slightly more important than the normalized score of temperature sensitivity (scale 2); the normalized score of failure mode is equally important than the normalized score of temperature sensitivity (scale 1).

[0078] Then, the judgment matrix is ​​normalized, and the weight coefficients of each evaluation index are calculated based on the normalized judgment matrix. The normalization process is as follows: first, the sum of the elements in each column of the judgment matrix is ​​calculated, then each element is divided by the sum of the corresponding column to obtain the normalized matrix; the normalized matrix is ​​then summed row by row and divided by the matrix order. ( =3), thus obtaining the weight vector.

[0079] After calculation, the weighting coefficients were determined to be: , , ,satisfy The normalization requirement. Among them... The corresponding normalized score of inter-layer shear strength Corresponding failure mode normalized score, The corresponding temperature sensitivity normalized score.

[0080] The weighting coefficients are determined as follows: interlaminar shear strength is the most direct and core mechanical indicator, reflecting the ultimate bearing capacity of the interlaminar interface under shear load, and is assigned the highest weight of 0.40; failure mode diagnosis provides information at the "cause" level, and its value lies in guiding the direction of engineering improvement, and is assigned a weight of 0.30; temperature sensitivity evaluation reflects the performance stability of the bonding system within the service temperature range, and is assigned a weight of 0.30; this weight is the default recommended weight, and in actual application, it can be appropriately increased according to specific engineering needs, such as in high-temperature areas. For heavy traffic sections, the weighting of inter-story shear strength can be appropriately increased. The calibration was performed using the AHP method, but a consistency check was still required after the adjustment.

[0081] Perform a consistency check on the judgment matrix: Calculate the largest eigenvalue of the judgment matrix. In this embodiment ; Calculate the consistency index ; Calculate the consistency ratio ,in As a random consistency indicator, =3 =0.58, then =0 < 0.1, the consistency of the judgment matrix is ​​acceptable.

[0082] In some embodiments, a comprehensive score for interlayer bonding quality is calculated based on each evaluation index and the weighting coefficients, specifically including: The normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode are multiplied by their respective weighting coefficients to obtain the weighted scores for each evaluation index. The weighted scores for each evaluation index are then summed to obtain the comprehensive score for interlaminar bond quality.

[0083] In application, the process of calculating the comprehensive score of interlayer bonding quality based on each evaluation index and the weighting coefficient is as follows.

[0084] In the above, the weight coefficients of each evaluation index have been determined using the analytic hierarchy process (AHP). , , Furthermore, the normalized score of the interlayer shear strength has been obtained. Failure Mode Normalization Score and temperature sensitivity normalized score This step involves multiplying the three normalized scores by their corresponding weighting coefficients and summing the results to obtain the comprehensive interlayer bonding quality score P.

[0085] Specifically, the normalized score of the interlayer shear strength is... With the corresponding weighting coefficients Multiplying them together yields the weighted score corresponding to the interlayer shear strength. Normalize the failure mode score With the corresponding weighting coefficients Multiply to obtain the weighted score corresponding to the failure mode. Normalize the temperature sensitivity score With the corresponding weighting coefficients Multiply by this to obtain the weighted score corresponding to the temperature sensitivity. .

[0086] Summing the three weighted scores yields the comprehensive interlayer bond quality score P: ; In the formula: This represents the normalized score for interlayer shear strength. The failure mode normalization score; This represents the normalized score for temperature sensitivity. , , For the weighting coefficients, satisfying .

[0087] Taking the measured data of the second-order reactive epoxy resin adhesive (shot blasting, texture depth 0.5 mm) in this embodiment as an example, =96.1, calculated based on a shear strength of 1.73 MPa at 25℃. =100, the fracture surface is located inside the SMA mixture, and the diagnosis is an internal fracture mode of asphalt mixture. =33.8, calculated based on the exponential decay model. =0.40, =0.30, =0.30, then: ; After rounding, P = 78.5.

[0088] S60: Based on the preset range of comprehensive scores, classify the interlayer bonding quality level.

[0089] In application, the interlayer bonding quality level is divided according to the preset comprehensive score range.

[0090] Specifically, in this embodiment, the interlayer bonding quality level is divided into four levels: Grade I: Overall score P≥90, indicating excellent interlayer bonding quality; Grade II: 75≤P<90, good interlayer bonding quality; Grade III: 60≤P<75, interlayer bonding quality is average; Grade IV: P < 60, poor interlayer bonding quality.

[0091] The grading thresholds are determined based on the following criteria: the commonly used grading system of "Excellent (≥90), Good (≥75), Pass (≥60), Poor (<60)" is adopted, and the sub-item inspection and evaluation standards in the "Highway Engineering Quality Inspection and Evaluation Standard" (JTG F80 / 1-2017) are referenced for calibration. In practical applications, users can adjust the thresholds appropriately according to the climate and traffic conditions of the specific project location.

[0092] Taking P=78.5 calculated based on measured data in this embodiment as an example, it falls within the range of 75≤P<90 and is judged as Grade II, indicating good interlayer bonding quality. This grade indicates that although the high-viscosity and high-elasticity modified asphalt has excellent room temperature strength, its performance retention rate under extreme high temperature conditions needs to be improved, providing a clear direction for material optimization.

[0093] This invention also provides a quantitative grading and evaluation system for the interlayer bonding quality of rigid-flexible composite pavement, comprising: Specimen preparation module 11 is used to prepare oblique shear specimens; The oblique shear test module 12 is used to conduct oblique shear tests, measure the oblique shear strength value at each temperature, normalize the oblique shear strength value measured at the lowest temperature among the multiple temperature conditions according to the preset oblique shear strength benchmark value, obtain the normalized score of interlaminar oblique shear strength, and record the fracture surface position. Temperature sensitivity calculation module 13 is used to establish an exponential decay model of shear strength-temperature, and to obtain the temperature decay rate constant by fitting it. Based on the temperature decay rate constant, the temperature sensitivity normalization score is calculated. The failure mode diagnosis module 14 is used to determine the failure mode based on the location of the fracture surface, and to determine the failure mode normalization score corresponding to the failure mode according to the preset correspondence between failure modes and normalization scores. The comprehensive scoring module 15 is used to calculate the comprehensive score of interlaminar bond quality by using the normalized score of interlaminar shear strength, the normalized score of temperature sensitivity and the normalized score of failure mode as evaluation indicators, and using the analytic hierarchy process to determine the weight coefficients of each evaluation indicator. The grading and judgment module 16 is used to classify the interlayer bonding quality level according to the preset comprehensive score range.

[0094] It should be understood that the quantitative grading and evaluation system for the interlayer bond quality of rigid-flexible composite pavement achieves automated and standardized evaluation of interlayer bond quality through the collaborative work of the specimen preparation module 11, oblique shear test module 12, temperature sensitivity calculation module 13, failure mode diagnosis module 14, comprehensive scoring module 15, and grading determination module 16. Each module is responsible for specimen preparation, oblique shear test and normalization, temperature sensitivity calculation, failure mode diagnosis, comprehensive scoring, and grading determination, respectively. Data transfer between modules is clear, and the evaluation process is standardized, avoiding the result dispersion caused by operational differences in manual evaluation. This system can be integrated into computer equipment to achieve rapid evaluation and grading of interlayer bond quality, and is suitable for various application scenarios such as on-site engineering testing and laboratory evaluation.

[0095] The present invention also provides an electronic device, including a processor 21 and a memory 22, wherein the memory 22 stores a computer program, and the processor 21 executes the computer program to implement the quantitative grading evaluation method for the interlayer bonding quality of rigid-flexible composite pavement described above.

[0096] It should be understood that the electronic device may be a computer, server, or other device with data processing capabilities. When the computer program stored in the memory 22 is executed by the processor, it performs all the operations described in the above method steps; the processor 21 may be a central processing unit (CPU), microprocessor, or the like.

[0097] The electronic device executes the computer program stored in the memory 22 through the processor 21, and can perform the following functions: process the shear strength values ​​of the oblique shear specimen measured under multiple temperature conditions, normalize the shear strength value at the lowest temperature into a normalized score for interlaminar shear strength; establish an exponential decay model of shear strength-temperature based on the shear strength values ​​at each temperature, and calculate the normalized score for temperature sensitivity; determine the failure mode and the corresponding normalized score for failure mode based on the fracture surface location; use the three normalized scores as evaluation indicators, determine the weighting coefficients using the analytic hierarchy process (AHP), and calculate the comprehensive score for interlaminar bond quality; and classify the interlaminar bond quality level according to the preset numerical range of the comprehensive score. The electronic device automates and standardizes the evaluation process, reduces the workload and errors of manual calculations, and improves evaluation efficiency and consistency of results.

[0098] The present invention also provides a non-transitory computer-readable storage medium storing a computer program, which, when executed by a processor, implements the above-described quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement.

[0099] It should be understood that the computer-readable storage medium may be a non-transitory storage medium such as a disk, optical disk, or semiconductor memory; when the computer program stored on the computer-readable storage medium is executed by a processor, it performs all the above-mentioned method steps; when the computer program is executed by a processor, it can realize a multi-dimensional comprehensive quantitative grading evaluation of interlayer bonding quality, including shear strength normalization, temperature sensitivity calculation, failure mode diagnosis, AHP weighting, and comprehensive scoring, thereby achieving standardization and automation of the evaluation process.

[0100] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement, characterized in that, Includes the following steps: The surface of the rigid base test plate is roughened, an adhesive material is applied, an asphalt mixture surface layer is formed on the adhesive material to form a composite plate, and oblique shear test specimens are cut from the composite plate. The oblique shear specimen is placed on a universal testing machine and oblique shear tests are carried out under multiple temperature conditions. The oblique shear strength value at each temperature is measured. The oblique shear strength value measured at the lowest temperature among the multiple temperature conditions is normalized according to the preset oblique shear strength benchmark value to obtain the normalized score of interlaminar oblique shear strength, and the fracture surface position is recorded. Based on the measured shear strength values ​​at various temperatures, an exponential decay model of shear strength-temperature is established, and the temperature decay rate constant is obtained by fitting. The temperature sensitivity normalization score is calculated based on the temperature decay rate constant. Based on the recorded fracture surface location, the failure mode is determined, and according to the preset correspondence between failure modes and normalized scores, the failure mode normalized score corresponding to the failure mode is determined. The normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode were used as evaluation indicators. The weight coefficients of each evaluation indicator were determined by the analytic hierarchy process (AHP). The comprehensive score of interlaminar bond quality was calculated based on the normalized scores of each evaluation indicator and the weight coefficients. Based on the preset range of comprehensive scores, the interlayer bonding quality is classified into different grades.

2. The quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to claim 1, characterized in that, The step of normalizing the shear strength value measured at the lowest temperature among the multiple temperature conditions according to a preset shear strength benchmark value to obtain the normalized score of interlayer shear strength specifically includes: Divide the shear strength value measured at the lowest temperature by the preset shear strength benchmark value to obtain the strength ratio. Multiply the strength ratio by 100 to obtain the normalized score of the interlaminar shear strength; When the strength ratio is greater than 1, the normalized score of the interlaminar shear strength is 100.

3. The quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to claim 1, characterized in that, The step involves establishing an exponential decay model of oblique shear strength versus temperature based on the measured oblique shear strength values ​​at various temperatures, specifically including: The shear strength measured at each temperature is used as the fitting data. The lowest temperature among all temperature points is used as the reference temperature. The shear strength at the reference temperature is used as the reference value of the model. The shear strength decreases exponentially with increasing temperature as the fitting form. An exponential decay model with the temperature decay rate constant as the undetermined parameter is constructed. Using the reference temperature as the fitting reference point, the oblique shear strength values ​​measured at each temperature point are substituted into the exponential decay model, and the least squares method is used for fitting to obtain the exponential decay model of oblique shear strength-temperature and the temperature decay rate constant.

4. The quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to claim 1, characterized in that, The calculation of the temperature sensitivity normalized score based on the temperature decay rate constant specifically includes: The product of the temperature decay rate constant and the difference between the preset upper temperature limit and the reference temperature is used as the exponential decay factor, where the reference temperature is the lowest temperature among all temperature conditions. The exponential decay factor is negatively represented as the exponential term, and the exponential function value is calculated. The exponential function value is then multiplied by 100 to obtain the normalized score of temperature sensitivity.

5. The quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to claim 1, characterized in that, The failure modes specifically include: The failure modes include internal fracture modes of the bonding layer, internal fracture modes of the asphalt mixture, and interface fracture modes of the rigid base layer. When the fracture surface is located inside the adhesive layer, it is diagnosed as an internal fracture mode of the adhesive layer; When the fracture surface is located inside the asphalt mixture, it is diagnosed as an internal fracture mode of the asphalt mixture. When the fracture surface is located at the interface of a rigid base layer, it is diagnosed as a rigid base layer interface fracture mode.

6. The quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to claim 1, characterized in that, The evaluation indicators are the normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode. The weighting coefficients of each indicator are determined using the analytic hierarchy process (AHP), specifically including: A hierarchical structure model is constructed, with interlaminar bonding quality as the target layer of the hierarchical structure model, and the normalized score of interlaminar shear strength, the normalized score of temperature sensitivity, and the normalized score of failure mode as the evaluation indicators of the criterion layer of the hierarchical structure model. The Saaty scaling method is used to compare the relative importance of each evaluation index in the criterion layer pairwise, and a judgment matrix is ​​constructed. The judgment matrix is ​​normalized, and the weight coefficients of each evaluation index are calculated based on the normalized judgment matrix.

7. The quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement according to claim 6, characterized in that, The calculation of the comprehensive score for interlayer bonding quality based on each evaluation index and the weighting coefficients specifically includes: The normalized scores of the interlaminar shear strength, temperature sensitivity, and failure mode are multiplied by their respective weighting coefficients to obtain the weighted scores for each evaluation index. The weighted scores of each evaluation indicator are summed to obtain the comprehensive score of interlayer bonding quality.

8. A quantitative grading and evaluation system for the interlayer bonding quality of rigid-flexible composite pavement, characterized in that, include: The specimen preparation module is used to prepare oblique shear specimens; The oblique shear test module is used to conduct oblique shear tests, measure the oblique shear strength value at various temperatures, normalize the oblique shear strength value measured at the lowest temperature among multiple temperature conditions according to the preset oblique shear strength benchmark value, obtain the normalized score of interlaminar oblique shear strength, and record the fracture surface location. The temperature sensitivity calculation module is used to establish an exponential decay model of shear strength-temperature, and fit it to obtain the temperature decay rate constant. Based on the temperature decay rate constant, the normalized score of temperature sensitivity is calculated. The failure mode diagnosis module is used to determine the failure mode based on the location of the fracture surface, and to determine the failure mode normalization score corresponding to the failure mode according to the preset correspondence between failure modes and normalization scores. The comprehensive scoring module is used to evaluate the interlaminar bond quality by using the normalized scores of interlaminar shear strength, temperature sensitivity, and failure mode as evaluation indicators, and employing the analytic hierarchy process (AHP) to determine the weight coefficients of each evaluation indicator. The grading and determination module is used to classify the interlayer bonding quality level according to the preset comprehensive score range.

9. An electronic device, characterized in that, It includes a processor and a memory, the memory storing a computer program, and the processor executing the computer program to implement the quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement as described in any one of claims 1 to 7.

10. A non-transitory computer-readable storage medium, characterized in that, The computer-readable storage medium stores a computer program that, when executed by a processor, implements the quantitative grading and evaluation method for the interlayer bonding quality of rigid-flexible composite pavement as described in any one of claims 1 to 7.