Method for determining water erosion resistance of inner surface of glass liquor bottle

By combining ICP-OES technology with acetic acid aqueous solution immersion treatment and optimizing immersion conditions, the accuracy and efficiency issues of water erosion resistance determination of the inner surface of glass liquor bottles have been solved. This has enabled efficient and convenient multi-element detection, which is suitable for quality control of glass liquor bottles and quality inspection of liquor production enterprises.

CN123135682APending Publication Date: 2026-11-20GUIZHOU MOUTAI WINERY GRP XIJIU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611564347.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing methods for determining the water resistance of the inner surface of glass liquor bottles are cumbersome to operate, slow to detect, and have low sensitivity. They are difficult to accurately reflect the degree of corrosion on the inner surface of the glass and suffer from significant matrix interference, which cannot meet the requirements for accurate determination of low-content ions.

Method used

The target elements in glass liquor bottles were extracted by using ICP-OES technology combined with acetic acid aqueous solution immersion treatment, ultrasonic treatment and constant temperature immersion. The leaching concentration of the target elements was detected by ICP-OES, the total amount of oxides was calculated, and factors such as immersion volume, ultrasonic time, immersion time, immersion solution concentration and immersion temperature were optimized to ensure the simplicity and accuracy of the determination method.

Benefits of technology

It improves the accuracy and efficiency of measuring the corrosivity of the inner surface of glass liquor bottles, enables simultaneous measurement of multiple elements, reduces human interference, simplifies the operation process, and is suitable for quality control of glass liquor bottles and quality inspection of liquor production enterprises, ensuring the safety of liquor storage and consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The application provides a kind of glass white liquor bottle inner surface water erosion resistance determination method, comprising the following steps: A) to the treated glass white liquor bottle is added soaking liquid, seal, after ultrasonic treatment, carry out soaking treatment, obtain soaking treatment liquid, the soaking liquid is acetic acid aqueous solution, volume concentration is 2~15%;B) the soaking treatment liquid is filtered and then detected by ICP-OES, and the total amount of oxide is calculated according to the target element dissolution concentration obtained by detection.The determination method provided by the application ensures the extraction effect of target elements in glass white liquor bottles, without setting high temperature and high pressure device in the pretreatment process, the determination is simple, and the accuracy is higher.The application provides practical data support and reference for liquor production enterprises in bottle selection and quality control, and has important practical significance and application value for promoting the standardization and standardization development of liquor industry and improving the quality level of the whole industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of analytical testing technology, specifically relating to a method for determining the water erosion resistance of the inner surface of a glass liquor bottle. Background Technology

[0002] Glass, due to its excellent chemical stability, barrier properties, and recyclability, is widely used in the packaging of baijiu (Chinese liquor). It serves as a crucial packaging container in the production, storage, and sale of baijiu, and its quality directly impacts the quality and safety of the liquor. However, during long-term storage and transportation, the moisture in baijiu undergoes hydrolysis with alkali metal oxides and other components on its surface, leading to the dissolution of ions. If the glass's water resistance is poor, these dissolved ions can enter the baijiu, altering its composition, affecting its taste, aroma, and stability, and shortening its shelf life. Therefore, from a quality control perspective, accurately measuring the water resistance of the inner surface of glass baijiu bottles helps baijiu producers select high-quality bottle suppliers, ensuring that packaging materials meet requirements. This is crucial for guaranteeing the stability and consistency of baijiu product quality and ensuring food safety.

[0003] The water resistance of the inner surface of glass liquor bottles is one of the key indicators for measuring their quality. Traditional testing methods mainly include chemical titration or flame atomic emission / absorption spectroscopy. However, titration is cumbersome, slow, time-consuming, and subjective, and has low detection sensitivity, making it difficult to meet the needs of accurate determination of low-content ions. Flame atomic emission / absorption spectroscopy suffers from significant matrix interference, limitations in simultaneous determination of multiple elements, and difficulty in accurately detecting subtle erosion changes. It cannot efficiently and comprehensively reflect the degree of erosion on the inner surface of the glass, resulting in poor accuracy and reliability of the test results.

[0004] Therefore, providing an efficient, accurate method suitable for determining the water resistance of the inner surface of glass liquor bottles has become a problem that needs to be solved. Summary of the Invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a method for determining the water erosion resistance of the inner surface of a glass liquor bottle. The method provided by the present invention ensures the extraction effect of the target elements in the glass liquor bottle, does not require the setting of a high temperature and high pressure device in the pretreatment process, is simple to operate, has a short detection cycle, and the determination method has strong pertinence and reliability.

[0006] This invention provides a method for determining the water resistance of the inner surface of a glass liquor bottle, comprising the following steps: A) Add soaking solution to the treated glass liquor bottle, seal it, and after ultrasonic treatment, perform soaking treatment to obtain soaking solution. The soaking solution is an aqueous solution of acetic acid with a volume concentration of 2-15%. B) After filtering the soaking solution, perform ICP-OES detection, and calculate the total amount of oxides based on the detected dissolution concentration of the target element.

[0007] Preferably, the treated glass liquor bottle is treated according to the following method: After rinsing the inner surface of the bottle with deionized water 3-5 times, place it in an oven at 60-80℃ to dry to constant weight, and then cool to room temperature.

[0008] Preferably, the amount of the soaking solution added is 20% to 100% of the nominal capacity of the glass liquor bottle.

[0009] Preferably, the ultrasonic treatment has a power of 700W and a duration of 10-50 minutes.

[0010] Preferably, the soaking temperature is 25~100℃ and the soaking time is 30~180min.

[0011] Preferably, the filtration is performed using a 0.22 μm filter membrane.

[0012] Preferably, the ICP-OES detection parameters are: RF power 1147W, carrier gas flow rate 0.50L / min, carrier gas pressure 2.13bar, auxiliary gas flow rate 0.50L / min, and cooling gas flow rate 12.5L / min.

[0013] Preferably, the target elements include Na, K, and Ca.

[0014] Preferably, the method for calculating the total amount of oxides includes: calculating the average concentration of each oxide in each sample by comparing it with a standard curve, expressing it as the number of micrograms of sodium oxide contained in each milliliter of extract, and then calculating the total content of oxides.

[0015] Preferably, the formula for calculating the total amount of oxides is shown in Equation I: Formula I In Formula I: X: Total amount of oxides in the sample solution, μg / mL; C Na : The detected value of sodium oxide in the sample solution, in μg / mL; C K : The detected value of potassium oxide in the sample solution, in μg / mL; C Ca : Detection value of calcium oxide in the sample solution, μg / mL; σ K Conversion factor: 0.658; σ Ca Conversion factor: 1.105.

[0016] Compared with existing technologies, this invention provides a method for determining the water resistance of the inner surface of a glass liquor bottle, comprising the following steps: A) adding an immersion solution to a treated glass liquor bottle, sealing it, ultrasonically treating it, and then immersing it to obtain an immersion solution, wherein the immersion solution is an aqueous solution of acetic acid with a volume concentration of 2-15%; B) filtering the immersion solution and performing ICP-OES detection, and calculating the total amount of oxides based on the detected dissolution concentration of the target element. The determination method provided by this invention ensures the extraction effect of the target element in the glass liquor bottle, eliminates the need for high-temperature and high-pressure devices during pretreatment, and is simpler and more accurate. This invention provides practical data support and reference for liquor producers in bottle selection and quality control, and has significant practical significance and application value for promoting the standardization and normalization of the liquor industry and improving the overall quality level of the industry. Attached Figure Description

[0017] Figure 1 A schematic diagram showing the effect of different immersion volumes on the water resistance of the inner surface of a glass liquor bottle. Figure 2 A schematic diagram showing the effect of different ultrasonic times on the water resistance of the inner surface of a glass liquor bottle. Figure 3 A schematic diagram showing the effect of different immersion times on the water resistance of the inner surface of a glass liquor bottle. Figure 4 A schematic diagram showing the effect of different immersion solution concentrations on the water resistance of the inner surface of a glass liquor bottle. Figure 5 This is a schematic diagram showing the effect of different immersion temperatures on the water resistance of the inner surface of a glass liquor bottle. Detailed Implementation

[0018] This invention provides a method for determining the water resistance of the inner surface of a glass liquor bottle, comprising the following steps: A) Add soaking solution to the treated glass liquor bottle, seal it, and after ultrasonic treatment, perform soaking treatment to obtain soaking solution. The soaking solution is an aqueous solution of acetic acid with a volume concentration of 2-15%. B) After filtering the soaking solution, perform ICP-OES detection, and calculate the total amount of oxides based on the detected dissolution concentration of the target element.

[0019] This invention first processes the glass liquor bottle, specifically including the following steps: Rinse the inside of the glass liquor bottle with deionized water 3-5 times to remove all dirt and packaging debris. Place it in an oven at 60-80℃ to dry to constant weight and cool to room temperature for later use.

[0020] Then, a soaking solution is added to the treated glass liquor bottle. The soaking solution is an aqueous acetic acid solution with a volume concentration of 2-15%, which can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or any value between 3% and 15%. Preferably, it is 3% to 5%, more preferably 4%.

[0021] The amount of the soaking solution added is 20% to 100% of the nominal capacity of the glass liquor bottle, and can be 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%, or any value between 20% and 100%. Preferably, it is 60% to 80%, more preferably 80%.

[0022] After adding the soaking solution, the glass liquor bottle is sealed and subjected to ultrasonic treatment. The ultrasonic treatment power is 700W, and the time is 10-50 minutes, which can be any value between 10, 20, 30, 40, 50 minutes, or 10-50 minutes. Preferably, it is 20-40 minutes, more preferably 30 minutes.

[0023] Next, the glass liquor bottle is immersed in a soaking solution to extract the target element. The immersion process preferably maintains a constant temperature; therefore, the glass liquor bottle can be placed in a constant-temperature water bath for extraction. The immersion temperature is 25~100℃, and can be any value between 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, and 100℃. Preferably, it is 80~100℃, more preferably 100℃. The immersion time is 30~180 min, and can be any value between 30, 60, 90, 120, 150, and 180 min. Preferably, it is 90~150 min, more preferably 120 min.

[0024] After soaking, cool to room temperature to obtain the soaking solution.

[0025] Next, the soaking solution is filtered to obtain the solution to be tested. The filtration is performed using a 0.22 μm filter membrane.

[0026] The test solution is subjected to ICP-OES detection, and the total amount of oxides is calculated based on the detected dissolution concentration of the target element.

[0027] The principle of ICP-OES for determining the water resistance of the inner surface of glass liquor bottles is as follows: Sodium, calcium, and silicon in the inner wall of glass liquor bottles undergo ion exchange and skeletal hydrolysis reactions under aqueous conditions and long-term storage. Components such as sodium, potassium, and calcium in the glass network can slowly dissolve, which is the main reason for the failure of the glass container's water resistance. This invention conducts accelerated extraction tests on clean glass liquor bottles. Using ultrasonic equipment, an acetic acid aqueous solution is used for extraction under specific temperature conditions to simulate the corrosive effect of liquor components on the inner wall of the glass during long-term storage, allowing the soluble components on the glass surface to fully dissolve and transfer to the extraction solution.

[0028] The extract to be tested is nebulized and introduced into ICP-OES high-temperature argon plasma, where sample evaporation, dissociation, atomization, and excitation are achieved at high temperatures of 6000–10000 K. When excited-state atoms of each element transition back to the ground state, they emit characteristic wavelength spectra, and the spectral intensity is linearly related to the concentration of the corresponding element in the solution. The instrument collects the characteristic emission spectra of each element through a spectroscopic system, and quantifies the content of sodium, potassium, and calcium in the extract using standard curves.

[0029] The total amount of oxides is calculated based on the leaching of each element, and its level characterizes the water resistance of the inner surface of the glass liquor bottle: under the same experimental conditions, the lower the total amount of oxides, the better the density of the glass's silica-oxygen network structure, and the stronger the resistance of the inner wall to water erosion; conversely, the glass surface has poor stability, and long-term storage of liquor can easily lead to changes in the composition of the liquor, alkali precipitation, or even delamination. Compared with the traditional acid-base titration method, inductively coupled plasma optical emission spectrometry (ICP-OES) technology has advantages such as high detection sensitivity, high accuracy, low matrix interference, the ability to detect extremely low concentrations of elements, and fast simultaneous determination of multiple elements. It reduces the interference of human factors, greatly improves detection efficiency and the comprehensiveness of information acquisition, and enhances data repeatability and stability. Therefore, ICP-OES can achieve accurate and independent quantification of multiple elements, distinguish the differences between surface ion exchange and deep framework hydrolysis erosion, and more comprehensively and objectively evaluate the water resistance of the inner surface of the glass liquor bottle.

[0030] The specific steps involved in performing ICP-OES testing are as follows: 1) Take appropriate amounts of Na, K, and Ca mixed standard stock solution (concentration 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions with concentration gradients of 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Analyze the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and use the instrument's built-in analysis software to plot standard curves. Obtain the standard curve equations and correlation coefficients for each element through linear regression analysis.

[0031] The ICP-OES detection parameters are as follows: RF power 1147W, carrier gas flow rate 0.50L / min, carrier gas pressure 2.13bar, auxiliary gas flow rate 0.50L / min, and cooling gas flow rate 12.5L / min.

[0032] 2) Following the same instrument reference conditions and operating procedures as when establishing the standard curve, the glass liquor bottle soaking solution was tested using an ICP-OES instrument to determine the signal response values ​​of the elements to be tested. The detection values ​​of Na, K and Ca in the test solution were obtained according to the standard curve.

[0033] The average concentration of each oxide in each sample was calculated by comparing it with the standard curve, and expressed as the number of micrograms of sodium oxide contained in each milliliter of extract. Then the total content of oxides was calculated.

[0034] According to Formula I, the content of oxides in the glass liquor bottle sample is calculated based on the detected values ​​of Na, K, and Ca in the soaking solution. The calculation method is as follows: Formula I In Formula I: X: Total amount of oxides in the sample solution, μg / mL; C Na : The detected value of sodium oxide in the sample solution, in μg / mL; C K : The detected value of potassium oxide in the sample solution, in μg / mL; C Ca : Detection value of calcium oxide in the sample solution, μg / mL; σ K Conversion factor: 0.658; σ Ca Conversion factor: 1.105.

[0035] The calculation method refers to the calculation method in GB / T 4548.2-2003 Determination and classification of water erosion resistance of inner surface of glass products and glass containers by flame spectroscopy.

[0036] The total amount of oxides is used to evaluate the water resistance of the inner surface of glass liquor bottles. The lower the total amount of oxides, the better the water resistance of the inner surface of the glass.

[0037] Compared with the prior art, the present invention has the following beneficial technical effects: 1. This invention is the first to apply ICP-OES technology to the determination of water erosion resistance of the inner surface of glass liquor bottles. By utilizing its advantages of high sensitivity, low matrix interference, and simultaneous determination of multiple elements, it significantly improves the accuracy and efficiency of ion dissolution detection and can accurately reflect the degree of erosion of the inner surface of glass. 2. The effects of five key factors on the test results were systematically studied: immersion volume, ultrasonic time, immersion time, immersion solution concentration, and immersion temperature. The optimal experimental conditions were determined through optimization, making the test method more targeted and reliable, and applicable to the detection of different types of glass liquor bottles. 3. The method of this invention is simple to operate, has a short testing cycle, requires no complex sample pretreatment process, and does not require high-temperature and high-pressure devices during pretreatment. It can be widely applied to quality control in glass liquor bottle manufacturing enterprises and other fields. Specifically, the optimized testing method is applied to the factory quality inspection, warehousing acceptance, or performance monitoring during the use of glass liquor bottles to screen out glass liquor bottles that meet the requirements for water resistance, ensuring the safety of liquor storage and consumption, and has significant practical value.

[0038] To further understand the present invention, the method for determining the water erosion resistance of the inner surface of a glass liquor bottle provided by the present invention will be described below with reference to embodiments. The scope of protection of the present invention is not limited by the following embodiments.

[0039] I. Materials and Reagents

[0040] (1) Acetic acid (CH3COOH): analytical grade, purchased from Tianjin Kemei Chemical Reagent Co., Ltd.; (2) Nitric acid (HNO3): Superior grade, purchased from Chengdu Kelong Chemical Co., Ltd.; (3) Argon (Ar): Argon (purity ≥ 99.999%); (4) Helium (He): Helium (purity ≥ 99.999%); (5) Nitric acid solution (6+94): Take 60 mL of nitric acid and slowly add it to 940 mL of water, then mix well.

[0041] (6) Multi-element mixed standard (GSB 04-1767-2004): Na, K, Ca, etc., with a mass concentration of 1000 μg / mL, purchased from the National Nonferrous Metals and Electronic Materials Analysis and Testing Center. When using, dilute with 6% HNO3 to prepare a mixed standard solution of appropriate concentration as needed.

[0042] II. Equipment

[0043] (1) EQ7000 ultrapure water system: Merck Millipore China Co., Ltd.; (2) WGLL-230E electric thermostatic drying oven: Fisford Instruments (Hebei) Co., Ltd.; (3) Ultrasonic cleaning machine: Shanghai Chenhui Instrument Co., Ltd.; (4) Digital display constant temperature water bath: Shandong Oulaibo Instrument Co., Ltd.; (5) iCAP PRO 13728 Inductively Coupled Plasma Emission Spectrometer: Thermo Fisher Scientific.

[0044] III. Optimization of Preprocessing Methods

[0045] 3.1 Preparation of standard solutions

[0046] Take appropriate amounts of Na, K, and Ca mixed standard stock solutions (each with a concentration of 1000 μg / mL) and dilute them stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set as 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL.

[0047] 3.2 ICP-OES Analysis Procedure

[0048] (1) Start-up and preheating: Before starting the machine, purge the gas for 2 hours, turn on the circulating water cooling system and the fan, and install the sample inlet tube and waste liquid tube. (2) Ignition and sequence editing: Ignite the plasma, cool the detector to -44℃, wait for 30 minutes, edit the sample injection program, and put the sample inlet tube into the extract to be tested. Before the sample is tested, 3-4 blank samples need to be prepared to balance the instrument. (3) Cleaning and shutdown: After the sample is tested, put the sample in dilute nitric acid solution and ultrapure water for cleaning for 2-3 minutes to ensure that there is no residual reagent or sample contamination or corrosion of the instrument. Finally, turn off the plasma, loosen the peristaltic pump, place the sample inlet tube in ultrapure water, and turn off the argon valve, fan and circulating water cooling system.

[0049] 3.3 Preprocessing

[0050] 3.3.1 Selection of Immersion Volume

[0051] This section uses the total amount of final oxides to measure whether the extraction is complete.

[0052] (1) Sample pretreatment: Randomly select a batch of glass liquor bottles of the same specification (500mL) from the same manufacturer, rinse the inner surface of the bottle with deionized water 3-5 times to remove all dirt and packaging debris and other impurities, place them in an oven at 60-80℃ to dry to constant weight, and cool to room temperature for later use.

[0053] (2) Immersion Test: In this test, 100 mL, 200 mL, 300 mL, 400 mL, and 500 mL of 4% acetic acid aqueous solution were added to a batch of 500 mL glass liquor bottles to extract the target elements. The corresponding immersion volume ratios were 20%, 40%, 60%, 80%, and 100% of the nominal capacity of the glass liquor bottles, respectively. This was to investigate the effect of different immersion volumes on the extraction efficiency of the target elements in the glass liquor bottles. The specific experimental steps were as follows: 100 mL, 200 mL, 300 mL, 400 mL, and 500 mL of 4% acetic acid aqueous solution were added to the pretreated glass liquor bottle samples, respectively. After sealing, the samples were sonicated for 30 min and then immersed in a constant temperature water bath at 100±1℃ for 120 min. After immersion, the samples were cooled. Three parallel samples were set up for each group.

[0054] (3) Soaking solution collection: Take out the soaking solution, filter it with a 0.22μm filter membrane to remove suspended impurities, and obtain the test solution.

[0055] (4) ICP-OES detection

[0056] To prepare a standard curve: Take appropriate amounts of the mixed standard stock solution (concentration of 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set to 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Detect the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and use the instrument's built-in analysis software to plot the standard curve. Through linear regression analysis, obtain the standard curve equation and correlation coefficient for each element.

[0057] Sample determination: Before each sample determination, the system was rinsed with nitric acid. After the analytical signal value stabilized, the soaking solution was tested by ICP-OES under the same instrument reference conditions and operating procedures as when establishing the standard curve. The signal response value of the target element was determined. The concentration of the target element in the extract was obtained according to the standard curve. Laboratory blank samples were determined under the same instrument reference conditions and operating procedures.

[0058] ICP-OES detection parameter settings: The above-mentioned test liquid was tested by ICP-OES to detect the leaching concentration of the target element in the glass; the ICP-OES detection parameters were: radio frequency power: 1147 W; carrier gas flow rate: 0.50 L / min; carrier gas pressure: 2.13 bar; auxiliary gas flow rate: 0.50 L / min; cooling gas flow rate: 12.5 L / min.

[0059] (5) Calculation of results: The total amount of oxides in the glass liquor bottle sample was calculated according to Formula I based on the detected values ​​of Na, K and Ca in the soaking solution. The total amount of oxides in the sample was expressed as the number of micrograms of sodium oxide contained in each milliliter of extract.

[0060] (6) Results Analysis: In the simulated erosion test, the immersion volume can change the solid-liquid contact state and interfacial reaction intensity inside the bottle, which is a key factor affecting the degree of water erosion on the inner wall of the glass. The results of the effect of different immersion liquid volume ratios on the water erosion resistance of the inner surface of the glass liquor bottle are as follows: Figure 1 As shown, by Figure 1 It was found that different immersion solution volume ratios significantly affected the detection results of the total oxide content in glass liquor bottles, ranging from 3.757 to 11.638 μg / mL. When the immersion solution volume ratio was below 40% (100–200 mL), the solid-liquid contact area was small, and the target ions, after dissolving, would rapidly accumulate at the narrow solid-liquid interface, resulting in an inflated detection result for the total oxide content in the sample. However, when the immersion solution volume ratio was 80%, the immersion solution covered most of the inner wall of the bottle, diluting the interfacial ion enrichment effect, essentially eliminating the wet-dry interface, and significantly improving the uniformity of erosion. This not only allowed for better extraction of target ions but also reduced the generation of extraction waste liquid to some extent, contributing to resource conservation and environmental protection. Overall, an immersion solution volume ratio of 80% was optimal.

[0061] 3.3.2 Selection of Ultrasound Time

[0062] (1) Sample pretreatment: Randomly select a batch of glass liquor bottles of the same specification (500mL) from the same manufacturer, rinse the inner surface of the bottle with deionized water 3-5 times to remove all dirt and packaging debris and other impurities, place them in an oven at 60-80℃ to dry to constant weight, and cool to room temperature for later use.

[0063] (2) Immersion test: Ultrasonic equipment was used in the experiment, and ultrasonic treatment times of 0 min, 10 min, 20 min, 30 min, 40 min and 50 min were set to investigate the effect of different ultrasonic times on the extraction effect of target elements in glass liquor bottles. The specific experimental steps are as follows: 400 mL of 4% acetic acid aqueous solution was added to the pretreated glass liquor bottle sample, sealed, and ultrasonicated for 0 min, 10 min, 20 min, 30 min, 40 min and 50 min respectively. After immersion extraction in a constant temperature water bath at 100±1℃ for 120 min, the sample was cooled after immersion. Three parallel samples were set for each group.

[0064] (3) Soaking solution collection: Take out the soaking solution, filter it with a 0.22μm filter membrane to remove suspended impurities, and obtain the test solution.

[0065] (4) ICP-OES detection

[0066] To prepare a standard curve: Take appropriate amounts of the mixed standard stock solution (concentration of 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set to 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Detect the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and use the instrument's built-in analysis software to plot the standard curve. Through linear regression analysis, obtain the standard curve equation and correlation coefficient for each element.

[0067] Sample determination: Before each sample determination, the system was rinsed with nitric acid. After the analytical signal value stabilized, the soaking solution was tested by ICP-OES under the same instrument reference conditions and operating procedures as when establishing the standard curve. The signal response value of the target element was determined. The concentration of the target element in the extract was obtained according to the standard curve. Laboratory blank samples were determined under the same instrument reference conditions and operating procedures.

[0068] ICP-OES detection parameter settings: The above-mentioned test liquid was tested by ICP-OES to detect the leaching concentration of the target element in the glass; the ICP-OES detection parameters were: radio frequency power: 1147 W; carrier gas flow rate: 0.50 L / min; carrier gas pressure: 2.13 bar; auxiliary gas flow rate: 0.50 L / min; cooling gas flow rate: 12.5 L / min.

[0069] (5) Calculation of results: The total amount of oxides in the glass liquor bottle sample was calculated according to Formula I based on the detected values ​​of Na, K and Ca in the soaking solution. The total amount of oxides in the sample was expressed as the number of micrograms of sodium oxide contained in each milliliter of extract.

[0070] (6) Results Analysis: Ultrasonic treatment can alter the microstructure and chemical stability of the inner surface of glass liquor bottles through cavitation and microjets. The effects of different ultrasonic times on the water resistance of glass liquor bottles are shown in the following figures. Figure 2 As shown, the inner surface of the blank group of glass bottles without ultrasound treatment (0 min) remained in its original, molded state, with the lowest total oxide content. After a short ultrasound treatment of 10–20 min, the micro-impact generated by ultrasonic cavitation effectively removed residual dust and loose silicate particles adhering to the inner surface of the bottle, significantly increasing the total oxide content. When the ultrasound time was extended to 30 min, the continuous cavitation impact began to cause slight damage to the inner surface of the glass, and the repeated impact of the high-frequency micro-jets on the surface caused the total oxide content to continue to increase. When the ultrasound time was increased to 40–50 min, ion dissolution tended to stabilize. In summary, ultrasound treatment for 30 min is preferred for extracting the target elements from glass liquor bottles.

[0071] 3.3.3 Selection of soaking time

[0072] (1) Sample pretreatment: Randomly select a batch of glass liquor bottles of the same specification (500mL) from the same manufacturer, rinse the inner surface of the bottle with deionized water 3-5 times to remove all dirt and packaging debris and other impurities, place them in an oven at 60-80℃ to dry to constant weight, and cool to room temperature for later use.

[0073] (2) Immersion test: The extraction of target elements from glass liquor bottles was investigated at immersion times of 0 min, 30 min, 60 min, 90 min, 120 min, 150 min, and 180 min. The specific experimental steps were as follows: 400 mL of 4% acetic acid aqueous solution was added to the pretreated glass liquor bottle sample, sealed, sonicated for 30 min, and then placed in a constant temperature water bath at 100±1℃ for immersion and extraction at 0 min, 30 min, 60 min, 90 min, 120 min, 150 min, and 180 min, respectively. The sample was cooled after immersion. Three parallel samples were set up for each group.

[0074] (3) Soaking solution collection: Take out the soaking solution, filter it with a 0.22μm filter membrane to remove suspended impurities, and obtain the test solution.

[0075] (4) ICP-OES detection

[0076] To prepare a standard curve: Take appropriate amounts of the mixed standard stock solution (concentration of 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set to 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Detect the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and use the instrument's built-in analysis software to plot the standard curve. Through linear regression analysis, obtain the standard curve equation and correlation coefficient for each element.

[0077] Sample determination: Before each sample determination, the system was rinsed with nitric acid. After the analytical signal value stabilized, the test solution was tested by ICP-OES under the same instrument reference conditions and operating procedures as when establishing the standard curve. The signal response value of the analyte was measured, and the concentration of the analyte in the extract was obtained according to the standard curve. Laboratory blank samples were determined under the same instrument reference conditions and operating procedures.

[0078] ICP-OES detection parameter settings: The above-mentioned test liquid was tested by ICP-OES to detect the leaching concentration of the target element in the glass; the ICP-OES detection parameters were: radio frequency power: 1147 W; carrier gas flow rate: 0.50 L / min; carrier gas pressure: 2.13 bar; auxiliary gas flow rate: 0.50 L / min; cooling gas flow rate: 12.5 L / min.

[0079] (5) Calculation of results: The total amount of oxides in the glass liquor bottle sample was calculated according to Formula I based on the detected values ​​of Na, K and Ca in the soaking solution. The total amount of oxides in the sample was expressed as the number of micrograms of sodium oxide contained in each milliliter of extract.

[0080] (6) Results Analysis: The effects of different soaking times on the water resistance of the inner surface of glass liquor bottles are as follows: Figure 3 As shown in the figure, the inner surface of the blank sample bottle after soaking for 0 min is intact and dense, with no obvious traces of hydrolysis. Na + K + The leaching amount of alkali metal ions was initially at an extremely low level. When the immersion time increased to the range of 30–90 min, the ion exchange depth continued to increase with time, leading to a rise in the leaching amount of alkali metal ions. Localized corrosion preferentially occurred at microscopic defects on the inner wall of the bottle and at microcracks in the molding process, resulting in a significant increase in the total amount of oxides. After the immersion time reached 120 min, the high-temperature immersion environment continuously damaged the surface hydration layer, leading to an increase in OH... -The gradual attack on the Si–O–Si covalent bonds leads to localized dissolution of the glass network framework, with alkali metals and silicon simultaneously leaching out in large quantities. After immersion for 150–180 minutes, the etching process gradually reaches a stable state. In summary, short-term immersion only results in reversible surface ion exchange, having a limited impact on the substrate's durability, but continuously extending the immersion time exacerbates the deterioration of the inner surface. Therefore, an immersion time of 120 minutes is preferred for extracting the target elements from the glass liquor bottle, as this not only fully reflects the water corrosion resistance of the inner surface of the glass liquor bottle but also shortens the detection cycle.

[0081] 3.3.4 Selection of Immersion Solution Concentration

[0082] (1) Sample pretreatment: Randomly select a batch of glass liquor bottles of the same specification (500mL) from the same manufacturer, rinse the inner surface of the bottle with deionized water 3-5 times to remove all dirt and packaging debris and other impurities, place them in an oven at 60-80℃ to dry to constant weight, and cool to room temperature for later use.

[0083] (2) Immersion test: The experiment set up immersion solutions of acetic acid aqueous solution with concentrations of 0%, 2%, 3%, 4%, 5%, 10% and 15% to extract the target elements in glass liquor bottles, and investigated the effect of different concentrations of acetic acid solution on the total amount of oxides, and selected the optimal acetic acid concentration. The specific experimental steps are as follows: 400 mL of acetic acid aqueous solution with concentrations of 0 (ultrapure water), 2%, 3%, 4%, 5%, 10% and 15% were added to the pretreated glass liquor bottle samples, sealed, sonicated for 30 min, and then immersed in a constant temperature water bath at 100±1℃ for 120 min. After immersion, the samples were cooled. Three parallel samples were set up for each group.

[0084] (3) Soaking solution collection: Take out the soaking solution, filter it with a 0.22μm filter membrane to remove suspended impurities, and obtain the test solution.

[0085] (4) ICP-OES detection

[0086] To prepare a standard curve: Take appropriate amounts of the mixed standard stock solution (concentration of 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set to 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Detect the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and use the instrument's built-in analysis software to plot the standard curve. Through linear regression analysis, obtain the standard curve equation and correlation coefficient for each element.

[0087] Sample determination: Before each sample determination, the system was rinsed with nitric acid. After the analytical signal value stabilized, the test solution was tested by ICP-OES under the same instrument reference conditions and operating procedures as when establishing the standard curve. The signal response value of the analyte was measured, and the concentration of the analyte in the extract was obtained according to the standard curve. Laboratory blank samples were determined under the same instrument reference conditions and operating procedures.

[0088] ICP-OES detection parameter settings: The above-mentioned test liquid was tested by ICP-OES to detect the leaching concentration of the target element in the glass; the ICP-OES detection parameters were: radio frequency power: 1147 W; carrier gas flow rate: 0.50 L / min; carrier gas pressure: 2.13 bar; auxiliary gas flow rate: 0.50 L / min; cooling gas flow rate: 12.5 L / min.

[0089] (5) Calculation of results: The total amount of oxides in the glass liquor bottle sample was calculated according to Formula I based on the detected values ​​of Na, K and Ca in the soaking solution. The total amount of oxides in the sample was expressed as the number of micrograms of sodium oxide contained in each milliliter of extract.

[0090] (6) Results Analysis: Acetic acid, as the main organic acid naturally generated during the storage of baijiu, directly affects the degree of corrosion on the inner surface of the glass due to the concentration of its aqueous solution. The results of the effect of different soaking solution concentrations on the water corrosion resistance of the inner surface of the glass baijiu bottle are as follows: Figure 4 As shown, with pure water as a blank control, the dissolution of alkali metal ions in the glass network is relatively slow, and the total amount of oxides is the lowest. In the low-concentration acetic acid (2%~5%) system, the trace hydrogen ions generated by solution dissociation can exacerbate the displacement dissolution reaction of metal ions on the glass surface, and the degree of glass matrix corrosion gradually intensifies with a slight increase in acetic acid concentration. When the acetic acid concentration is increased to 10% and 15%, the amount of ion precipitation on the glass surface does not continue to increase with the increase in acidity, but instead shows a decreasing trend. This phenomenon is mainly due to the weak electrolyte dissociation characteristics of acetic acid and the role of interfacial reaction equilibrium regulation. With a significant increase in system concentration, the concentration of acetate ions in the solution increases significantly, producing a strong common ion effect, inhibiting the dissociation process of acetic acid molecules, and effectively reducing the destruction of glass silicon-oxygen bonds by hydrogen ions and the driving force of metal ion displacement. In addition, the salting-out effect of high-concentration systems will reduce the solubility of metal ions in the immersion solution and weaken the macroscopic manifestation of ion precipitation. Overall, an acetic acid solution concentration of 3%~5% is better, preferably 4%.

[0091] 3.3.5 Selection of Immersion Temperature

[0092] (1) Sample pretreatment: Randomly select a batch of glass liquor bottles of the same specification (500mL) from the same manufacturer, rinse the inner surface of the bottle with deionized water 3-5 times to remove all dirt and packaging debris and other impurities, dry them in an oven at 60-80℃ until constant weight, and cool them to room temperature for later use.

[0093] (2) Immersion test: The extraction of target elements from glass liquor bottles was investigated at immersion temperatures of 25℃, 40℃, 60℃, 80℃ and 100℃. The specific experimental steps are as follows: 400mL of 4% acetic acid aqueous solution was added to the pretreated glass liquor bottle sample, sealed, and sonicated for 30 min. Then, the sample was immersed in a constant temperature water bath at 25℃, 40℃, 60℃, 80℃ and 100℃ for 120 min, respectively, and cooled after immersion. Three parallel samples were set up for each group.

[0094] (3) Soaking solution collection: Take out the soaking solution, filter it with a 0.22μm filter membrane to remove suspended impurities, and obtain the test solution.

[0095] (4) ICP-OES detection

[0096] To prepare a standard curve: Take appropriate amounts of the mixed standard stock solution (concentration of 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set to 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Detect the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and use the instrument's built-in analysis software to plot the standard curve. Through linear regression analysis, obtain the standard curve equation and correlation coefficient for each element.

[0097] Sample determination: Before each sample determination, the system was rinsed with nitric acid. After the analytical signal value stabilized, the test solution was tested by ICP-OES under the same instrument reference conditions and operating procedures as when establishing the standard curve. The signal response value of the analyte was measured, and the concentration of the analyte in the extract was obtained according to the standard curve. Laboratory blank samples were determined under the same instrument reference conditions and operating procedures.

[0098] ICP-OES detection parameter settings: The above-mentioned test liquid was tested by ICP-OES to detect the leaching concentration of the target element in the glass; the ICP-OES detection parameters were: radio frequency power: 1147 W; carrier gas flow rate: 0.50 L / min; carrier gas pressure: 2.13 bar; auxiliary gas flow rate: 0.50 L / min; cooling gas flow rate: 12.5 L / min.

[0099] (5) Calculation of results: The total amount of oxides in the glass liquor bottle sample was calculated according to Formula I based on the detected values ​​of Na, K and Ca in the soaking solution. The total amount of oxides in the sample was expressed as the number of micrograms of sodium oxide contained in each milliliter of extract.

[0100] (6) Results Analysis: Sodium-calcium silicate glass is the mainstream substrate for liquor packaging. The long-term synergistic effect of acetic acid and water in the liquor can lead to ion dissolution and skeletal corrosion of the inner wall. Immersion temperature, as a key variable in corrosion kinetics, directly regulates the ion exchange rate and the degree of silicon-oxygen network damage. The results of the influence of different immersion temperatures on the water resistance of the inner surface of glass liquor bottles are as follows: Figure 5 As shown, under immersion conditions at 25℃, the corrosion reaction on the glass surface is in the low activation energy range, and the total amount of ion precipitation is extremely low. When the temperature is raised to 40℃ and 60℃, H... + Interdiffusion efficiency with alkali metals is significantly enhanced, and the amount of ion dissolution increases significantly with increasing temperature. When the immersion temperature reaches 80℃ and 90℃, on the one hand, the high temperature accelerates ion exchange, and a large amount of alkali metals continuously migrate out; on the other hand, water molecules and hydrogen ions synergistically attack Si-O-Si bonds, resulting in the continuous dissolution of metal ions. The erosion effect reaches its peak at 100℃, with a large amount of calcium and sodium migrating out. Overall, temperature is significantly positively correlated with the degree of erosion on the inner surface of the glass. At low temperatures, the passivation layer maintains chemical stability, while at high temperatures, the water and acid erosion resistance of the soda-lime-silica glass bottle is significantly weakened. To better simulate the accelerated erosion test, the optimal immersion temperature was determined to be 100℃.

[0101] 3.4 Specific steps of optimized preprocessing

[0102] The inner surface of the glass liquor bottle was rinsed with deionized water 3-5 times to remove all dirt and packaging debris. The bottle was then dried in an oven at 60-80℃ until constant weight. After cooling to room temperature, 400mL of 4% acetic acid aqueous solution was added, the bottle was sealed, and ultrasonically treated for 30min. The bottle was then immersed and extracted in a digital display constant temperature water bath at 100±1℃ for 120min. After extraction, the bottle was cooled to room temperature, the soaking solution was removed, and the solution was filtered through a 0.22μm filter membrane to remove suspended impurities, thus obtaining the solution to be tested.

[0103] 3.5 Analytical and Testing Procedures

[0104] ICP-OES was used to analyze the test solution to obtain the leaching concentration of the target elements (Na, K and Ca) in the test solution, and the total amount of oxides in the immersion solution of the glass liquor bottle sample was calculated based on the detected values ​​of Na, K and Ca in the test solution.

[0105] Specifically: Take appropriate amounts of Na, K, and Ca mixed standard stock solution (concentration 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions with concentration gradients of 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. Analyze the prepared mixed standard solutions sequentially, record the emission intensity of each element at the selected wavelength, and plot the standard curve using the instrument's built-in analysis software. Obtain the standard curve equation and correlation coefficient for each element through linear regression analysis. Following the same instrument reference conditions and operating procedures as when establishing the standard curve, analyze the glass liquor bottle soaking solution using ICP-OES to determine the signal response values ​​of the analytes. Calculate the detection values ​​of Na, K, and Ca in the test solution based on the standard curve.

[0106] According to Formula I, the content of oxides in the glass liquor bottle sample was calculated based on the detected values ​​of Na, K, and Ca in the soaking solution. The formula for calculating the total amount of oxides is shown in Formula I: Formula I In Formula I: X: Total amount of oxides in the sample solution, μg / mL; C Na : The detected value of sodium oxide in the sample solution, in μg / mL; C K : The detected value of potassium oxide in the sample solution, in μg / mL; C Ca : Detection value of calcium oxide in the sample solution, μg / mL; σ K Conversion factor: 0.658; σ Ca Conversion factor: 1.105.

[0107] IV. Methodological Validation

[0108] In some embodiments, a specific method for determining the water resistance of the inner surface of a glass liquor bottle is as follows: Pretreatment steps: Randomly select a batch of glass liquor bottles of the same specification (500mL) from the same manufacturer, rinse the inner surface of the bottles with deionized water 3-5 times to remove all dirt and packaging debris and other impurities, dry them in an oven at 60~80℃ until constant weight, cool them to room temperature, add 400mL of 4% acetic acid aqueous solution, seal, sonicate for 30min, and soak and extract in a digital display constant temperature water bath at 100±1℃ for 120min. After that, cool to room temperature, take out the soaking solution, filter it through a 0.22μm filter membrane to remove suspended impurities, and obtain the test solution.

[0109] 4.1 Method linear range and detection limit

[0110] A series of standard working solutions with concentrations of 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL were analyzed according to the ICP-OES detection procedure to obtain the standard curve regression equations for the three target elements Na, K, and Ca. Table 1 shows that the correlation coefficients for Na, K, and Ca in the range of 0–20 μg / mL were 0.9997, 1.0000, and 0.9990, respectively, indicating good linearity.

[0111] Table 1. Linear equations and detection limits for the three target elements.

[0112] 4.2 Precision Test

[0113] Three glass liquor bottles (500mL each) from different manufacturers were selected as test samples for the precision experiment. The extract was prepared according to the pretreatment method described in 3.4. The extracts from the glass liquor bottles of each manufacturer were prepared repeatedly for 6 times. The total amount of oxides in each of the 6 tests of the glass liquor bottles of each manufacturer was calculated according to the calculation method of Formula I.

[0114] The relative standard deviation (RSD) was calculated based on the test results, and the results are shown in Table 2. Table 2 shows that the RSD values ​​of the precision test for glass liquor bottles from the three manufacturers are all <5%, indicating that the test method has good precision and repeatability, and can well meet the requirements for testing the water resistance of the inner surface of glass liquor bottles.

[0115] Table 2. Results of Precision and Repeatability Tests

[0116] 4.3 Stability Test

[0117] Three glass liquor bottles (500mL each) from different manufacturers were selected for pretreatment. Analysis was performed at 0h, 1h, 5h, 12h, and 24h after pretreatment. The RSD values ​​were calculated based on the results, as shown in Table 3. Table 3 shows that the total oxide content of the tested glass liquor bottle samples did not differ significantly within 0–24h, and the RSD of the stability test results ranged from 0.655% to 0.764%, indicating good stability of the method.

[0118] Table 3 Stability test results

[0119] Note: The letter 'a' in Table 3 represents the results of the significance analysis. If both are marked with 'a', it indicates that there is no significant difference between the measurement results.

[0120] 4.4 Spike Recovery Test

[0121] To verify the accuracy of the detection method, the standard addition method was used. A 500mL glass liquor bottle sample was selected for the spiked recovery experiment. After sample pretreatment, mixed standard solutions with low, medium, and high concentrations were added to the extract. The samples were then analyzed according to the established method, and the detection results and spiked recoveries of each target element were calculated. The results are shown in Table 4. As can be seen from Table 4, at the three concentration levels, the spiked recoveries of each target element in this method were between 90.476% and 107.240%, which met the methodological requirements and indicated that the detection method had good accuracy.

[0122] Table 4 Results of Spiked Recovery Test

[0123] In summary, the method of the present invention has good precision and accuracy, and can meet the requirements for determining the water resistance of the inner surface of glass liquor bottles.

[0124] 4.5 Comparison of test results with the pretreatment methods in the national standard testing methods

[0125] The test, conducted according to the pretreatment methods (i.e., 4.5.1 and 4.5.2 below) in GB / T 4548.2-2003 "Determination and Classification of Water Erosion Resistance of Inner Surface of Glass Products and Glass Containers by Flame Spectrometry" combined with the sample testing method of this invention, determined the water erosion resistance of the inner surface of three glass liquor bottles from different manufacturers for comparison. The specific test steps are as follows: 4.5.1 Reagent Preparation (1) Test water: free of heavy metals.

[0126] (2) Hydrochloric acid solution.

[0127] (3) Spectrochemical buffer solution (cesium chloride CsCl solution): Dissolve 80 g of cesium chloride in about 300 mL of test water, add 10 mL of hydrochloric acid, and then transfer to a 1000 mL volumetric flask and shake well.

[0128] (4) Standard solution: Dilute the base solution with test water to a certain appropriate concentration.

[0129] (5) Reference solution: Dilute the appropriate concentration of the standard solution with test water to obtain a series of reference solutions that constitute the standard curve.

[0130] 4.5.2 Preparation of Sample Solution and Standard Solution

[0131] (1) Sample preparation: Randomly select a batch of glass liquor bottles of the same specifications from 3 manufacturers, remove all dirt and packaging debris from the container, rinse the inner surface of the bottle with deionized water 3-5 times, fill with test water, seal and place it in a high temperature and high pressure vessel containing distilled water, heat to 121℃, keep the temperature constant for 60min, take it out after the temperature drops to 100℃, put it in an 80℃ water bath, inject cooling water to make the sample cool to room temperature as soon as possible before testing.

[0132] (2) Preparation of standard solutions: Take appropriate amounts of mixed standard stock solution (concentration of 1000 μg / mL) and dilute it stepwise with 6% nitric acid solution to prepare a series of mixed standard solutions of different concentrations. The specific concentration gradients are set to 0 μg / mL, 2 μg / mL, 4 μg / mL, 6 μg / mL, 8 μg / mL, 10 μg / mL, and 20 μg / mL. The prepared mixed standard solutions are detected sequentially, and the emission intensity of each element at the selected wavelength is recorded. The standard curve is plotted using the instrument's built-in analysis software. The standard curve equation and correlation coefficient of each element are obtained through linear regression analysis.

[0133] 4.5.3 Sample Determination

[0134] Following the same instrument reference conditions and operating procedures as when establishing the standard curve, the test solution was tested using an ICP-OES instrument to determine the signal response value of the analyte. The concentration of the analyte in the extract was obtained according to the standard curve. The blank sample was then tested under the same instrument reference conditions and operating procedures.

[0135] ICP-OES detection parameter settings: The above-mentioned test liquid was tested by ICP-OES to detect the leaching concentration of the target element in the glass; the ICP-OES detection parameters were: radio frequency power: 1147 W; carrier gas flow rate: 0.50 L / min; carrier gas pressure: 2.13 bar; auxiliary gas flow rate: 0.50 L / min; cooling gas flow rate: 12.5 L / min.

[0136] 4.5.4 Result Calculation

[0137] Calculate according to the formula shown in Equation I.

[0138] 4.5.5 Results Analysis

[0139] As shown in Table 5, the deviation between the total oxide content in the three manufacturers' glass liquor bottles measured by the national standard pretreatment method and the pretreatment method of this method (3.4 optimized pretreatment steps) is between 2.426% and 4.226%, all less than 5%, indicating that the test results are accurate and reliable. In summary, this method can achieve accurate and rapid determination of the water resistance of the inner surface of glass liquor bottles.

[0140] Table 5. Test results of water resistance of the inner surface of glass liquor bottles

[0141] This invention provides a method for determining the water resistance of the inner surface of a glass liquor bottle using ICP-OES. By systematically optimizing five experimental factors—immersion volume, ultrasonic time, immersion time, immersion solution concentration, and immersion temperature—the method achieves accurate and efficient determination of the water resistance of the inner surface of the glass liquor bottle. In summary, this application provides a rapid and efficient method for determining the water resistance of the inner surface of a glass liquor bottle. In this embodiment, only an acidic solution is used for ultrasonic extraction followed by heating to extract the target elements, eliminating the need for high-temperature and high-pressure equipment. ICP-OES is then used to detect Na, K, and Ca in the extract, thereby achieving rapid determination of the water resistance of the inner surface of the glass liquor bottle. This extraction method offers higher accuracy compared to titration methods.

[0142] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for determining the water resistance of the inner surface of a glass liquor bottle, characterized in that, Includes the following steps: A) Add soaking solution to the treated glass liquor bottle, seal it, and after ultrasonic treatment, perform soaking treatment to obtain soaking solution. The soaking solution is an aqueous solution of acetic acid with a volume concentration of 2-15%. B) After filtering the soaking solution, perform ICP-OES detection, and calculate the total amount of oxides based on the detected dissolution concentration of the target element.

2. The method according to claim 1, characterized in that, The treated glass liquor bottles are processed according to the following method: After rinsing the inner surface of the bottle with deionized water 3-5 times, place it in an oven at 60-80℃ to dry to constant weight, and then cool to room temperature.

3. The method according to claim 1, characterized in that, The amount of the soaking solution added is 20% to 100% of the nominal capacity of the glass liquor bottle.

4. The method according to claim 1, characterized in that, The ultrasonic treatment has a power of 700W and a duration of 10-50 minutes.

5. The method according to claim 1, characterized in that, The soaking temperature is 25~100℃ and the soaking time is 30~180min.

6. The method according to claim 1, characterized in that, The filtration process uses a 0.22 μm filter membrane.

7. The method according to claim 1, characterized in that, The ICP-OES detection parameters are: RF power 1147W, carrier gas flow rate 0.50L / min, carrier gas pressure 2.13bar, auxiliary gas flow rate 0.50L / min, and cooling gas flow rate 12.5L / min.

8. The method according to claim 1, characterized in that, The target elements include Na, K, and Ca.

9. The method according to claim 1, characterized in that, The method for calculating the total amount of oxides includes: calculating the average concentration of each oxide in each sample by comparing it with the standard curve, and expressing it as the number of micrograms of sodium oxide contained in each milliliter of extract, and then calculating the total content of oxides.

10. The method according to claim 1, characterized in that, The formula for calculating the total amount of oxides is shown in Equation I: Equation I In Formula I: X: Total amount of oxides in the sample solution, μg / mL; C Na : The detected value of sodium oxide in the sample solution, in μg / mL; C K : The detected value of potassium oxide in the sample solution, in μg / mL; C Ca : Detection value of calcium oxide in the sample solution, μg / mL; σ K Conversion factor: 0.658; σ Ca Conversion factor: 1.105.