A method and system for in-situ field aging test of stay cable PE

By combining multi-dimensional environmental conditions and correcting spectral signals using contact transfer functions, the problem of misjudgment caused by surface contamination and changes in contact conditions in on-site infrared detection was solved, enabling accurate stratified evaluation of the aging state of the PE sheath of the cable-stayed bridge and scientific operation and maintenance decisions.

CN123135733APending Publication Date: 2026-11-20JSTI GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611278529.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In on-site in-situ contact infrared spectroscopy testing, misjudgments caused by surface contamination and changes in contact conditions have led to normally functioning cable stays being mistakenly identified as requiring emergency replacement, resulting in unnecessary maintenance costs and traffic disruptions.

Method used

By constructing a multi-dimensional environmental state combination and using the contact transfer function to correct the spectral signal, we can achieve accurate hierarchical analysis of the degree of aging and oxidation and prediction of oxidation induction time. By using dual-probe depth in-situ sampling and synchronous binding of multi-dimensional environmental state combination data, we can eliminate the misjudgment of the degree of aging caused by overall spectral intensity distortion and surface contamination.

Benefits of technology

It significantly avoids misjudging the degree of aging due to surface-limited contamination, enables quantitative and stratified evaluation of the aging state of cable sheaths, improves the accuracy of detection and the scientific nature of operation and maintenance decisions, and meets the needs of non-destructive assessment of material aging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123135733A_ABST
    Figure CN123135733A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of cable detection, and discloses a cable PE in-situ aging test method and system, which comprises the following steps: synchronously binding contact load values, surface temperature values and sheath geometric curvature values through double-probing-depth sampling, performing contact state correction and pollution discrimination, performing differential layer analysis calculation according to an effective probing depth constant, separating surface layer oxidation physical values, subsurface layer oxidation physical values and oxidation depth gradient values, inputting the values into a preset constraint regression equation to output oxidation induction time prediction values and trigger a maintenance instruction; through the contact transfer function correction of the double-probing-depth sampling and the multi-dimensional environmental state binding, the evaluation distortion problem caused by the contact state difference and surface attachment interference under single-probing-depth sampling is solved, and the layered quantitative evaluation of the aging degree under the condition of not cutting the sample is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cable-stayed bridge testing technology, and in particular to a method and system for in-situ aging testing of PE cables in cable-stayed bridges. Background Technology

[0002] As cable-stayed bridges age, aging detection of the PE sheaths of the cables has become a crucial step in assessing their safety. In-situ contact infrared spectroscopy is widely used. This technique involves pressing a handheld probe against the sheath surface to collect the infrared reflectance spectrum of the polyethylene material. The carbonyl index is calculated based on the area of ​​characteristic absorption bands, thus quantitatively determining the degree of oxidative degradation of the PE sheath. This portable testing method can quickly obtain surface chemical information without opening the sheath, providing a reference for cable maintenance.

[0003] In actual testing, when the probe is pressed against an inclined sheath surface with different curvatures and surface temperatures, and the sheath surface has naturally attached contaminants such as dust or rain streaks, the collected spectral data will fluctuate wildly and irregularly with slight changes in probe contact pressure. For example, when testing the sun-facing side of a large-diameter cable, the sheath surface is covered with a visible powdery layer. Even slight changes in the force applied by the operator holding the probe, or instability caused by changes in cable diameter, will immediately cause the carbonyl index of the collected spectrum to rise. If the detection system judges solely based on the average spectrum of this surface, it will directly classify the area as severely aged and trigger a high-risk alarm. However, on-site sampling revealed that the powdery contamination was only present in the surface layer of a few micrometers, and the subsurface PE material had not undergone substantial structural degradation. This misjudgment led the operator to mistakenly identify a normally functioning cable as a critically damaged component requiring urgent replacement, resulting in unnecessary maintenance investment and traffic disruption. Therefore, how to avoid misjudgments caused by surface contamination and changes in contact conditions during on-site in-situ contact infrared spectroscopy testing is a problem that urgently needs to be solved in this field. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the present invention aims to provide an in-situ aging test method for PE cables. By constructing a multi-dimensional combination of environmental states and using contact transfer function to correct the spectral signal, the method achieves accurate hierarchical analysis of the degree of aging and oxidation and prediction of oxidation induction time.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] In a first aspect, the present invention provides a method for in-situ aging test of PE for cable-stayed bridges, comprising:

[0007] The first and second depth infrared spectral signals are acquired by infrared acquisition equipment, and the contact load value, surface temperature value and sheath geometric curvature are read simultaneously to generate a multi-dimensional environmental state combination.

[0008] Substitute the multidimensional environmental state combination into the contact transfer function to calculate the absorption band integral correction coefficient, and use the absorption band integral correction coefficient to correct the first depth infrared spectral signal and the second depth infrared spectral signal to generate the first carbonyl index estimate and the second carbonyl index estimate.

[0009] By combining the effective detection depth constant of the dual channels, differential stratification is performed on the first carbonyl index estimate and the second carbonyl index estimate to separate the surface oxidation physical properties, subsurface oxidation physical properties and oxidation depth gradient value.

[0010] Substitute the surface oxidation physical quantity, the subsurface oxidation physical quantity, and the oxidation depth gradient value into a preset constraint regression equation to calculate the oxidation induction time prediction and trigger a maintenance command.

[0011] Furthermore, acquiring the first depth infrared spectral signal and the second depth infrared spectral signal through the infrared acquisition device includes: switching the indexing disk inside the infrared acquisition device so that attenuated total internal reflection crystals with different refractive index physical properties are successively attached to the detection surface at the same detection point and on the same loading axis; driving the indexing disk to sequentially switch to the first indexing position and the second indexing position so that the germanium crystal and the diamond crystal are attached at the same detection point, and acquiring the first depth original spectrum and the second depth original spectrum; and sequentially acquiring and outputting the first depth infrared spectral signal and the second depth infrared spectral signal.

[0012] Furthermore, the step of sequentially attaching attenuated total internal reflection crystals with different refractive index physical properties to the detection surface at the same detection point and on the same loading axis includes: pressing the infrared acquisition device onto the sheath detection point using an independent fixing component and a curved self-centering positioning component; adjusting the contact load value into the contact stability platform range using a constant pressure floating loading component and outputting the load time series; and setting the contact state ready flag when all continuous sampling points of the pressure sensor fall into the contact stability platform range and the duration is not less than the single spectral cumulative scan duration.

[0013] Furthermore, the contact stability platform interval includes: a lower and upper boundary of the contact stability platform interval determined by load step calibration; the contact load value is increased from 6 Newtons to 34 Newtons in 2-Newton steps, the integral area of ​​the polyethylene reference absorption band is collected once for each load level, and the relative change rate of the reference band area between adjacent levels is calculated. The load level where the relative change rate first falls below 1% per Newton is taken as the lower boundary of the contact stability platform interval; after the pressure is released, the indentation depth is measured with a portable profilometer, and the lowest load level with an indentation depth exceeding 5 micrometers is taken minus one step as the upper boundary of the contact stability platform interval.

[0014] Furthermore, after acquiring the first depth original spectrum and the second depth original spectrum, the method further includes: selecting a stable window based on the load time series, including only interferograms falling within the stable window in the cumulative scan, discarding interferograms falling outside the window and automatically rescanning them; acquiring the pre-detection reference spectrum and post-detection reference spectrum of the reference material block in the same optical path, and extracting the pre-detection reference band area and post-detection reference band area respectively; calculating the drift correction coefficient based on the ratio of the reference band area to the current reference band area obtained by time linear interpolation, performing drift correction on the first depth original spectrum and the second depth original spectrum, and outputting the first depth infrared spectral signal and the second depth infrared spectral signal.

[0015] Furthermore, the synchronous reading of contact load value, surface temperature value, and sheath geometric curvature includes: reading the electrical signal of the pressure sensor at the end of the clamping mechanism and converting it into a contact load value; taking the arithmetic mean of all sampling points within the stable window as the contact load value of this measuring point; reading the thermoelectric potential signal of the thermocouple sensor and converting it into a surface temperature value according to the K-type thermocouple calibration table after cold junction compensation; receiving the outer diameter of the sheath measured by the handheld laser diameter gauge and transmitted through the serial interface, and converting it into the sheath geometric curvature by dividing the sheath geometric curvature by 2.

[0016] Furthermore, the generation of multidimensional environmental state combinations includes: performing a continuous memory packaging operation on the contact load value, surface temperature value, and sheath geometric curvature value according to a preset data structure; the preset data structure is a fixed-length structure, and the field order is fixed as measurement point number, acquisition time, contact load value, surface temperature value, sheath geometric curvature value, and channel identifier; generating one multidimensional environmental state combination record for each of the first depth infrared spectral signal and the second depth infrared spectral signal, with the two records sharing the same measurement point number, and the acquisition time being the midpoint time of two cumulative scans respectively.

[0017] Further, the calculation of the absorption band integral correction coefficient includes: extracting the contact load value, surface temperature value, and sheath geometric curvature from the multidimensional environmental state combination; substituting the contact load value, surface temperature value, and sheath geometric curvature into the contact transfer function composed of a quadratic polynomial to perform multivariate algebraic operations to obtain the contact transfer function output value; and calculating the first absorption band integral correction coefficient and the second absorption band integral correction coefficient of the corresponding germanium crystal channel and the corresponding diamond crystal channel by using the ratio of the calibration reference band area to the contact transfer function output value.

[0018] Further, generating the first carbonyl index estimate and the second carbonyl index estimate includes: multiplying the absorption band integral correction coefficient by the spectral intensity amplitude sequences of the first and second deep infrared spectral signals respectively, and outputting the corrected infrared spectral signal; extracting the integral area of ​​the corrected infrared spectral signal in a preset interference wavenumber range and dividing it by a preset polyethylene reference band area to obtain a non-target interference parameter; generating a pollution alarm flag and terminating subsequent calculations when the non-target interference parameter is greater than a preset pollution judgment threshold; and extracting the integral area of ​​the carbonyl characteristic absorption band and dividing it by the integral area of ​​the polyethylene reference absorption band when the non-target interference parameter is less than or equal to the preset pollution judgment threshold, thereby generating the first carbonyl index estimate and the second carbonyl index estimate respectively.

[0019] Further, the differential analysis calculation includes: obtaining the crystal refraction parameters stored in the internal hardware register, substituting them into the attenuation total internal reflection penetration depth formula to calculate the first effective detection depth constant and the second effective detection depth constant; assigning the estimated value of the first carbonyl index to the surface oxidation physical quantity; multiplying the estimated value of the second carbonyl index by the second effective detection depth constant, subtracting the product of the estimated value of the first carbonyl index and the first effective detection depth constant, and then dividing by the difference between the second effective detection depth constant and the first effective detection depth constant to calculate the subsurface oxidation physical quantity, and calculating the ratio of the estimated value of the first carbonyl index to the estimated value of the second carbonyl index to output the oxidation depth gradient value.

[0020] Further, the calculation of the oxidation induction time prediction and triggering of the maintenance command includes: extracting the pre-configured multivariate constraint regression prediction equation in the data storage unit, wherein the coefficients corresponding to the subsurface oxidation physical quantities in the multivariate constraint regression prediction equation are forcibly constrained to non-positive polarity by hardware-level code; substituting the surface oxidation physical quantities, subsurface oxidation physical quantities, and oxidation depth gradient values ​​as independent variables into the multivariate constraint regression prediction equation to calculate the oxidation induction time prediction and outputting the confidence interval according to the calibrated residual standard deviation; comparing the oxidation induction time prediction with the safety period threshold; if the oxidation induction time prediction is lower than the safety period threshold, outputting a high-frequency eddy current verification command to start the external mechanical flaw detection equipment to perform physical verification operation; otherwise, maintaining the low-power standby state of the current detection equipment.

[0021] Secondly, the present invention provides an in-situ aging test system for PE cables, used to implement the above-mentioned in-situ aging test method for PE cables, the system comprising:

[0022] The spectral acquisition and environmental state combination generation module is used to acquire first-depth infrared spectral signals and second-depth infrared spectral signals through infrared acquisition equipment, and simultaneously read contact load values, surface temperature values ​​and sheath geometric curvature to generate multi-dimensional environmental state combinations.

[0023] The correction and carbonyl index estimation module is used to substitute the multidimensional environmental state combination into the contact transfer function to calculate the absorption band integral correction coefficient, and use the absorption band integral correction coefficient to correct the first depth infrared spectral signal and the second depth infrared spectral signal to generate the first carbonyl index estimation value and the second carbonyl index estimation value.

[0024] The differential stratification module is used to combine the effective detection depth constant of the dual channels to perform differential stratification on the first carbonyl index estimate and the second carbonyl index estimate, and separate the surface oxidation physical quantity, subsurface oxidation physical quantity and oxidation depth gradient value.

[0025] The oxidation induction time prediction and maintenance triggering module is used to substitute the surface oxidation physical quantity, the subsurface oxidation physical quantity and the oxidation depth gradient value into a preset constraint regression equation, calculate the oxidation induction time prediction, and trigger maintenance instructions.

[0026] Compared to existing technologies, the advantages of this invention are as follows: This invention solves the problems of overall spectral intensity distortion caused by fluctuations in contact load, surface temperature, and sheath curvature during on-site testing of PE sheaths for cable stays by simultaneously binding in-situ sampling with dual-probe depth and multi-dimensional environmental state data. It also addresses the mixing of surface dust, rain marks, or powdery layers with internal aging absorption. Through a pre-established contact transfer function, the on-site spectrum can calculate the absorption band integral correction coefficient in real time based on the simultaneously acquired contact load, surface temperature, and sheath geometric curvature values. This normalizes the spectra under different testing conditions to a unified benchmark, eliminating the incomparability caused by variations in hand-held pressing force and differences in cable diameter. Simultaneously, by using the effective probe depth constant of the dual channels for differential analysis, the surface contamination and the true oxidation state of the subsurface layer in the attenuated total reflection spectrum can be separated, obtaining the physical quantities of surface oxidation, the physical quantities of subsurface oxidation, and the oxidation depth gradient value, significantly avoiding misjudgments of aging degree due to surface-limited contamination. Furthermore, by outputting the oxidation induction time prediction through a regression equation with sign constraints, the on-site test results are directly correlated with the remaining antioxidant capacity of the sheath. This can provide proactive early warning for high-frequency eddy current verification, realize quantitative and hierarchical evaluation of the aging state of the cable sheath, improve the accuracy of testing and the scientific nature of operation and maintenance decisions, and meet the testing requirements for in-situ non-destructive assessment of material aging. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 This is a flowchart of an in-situ aging test method for PE cables in cable stays, as described in this invention.

[0029] Figure 2 This is a schematic diagram of the independent fixing component and the self-centering positioning component in an embodiment of the present invention;

[0030] Figure 3 This is a schematic diagram of the coaxial bonding installation of the sensor in an embodiment of the present invention;

[0031] Figure 4 This is a schematic diagram of the multi-dimensional environmental state combination data structure in an embodiment of the present invention;

[0032] Figure 5 This is a schematic diagram of the differential layer analysis depth coverage in an embodiment of the present invention;

[0033] Figure 6This is a schematic diagram of the high-frequency eddy current flaw detection equipment verification in an embodiment of the present invention;

[0034] Figure 7 This is a functional block diagram of an in-situ aging test system for cable-stayed PE in this invention. Detailed Implementation

[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] Example 1:

[0037] Please see Figure 1 As shown, this embodiment provides a method for in-situ aging testing of PE cables for cable stays, including:

[0038] This embodiment provides an in-situ aging test method for PE sheaths of cable-stayed bridges, used for quantitative evaluation of the aging degree of polyethylene sheaths on cable-stayed bridge cables under conditions where no samples are taken. For ease of understanding, the core terms with specific meanings in this embodiment are defined first. The multidimensional environmental state combination refers to a fixed-length data structure composed of contact load values, surface temperature values, and sheath geometric curvature values ​​acquired synchronously at the same spectral acquisition time, arranged in a fixed field order. The contact transfer function refers to a quadratic polynomial, fitted in advance on a polyethylene calibration sample of the same material and known curvature, with contact load values, surface temperature values, and sheath geometric curvature as independent variables and the integral area of ​​the polyethylene reference absorption band as the dependent variable. The absorption band integral correction coefficient is the ratio of the index-defined reference band area to the output value of the contact transfer function under the current multidimensional environmental state combination. The non-target interference parameter refers to the ratio of the integral area of ​​the corrected infrared spectral signal in the interference wavenumber interval unrelated to polyethylene skeleton absorption and carbonyl absorption to the integral area of ​​the polyethylene reference absorption band. The effective detection depth constant refers to the equivalent uniform thickness of infrared light effectively sampled within the sheath material when the attenuating total reflection crystal forms optical contact with the sheath surface. The differential stratification calculation refers to the algebraic operation that separates two carbonyl index estimates into oxidation indices in two thickness ranges—the surface layer and the subsurface layer—using the difference between the two effective detection depth constants.

[0039] The specific causes of spectral distortion in the field are as follows: The optical contact between the attenuating total reflectance crystal and the sheath is formed by compression. A change in the contact load value of a few tenths of a Newton alters the actual contact area and the residual contact gap, causing the integral area of ​​the polyethylene reference absorption band to rise or fall accordingly. The surface temperature of the sheath facing the sun can reach over 60 degrees Celsius, softening the polyethylene surface and causing the contact area to continue to expand under the same contact load value. Different cable diameters have different outer cylindrical surface curvatures, meaning that only a strip-shaped contact area can be formed between the planar crystal and the cylindrical surface, and the strip width narrows as the curvature increases. The combination of these three factors makes the ratio of the carbonyl characteristic absorption band area to the polyethylene reference absorption band area incomparable across cable diameters and environments. Another parallel cause is that dust, rain streaks, and powdery substances accumulate on the surface layer for several micrometers. Attenuating total reflectance spectra at a single detection depth mix the absorption from surface deposits with the absorption from internal materials, making it impossible to distinguish whether the carbonyl signal originates from surface deposits or subsurface structure degradation.

[0040] To address the two causes mentioned above, this embodiment is based on dual-probe depth sampling at the same point and on the same loading axis. The contact load value, surface temperature value, and sheath geometric curvature are synchronously bound to the spectral data. First, the spectral data is corrected for contact status and contamination is determined. Then, differential analysis is performed according to the effective probe depth constant. Finally, the oxidation induction time prediction is output as a regression equation with sign constraints, and maintenance instructions are triggered.

[0041] S1: Acquire first-depth infrared spectral signals and second-depth infrared spectral signals through infrared acquisition equipment, and simultaneously read contact load values, surface temperature values ​​and sheath geometric curvature to generate a multi-dimensional environmental state combination.

[0042] The sheath surface is an inclined cylindrical surface. When the probe is held by hand or supported by a basket, the contact load value fluctuates within a few Newtons due to hand tremors and slight wind-induced vibrations of the cable. If only the spectrum is stored without simultaneously recording the contact load value, surface temperature value, and sheath geometric curvature at the moment of acquisition, it is impossible to determine later whether a higher absorption band area in a particular acquisition is due to strong absorption of the material itself or a favorable fit. Furthermore, the difference in results between two re-measurements at the same point cannot be explained. Therefore, this step bundles the optical, mechanical, and thermal quantities for output at the same time, providing a verifiable record of physical conditions for subsequent corrections.

[0043] Further, step S1 includes:

[0044] S11: Switch the indexing plate inside the infrared acquisition device to allow attenuated total reflection crystals with different refractive index physical properties to be attached to the detection surface, and sequentially acquire and output the first depth infrared spectrum signal and the second depth infrared spectrum signal.

[0045] If the two attenuated total internal reflection channels are set at two different measurement points, the distribution of powdery spots and rain marks on the sheath surface itself has centimeter-level inhomogeneity. The spectral differences between the channels will be mixed with the positional differences, making it unusable for subsequent thickness-based differential calculations. Therefore, this step requires two crystals with different refractive indices to be bonded sequentially at the same detection point and on the same loading axis, switching only the crystals without moving the positioning base.

[0046] Further, step S11 includes:

[0047] S111: The infrared acquisition device is pressed onto the sheath detection point by an independent fixing component and a curved self-centering positioning component. The constant pressure floating loading component adjusts the contact load value into the contact stability platform range and outputs the contact status ready indicator and load time series.

[0048] Specifically, the independent fixing component is an elastic clamp that surrounds the sheath. The clamping force of the clamp is closed along the circumference of the sheath and is not transmitted to the crystal indenter along the loading axis, so that the fixing action and the loading action do not affect each other. The curved self-centering positioning component consists of two sets of V-shaped roller supports that can swing around the pin shaft. After the two sets of V-shaped roller supports are in contact with the outer cylindrical surface of the sheath, the loading axis of the crystal indenter passes through the center of the cross-section of the sheath. The working surface of the crystal and the cylindrical surface have symmetrical strip contact in the contact area, avoiding one-sided point contact at the edge of the crystal when the loading axis deviates from the normal.

[0049] The constant pressure floating loading assembly includes a constant force elastic element in the form of a pre-compressed helical spring and an anti-rotation guide element in the form of a linear ball bearing guide sleeve. The constant force elastic element has a stiffness of 2 Newtons per millimeter, and the anti-rotation guide element has an anti-rotation keyway to prevent the crystal from rotating around the loading axis during compression. If the crystal does rotate around the axis, the crystal edges will scratch the polyethylene surface and bring up powdery material, causing the subsequently collected spectrum to be infiltrated by the newly generated deposits. See also Figure 2 , Figure 2 This diagram illustrates the independent fixing component and the self-centering positioning component. The diagram shows the elastic clamp of the sheath, with the clamping force closed circumferentially through the sheath and not transmitted to the crystal indenter along the loading axis. Two sets of V-shaped rollers, capable of swinging around a pivot, support the outer cylindrical surface of the sheath, ensuring the loading axis of the crystal indenter passes through the center of the sheath's cross-section. The crystal's working surface and the cylindrical surface form symmetrical strip contact within the contact area. The constant-force elastic element is a pre-compressed helical spring, and the anti-rotation guide element is a linear ball bearing guide sleeve with an internal anti-rotation keyway, preventing the crystal from rotating around the loading axis during clamping. This structure ensures that the fixing and loading actions do not interfere with each other, avoiding one-sided point contact at the crystal edge when the loading axis deviates from the normal, and preventing scratches and powdering on the polyethylene surface caused by the crystal rotating around the axis, thus preventing the absorption of newly generated deposits in the subsequently collected spectrum.

[0050] The contact stability plateau interval is determined through load step calibration. During calibration, on the test section of the same specification sheath to be tested, the contact load value is increased from 6 Newtons to 34 Newtons in 2-Newton increments. The integrated area of ​​the polyethylene reference absorption band is collected every 5 seconds at each load level. The relative change rate of the reference band area between adjacent levels is calculated. The load level where the relative change rate first falls below 1% per Newton is taken as the lower boundary of the contact stability plateau interval. After pressure is released, the indentation depth is measured using a portable profilometer. The profilometer has a single-point repeatability accuracy of 2 micrometers. The lowest load level where the indentation depth exceeds 2.5 times the repeatability accuracy (5 micrometers) is subtracted from the lowest load level and taken as the upper boundary of the contact stability plateau interval. When the load is below the lower boundary, the contact area still increases rapidly with the load, and the spectrum is unreproducible. When the load is above the upper boundary, a measurable indentation is left on the polyethylene surface, constituting secondary damage. For example, the contact stability plateau interval is 12 Newtons to 22 Newtons.

[0051] The load time series refers to a one-dimensional array of contact load values ​​continuously output by the pressure sensor at a sampling rate of 200 Hz and arranged by timestamps. When all continuous sampling points fall within the contact stability platform range and the duration is not less than the duration of a single spectral cumulative scan, the control unit sets the contact state ready flag, which is a Boolean value.

[0052] S112: In response to the contact state ready flag, drive the indexing disk to switch sequentially to the first indexing position and the second indexing position, so that the germanium crystal and the diamond crystal are attached at the same detection point, and the first depth raw spectrum and the second depth raw spectrum are collected.

[0053] Specifically, the indexing disk is a two-position rotating indexing disk that rotates around the loading axis. A germanium crystal with a refractive index of 4.0 is installed at the first indexing position, and the angle between the crystal's working surface normal and the infrared incident light is set to 60 degrees. A diamond crystal with a refractive index of 2.4 is installed at the second indexing position, and the incident angle is set to 45 degrees. The indexing disk is driven by a stepper motor, with a repeatability deviation of no more than 0.05 degrees. During switching, the crystal pressure head retracts 1 mm along the loading axis and then resets and presses firmly, with the center offset of the contact imprint between the two contacts not exceeding 0.3 mm.

[0054] Data acquisition was performed using a portable Fourier transform infrared spectrometer with a spectral resolution of 4 wavenumbers. Each acquisition consisted of 32 scans, with an accumulation time of approximately 3 seconds. The effective wavenumber range of the first depth raw spectrum was 4000 to 900 wavenumbers, arranged in a one-dimensional absorbance array of length 776 at 4 wavenumber intervals. The effective wavenumber range of the second depth raw spectrum was 4000 to 652 wavenumbers, arranged in a one-dimensional absorbance array of length 838. Both wavenumber ranges collectively cover the carbonyl characteristic absorption band of 1700 to 1740 wavenumbers, the polyethylene reference absorption band of 1460 to 1480 wavenumbers, and the interfering wavenumber range used in subsequent determination.

[0055] Throughout the data acquisition process, the elastic lip rubber cover of the light-shielding and dust-proof module is pressed tightly against the surface of the protective sleeve. The inside of the cover is maintained with a slight positive pressure by purging with dry nitrogen at a rate of 0.2 liters per minute, blocking direct sunlight and dust from falling into the contact area. The infrared component of sunlight leaks into the detector laterally through the crystal, raising the baseline, while the slight positive pressure inside the cover prevents dust from entering the contact area during the interval between the two indexing switches.

[0056] S113: Based on the load time series, a stable window is selected, and the drift correction coefficient is calculated by time interpolation of the reference spectrum before and after detection of the reference material block with the same optical path. Drift correction is performed on the original spectrum of the first depth and the original spectrum of the second depth, and the infrared spectrum signal of the first depth and the infrared spectrum signal of the second depth are output.

[0057] During the on-site operation, the ambient temperature and the internal temperature of the instrument continuously change, causing the light source radiation intensity and detector response to change slowly. If the spectra collected in the morning and afternoon are directly compared on the same scale, the area of ​​the reference band will show an overall increase or decrease independent of the material. Therefore, this step involves collecting the spectrum of the reference material block along the same optical path before and after the test to account for the overall increase or decrease caused by time.

[0058] Specifically, the stabilization window refers to the time period in the load time series where the range of contact load values ​​at consecutive sampling points does not exceed the load range limit and the duration is not less than 3 seconds. The load range limit is taken as 5% of the width of the contact stabilization platform interval, which is 10 Newtons; therefore, the load range limit is 0.5 Newtons. Only interferograms falling within the stabilization window are included in the 32-scan accumulation; interferograms falling outside the window are discarded and automatically rescanned.

[0059] The reference material block with the same optical path is an unaged polyethylene block fixedly installed beside the indexing plate and can be flipped to face the crystal working face by a stepper motor. The reference material block and the sheath under test share the same optical path and the same detector. Before the test begins, the spectrum of the reference material block is acquired once to obtain the pre-test reference spectrum. After the test, it is acquired again to obtain the post-test reference spectrum. The wavenumber integration area from 1460 to 1480 is extracted and recorded as the pre-test reference band area and the post-test reference band area, respectively. The drift correction coefficient is calculated using time linear interpolation.

[0060]

[0061] In the formula, The reference reference band area is measured and written into the non-volatile memory by the reference material block under factory calibration conditions. The area of ​​the reference band before detection. The area of ​​the reference band after detection. This is the current data acquisition time at the measuring point. and These are the acquisition times of the reference spectra before and after detection, respectively, all taken from the same system clock of the spectrometer. The drift correction coefficient calculation expression uses linear time interpolation instead of averaging the two endpoints because the response changes of the light source and detector are monotonically gradual on the order of several hours; linear interpolation can restore the intermediate state at the acquisition time of the measurement point. Using the area of ​​the reference band as a molecular ratio, the correction result is a dimensionless multiplicative factor that can be directly applied to the absorbance array. For example, It is 10.00. It is 9.95. The value is 9.75, the measurement point acquisition time is located at the midpoint between the two reference acquisition times, the interpolation result is 9.85, and the drift correction coefficient is 1.015.

[0062] The drift correction coefficient is multiplied by the total absorbance values ​​of the original spectra at the first and second depths, respectively, to output the infrared spectrum signals at the first and second depths, which are still one-dimensional arrays of length 776 and 838, respectively.

[0063] S12: Reads the electrical signal from the pressure sensor at the end of the clamping mechanism and converts it into a contact load value; reads the thermoelectric potential signal from the thermocouple sensor and converts it into a surface temperature value; and receives the sheath geometric curvature measured by an external measuring instrument.

[0064] Specifically, the pressure sensor is a strain gauge miniature pressure sensor, installed at the end of the clamping mechanism, between the crystal indenter and the constant-force elastic element. The sensitive axis is coaxial with the loading axis, with a range of 0 to 50 Newtons and a resolution of 0.05 Newtons. The coaxial arrangement of the sensor and the crystal indenter prevents lateral friction components from entering the reading; the obtained value is the normal contact load value transmitted to the sheath via the crystal working surface. The millivolt-level voltage signal output by the pressure sensor is converted to a contact load value in Newtons using a 24-bit analog-to-digital converter and the factory-calibrated linear scale coefficient. The arithmetic mean of all sampling points within the stable window is taken as the contact load value at that measurement point.

[0065] Temperature acquisition utilizes a type K thin-film thermocouple. The hot junction of the thermocouple is attached to the sidewall of the crystal indenter, within 2 mm of the crystal's working surface. The measurement range is -40°C to 150°C. After cold junction compensation, the thermoelectric potential signal is converted to a surface temperature value in degrees Celsius according to the type K thermocouple calibration table. The hot junction of the thermocouple is placed close to the crystal's working surface rather than exposed to the air inside the enclosure because the interface temperature of the contact area affects the softening degree of the polyethylene surface layer, and the air temperature inside the enclosure and the interface temperature can differ by more than 10°C on the sun-facing side. Figure 3This diagram illustrates the coaxial mounting of the sensor. The strain gauge miniature pressure sensor is installed at the end of the clamping mechanism, between the crystal indenter and the constant-force elastic element, with the sensitive axis and loading axis coaxial. The hot end of a K-type thin-film thermocouple is attached to the side wall of the crystal indenter, within 2 mm of the crystal working surface. This arrangement ensures the sensor and crystal indenter are coaxial, preventing lateral friction components from entering the reading. The obtained value is the normal contact load value transmitted from the crystal working surface to the sheath. Because the thermocouple hot end is close to the crystal working surface rather than placed in the air inside the enclosure, it can collect the interface temperature of the contact area that affects the softening degree of the polyethylene surface. The air temperature inside the enclosure and the interface temperature can differ by more than 10 degrees Celsius on the sun-facing side.

[0066] The sheath geometric curvature is calculated from the sheath's outer diameter measured by a handheld laser diameter gauge. The conversion is 2 divided by the sheath's outer diameter, with units of millimeters. The handheld laser diameter gauge transmits the outer diameter value to the data receiving unit of the detection device via an RS485 serial interface. For example, when the sheath's outer diameter is 160 mm, the sheath geometric curvature is 0.0125 millimeters.

[0067] The time alignment of the above three data streams is based on the starting trigger pulse of the interferogram scan of the spectrometer. Both the pressure sensor and the thermocouple sensor start continuous sampling at 200 Hz on the rising edge of the trigger pulse and stop when the cumulative scan ends. The sheath geometric curvature remains unchanged within the same measurement point and is only reread when the measurement point changes.

[0068] S13: Perform a continuous memory packaging operation on the contact load value, surface temperature value, and sheath geometric curvature according to the preset data structure to generate a multi-dimensional environmental state combination.

[0069] Specifically, the preset data structure is a fixed-length structure with a fixed field order: measurement point number, acquisition time, contact load value, surface temperature value, sheath geometric curvature, and channel identifier. The contact load value, surface temperature value, and sheath geometric curvature are stored as 32-bit single-precision floating-point numbers, while the channel identifier is stored as an 8-bit unsigned integer. A value of 1 corresponds to the germanium crystal channel, and a value of 2 corresponds to the diamond crystal channel. The field order and field width of the preset data structure are determined during device firmware compilation and are consistent with the order in which the independent variables of the subsequent contact transfer function are read. This allows for direct addressing by memory offset during substitution calculations, eliminating the need for searching by field name. Figure 4This is a schematic diagram of a multi-dimensional environmental state combination data structure. The diagram shows a fixed-length structure with the following field order: measurement point number, acquisition time, contact load value, surface temperature value, sheath geometric curvature, and channel identifier. The contact load value, surface temperature value, and sheath geometric curvature are stored as 32-bit single-precision floating-point numbers, while the channel identifier is stored as an 8-bit unsigned integer. The field order and width of this data structure are determined during the device firmware compilation phase, consistent with the order of independent variables read in the subsequent contact transfer function. This allows for direct addressing based on memory offset during substitution calculations, eliminating the need for field name retrieval. The contact load value, surface temperature value, and sheath geometric curvature at the same moment are fixedly bound to the spectral data, ensuring that each field spectrum carries information on the contact strength, interface temperature, and cable diameter at the time of acquisition.

[0070] The packaging operation generates a multidimensional environmental state combination record for both the first-depth infrared spectral signal and the second-depth infrared spectral signal. The two records share the same measurement point number, and the acquisition time is the midpoint of the two cumulative scans. The generated multidimensional environmental state combination, along with the corresponding first-depth infrared spectral signal and second-depth infrared spectral signal, is written into the same measurement point record in the data storage unit.

[0071] The multi-dimensional environmental condition combination binds the contact load value, surface temperature value, and sheath geometric curvature value at the same moment to the spectral data, so that each field spectrum carries the contact strength, interface temperature, and cable diameter information at the time of acquisition. Under this binding relationship, when the reference zone area differs in two re-measurements of the same measuring point under different wind loads and different sunshine periods, it can be directly correlated by the difference in the recorded contact load value and surface temperature value, and the difference in contact conditions is no longer treated as a difference in material absorption. When measuring across cable diameters, the sheath geometric curvature value is saved as an independent field with the spectrum, so that the measuring points on cables of different diameters have a unified condition description.

[0072] S2: Substitute the combination of multidimensional environmental states into the contact transfer function to calculate the absorption band integral correction coefficient. Use the absorption band integral correction coefficient to correct the first and second depth infrared spectral signals, and generate the first and second carbonyl index estimates.

[0073] Before being used to calculate the carbonyl index, the first and second depth infrared spectral signals simultaneously contain two types of components unrelated to material aging: overall intensity distortion caused by contact state and interface temperature, and absorption by surface deposits in their characteristic wavelength bands. These two components act differently: the former alters absorbance across all wavenumber points multiplicatively, while the latter only superimposes absorption peaks in specific wavelength bands. Therefore, this step first subtracts the multiplicative distortion using the contact transfer function, then identifies deposit absorption using non-target interference parameters, and only after these two processing steps are completed is the carbonyl index estimate calculated.

[0074] Further, step S2 includes:

[0075] S21: Extract the contact load value, surface temperature value, and sheath geometric curvature from the multidimensional environmental state combination, substitute them into the contact transfer function composed of a quadratic polynomial, perform multivariate algebraic operations, and calculate the absorption band integral correction coefficient.

[0076] The polyethylene reference absorption band corresponds to methylene bending vibration at wavenumbers of 1460 to 1480. The total amount of methylene changes very little during material aging; therefore, the field fluctuations in the reference band area are mainly caused by the bonding condition. Using the reference band area as a measurable indicator of the contact state, the effects of contact load, surface temperature, and sheath geometric curvature on the reference band area are pre-fitted into a function. This allows for the on-site deduction of the strength deviation between the current acquisition conditions and the calibration reference conditions.

[0077] Specifically, the absorption band integral correction coefficient includes a first absorption band integral correction coefficient and a second absorption band integral correction coefficient, corresponding to the germanium crystal channel and the diamond crystal channel, respectively. The calculation formula is the ratio of the calibration reference band area to the contact transfer function output value:

[0078]

[0079]

[0080] In the formula, The contact load value read by S12 The surface temperature value read by S12. The sheath geometry curvature received by S12, the three are read out by field offset from the multidimensional environmental state combination in S13; , , To establish the calibration reference conditions, the reference load within the contact stability platform range was set at 15 Newtons, the laboratory calibration temperature at 25 degrees Celsius, and the calibration sample curvature at 0.0100 per millimeter. The integral area of ​​the polyethylene reference absorption band measured under calibration reference conditions is written into the non-volatile memory of the device. to These are the contact transfer function coefficients.

[0081] The design basis of the contact transfer function is as follows. The constant term represents the reference strip area under the reference conditions. The first term of the contact load value represents the enhanced absorption caused by the increase in the bonding area and the decrease in the optical contact gap due to the increase in load. This enhancement has slowed down but has not disappeared within the contact stability plateau region, so the first term is retained. The second term of the contact load value takes a negative sign, indicating that there is an upper limit to the bonding area with the increase of load. As the load continues to increase, the gain decreases. If only the first term is used, a systematic deviation will appear at both ends of the plateau region. The first term of the surface temperature value represents the net effect of the polyethylene softening effect and the characteristic absorption coefficient decay effect when the temperature rises. Although the temperature rise causes the bonding area to increase and the optical contact gap to decrease due to the softening effect, the molar absorption coefficient of the polyethylene methylene bending vibration itself decreases with the increase of temperature. Moreover, within the contact stability plateau region, the change of the bonding area with load and temperature has slowed down. The gain of the increased area on the reference strip area is insufficient to offset the loss caused by the decay of the absorption coefficient. After the two effects are superimposed, the reference strip area shows a net decreasing trend with the increase of temperature. Therefore, the coefficient of the first term of temperature takes a negative value. In actual measurements, the net effect is approximately linear within the range of 20 to 70 degrees Celsius, therefore a quadratic temperature term is not included. The linear term for the sheath geometric curvature represents how increased curvature narrows the contact strip between the crystal and the cylindrical surface, reducing the number of effective reflections. The cross term for load and curvature represents the different contact strip widths formed by the same load on surfaces with different curvatures. The greater the curvature, the smaller the increase in contact area gained by increasing the load. The cross term appears in a product form because both factors jointly determine the geometric dimensions of the contact strip; simply adding them together cannot express this mutual constraint. The overall design goal is to make the function output increase with increasing load, decrease with increasing temperature, and decrease with increasing curvature, and to prevent the output deviation from being amplified when both load and curvature deviate from the reference.

[0082] The contact transfer function coefficients were determined by regression fitting using historical calibration data. The target variable of the regression was the integral area of ​​the polyethylene reference absorption band, and the independent variables were the contact load value, surface temperature value, and sheath geometric curvature, constructed as a 6-item design matrix according to the previous formula. Calibration data were collected on polyethylene samples of the same material and with known curvature, covering four curvatures: outer diameter 120 mm, 160 mm, 200 mm, and 250 mm. The sample surface temperature was set to four levels (20, 35, 50, and 65 degrees Celsius) by a temperature control platform. The contact load value covered the entire plateau range of 12 to 22 Newtons in 2-Newton increments. Each condition combination was repeated 5 times, and the two channels were fitted independently. The solution criterion was ordinary least squares, minimizing the sum of squared residuals between the measured reference band area and the function output value. For example, the germanium crystal channel coefficient was taken as... , , , , , , Diamond crystal channel coefficient is taken as , , , , , , .

[0083] For example, if the contact load at a certain measuring point is 18.2 Newtons, the surface temperature is 41.5 degrees Celsius, and the sheath's geometric curvature is 0.0125 per millimeter, then... , , Substituting the germanium crystal channel yields... The integral correction factor for the first absorption band is Substituting the diamond crystal channel yields The integral correction factor for the second absorption band is .

[0084] The contact transfer function converts three field conditions—fluctuations in hand-held clamping force, temperature rise on the sunlit side, and differences in cable diameter—into two multiplicative coefficients that can be directly applied to the spectrum. When sampling with clamping forces of 16 N and 21 N on the same sheath, the reference zone area originally differed by about 2%. After multiplying by their respective absorption zone integral correction coefficients, they were brought to the same calibration reference conditions, ensuring that the carbonyl index estimate at the same measuring point under different clamping forces no longer drifted with the clamping action. For cables with outer diameters of 120 mm and 250 mm, the differences in the values ​​of the curvature and cross terms were included in the correction coefficients, allowing the spectra collected on the two cable diameters to be compared on the same scale.

[0085] S22: Multiply the absorption band integral correction coefficient by the spectral intensity amplitude sequences of the first and second depth infrared spectral signals respectively, and output the corrected infrared spectral signal.

[0086] Specifically, the spectral intensity amplitude sequence refers to the absorbance value sequence arranged in ascending wavenumber order in the first and second depth infrared spectral signals, with lengths of 776 and 838, respectively. The multiplication operation is a point-by-point scalar multiplication, where each absorbance value of the first depth infrared spectral signal is multiplied by a first absorption band integral correction factor, and each absorbance value of the second depth infrared spectral signal is multiplied by a second absorption band integral correction factor. The output corrected infrared spectral signal includes both the first and second corrected infrared spectral signals, and the array length is consistent with the input.

[0087] Before point-by-point multiplication, a two-point linear baseline correction is performed on the two spectral intensity amplitude sequences. This involves taking the average absorbance at three wavenumber points at each end of a specified band as the baseline endpoints. A straight line is then drawn connecting these endpoints, and the straight line value is subtracted point-by-point from the absorbance within the band. The baseline endpoints for the carbonyl characteristic absorption band are 1690 and 1760 wavenumbers; for the polyethylene reference absorption band, they are 1440 and 1500 wavenumbers; for the interference range of 1000 to 1100 wavenumbers, they are 980 and 1120 wavenumbers; and for the interference range of 3300 to 3500 wavenumbers, they are 3250 and 3550 wavenumbers. The two-point linear baseline correction subtracts the broad, gradual rise caused by scattering in the probe region and contamination on the crystal surface. This type of rise is nearly linear within a narrow band and can be removed by connecting the two endpoints without reducing the absorption peak located in the middle of the band.

[0088] The integral area is accumulated within the baseline-corrected bands using the trapezoidal method, which involves averaging the absorbance of two adjacent wavenumber points, multiplying it by the interval of 4 wavenumbers, and summing the results segment by segment to output the integral area of ​​each band.

[0089] S23: Extract the integral area of ​​the calibrated infrared spectral signal in the preset interference wavenumber range, and then divide it by the preset polyethylene reference band area to obtain the non-target interference parameter.

[0090] The surface dust of the sheath is mainly composed of silicate minerals. After rain marks dry, residual carbonate and sulfate crystals remain. Water films and water vapor leave broad peaks in the hydroxyl stretching region. The absorption locations of these three types of deposits do not overlap with the absorption of the polyethylene skeleton and carbonyl groups. By comparing the absorption intensity at these locations with the area of ​​the polyethylene reference band, the proportion of deposits in the contact area can be determined without moving the probe.

[0091] Specifically, the preset interference wavenumber range includes two segments: 1000 to 1100 wavenumbers and 3300 to 3500 wavenumbers. The former corresponds to the Si-O and SO stretching absorption of silicates and sulfates, while the latter corresponds to the stretching absorption of water and hydroxyl groups. Neither segment overlaps with the carbonyl characteristic absorption band at 1700 to 1740 wavenumbers or the polyethylene reference absorption band at 1460 to 1480 wavenumbers. The preset polyethylene reference band area refers to the area obtained by integrating the corrected infrared spectral signal at 1460 to 1480 wavenumbers using the trapezoidal method after baseline correction. The non-target interference parameter is calculated using the following formula:

[0092]

[0093] In the formula, , , The first The integrated area of ​​the calibrated infrared spectral signal in the corresponding band for each channel is output by S22. The sum of the two interference areas is divided by the reference band area because dust and watermarks often coexist and are independent in the field; an increase in either area indicates uncleanliness in the contact area. The polyethylene reference band area is used as the denominator so that the non-target interference parameter expresses the proportion of adhering substance absorption relative to matrix absorption, and does not change with the overall intensity level. The first non-target interference parameter corresponds to the germanium crystal channel, and the second non-target interference parameter corresponds to the diamond crystal channel.

[0094] For example, the integral area of ​​the first-corrected infrared spectral signal at a certain measuring point is 3.478 in the wavenumber range of 1000 to 1100, and 1.892 in the wavenumber range of 3300 to 3500. The reference band area is 12.005, and the first non-target interference parameter is... .

[0095] The non-target interference parameter, constructed using the area of ​​the polyethylene reference band as the denominator, not only identifies adhering substances but also provides a discriminant for detecting saturation distortion. When a thick powdery layer or residual water film exists on the shaded side of the sheath, the crystal and the substrate are separated by a low-refractive-index medium, causing a decrease in the measured area of ​​the reference absorption band. Simultaneously, the powdery layer and water film themselves exhibit strong absorption at wavenumbers of 1000-1100 and 3300-3500. The increase in the numerator and the decrease in the denominator act in the same direction with the same ratio. The increase in the non-target interference parameter is greater than the increase in any single change, thus crossing the judgment threshold before the carbonyl band shows obvious anomalies. At a deeper level, this discrimination addresses a deficiency in existing in-situ spectroscopic detection that is not associated with interference indicators: when the absorption band is compressed as a whole due to the isolation of the surface medium, the carbonyl area and the reference area shrink by approximately the same proportion, and the carbonyl index in ratio form does not report an error, leading the detector to believe the data is usable. This embodiment does not add any additional detection channels or additional parameters; the fractional structure of non-target interference parameters alone can expose this type of saturation distortion in the same acquisition.

[0096] S24: When the non-target interference parameter is greater than the preset pollution judgment threshold, generate a pollution alarm sign and terminate subsequent calculations; when the non-target interference parameter is less than or equal to the preset pollution judgment threshold, extract the integral area of ​​the carbonyl characteristic absorption band in the corrected infrared spectrum signal and divide it by the integral area of ​​the polyethylene reference absorption band to generate the first carbonyl index estimate and the second carbonyl index estimate, respectively.

[0097] The powdery material adhering to the surface is itself oxidized polyethylene debris, which has strong absorption in the carbonyl band. If the carbonyl index is calculated directly without branching, the measurement points in the powdery area will give the same value as those for severe aging. The branching decision removes unclean measurement points from the calculation link, allowing only the spectra that pass the cleanliness verification to enter the subsequent differential analysis calculation.

[0098] Further, step S24 includes:

[0099] S241: Compare the first non-target interference parameter with the preset contamination judgment threshold and output the contamination judgment result.

[0100] Specifically, the comparison is based on the first non-target interference parameter. The germanium crystal channel has the smallest effective detection depth constant, and the proportion of deposits in the contact area is the highest in the shallow channel spectrum, making the shallow channel the most sensitive to surface deposits. The second non-target interference parameter is also saved for verification before and after cleaning of S242.

[0101] The preset contamination threshold is determined by shifting the measured extreme value of the clean sheath towards the contamination side. Samples of the same model of sheath that have been completed but not yet put into operation, as well as measuring points on in-service sheaths wiped and dried with anhydrous ethanol, are taken as objects on the clean side. The first non-target interference parameter is collected from 30 measuring points on each side. The maximum value among all measuring points is taken as the clean upper limit. The clean upper limit is multiplied by the dust adhesion detection factor to obtain the preset contamination threshold. The dust adhesion detection factor is a real number between 2 and 3. If the value is too small, surface adsorption water caused by increased air humidity will trigger a contamination alarm; if the value is too large, thin layers of floating dust cannot be detected. For example, the clean upper limit is 0.10, the dust adhesion detection factor is 2.5, and the preset contamination threshold is 0.25.

[0102] S242: When the pollution judgment result is that the first non-target interference parameter is greater than the preset pollution judgment threshold, a pollution alarm sign is generated and the subsequent calculation is terminated. At the same time, the surface pretreatment and light-shielding dust prevention module is triggered to perform contact area cleaning. After cleaning is completed, return to step S1 to collect data again and calculate the difference in non-target interference parameters before and after cleaning.

[0103] Specifically, the pollution alarm identifier is a status word written into the measurement point record. A value of 1 indicates that the current data collection is determined to be surface contamination, and simultaneously invalidates the estimated values ​​of the first and second carbonyl indices for this measurement point. The surface pretreatment and light-shielding / dust-proof module has a built-in non-woven cloth wiping head impregnated with anhydrous ethanol. The wiping head is driven by a micro motor to reciprocate 10 times in the contact area, with a stroke of 20 mm, followed by purging with dry nitrogen gas inside the cover for 20 seconds. The wiping pressure is limited to within 3 Newtons by the same constant force elastic element to avoid creating new scratches on the polyethylene surface during wiping.

[0104] After cleaning, steps S1 to S23 are repeated to obtain the first and second non-target interference parameters after cleaning. These are then subtracted from their pre-cleaning values ​​to obtain the difference in non-target interference parameters before and after cleaning. If the first non-target interference parameter after cleaning is no greater than the preset contamination threshold, the contamination alarm is cleared and the process proceeds to S243. If, after two consecutive cleanings, the first non-target interference parameter is still greater than the preset contamination threshold, and the absolute value of the difference in non-target interference parameters before and after cleaning is less than the cleanliness limit, it is determined that the contact area contains a powdery layer bonded to the substrate, rather than removable deposits. A powdery layer marker is written into the measurement point record, and the contamination alarm is retained. This measurement point is then processed using methods other than manual window opening for verification. Removable dust and rain streaks show a significant reduction in interference absorption after a single wipe, while the powdery layer bonded to the substrate shows little change before and after wiping. The distinction between the two is based on the magnitude of the difference in non-target interference parameters before and after cleaning.

[0105] S243: When the pollution determination result is that the first non-target interference parameter is less than or equal to the preset pollution determination threshold, the integral area of ​​the carbonyl characteristic absorption band in the wavenumber range of 1700 to 1740 of the first corrected infrared spectral signal and the second corrected infrared spectral signal is extracted respectively, and each is divided by the integral area of ​​the polyethylene reference absorption band in the wavenumber range of 1460 to 1480 of the corresponding channel to generate the first carbonyl index estimate and the second carbonyl index estimate.

[0106] Specifically, the carbonyl index is taken in the wavenumber range of 1700 to 1740, covering the absorption of ketone carbonyl and carboxylic acid carbonyl groups generated by the oxidative degradation of polyethylene; the methylene bending absorption of 1460 to 1480 wavenumbers is used as the denominator, so that the ratio reflects the amount of carbonyl generated per unit polyethylene matrix, regardless of the sample thickness and bonding state. The estimated values ​​of the first and second carbonyl indices are both dimensionless real numbers, and the value on the unaged sheath does not exceed 0.05.

[0107] For example, following the aforementioned measurement points, after cleaning, the integrated area of ​​the carbonyl characteristic absorption band of the first corrected infrared spectral signal is 5.034, the reference band area is 12.005, and the estimated value of the first carbonyl index is 0.42; the integrated area of ​​the carbonyl characteristic absorption band of the second corrected infrared spectral signal is 1.540, the reference band area is 8.500, and the estimated value of the second carbonyl index is 0.181. After cleaning, the first non-target interference parameter decreases to 0.045, which is not greater than the preset contamination judgment threshold of 0.25, and the two carbonyl index estimates are set to valid.

[0108] The multiplicative correction mechanism consisting of S21 and S22, and the interference branching mechanism consisting of S23, S241 to S243, apply to two types of non-overlapping distortion components. The absence of either one results in errors of different natures in subsequent differential stratification calculations. Without the multiplicative correction mechanism, the Newton-level fluctuations of the contact load value within the plateau region and the tens of degrees Celsius temperature rise on the sunlit side remain in the spectrum as overall intensity deviations. The carbonyl index estimates for both channels are simultaneously inflated or deflated. When the differential stratification calculation is performed based on thickness, these two deviations cannot cancel each other out, resulting in subsurface oxidation physical quantities with opposite signs. Without the interference branching mechanism, the absorption of dust and powder in the carbonyl band is included in the molecular calculation. The carbonyl index estimate for shallow channels is artificially inflated, while the deep channels are less affected. The differential stratification calculation will misjudge pure surface adhesion as a steep oxidation depth gradient. There are two types of distortion: one is a proportional change in the continuity of all wavenumber points, and the other is a discrete superposition that only appears at specific measurement points and in specific wavebands. The former requires back-calculation of correction coefficients using physical condition quantities, while the latter requires setting blocking branches based on waveband ratios. Neither mechanism alone can cover the other type. After the two processes are cascaded, the two carbonyl index estimates entering S3 simultaneously satisfy both the premises of uniform intensity scale and clean contact area. The simultaneous fulfillment of these two premises is a necessary condition for the subtraction of the two channels in differential analysis to avoid amplifying the error.

[0109] S3: Combining the effective detection depth constant of the dual channels, differential stratification is performed on the estimated values ​​of the first carbonyl index and the second carbonyl index to separate the surface oxidation physical quantities, subsurface oxidation physical quantities and oxidation depth gradient values.

[0110] The germanium crystal channel and the diamond crystal channel sample different thicknesses. The readings of the shallow channel only reflect the material state within the outermost half-micrometer, while the readings of the deep channel are a mixed result of contributions from both the shallow and deeper layers. The difference between the two readings comes from the layer not covered by the shallow channel. By solving the contribution of this layer separately, it is possible to determine whether oxidation has only stopped at the outermost layer or has progressed inward.

[0111] Further, step S3 includes:

[0112] S31: Obtain the crystal refraction parameters stored in the internal hardware register, substitute them into the infrared penetration physics formula to calculate the first effective detection depth constant and the second effective detection depth constant.

[0113] Specifically, the crystal refractive parameters include a first crystal refractive index of 4.0, a first effective incident angle of 60 degrees, a second crystal refractive index of 2.4, a second effective incident angle of 45 degrees, and a polyethylene refractive index of 1.51. These five values ​​are written into the hardware register of the control unit during device assembly. The two crystal refractive indices and the two effective incident angles are given by the crystal supply technical documents, and the polyethylene refractive index is taken as the measured value of the sheath material in the mid-infrared band.

[0114] The effective detection depth constant is calculated using the formula for attenuated total internal reflection penetration depth:

[0115]

[0116] In the formula, The wavelength corresponding to the center wavenumber of 1720 in the carbonyl characteristic absorption band is 5.81 micrometers. For the first The refractive index of a crystal, For the first One effective angle of incidence, The refractive index of polyethylene is used. The reason for choosing this formula is that the thickness required in this step is exactly the equivalent sampling thickness of infrared light on the sample side under attenuated total internal reflection conditions. The formula is the standard calculation formula for this thickness in attenuated total internal reflection spectroscopy. The two channels differ only in the crystal refractive index and the incident angle. Substituting these values ​​will yield two thickness values.

[0117] For example, germanium crystal channel substitution , Spend, The square root contains The square root is 0.7794, and the denominator is... The first effective detection depth constant is Micrometers; diamond crystal channel substitution , Degree, the square root of The square root is 0.3231, and the denominator is... The second effective detection depth constant is Micrometers. The two thickness values ​​are written to the data storage unit for use by S33 and S34.

[0118] It should be noted that the above calculations use the wavelength corresponding to the center wavenumber of the carbonyl characteristic absorption band (1720 wavenumber) as the representative value, and are uniformly used to calculate the first and second effective detection depth constants. Calculations show that the penetration depth varies with wavenumber in the range of 1700 to 1740 wavenumbers, with the variation not exceeding 2% of the center value. The penetration depth corresponding to the polyethylene reference absorption band in the range of 1460 to 1480 wavenumbers differs from the corresponding value in the carbonyl band by approximately 15%. However, the differential analysis calculation uses the difference and ratio of the penetration depths of the two channels. The fluctuation range of this difference and ratio in both the carbonyl band and the reference band does not exceed 1%. Therefore, in S33 and S34, fixed first and second effective detection depth constants are substituted into the calculations involving the two bands respectively. The resulting systematic error is negligible within the engineering accuracy range.

[0119] S32: The estimated value of the first carbonyl index is directly assigned to the surface oxidation physical quantity to characterize the attenuation characteristics of shallow materials.

[0120] Specifically, the physical quantity of surface oxidation is numerically equal to the estimated value of the first carbonyl index output by S243. Physically, it represents the average carbonyl generation within a thickness range of 0 to 0.30 micrometers from the outer surface of the sheath inwards, and is a dimensionless real number. Due to the high refractive index and large incident angle of germanium crystals, the first effective detection depth constant is as small as 0.30 micrometers. The average range of shallow channel readings in the thickness direction coincides with the surface thickness range; therefore, a value is directly assigned without weighting. For example, the physical quantity of surface oxidation is 0.42.

[0121] S33: Multiply the estimated value of the second carbonyl index by the second effective detection depth constant, subtract the product of the estimated value of the first carbonyl index and the first effective detection depth constant, and then divide by the difference between the second effective detection depth constant and the first effective detection depth constant to calculate the physical quantity of subsurface oxidation.

[0122] Specifically, the formula for calculating the physical quantities of subsurface oxidation is as follows:

[0123]

[0124] In the formula, and These are the estimated values ​​of the first and second carbonyl indices output by S243, respectively. and These are the first and second effective detection depth constants output by S31, respectively. The construction process of the calculation formula is as follows: Deep channel sampling thickness Coverage from 0 to 1.19 micrometers, shallow channel sampling thickness Covering 0 to 0.30 micrometers, deep channel readings can be written as 0 to... interval and to The thickness-weighted average of the intervals, i.e. The formula is obtained by shifting the desired subsurface oxidation physical quantity to one side. In the formula, the two product terms in the numerator represent the total carbonyl content of the thickness sampled by the deep channel and the total carbonyl content of the thickness sampled by the shallow channel, respectively. Subtracting the two gives the total carbonyl content within the 0.30 to 1.19 micrometer layer. The denominator is the layer thickness, which, after division, reduces to the average carbonyl generation of that layer, having the same dimensions as the surface oxidation physical quantity and allowing for direct comparison. The overall design goal is to minimize the subsurface oxidation physical quantity when the surface reading is higher and the deep channel reading is lower, effectively removing oxidation limited to the outer surface from the mixed deep channel reading. Figure 5This diagram illustrates the depth coverage calculation for differential stratification. The diagram shows two intervals along the sheath thickness: the surface layer and the subsurface layer. The first effective detection depth constant covers the surface layer interval, and the second effective detection depth constant covers the combined interval of the surface and subsurface layers. The deep channel reading can be written as the thickness-weighted average of the interval from 0 to the first effective detection depth constant and the interval from the first effective detection depth constant to the second effective detection depth constant. This coverage relationship allows the total carbonyl content on the thickness sampled by the deep channel to be subtracted from the total carbonyl content on the thickness sampled by the shallow channel, restoring the average carbonyl generation in the 0.30 to 1.19 micrometer layer. This effectively removes oxidation limited to the outer surface from the deep channel mixed reading, allowing for a separate representation of the surface and internal states.

[0125] For example, substitute , , micrometers Micrometers, molecules are The denominator is Micrometer, the physical properties of subsurface oxidation are .

[0126] Differential analysis separates the previously mixed surface and internal states. The surface oxidation physical quantity at the aforementioned measurement point was 0.42. If evaluated solely based on the average spectrum of a single surface, the measurement point would be classified as heavily oxidized and trigger high-risk treatment. The calculated subsurface oxidation physical quantity was only 0.100, close to the level of unaged sheaths, indicating that carbonyl groups are concentrated on the outermost layer within 0.30 micrometers, and the polyethylene in the 0.30 to 1.19 micrometer range has not yet shown significant structural degradation. For large-diameter cable measurement points on the sun-facing side that have already shown powdering, the powdery residue remaining on the outermost layer after wiping with S242 is no longer included in the subsurface oxidation physical quantity. The criterion for determining whether the sheath needs replacement shifts from surface appearance to a layered numerical value.

[0127] S34: Calculate the ratio of the estimated value of the first carbonyl index to the estimated value of the second carbonyl index, and output the oxidation depth gradient value.

[0128] Specifically, the formula for calculating the oxidation depth gradient value is:

[0129]

[0130] In the formula, and These are the estimated values ​​of the first and second carbonyl indexes output by S243, respectively. The oxidation depth gradient value is a dimensionless real number, representing the relative concentration of carbonyl readings in the shallow and deep channels. A ratio greater than 1 and a larger value indicates that the carbonyl signal is more concentrated within the surface thickness covered by the shallow channel, and oxidation has not yet penetrated deeper; when the ratio approaches 1, it indicates that the readings of the shallow and deep channels are close, and oxidation has penetrated inward to a thickness above the second effective detection depth constant.

[0131] The reason for using a ratio instead of the difference between the surface oxidation physical quantity and the subsurface oxidation physical quantity divided by the difference between the second effective detection depth constant and the first effective detection depth constant is that the latter construction method is numerically equal to a linear combination of the surface oxidation physical quantity and the subsurface oxidation physical quantity with fixed coefficients, and does not have independent information increments between them. For a given device, the first effective detection depth constant and the second effective detection depth constant are both fixed values. Substituting the quantities obtained by this construction into the multivariate constraint regression prediction equation in S41 will cause the design matrix of the equation to be completely collinear, and the regression coefficients cannot be uniquely determined. The subsurface oxidation physical quantity is obtained by nonlinear operation in S33 using the estimated values ​​of the first carbonyl index and the second carbonyl index. Therefore, the ratio of the estimated values ​​of the first carbonyl index and the second carbonyl index does not constitute a linear correlation with the subsurface oxidation physical quantity. It can be used as a third independent variable, independent of the surface oxidation physical quantity and the subsurface oxidation physical quantity, and substituted into the regression equation, while still expressing the physical meaning of the concentration of oxidation along the thickness direction.

[0132] For example, substituting the estimated value of the first carbonyl index (0.42) and the estimated value of the second carbonyl index (0.181), the oxidation depth gradient value is... .

[0133] S4: Substitute the surface oxidation physical quantities, subsurface oxidation physical quantities, and oxidation depth gradient values ​​into the preset constraint regression equation to calculate the oxidation induction time prediction and trigger the maintenance command.

[0134] The carbonyl index itself only indicates the amount of oxidation products accumulated, not directly how long the sheath can resist further oxidation. The remaining antioxidant capacity of the sheath is determined by the residual antioxidant content, which is measured in the laboratory by oxidation induction time. By establishing a pre-defined numerical correspondence between the three measurable stratification indicators on-site and the laboratory oxidation induction time, the remaining antioxidant capacity, expressed as a relative value, can be read on-site, avoiding the direct application of an uncalibrated fixed carbonyl index threshold.

[0135] Further, step S4 includes:

[0136] S41: Extract the pre-configured multivariate constraint regression prediction equation within the data storage unit. The coefficients corresponding to the subsurface oxidation physical quantities in the multivariate constraint regression prediction equation are forcibly constrained to non-positive polarity by the hardware-level code.

[0137] Specifically, the multivariate constrained regression prediction equation is as follows:

[0138]

[0139] In the formula, The surface oxidation physical quantities output by S32 The physical quantities of subsurface oxidation output by S33 The oxidation depth gradient value output by S34 is the ratio of the estimated value of the first carbonyl index to the estimated value of the second carbonyl index, and is a dimensionless real number. The oxidation induction time is a predicted value, expressed as a relative value, and is defined as the ratio of the oxidation induction time of the sheath to be tested to the oxidation induction time of the unaged sheaths in the same batch. For constant terms, , , The firmware verifies the regression coefficients when they are written. and Coefficients that do not meet the polarity condition will not be written.

[0140] The regression coefficients were determined by regression fitting based on the calibration data of the artificially aged samples. The target variable was the relative value of oxidation induction time, obtained by comparing the measured oxidation exothermic onset time (measured by differential scanning calorimetry at 200 degrees Celsius under oxygen purging conditions) with that of unaged samples from the same batch. The independent variables were the surface oxidation physical properties, subsurface oxidation physical properties, and oxidation depth gradient values ​​measured according to procedures S1 to S3 on the same batch of artificially aged samples. The solution criterion was... and To minimize the sum of squared residuals under two linear inequality constraints, the Lawson-Hanson nonnegative least squares algorithm was used to solve for the negativeed independent variable series. Artificial aging samples were subjected to a coupled combination of three conditions: ultraviolet irradiation, damp heat, and temperature cycling. Five aging durations, three aging temperatures, two curvatures, and two material batches were set, resulting in a total of 60 samples. The enthalpy of fusion of each sample was simultaneously measured using a differential scanning calorimeter and converted into a relative crystallinity value. This relative crystallinity value was not included in the regression calculation and was used to eliminate outlier samples where the relative crystallinity value changed by more than 0.15 due to melt recrystallization, thus preventing outlier samples from skewing the regression coefficients. To control the impact of random errors in a single measurement on the regression coefficients, the calibration process verifies the overall goodness of fit of the 60 sets of samples based on the standard deviation of the calibration residuals. When the standard deviation of the calibration residuals does not exceed 10% of the range of the relative value of oxidation induction time, the resolution of the 60 sets of condition combinations is considered to meet the requirements for evaluating the remaining antioxidant capacity. For example, the standard deviation of the calibration residuals is 0.045, and the range of the relative value of oxidation induction time is approximately 0 to 1.02, which meets the above verification conditions.

[0141] For example, the calibration result is , , , The absolute value of the coefficient of physical properties of subsurface oxidation is greater than that of surface oxidation, which is consistent with the law that polyethylene antioxidants are consumed layer by layer from the surface to the interior. The fact that oxidation has progressed to the subsurface means that the antioxidants have been consumed over a larger thickness range.

[0142] A non-positive polarity constraint is applied to the subsurface oxidation physical quantity coefficients to ensure that the equation does not yield results indicating higher residual antioxidant capacity with heavier subsurface oxidation under any input. After the sheath surface is washed by rain or wiped with S242, the surface oxidation physical quantity at some measuring points may be low while the subsurface oxidation physical quantity is high. If unconstrained least squares fitting is used for such samples, the subsurface coefficients may be fitted as positive numbers, resulting in an overestimated oxidation induction time prediction when encountering measuring points with severe deep oxidation in the field. The polarity constraint prevents this situation during the coefficient writing stage, ensuring that the output always decreases as the two oxidation indicators increase.

[0143] S42: Substitute the surface oxidation physical quantity, subsurface oxidation physical quantity, and oxidation depth gradient value as independent variables into the multivariate constrained regression prediction equation to calculate the oxidation induction time prediction quantity, and output the confidence interval according to the standard deviation of the calibrated residuals.

[0144] Specifically, the substitution operation is performed as a scalar multiplication and addition, outputting the predicted oxidation induction time. The confidence interval is the predicted oxidation induction time plus or minus half the prediction interval width. The half-width of the prediction interval is equal to twice the standard deviation of the calibrated residuals. The standard deviation of the calibrated residuals is the standard deviation of the difference between the measured relative values ​​of the oxidation induction time of the 60 artificially aged samples after S41 regression fitting and the output value of the equation. A multiplier of 2 corresponds to approximately 95% coverage under large sample conditions. For example, the standard deviation of the calibrated residuals is 0.045, and the half-width of the prediction interval is 0.09.

[0145] For example, substituting the surface oxidation physical quantity of 0.42, the subsurface oxidation physical quantity of 0.100, and the oxidation depth gradient value of 2.320, we get... The confidence interval is 0.720 to 0.900. As a control, the estimated values ​​for the first carbonyl index and the second carbonyl index at another measurement point are 0.52 and 0.48, respectively. Solving S33 yields a subsurface oxidation physical quantity of 0.4665, and solving S34 yields an oxidation depth gradient value of... Substituting into The confidence interval is 0.041 to 0.221, indicating that oxidation has progressed to the subsurface layer and the antioxidant residue is very low. The surface oxidation physical properties at the two measurement points differ by less than 0.10, but the predicted oxidation induction time differs by 0.68. The difference mainly comes from the subsurface oxidation physical properties and the oxidation depth gradient value.

[0146] S43: Compare the predicted oxidation induction time with the safe period threshold stored in the internal bus. If the predicted oxidation induction time is lower than the safe period threshold, output a high-frequency eddy current verification command to start the external mechanical flaw detection equipment to perform physical verification operation. Otherwise, maintain the low-power standby state of the current detection equipment.

[0147] Specifically, the safety period threshold is determined by the observation results of artificially aged samples: Among the 60 artificially aged samples mentioned in S41, samples showing microcracks penetrating the surface for the first time under microscopic observation are selected. The maximum value of the relative value of oxidation induction time for this sample group is taken as the upper limit for crack initiation, and then a crack initiation warning margin of 0.05 is added to obtain the safety period threshold. The crack initiation warning margin is taken as the average decrease in the relative value of oxidation induction time within the on-site retest cycle, ensuring that the sheath does not directly jump from a qualified state to a cracked state between two tests. For example, the upper limit for crack initiation is 0.30, and the safety period threshold is 0.35.

[0148] After microcracks penetrate the surface of the sheath, the rate at which water vapor permeates inward along the crack channel increases by approximately an order of magnitude compared to the permeation rate of an intact sheath. This rate change has been confirmed by immersion permeation tests and electrochemical impedance spectroscopy (EIS) measurements of samples from the same sheath model. Once the permeation rate reaches this level, the corrosion rate of the internal galvanized steel wire in a humid environment is sufficient to generate a cross-sectional loss signal identifiable by high-frequency eddy current testing within one testing cycle. The field testing cycle is typically six months to one year. The safety period threshold is a crack initiation warning margin superimposed on the upper limit of crack initiation, i.e., taken from the average decrease in the relative value of oxidation induction time within one testing cycle. The purpose is to ensure that the review instruction is triggered before crack initiation and before the sheath's barrier performance substantially deteriorates, leaving an effective window for subsequent eddy current testing and possible replacement decisions.

[0149] When the predicted oxidation induction time is lower than the safety period threshold, the control unit sends a high-frequency eddy current verification command to the external high-frequency eddy current testing equipment via the CAN bus. The command message carries the test point number, the predicted oxidation induction time, the confidence interval, the physical quantities of subsurface oxidation, and the oxidation depth gradient value. After receiving the command, the high-frequency eddy current testing equipment scans within a 500 mm range above and below the test point along the cable axis to detect the cross-sectional loss and broken wire signals of the galvanized steel wire inside the sheath, in order to confirm whether the sheath's barrier failure has caused internal corrosion. After the subsurface oxidation of the sheath reaches a certain level, the water vapor penetration rate increases, and steel wire corrosion occurs before sheath cracking. Therefore, verifying the metal side condition using eddy current methods can corroborate the spectral results. If the lower limit of the confidence interval for the predicted oxidation induction time is lower than the safety period threshold, but the predicted value itself is higher than the safety period threshold, the control unit writes an encrypted retest mark in the test point record and includes the test point in the priority retest list for the next testing cycle. Figure 6 This is a schematic diagram of the verification process using a high-frequency eddy current (EDC) flaw detection device. The diagram shows that after receiving the EDC verification command, the device scans along the cable axis within a 500 mm range above and below the measuring point, detecting the cross-sectional loss and broken wire signals of the galvanized steel wires inside the sheath. The command message carries the measuring point number, the predicted oxidation induction time, the confidence interval, the physical quantities of subsurface oxidation, and the oxidation depth gradient value. This verification method uses eddy current to check the metal-side condition, corroborating the spectral results to confirm whether sheath barrier failure has triggered internal corrosion. Once the subsurface oxidation of the sheath reaches a certain level, the water vapor penetration rate increases, and steel wire corrosion occurs before sheath cracking, thus ensuring that the number of times the external flaw detection equipment is activated corresponds to the actual internal risk of the sheath.

[0150] When the comparison result shows that the predicted oxidation induction time is not lower than the safety period threshold, the control unit turns off the light source and indexing disk drive, maintains the low-power standby state of the data storage unit and communication unit, and waits to move to the next detection point.

[0151] The verification action is triggered directly by the predicted oxidation induction time rather than the carbonyl index, establishing a numerical correspondence between the on-site spectral results and the remaining antioxidant capacity of the sheath. The surface oxidation physical quantities at the two aforementioned measurement points are similar, but the treatment actions differ; the difference in treatment is determined by the subsurface oxidation physical quantities and the oxidation depth gradient value. After the polarity constraint of S41, the equation still outputs a lower predicted oxidation induction time when encountering abnormal measurement points where the surface reading is low and the deep reading is high after wiping. This ensures that the verification command is triggered at measurement points where deep oxidation has progressed, rather than at measurement points with only surface adhesion. The number of times the external flaw detection equipment is activated corresponds to the actual internal risk of the sheath.

[0152] Example 2:

[0153] This embodiment, based on Embodiment 1, provides an in-situ aging test system for PE cables used in cable stays. Figure 7 As shown, it includes:

[0154] The spectral acquisition and environmental state combination generation module is used to acquire first-depth infrared spectral signals and second-depth infrared spectral signals through infrared acquisition equipment, and simultaneously read contact load values, surface temperature values ​​and sheath geometric curvature to generate multi-dimensional environmental state combinations.

[0155] The correction and carbonyl index estimation module is used to substitute the multidimensional environmental state combination into the contact transfer function to calculate the absorption band integral correction coefficient, and use the absorption band integral correction coefficient to correct the first depth infrared spectral signal and the second depth infrared spectral signal to generate the first carbonyl index estimation value and the second carbonyl index estimation value.

[0156] The differential stratification module is used to combine the effective detection depth constant of the dual channels to perform differential stratification on the first carbonyl index estimate and the second carbonyl index estimate, and separate the surface oxidation physical quantity, subsurface oxidation physical quantity and oxidation depth gradient value.

[0157] The oxidation induction time prediction and maintenance triggering module is used to substitute the surface oxidation physical quantity, the subsurface oxidation physical quantity and the oxidation depth gradient value into a preset constraint regression equation, calculate the oxidation induction time prediction, and trigger maintenance instructions.

Claims

1. A method for in-situ aging test of PE cables for cable stays, characterized in that, include: The first and second depth infrared spectral signals are acquired by infrared acquisition equipment, and the contact load value, surface temperature value and sheath geometric curvature are read simultaneously to generate a multi-dimensional environmental state combination. Substitute the multidimensional environmental state combination into the contact transfer function to calculate the absorption band integral correction coefficient, and use the absorption band integral correction coefficient to correct the first depth infrared spectral signal and the second depth infrared spectral signal to generate the first carbonyl index estimate and the second carbonyl index estimate. By combining the effective detection depth constant of the dual channels, differential stratification is performed on the first carbonyl index estimate and the second carbonyl index estimate to separate the surface oxidation physical properties, subsurface oxidation physical properties and oxidation depth gradient value. Substitute the surface oxidation physical quantity, the subsurface oxidation physical quantity, and the oxidation depth gradient value into a preset constraint regression equation to calculate the oxidation induction time prediction and trigger a maintenance command.

2. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The acquisition of the first depth infrared spectral signal and the second depth infrared spectral signal through the infrared acquisition device includes: Switch the indexing plate inside the infrared acquisition device so that attenuated total internal reflection crystals with different refractive index physical properties are successively attached to the detection surface at the same detection point and on the same loading axis. The indexing disk is driven to switch sequentially to the first indexing position and the second indexing position, so that the germanium crystal and the diamond crystal are attached at the same detection point, and the first depth raw spectrum and the second depth raw spectrum are collected. The first depth infrared spectral signal and the second depth infrared spectral signal are acquired and output sequentially.

3. The in-situ aging test method for PE cables of cable stays according to claim 2, characterized in that, The process of sequentially attaching attenuated total internal reflection crystals with different refractive indices to the detection surface at the same detection point and on the same loading axis includes: The infrared acquisition device is pressed onto the detection point of the sheath using an independent fixing component and a curved self-centering positioning component. The constant pressure floating loading component adjusts the contact load value into the contact stability platform range and outputs the load time series. When all continuous sampling points of the pressure sensor fall within the contact stability platform range and the duration is not less than the duration of a single spectral cumulative scan, the contact state ready flag is set.

4. The in-situ aging test method for PE cables of cable stays according to claim 3, characterized in that, The contact stabilization platform range includes: The lower and upper boundaries of the contact stability platform range are determined by load step calibration. The contact load value was increased from 6 Newtons to 34 Newtons in increments of 2 Newtons. The integral area of ​​the polyethylene reference absorption band was collected once for each load level, and the relative change rate of the reference band area between adjacent levels was calculated. The load level where the relative change rate first fell below 1% per Newton was taken as the lower limit of the contact stability plateau interval. After the pressure is released, the indentation depth is measured with a portable profilometer. The lowest load level with an indentation depth exceeding 5 micrometers is taken, and then one step is subtracted as the upper limit of the contact stability platform range.

5. The in-situ aging test method for PE cables of cable stays according to claim 2, characterized in that, After acquiring the raw spectra at the first depth and the raw spectra at the second depth, the process also includes: Stable windows are selected based on the load time series. Only interferograms falling within the stable window are included in the cumulative scan, while interferograms falling outside the window are discarded and automatically re-scanned. Before and after detection, the reference spectrum of the same optical path reference material block was collected, and the reference band area before and after detection was extracted respectively. The drift correction coefficient is calculated by the ratio of the area of ​​the reference band to the area of ​​the current reference band obtained by linear interpolation over time. Drift correction is performed on the original spectra at the first depth and the original spectra at the second depth, and the infrared spectral signals at the first depth and the second depth are output.

6. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The synchronous reading of contact load values, surface temperature values, and sheath geometric curvature includes: Read the electrical signal of the pressure sensor at the end of the clamping mechanism and convert it into a contact load value. Take the arithmetic mean of all sampling points within the stable window as the contact load value of this measuring point. After cold junction compensation, the thermoelectric potential signal of the thermocouple sensor is read and converted into a surface temperature value according to the K-type thermocouple calibration table. The outer diameter of the sheath is received by a handheld laser diameter gauge and transmitted via a serial interface. The geometric curvature of the sheath is calculated by dividing the geometric curvature of the sheath by 2.

7. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The generated multidimensional environmental state combinations include: The contact load value, surface temperature value, and sheath geometric curvature are continuously packaged in memory according to a preset data structure. The preset data structure is a fixed-length structure, and the fields are in a fixed order as follows: measurement point number, acquisition time, contact load value, surface temperature value, sheath geometric curvature, and channel identifier. A multidimensional environmental state combination record is generated for each of the first and second depth infrared spectral signals. The two records share the same measurement point number, and the acquisition time is the midpoint time of the two cumulative scans.

8. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The calculation of the absorption band integral correction factor includes: Extract contact load values, surface temperature values, and sheath geometric curvature from the multidimensional environmental condition combination; Substitute the contact load value, the surface temperature value, and the sheath geometric curvature into the contact transfer function composed of a quadratic polynomial and perform multivariate algebraic operations to obtain the contact transfer function output value; The integral correction coefficients of the first absorption band and the second absorption band of the corresponding diamond crystal channel are calculated by using the ratio of the calibration reference band area to the output value of the contact transfer function.

9. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The generation of the first carbonyl index estimate and the second carbonyl index estimate includes: The absorption band integral correction coefficient is multiplied by the spectral intensity amplitude sequences of the first and second depth infrared spectral signals, respectively, and the corrected infrared spectral signal is output. The integral area of ​​the corrected infrared spectral signal in the preset interference wavenumber range is extracted and divided by the area of ​​the preset polyethylene reference band to obtain the non-target interference parameter. When the non-target interference parameter is greater than the preset pollution judgment threshold, a pollution alarm is generated and subsequent calculations are terminated. When the non-target interference parameter is less than or equal to the preset pollution judgment threshold, the integral area of ​​the carbonyl characteristic absorption band is extracted and divided by the integral area of ​​the polyethylene reference absorption band to generate the first carbonyl index estimate and the second carbonyl index estimate, respectively.

10. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The execution differential layer analysis solution includes: Obtain the crystal refraction parameters stored in the internal hardware registers, substitute them into the attenuation total internal reflection penetration depth formula to calculate the first effective detection depth constant and the second effective detection depth constant; The estimated value of the first carbonyl index is assigned to the surface oxidation physical quantity; Multiply the estimated value of the second carbonyl index by the second effective detection depth constant, subtract the product of the estimated value of the first carbonyl index and the first effective detection depth constant, and then divide by the difference between the second effective detection depth constant and the first effective detection depth constant to calculate the subsurface oxidation physical quantity. Calculate the ratio of the estimated value of the first carbonyl index to the estimated value of the second carbonyl index and output the oxidation depth gradient value.

11. The in-situ aging test method for PE cables of cable stays according to claim 1, characterized in that, The calculation of the predicted oxidation induction time and the triggering of the maintenance command include: Extract the pre-configured multivariate constraint regression prediction equation within the data storage unit. The coefficients corresponding to the subsurface oxidation physical quantities in the multivariate constraint regression prediction equation are forcibly constrained to non-positive polarity by hardware-level code. Substitute the surface oxidation physical quantity, subsurface oxidation physical quantity, and oxidation depth gradient value as independent variables into the multivariate constrained regression prediction equation to calculate the oxidation induction time prediction and output the confidence interval according to the calibrated residual standard deviation. The predicted oxidation induction time is compared with the safety period threshold. If the predicted oxidation induction time is lower than the safety period threshold, a high-frequency eddy current verification command is output to start the external mechanical flaw detection equipment to perform physical verification operation. Otherwise, the current detection equipment is kept in low-power standby mode.

12. A system for in-situ aging testing of PE for cable-stayed bridges, used to implement the method for in-situ aging testing of PE for cable-stayed bridges as described in any one of claims 1 to 11, characterized in that, The system includes: The spectral acquisition and environmental state combination generation module is used to acquire first-depth infrared spectral signals and second-depth infrared spectral signals through infrared acquisition equipment, and simultaneously read contact load values, surface temperature values ​​and sheath geometric curvature to generate multi-dimensional environmental state combinations. The correction and carbonyl index estimation module is used to substitute the multidimensional environmental state combination into the contact transfer function to calculate the absorption band integral correction coefficient, and use the absorption band integral correction coefficient to correct the first depth infrared spectral signal and the second depth infrared spectral signal to generate the first carbonyl index estimation value and the second carbonyl index estimation value. The differential stratification module is used to combine the effective detection depth constant of the dual channels to perform differential stratification on the first carbonyl index estimate and the second carbonyl index estimate, and separate the surface oxidation physical quantity, subsurface oxidation physical quantity and oxidation depth gradient value. The oxidation induction time prediction and maintenance triggering module is used to substitute the surface oxidation physical quantity, the subsurface oxidation physical quantity and the oxidation depth gradient value into a preset constraint regression equation, calculate the oxidation induction time prediction, and trigger maintenance instructions.