Cement-silica two-time-point correction determination method and system thereof

By employing a dual-time-point strategy of adding Ge tracer and Cd internal standard to cement, combined with the internal standard method and failure threshold determination, the problem of separately observing pretreatment loss and measurement fluctuation in cement silica determination was solved, achieving accurate determination of cement silica content and improving the reliability of analytical results.

CN123135784APending Publication Date: 2026-11-20CHINA RAILWAY 20TH BUREAU GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611492873.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies for determining silica in cement cannot effectively separate and address pretreatment losses from ICP-OES measurement fluctuations, leading to a confusion of errors and an inability to accurately determine the source of deviations. Furthermore, they cannot identify the conversion relationship between Si and Ge under different cement matrices, which can easily mask abnormal sample results.

Method used

A dual-time-point strategy was adopted, in which Ge tracer was added before alkali fusion and Cd internal standard was added before volume adjustment. The spectral intensities of Si, Ge and Cd were determined by inductively coupled plasma atomic emission spectrometry. The recovery rate of Ge pretreatment was calculated by combining the internal standard method, and a failure threshold was set to determine the effectiveness of pretreatment and avoid forced correction.

Benefits of technology

It enables separate observation and processing of pretreatment losses and measurement fluctuations, improves the reliability of analysis results, accurately identifies the source of deviation, prevents misjudgment, and significantly improves the accuracy and reliability of cement silica content determination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123135784A_ABST
    Figure CN123135784A_ABST
Patent Text Reader

Abstract

The application discloses a method and system for determining the content of silicon dioxide in cement. The method adds Ge tracer at the first time point before alkali fusion treatment, so that the Ge tracer and Si to be measured jointly experience the whole process of melting, leaching, acidification and transfer. Cd internal standard is added at the second time point after the test solution is transferred to the volumetric flask and before constant volume, so that the Cd internal standard only corrects the fluctuation in the measurement stage. After the spectral intensity of Si, Ge and Cd is determined, the internal standard method is used to calculate the Ge pretreatment recovery rate, and the recovery rate is compared with the preset threshold value. When the recovery rate is within the threshold value range, the silicon content data is corrected to calculate the content of silicon dioxide. When the recovery rate is lower than the threshold value, it is determined that the pretreatment is invalid, the correction is prohibited, and re-sampling is prompted. The application realizes independent identification of pretreatment loss and measurement fluctuation through a double-time-point separation strategy, and significantly improves the accuracy and reliability of the determination of the content of silicon dioxide in cement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of cement chemical analysis and inductively coupled plasma atomic emission spectrometry (ICP-AES) detection technology, specifically relating to a method and system for determining cement silica with dual time-point calibration. Background Technology

[0002] In cement, SiO2 is typically found in various structures formed by silicate clinker minerals, glass phases, and admixtures. Direct acid dissolution is insufficient to guarantee complete decomposition. Inductively Coupled Plasma Optical Emission Spectrometer (ICP-OES) typically employs a process of NaOH alkali fusion, hot water leaching, hydrochloric acid acidification, quantitative transfer, and volume adjustment before determination. Current methods enable rapid multi-element determination, but high salt and acid content can alter atomization efficiency and plasma load. Continuous injection can also lead to pump tube fatigue, atomizer salting out, and spectral response drift. Adding internal standards such as Cd after volume adjustment only corrects for injection and excitation fluctuations after the addition point, failing to reflect incomplete frit formation, leaching residues, localized gelation during acidification, liquid residue buildup in the crucible or beaker, and incomplete transfer. Furthermore, when evaluating analytical quality solely based on total oxide count, positive and negative biases for multiple elements may cancel each other out, and it's impossible to determine whether the bias originates from chemical pretreatment or spectroscopic measurement. The existing alkali fusion multi-element method often combines the above errors into a total correction coefficient, which makes it easy to implement numerical compensation from the result end when the pretreatment has failed, so that the abnormal sample surface meets the closure requirements and the true SiO2 content is masked. Summary of the Invention

[0003] To overcome the shortcomings of the prior art, the present invention aims to provide a method and system for determining cement silica with dual-time-point calibration. This method allows for the separate observation and processing of pretreatment losses and ICP-OES measurement fluctuations without altering the main cement NaOH alkali fusion process. It solves the problems of Ge and Si recovery not being naturally equivalent and the need for calibration of conversion relationships under different cement matrices. Furthermore, the method of the present invention establishes a failure boundary that cannot be replaced by mathematical corrections for re-sample preparation, thereby preventing forced compensation at the result end for severe melting or transfer anomalies.

[0004] To achieve the above objectives, the present invention employs the following technical solution: A first aspect of the present invention provides a method for determining the silica content in cement, comprising the following steps: S1. Obtain a cement sample and add a predetermined amount of Ge tracer to the cement sample at the first time point, and collect sample information containing Ge tracer. S2. The sample containing the Ge tracer is subjected to alkali fusion treatment, leaching treatment and acidification treatment, and the resulting test solution is transferred to a volumetric flask; S3. At the second time point, inject a predetermined amount of Cd internal standard into the volumetric flask and make up to volume to obtain the test solution; S4. The spectral intensities of Si, Ge, and Cd in the test solution were determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). After background correction, the net intensities of Si, Ge, and Cd were obtained, respectively. S5. Based on the net strength data of Ge and the net strength data of Cd, calculate the Ge pretreatment recovery rate using the internal standard method. And the obtained Ge pretreatment recovery rate Compare with a preset threshold range. Wherein, when the Ge pretreatment recovery rate When within the preset threshold range, based on the Ge pretreatment recovery rate The silicon content data obtained from the net strength data of Si is corrected to calculate the silica content in the cement sample; and, when the Ge pretreatment recovery rate... If the sample content exceeds the preset threshold range, an invalid sample pretreatment determination message is generated, the correction calculation of the silicon content data is prohibited, and a prompt message for re-sample preparation is output. The first time point is before the alkali fusion treatment of the sample, and the second time point is after the obtained test solution is transferred to a volumetric flask and before the test solution is diluted to volume.

[0005] In some embodiments, the amount of Ge tracer added is 2.000 mg / L based on the theoretical Ge concentration in the final diluted solution, the amount of Cd internal standard added is 1.000 mg / L based on the theoretical Cd concentration in the final diluted solution, and the Ge pretreatment recovery rate is... It was determined by performing conventional subtraction calculations on the Ge / Cd ratio of the sample, the Ge / Cd ratio of the blank sample, and the natural Ge background.

[0006] In some implementations, the Ge pretreatment recovery rate Determine according to the following formula (1): (1) in, The Ge / Cd strength ratio of the sample; This represents the blank corresponding ratio without Ge; ; The Ge / Cd theoretical mass concentration ratio is set to 2; It is the equivalent concentration of natural Ge; and Determined according to the following formula (2), (2), in, The average Ge / Cd ratio after adding a reference is Ge.

[0007] In some implementations, the preset threshold range is between the low-side failure threshold and the low-side failure threshold. With high side movement limit Between, wherein the high-side movement limit Set as And the low-side failure threshold Determine using the following formula (3): (3) In the formula, To allow for the minimum Ge recovery rate required for conversion correction, The average recovery rate of Ge pretreatment for the standard sample and This represents the standard deviation within the laboratory. Wherein, when the Ge pretreatment recovery rate is at the low-side failure threshold With the aforementioned high side movement limit Correction is permitted when the Ge pretreatment recovery rate exceeds the low-side failure threshold. With the aforementioned high side movement limit When the range is within a certain range, invalid preprocessing information is generated.

[0008] In some implementations, based on the Ge pretreatment recovery rate Correcting the silicon content data obtained from the net Si strength data includes: fitting the Ge recovery loss data and Si recovery loss data of multiple standard samples using the least squares method to establish a conversion model and determine the conversion coefficient κ; and, based on the conversion model and the Ge pretreatment recovery rate of the samples... Calculate the predicted recovery rate of Si. and utilize predicted recovery rate Correct the silica content.

[0009] In some implementations, the conversion coefficient κ is determined according to the following formula (4): (4) in, The weighted data are determined based on the uncertainty and repeated measurement variance of each standard sample. For Ge recycling losses, 0.94≤ ≤1.02; and, The Si recovery loss is calculated based on the weight of the cement sample, and is the ratio of the uncorrected SiO2 result to the value of the standard sample.

[0010] In some implementations, the predicted recovery rate of Si is determined according to the following formula (5). : (5).

[0011] In some implementations, after obtaining the silicon content data from the net Si intensity data, the uncorrected silicon dioxide mass fraction is calculated according to the following formula (6): (6) in, This refers to the final volume of the test solution, in liters (L). This represents the weight of the cement sample, in grams. This refers to the dilution factor; Here is the molar mass of Si, expressed in g / mol. The molar mass of SiO2 is expressed in g / mol; and, The silicon concentration data obtained from the Si calibration curve without pretreatment recovery correction; When correction is allowed, the corrected silica mass fraction Calculate according to the following formula (7): (7).

[0012] In some implementations, step S4 further includes the following steps: Obtain the net intensity data of Cd and the intensity ratio data of Ge / Cd; The net intensity data of Cd is compared with a preset normal range, and the Ge / Cd intensity ratio data is compared with a preset threshold. Based on the comparison results, the following judgment information is generated: When the Cd net intensity data is abnormal but the Ge / Cd intensity ratio data is normal, a first judgment information is generated to indicate an abnormality in sample introduction or plasma and to trigger a retest command for the original sample solution; when the Cd net intensity data is normal but the Ge / Cd intensity ratio data is low, a second judgment information is generated to indicate an abnormality in melting, leaching, or transfer and to trigger a resample preparation command; when both the Cd net intensity data and the Ge / Cd intensity ratio data are abnormal, a third judgment information is generated to trigger a retest command for the original sample solution; if the Cd net intensity data recovers after retesting but the Ge / Cd intensity ratio data is still low, the third judgment information is updated to indicate a pretreatment failure and to trigger a resample preparation command; if both recover after retesting, the third judgment information is updated to indicate an instantaneous measurement failure.

[0013] A second aspect of the present invention provides a system for determining the silica content in cement, comprising: The sample pretreatment module is used to add a predetermined amount of Ge tracer to the cement sample at a first time point, collect sample information containing Ge tracer, perform alkali fusion treatment, leaching treatment and acid treatment on the sample containing Ge tracer, and transfer the resulting test solution to a volumetric flask; and inject a predetermined amount of Cd internal standard into the volumetric flask at a second time point and make up the volume of the test solution to obtain the test solution. The spectral measurement module is used to measure the spectral intensities of Si, Ge and Cd in the test solution using inductively coupled plasma atomic emission spectrometry. After background correction, the net intensity data of Si, Ge and Cd are obtained respectively. The data processing module is used to calculate the Ge / Cd intensity ratio based on the net Ge intensity data and the net Cd intensity data, and to determine the Ge pretreatment recovery rate based on the Ge / Cd intensity ratio data. and the Ge pretreatment recovery rate Compare with a preset threshold; The calibration calculation module is used to calculate the Ge pretreatment recovery rate. When within the preset threshold range, based on the Ge pretreatment recovery rate The silicon content data obtained from the net strength data of Si is corrected, and the corrected silicon dioxide content data is calculated. The determination output module is used when the... When the sample content is below the preset threshold, a determination message indicating invalid sample pretreatment is generated, the correction calculation of the silicon content data is prohibited, and a prompt message indicating that the sample should be prepared again is output. Wherein, the first time point is the time point before the sample undergoes alkali fusion treatment, and the second time point is the time point after the test solution is transferred to the volumetric flask and before the test solution is brought to volume.

[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention employs a dual-time-point strategy, adding Ge tracer before alkali fusion and Cd internal standard before volume adjustment, to separate the sources of uncertainty in a single measurement according to time boundaries: Cd only corrects for measurement fluctuations occurring after its addition, such as injection, nebulization, and excitation; while Ge undergoes the complete melting, leaching, acidification, and transfer process together with the Si to be measured. The combined use of these two methods allows operators to clearly determine whether the deviation originates from the chemical pretreatment stage or the instrument measurement stage, avoiding misjudgments caused by the traditional method of conflating the two types of errors.

[0015] (2) This invention sets a failure threshold for Ge pretreatment recovery rate. When the Ge pretreatment recovery rate... When the sample exceeds the threshold range, the pretreatment is directly deemed invalid, correction calculations are prohibited, and a new sample is forced to be prepared, instead of forcibly incorporating the deviation into the total correction factor for numerical compensation as in existing technologies. This mechanism fundamentally avoids the situation where "the pretreatment has failed but the results still provide qualified data," significantly improving the reliability of the analytical results.

[0016] (3) This invention does not simply equate Ge recovery rate with Si recovery rate. Instead, it establishes the conversion coefficient between Ge recovery loss and Si recovery loss through actual measurement of standard samples, and uses the weighted least squares method through the origin for fitting, which objectively reflects the differences between Si and Ge in terms of lattice decomposition difficulty and acidification polymerization tendency under different cement matrices.

[0017] (4) This invention establishes a three-level fault location logic by combining the absolute intensity of Cd with the Ge / Cd ratio: distinguishing between sample injection / plasma faults, pretreatment (melting / leaching / transfer) faults, and instantaneous measurement faults. Operators can directly implement the corresponding treatment measures (retest the original sample or re-prepare the sample) based on the judgment results, without relying on empirical guesswork.

[0018] (5) When conventional methods rely on the total amount of multi-element oxides to evaluate the quality of analysis, the deviations of different elements may cancel each other out. The Ge recovery index of the present invention can independently monitor the loss of Si in the pretreatment, and can identify the case where the SiO2 content is low even if the total amount of oxides is still within the closed range.

[0019] (6) Without changing the main process of cement NaOH alkali fusion and ICP-OES determination, the present invention can achieve all the above functions by adding only two quantitative additions and corresponding ratio calculations. No additional equipment is required, and it has good applicability for promotion. Attached Figure Description

[0020] Figure 1 This is a schematic flowchart of the method for determining the silica content in cement according to the present invention. Detailed Implementation

[0021] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0022] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0023] When numerical ranges are provided, it should be understood that, unless the context explicitly specifies otherwise, every intermediate value between the upper and lower limits of the range (to one-tenth of the lower limit unit), as well as any other specified or intermediate value within the specified range, is included in this invention. The upper and lower limits of these smaller ranges may be independently included within the smaller ranges and also within this invention, but must comply with any explicitly excluded limits within the specified range. When a specified range includes one or two limits, the range excluding any one or both of these included limits is also included in this invention.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Although any methods and materials similar to or equivalent to those described herein may also be used in the practice or testing of this invention, preferred methods and materials are now described.

[0025] Upon reading this invention, it will be apparent to those skilled in the art that each individual embodiment described and illustrated herein has discrete components and features that can be readily separated from or combined from features of any other several embodiments without departing from the scope or spirit of the invention. Any of the described methods may be performed in the order of the events or in any other logically possible order.

[0026] The following examples are provided to demonstrate to those skilled in the art how to perform the disclosed and claimed methods and how to use the disclosed and claimed compositions and compounds in accordance with the full disclosure and description. Efforts have been made to ensure the accuracy of figures (e.g., quantities, temperatures, etc.), but some errors and deviations should be taken into account.

[0027] See Figure 1 The first aspect of the present invention provides a method for determining the silica content in cement, comprising the following steps: S1. Obtain a cement sample and add a predetermined amount of Ge tracer to the cement sample at the first time point, and collect sample information containing Ge tracer. S2. The sample containing the Ge tracer is subjected to alkali fusion treatment, leaching treatment and acidification treatment, and the resulting test solution is transferred to a volumetric flask; S3. At the second time point, inject a predetermined amount of Cd internal standard into the volumetric flask and make up to volume to obtain the test solution; S4. The spectral intensities of Si, Ge, and Cd in the test solution were determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). After background correction, the net intensities of Si, Ge, and Cd were obtained, respectively. S5. Based on the net strength data of Ge and the net strength data of Cd, calculate the Ge pretreatment recovery rate using the internal standard method. And the obtained Ge pretreatment recovery rate Compare with a preset threshold range. Wherein, when the Ge pretreatment recovery rate When within the preset threshold range, based on the Ge pretreatment recovery rate The silicon content data obtained from the net strength data of Si is corrected to calculate the silica content in the cement sample; and, when the Ge pretreatment recovery rate... If the sample content exceeds the preset threshold range, an invalid sample pretreatment determination message is generated, the correction calculation of the silicon content data is prohibited, and a prompt message for re-sample preparation is output. The first time point is before the alkali fusion treatment of the sample, and the second time point is after the obtained test solution is transferred to a volumetric flask and before the test solution is diluted to volume.

[0028] This invention, without altering the main process of NaOH alkali fusion for cement, separates the observation and handling of pretreatment losses from ICP-OES measurement fluctuations: one tracer element enters the sample before melting and undergoes melting, leaching, acidification, and transfer together with Si, while another internal standard enters the sample solution only after pretreatment and before volume adjustment; first, the Si / Cd strength ratio is used to eliminate sample injection and plasma fluctuations, and then the Ge / Cd relative theoretical addition ratio is used to characterize pretreatment recovery, addressing the issue that Ge and Si recovery are not naturally equivalent and that the conversion relationship under different cement matrices requires calibration; simultaneously, a failure boundary is set that cannot be replaced by mathematical correction to allow for re-sample preparation, thereby preventing forced compensation at the result end for severe melting or transfer anomalies.

[0029] This invention addresses uncertainties in a single determination by separating them at the point of addition. Specifically, the first point is before the sample comes into contact with the NaOH flux. A quantitative Ge tracer, whose natural cement content is negligible relative to the added amount and which can be converted into water-soluble germanate under alkaline melting conditions, is added to the weighed sample. Ge then undergoes the same crucible heating, melt formation, cooling, hot water leaching, hydrochloric acid acidification, vessel wall washing, quantitative transfer, and temperature equilibration process as the Si being measured. The second point is after the above processes are completed but before the volumetric flask is brought to volume. A quantitative Cd internal standard is added to the volumetric flask. Cd does not undergo melting, leaching, or transfer; it only undergoes final mixing, sample delivery, atomization, plasma excitation, and optical detection. During measurement, the content is not directly calculated using the absolute emission intensity of Si, but rather by dividing the background-corrected net intensity of Si by the net intensity of Cd; similarly, the net intensity of Ge is divided by the net intensity of Cd. The first ratio is used for Si quantification and to offset the common measurement fluctuations that occur after Cd is added. The second ratio is compared with the Ge / Cd ratio of the same batch with 100% theoretical recovery reference to obtain the Ge pretreatment recovery rate after the Cd measurement fluctuations have been eliminated. Therefore, if the absolute Cd intensity is abnormal but the Ge / Cd ratio is normal, the problem is primarily identified as an injection or plasma issue; if the absolute Cd intensity is normal but the Ge / Cd ratio is low, the problem is primarily identified as a melting, leaching, or transfer issue; if both are abnormal, the original sample solution is retested to rule out measurement stage faults, and then the decision on whether to re-prepare the sample is made based on the retested Ge / Cd ratio.

[0030] Therefore, this invention does not directly equate Ge recovery rate with Si recovery rate. Both GeO2 and germanates and SiO2 form oxyacid salts in alkaline melts, but the Si content in cement is affected by the clinker mineral lattice, the degree of glass phase polymerization, and the activity of the admixtures. After acidification, the hydrolysis and polymerization tendencies of Si and Ge are not entirely the same. Therefore, certified standard samples covering the range of SiO2 content in the tested cement matrix are used to measure the conversion factor between Ge recovery deficit and Si recovery deficit. This conversion is only applied to samples that are determined to be within a slight, modelable deviation range; when Ge recovery is below a predetermined failure threshold, no correction result is calculated, and the pretreatment is directly deemed invalid and a new sample is weighed. Thus, "whether the sample preparation is acceptable" is placed before "how to correct the values."

[0031] In the melting reaction, the idealized reactions of free oxides are SiO2 + 2NaOH → Na2SiO3 + H2O and GeO2 + 2NaOH → Na2GeO3 + H2O. Not all Si in cement exists as free SiO2; NaOH also needs to disrupt the Si-O-Ca, Si-O-Al, and Si-O-Si bonds in calcium silicates, aluminosilicates, and the glass phase. Therefore, Ge can only serve as a tracer rather than a stoichiometric substitute. The advantage of choosing Ge lies in its measurability within the same alkali-fusion and acidification windows, and its naturally low background, ensuring that melt loss, leaching residue, and transfer residue leave consistent defects in the Ge signal. The conversion factor specifically addresses the difficulty of lattice decomposition and the differences in acidification polymerization. The amount of Ge added corresponds to approximately 0.500 mg Ge, only 0.01% of the mass of 5.00 g flux, and will not substantially change the melt basicity or cement decomposition conditions.

[0032] The following section will describe in detail each step of the method for determining the silica content in cement.

[0033] In step S1, the sample is reduced according to the general requirements for cement chemical analysis, and all samples are passed through a 0.080 mm sieve. The sample is then dried at 105℃~110℃ for 2 h and cooled to room temperature in a desiccator. For samples containing easily oxidized sulfides or high-organic admixtures, the ignition temperature is not increased beforehand to avoid altering the components to be tested. If a dry basis result is required, a separate sample is taken to determine the moisture content and the result is converted to a dry basis.

[0034] Weigh 0.4000 g for each sample, with an allowable range of 0.3990 g to 0.4010 g, accurate to 0.0001 g. Use a 30 mL to 50 mL covered silver crucible; before use, the crucible should be rinsed with dilute HCl, washed with water, and dried at 105 °C. Empty crucibles should not have a peelable corrosion layer. The silver crucible should be able to withstand the 650 °C to 700 °C NaOH melting conditions of this method, and avoid the spectral background and matrix load caused by a large amount of Ni entering the test solution when using a Ni crucible.

[0035] Before weighing, each laboratory sample should be rolled and mixed in a sealed container for 60 seconds. Then, use a clean spoon to take samples alternately from the top, middle, and bottom of the container to prevent stratification of denser clinker particles and lighter mixtures due to transport vibration. Two parallel samples should be taken from different surface areas, and the sample bottle should be immediately replaced after weighing. If the sample contains visible fibers, metal shavings, or foreign matter larger than 0.080 mm, it should be re-prepared according to the applicable product method; do not attempt to address sample inhomogeneity by increasing the amount of NaOH. The interval between weighing and Ge addition should not exceed 30 minutes to prevent the dried sample from reabsorbing moisture from the air, which could cause changes in sample mass.

[0036] The flux was analytical grade NaOH granules or tablets, 5.00 g per sample, with the same reagent batch number used for each batch of tests. HCl was of analytical grade, with density and mass fraction recorded according to the reagent certificate; analytical water was of grade II or higher. Si, Ge, and Cd single-element standard solutions were all 1000 mg / L stock solutions with traceability certificates. The Cd working solution was prepared to 100.0 mg / L, with 2% HNO3 as the medium; Ge was then prepared to 100.0 mg / L with reference working solution added, using the same medium as the Cd working solution. All volumetric flasks and pipettes were calibrated to their ranges; Ge and Cd were added using calibrated pipettes or Grade A single-mark pipettes.

[0037] For the initial addition of Ge, a sodium germanate tracer working solution with a concentration of 1000 mg / L (based on Ge) is preferred. 0.500 mL of this solution is added per sample, ensuring a theoretical Ge concentration of 2.000 mg / L in the final 250 mL solution. This working solution is prepared from a Ge single-element stock solution using NaOH medium, with the NaOH mass concentration controlled between 2 g / L and 5 g / L. After adding the sample, gently rotate the crucible to ensure the droplets evenly wet the sample. Evaporate on a heating plate at 105℃–110℃ until no visible free liquid remains on the surface. After cooling, add the NaOH flux. Evaporate to dryness to fix the Ge to the sample particles and the bottom of the crucible, preventing splashing or residue along the crucible walls during flux addition. When increased sensitivity to incomplete melting is required, a GeO2 microdispersed tracer solution can be used: Prepare a uniform microdispersion solution of 1000 mg / L (based on Ge) using high-purity GeO2, with a median particle size of 5 μm–20 μm. Before use, sonicate at 20 kHz–40 kHz for 5 min and transfer 0.500 mL within 30 s; evaporate to dryness after addition. The two tracer forms must not be mixed in the same conversion model; the conversion coefficient and threshold must be re-determined after changing the form. For routine batch detection, sodium germanate working solution is preferred to reduce dispersion sampling errors; GeO2 microdispersion solution is used when establishing the method or when enhanced melt fault identification is required.

[0038] Sodium germanate tracer working solution was prepared stepwise by mass method. First, weigh a stoppered bottle containing water, then add Ge stock solution transferred using a calibrated pipette. Verify the transferred volume by checking the mass difference before and after addition and the water density at 20°C. Add NaOH and bring to volume. Observe after 12 hours; no turbidity or surface crystallization should appear. Before each use, take 0.500 mL and add it to an empty silver crucible, prepare according to the complete process, and compare with the Ge-added reference. The average recovery of the freshly prepared working solution from three consecutive processes should be 0.985–1.015, with a range not exceeding 0.010. Store the working solution in a polyethylene bottle protected from light; shelf life is 30 days. If precipitation, evaporation crystallization at the bottle neck, or process blank deviation occurs, discard immediately. Cd working solution was diluted using the same mass method and has a shelf life of 90 days. Ge and Cd are added using dedicated pipette tip boxes of different colors. First, the entire batch of Ge is added and the sample number is checked. After all the samples are transferred into the volumetric flask, Cd is added later to prevent confusion between the two addition points due to overlapping operations by personnel.

[0039] Cd is added after each sample has been completely transferred and cooled to room temperature. Add 2.500 mL of 100.0 mg / L Cd working solution to a 250 mL volumetric flask to bring the final theoretical Cd concentration to 1.000 mg / L. The volumetric flask should contain approximately 200–230 mL of liquid at the time of addition, and then dilute to volume with water. Cd must not be added to the crucible, leaching beaker, or before transfer, nor should Cd be premixed with HCl washing solution; otherwise, Cd will undergo partial pretreatment, disrupting the two-timepoint separation relationship.

[0040] In step S2, the alkali fusion treatment is as follows: 0.4000 g of sample is placed in the center of a silver crucible, and 0.500 mL of Ge tracer working solution is added to cover the sample without dispersing it. The solution is then evaporated to dryness under the conditions described above. After cooling, approximately 1.0 g of NaOH is added, and the sample and flux are gently mixed using a PTFE rod. The remaining 4.0 g of NaOH is then used to cover the mixture, and the crucible lid is closed, leaving a gap of approximately 1 mm. The purpose of layering the addition is to prevent the sample from being directly exposed to the airflow during the initial heating phase, and to avoid splashing caused by instantaneous contact between all the flux and the wet sample. The Ge addition time, NaOH addition time, and furnace position for each crucible are recorded in the sample sequence.

[0041] Preheat the high-temperature furnace to 300–350°C. After placing the crucible in the furnace, increase the temperature to 675°C at a rate of 8–15°C / min, with a stable range of 650–700°C. Start timing when the temperature reaches 650°C, with a total melting time of 20 min. At the 10-minute mark, remove the crucible using preheated crucible tongs, keeping the lid in place, and gently shake it in small circular motions 3–5 times to allow unreacted particles adhering to the wall to re-enter the melt. This operation should be completed within 30 seconds. Then, return the crucible to its original furnace position. At the end of the melting process, the melt should be continuous, without obvious powdery islands or black unmelted material. Visual observation is only supplementary information and cannot replace Ge recovery criteria. If melt overflows, the crucible tipps over, or large-area splashing and deposition occurs on the lid, the sample is immediately discarded.

[0042] High-temperature furnaces should undergo temperature uniformity verification of the working area at least every 6 months. Calibrated thermocouples should be placed at each furnace position planned for use, and the furnace should be held at 650℃, 675℃, and 700℃ for 20 minutes each. The deviation between the measured temperature and the set value at each furnace position should not exceed 10℃, and the range between furnace positions at any given time should not exceed 15℃. For routine batches, an independent temperature recording probe should be placed at the central furnace position. The time before the actual temperature reaches 650℃ is not included in the melting time. The time required for the temperature to return to 650℃ after opening the door and shaking should be less than 3 minutes. If it exceeds this time, it should be marked in the record, and the Ge recovery distribution of that batch should be checked. Crucibles should be placed in a serpentine pattern within the furnace. Certified standard samples should be arranged at both the relatively lower and higher furnace positions to identify system differences caused by furnace position. If the Ge recovery of the same batch shows a monotonous change with furnace position, even if individual samples have not yet exceeded the threshold, the release of results should be suspended, and the furnace temperature uniformity should be checked.

[0043] The leaching process is as follows: Remove the crucible and cool it on a heat-resistant plate for 3–5 minutes to allow the melt to solidify without prolonged moisture absorption. Place the crucible sideways into a 300 mL PTFE or alkali-resistant beaker pre-filled with 100 mL of boiling water, immediately cover with a watch glass, and maintain a temperature of 90–98°C on a controlled heating plate. Gently touch the outer wall of the crucible with a PTFE rod to promote the shedding of the molten material; do not scrape the crucible with metal utensils. After leaching for 8–12 minutes, check the inner wall of the crucible and the bottom of the beaker; there should be no hard, transparent, or milky white molten material. If molten material is still present, continue heating for a cumulative total of 15 minutes, but do not use methods such as increasing the amount of acid to mask incomplete leaching.

[0044] The acidification treatment is as follows: After the molten metal is completely leached out, 27.5 mL of concentrated HCl is added along the beaker wall in one go while continuously stirring. The allowable range is 25.0–30.0 mL. The acid addition rate is controlled at 15–30 s to avoid localized high acidity that could cause Si to form a gel that is difficult to redisperse. Immediately after adding acid, stir for 60 s, then gently boil at 90–98 °C for 1 min to allow the attached particles and hydrolysis intermediates to redisperse uniformly. The crucible and crucible lid are rinsed three times with approximately 20 mL of hot HCl solution (volume ratio 1+5), ensuring that the washing solution covers the entire inner surface and flows back into the original beaker each time. Then, the crucible is washed three times with water, approximately 10 mL each time. Before the crucible is removed from the beaker, the final washing solution is observed to ensure continuous flow and that there are no visible beads. If the solution contains flocculent silica that can entangle the stirring rod, insoluble particles are present at the bottom of the beaker, or visible loss occurs during transfer, even if the subsequent Ge signal may still be near the threshold, the sample is marked as manually rejected and will not be included in the numerical correction.

[0045] Cool the solution in the beaker to 20–25°C and quantitatively transfer it to a 250 mL volumetric flask along a glass rod. Wash the beaker, watch glass, and glass rod with water at least four times, 10–15 mL each time, and add all the washings to the volumetric flask. Ensure the liquid volume does not exceed 230 mL. Add 2,500 mL of Cd working solution, gently shake to mix, and then dilute to the mark with water. Tightly stopper the flask and invert it 20 times, ensuring all air bubbles pass completely through the liquid column each time. Let it stand for 10 minutes until the temperature returns to 20–25°C. Check the liquid level; if necessary, add more water to the mark and invert it 10 times again. If visible particles are still present in the solution, do not filter directly, as filtration may introduce new differential adsorption of Si and Ge. Discard the solution based on Ge recovery and visual inspection records, and prepare a new sample.

[0046] The final matrix after acidification is centered on 5.00 g NaOH and 27.5 mL concentrated HCl per sample. If the actual amount of NaOH added changes due to moisture absorption, it is not adjusted by adding additional acid per sample; instead, small changes are absorbed by the batch blank reagent and matrix matching calibration. If the NaOH surface shows significant deliquescence or the titration purity is lower than the reagent's labeled lower limit, the reagent is replaced. Three samples (first, middle, and last) from each batch are randomly selected, and their density or mass per unit volume after volume adjustment is measured at 20°C. The relative range of these three measurements should not exceed 1.0%, used to check for missed acid, missed flux, or volume adjustment errors. This density check is only used as a batch consistency indicator, does not participate in SiO2 calculations, and does not cover the Ge low recovery rejection rule.

[0047] In step S3, each batch contains no more than 20 samples, and four types of solutions are prepared. The first type is a Ge-free reagent blank, which undergoes melting, leaching, acidification, and transfer with 5.00 g NaOH, with 1.000 mg / L Cd added only before volume adjustment to subtract reagent and vessel background from Si and Ge. The second type is a pre-Ge addition blank, in which 2.000 mg / L of Ge equivalent is added to an empty crucible at the same time as the sample and the entire process is carried out, used to monitor Ge reagent stability, crucible adsorption, and batch consistency. The third type is a Ge-added 100% recovery reference, in which a blank matrix with the same NaOH and HCl loading as the sample is first prepared, and after being transferred to a volumetric flask, 2.000 mg / L Ge and 1.000 mg / L Cd are added simultaneously, without subjecting Ge to pretreatment; its Ge / Cd response is defined as the theoretical complete recovery response for that batch. The fourth category is the Si calibration series. Before volume adjustment in the same blank matrix, Si standard and fixed Cd are added. Si concentrations are set at 0 mg / L, 25 mg / L, 50 mg / L, 100 mg / L, 150 mg / L, 200 mg / L, and 250 mg / L. An additional 2,000 mg / L of fixed Ge is added to simultaneously verify the Ge response factor. The differences in Na, Cl, and residual acid concentrations between all calibration solutions and the sample solutions are controlled within 5%.

[0048] At least one certified cement standard sample should be prepared for each batch as an independent monitoring sample, with Ge added before the sample preparation. This sample is not used for fitting the Si working curve for that batch and is used to determine whether the established Ge-Si conversion relationship is still applicable. When initially establishing the conversion model, at least three certified cement standard samples should be selected, with SiO2 certified values ​​covering 15-40%, and including at least two matrices from silicate cement, slag-containing cement, and pozzolanic cement. At least six samples of each standard sample should be prepared independently under normal conditions and pre-designed slight perturbation conditions. Slight perturbations are only used for modeling, including melting times of 16, 18, 20, and 22 minutes, melting temperatures of 650°C, 675°C, and 700°C, and a 10% change in total washing volume near the specified value; data that has already experienced spillage, visible residue, or Ge recovery below the hard failure line should not be used for fitting. This design allows the model to cover common small chemical recovery variations without including severe failures in the compensable region.

[0049] The Si calibration series does not use pure water as a solvent directly. First, a cement-free NaOH molten blank mother liquor is prepared following the sample procedure. Multiple blanks are combined, cooled, and mixed thoroughly. Then, they are dispensed according to calculated volumes, with Si standard solution, Ge followed by reference solution, and Cd working solution added separately. Matrix dilution caused by the added standard solution volume is compensated for with blank acid matrix at all calibration points, ensuring the total volume of added solution in each volumetric flask is the same. The blank matrix is ​​measured immediately after measuring the highest Si calibration point; the residual Si signal should not exceed 0.2% of the highest point. If it does, the rinsing process is prolonged, and the affected low-concentration calibration points are re-measured. Since the Si concentration of the test solution is typically between 100 mg / L and 200 mg / L, the calibration check solution is set around 150 mg / L to avoid evaluating drift only at the lower end of the curve.

[0050] In step S4, the ICP-OES should have background correction, multi-wavelength observation, and internal standard calculation functions. It is recommended to use Si I 251.611 nm as the main analytical line and Si I 288.158 nm as the confirmation line; Ge I 209.426 nm as the main tracer line and Ge I 265.118 nm as the confirmation line; and Cd II 214.438 nm as the main internal standard line and Cd II 226.502 nm as the confirmation line. If the specific instrument has different resolutions or optical structures, wavelength scanning should be performed using a single-element solution and a cement blank matrix to confirm that the background points on both sides of the analytical peak do not fall on the structures of Fe, Al, Ti, P, Ni, or molecular bands. The results of the main and confirmation spectra should be calculated separately. For normal samples, the relative difference in SiO2 should not exceed 0.8%, and the absolute difference in Ge recovery should not exceed 0.015. If these values ​​are exceeded, check for spectral interference; do not use the average of the two lines to mask anomalies.

[0051] Recommended parameters include: RF power 1.20–1.35 kW, plasma gas flow rate 12–15 L / min, auxiliary gas flow rate 0.8–1.2 L / min, nebulizing gas flow rate 0.60–0.75 L / min, sample rise rate 0.8–1.2 mL / min, stabilization time 25–40 s, single integration time 3–5 s, and three parallel readings per solution. For high-salt matrices, a high-salt-resistant concentric nebulizer, a cyclone chamber, and a central tube with an inner diameter of at least 1.0 mm are preferred. Before each sample injection, rinse with 2% HNO3 for 20 s, followed by a 20 s pre-rinse with the same batch of blank matrix. After each sample injection, alternately rinse with water and 2% HNO3 until the Si, Ge, and Cd signals drop below 0.2% of the previous sample signal. After measuring 10 consecutive samples, insert one intermediate concentration calibration check solution.

[0052] Spectral confirmation employs a two-stage check involving single-element spikes and spikes with high-content coexisting elements. First, matrix-matched solutions containing only Si, Ge, or Cd are measured to determine the peak center and left and right background windows. Then, interference solutions containing Ca, Al, Fe, Mg, Ti, P, and S are prepared according to common high-content levels in cement, and the target wavelength ±0.050 nm range is scanned without adding the target element. If the equivalent concentration of any coexisting element within the target integration window exceeds 0.5% of the working concentration of the target element, the background point is moved, spectral line fitting is used for subtraction, or the confirmation line is switched. When using mathematical interference correction, the interference coefficient is fitted with five concentration points of a single coexisting element and verified using an independent mixed matrix; the physical meaning of the low recovery threshold of Ge must not be changed before or after correction. For each batch, one sample is added with a Si standard equivalent to 5% of the original Si concentration and a Ge standard equivalent to 10% of the added Ge concentration. The incremental recovery should be 97–103%, used to identify spectral line suppression or background fitting errors. Spiked samples are only used to evaluate the spectral response and are not used to correct the original sample results.

[0053] After the instrument has been ignited and stabilized for 30 minutes, first measure the blank without Ge reagent, then measure the Si calibration series, the Ge-added 100% recovery reference, the process blank, the independent monitoring sample, and the test sample. The calibration curve is fitted with the intensity ratio after Cd normalization, not with the absolute elemental intensity. The coefficient of determination of the Si curve should not be less than 0.9995, and the relative deviation of each non-zero calibration point should not exceed 2.0%. The relative standard deviation of the Ge / Cd ratio obtained from five consecutive measurements with the Ge-added reference should not exceed 1.0%. The absolute net Cd intensity is based on the net Cd intensity of the intermediate verification solution of the batch. The Cd response coefficient of the sample should be between 0.80 and 1.20, and the relative standard deviation of the net Cd intensity from three readings should not exceed 3.0%. If it exceeds this range, first dilute or clean the injection system and retest the same solution; do not rely solely on ratio correction to continue issuing results.

[0054] The deviation of the Si / Cd ratio of the intermediate verification solution from the initial value must not exceed 2.0%, and the deviation of the Ge / Cd ratio must not exceed 1.5%. If the limit is exceeded for the first time, the verification solution should be remeasured; if the limit is still exceeded after remeasurement, all subsequent samples should be remeasured after recalibration, using the last qualified verification solution as the cutoff. There should be no Ge blank at the end of the batch measurement, and the residual Si and Ge should not exceed 20% of the response of the lowest non-zero calibration point and 0.2% of the response of Ge addition, respectively. If only the residual Si exceeds the limit, extend the rinsing process and check for silicate deposition; if Si, Ge, and Cd all show memory effects, check the nebulizer drain and pump backflow. The above drift handling only changes the measurement sequence and does not alter the completed Ge pretreatment information.

[0055] The intensity of the original integral over element e is denoted as The background intensity obtained by fitting adjacent background points is denoted as . The corresponding net strength is: (a) In the formula, Take Si, Ge, or Cd respectively. The unit is cps. The net intensity of the Ge reagent-free blank was calculated in the same manner and processed in the intercept of the ratio fit.

[0056] In step S5, the ratio is calculated for each parallel read: (b).

[0057] When atomization efficiency, pump speed, or plasma load causes the three spectral lines to change in approximately the same proportion over a short period of time, the common multiplicative change in equation (b) is eliminated. (Calculate 3 times respectively.) and The average value; if the relative standard deviation of any ratio is greater than 1.5%, check for transient bubbles, salting out or integration anomalies, discard the readings. There must be an identifiable instrument event record, and at least 3 valid readings must be retained, otherwise re-inject.

[0058] The Si matrix matching calibration relationship is expressed as follows: (c) In the formula, The slope of the Si / Cd response is expressed in L / mg. The intercept of the curve; The final Si concentration in the test solution is expressed in mg / L. The Si concentration of the sample before pretreatment and recovery correction is: (d).

[0059] If the Si concentration in the sample exceeds 250 mg / L, take a quantitative volume of the test solution and dilute it with the same batch of blank matrix, then add Cd to the diluent to maintain a concentration of 1.000 mg / L; the dilution factor is recorded as follows: Do not dilute with water alone, as this may alter the Na and acid matrix and create new differences in atomization.

[0060] The theoretical mass concentration ratio of Ge / Cd is denoted as... Within this scope of implementation , Therefore The response factor was obtained by adding 100% recovered reference material to Ge. (2) In the formula, The average Ge / Cd ratio after adding a reference is given to Ge. This represents the ratio corresponding to the blank without Ge.

[0061] Preliminary screening of natural Ge in the cement to be tested: For each new cement variety or raw material system, at least one representative test solution without Ge but with the other steps identical was prepared, and the equivalent concentration of natural Ge obtained was recorded as follows. When it is less than When the concentration is 0.5%, it should be treated as 0 in regular batches; when it is 0.5% to 5.0%, one parallel sample without Ge should be retained in each batch of the same variety and deducted; when it exceeds 5.0%, the Ge addition level is not applicable, the amount of Ge added should be increased and the spectral linearity should be re-verified, or another pretreatment tracer element that has been verified and has no significant overlap with the Si and Ge spectral lines should be used instead.

[0062] The pretreatment recovery rate after deducting natural Ge was: (1) In the formula, The measured Ge / Cd ratio of the sample; The recovery rate of Ge after pretreatment is dimensionless.

[0063] Process blank The value should be between 0.985 and 1.015 to demonstrate that the batch of reagents and glassware did not cause systematic Ge loss; the process blank was qualified and the sample... The low value indicates that the loss is related to sample melting or sample transfer. Equation (1) uses the Cd normalized ratio, so a simple decrease in atomization efficiency will not be misjudged as a Ge pretreatment loss.

[0064] For the first A certified standard sample measurement unit is used to first calculate the uncorrected SiO2 result using equation (d) and the sample weight. Then use the certificate value The apparent recovery rate of Si was obtained as follows: (e) Define Ge recycling loss Si recycling losses In a lossless state, both should approach 0; therefore, a weighted relationship passing through the origin is used, instead of setting a free constant that can mask the fixed system deviation into the intercept. (f) In the formula, The conversion factor for converting Ge recycling losses to Si recycling losses; These are the residuals not explained by the model. Weights are determined based on the certificate uncertainty and repeated measures variance for each standard sample. The conversion factor is obtained by the following formula: (4).

[0065] The modeling data should have at least 12 measurement units that satisfy 0.94 ≤ ≤1.02, and derived from no fewer than 3 certified standard samples. The model coefficient of determination is not less than 0.90; the relative deviation of SiO2 after correction for independently retained standard samples does not exceed 0.8%; the values ​​calculated separately for different matrices... When the relative difference does not exceed 10%, a unified coefficient can be used; otherwise, separate models should be created for silicate cement, slag cement, or pozzolanic cement. After changing the Ge tracer morphology, NaOH batch type, crucible material, main acidification volume, or ICP-OES injection structure, at least two certified standard samples must be used for reconfirmation. Historical coefficients cannot be used.

[0066] To avoid overestimating apparent performance due to simultaneous use of the same batch of perturbation samples in fitting and validation, cross-validation was performed using "standard sample type" as the grouping unit during modeling. That is, all data for one type of standard sample were reserved each time, and only the data from the other standard samples were used to obtain the results. Then predict and reserve samples. Results from each round... A unified model can only be established if the relative standard deviation of the samples does not exceed 8% and the average relative deviation of the retained samples does not exceed 0.8%. After the model is activated, if the corrected results of independent monitoring samples exceed the combined range of the certificate value and its expanded uncertainty for two consecutive batches, or if there are three instances of exceeding the limit in the same direction among 20 batches, the model should be suspended and revalidated. Before revalidation, results without Ge conversion can be reported according to current standard methods, but expired historical data must not be used. Continue to provide compensation.

[0067] The predicted Si pretreatment recovery rate of the sample to be tested is: (5), The formula only reflects the loss magnitude of the chemical process represented by Ge; the difference between Si and Ge is determined by actual measurements. absorb.

[0068] like This indicates that the same Ge recovery loss corresponds to a larger Si loss, consistent with the situation where Si is more susceptible to the effects of unmelted particles or acid polymerization in some cement matrices; if a specific matrix obtains The value should be based on the verified data and should not be arbitrarily fixed at 1.

[0069] Under normal operating conditions, prepare no fewer than 60 certified standard samples or stable quality control samples continuously, and calculate... mean and laboratory standard deviation The low-side failure threshold of Ge is determined by the following formula: (3), In the formula, The minimum Ge recovery rate allowed for conversion correction is set at 0.950 to prevent a laboratory from obtaining an excessively low threshold due to excessive fluctuations in the historical process itself. When there are fewer than 60 normal data sets, 0.970 is temporarily used; once the accumulated data reaches the required level, it is confirmed according to equation (3). The high-side action limit is set to... It is used to identify repeated addition of Ge, failure to subtract natural Ge, insufficient volume determination, or positive interference in the spectral lines.

[0070] Only when Calculations are only permitted when the process blank is satisfactory, the Cd response coefficient is between 0.80 and 1.20, and there are no instances of manual rejection of the test solution. .like Regardless of whether the total amount of oxides is closed, the melting or transfer of this sample is deemed invalid and compensation using formula (5) is not applied; if the original sample is still below the threshold after retesting, the sample is weighed and melted again. First, check the Ge sample addition record, the natural Ge blank, and the volumetric flask liquid level. The recovery rate cannot be cut off to 1.000 for further calculation. If obtained according to formula (5)... If the value is not within the range of 0.960 to 1.030, it indicates that the required correction exceeds the range of minor deviations in the validated model, and the preprocessing is also deemed invalid. This triple boundary prevents the mathematical model from transforming from a quality control tool into a tool for masking serious operational errors.

[0071] Judgment is performed in a fixed sequence at the individual sample level. First, check for spillage, visible residue, silica gel, and transfer records; stop calculations immediately upon any manual rejection event. Next, check the Cd response coefficient and stability across three readings; if unsatisfactory, simply retest the original solution. Then, check the process blank and Ge reference after adding it; suspend the entire batch if batch control fails. Finally, calculate the sample... and , The comparison is performed first; only then are the Si recovery conversion and SiO2 results calculated. The software should retain the original intensity, background, ratio, decision code, and operator for each step, and operators should not be allowed to directly enter "qualified" to override the automatic threshold. New samples are prepared using new sample sub-numbers; the original failure data is retained but not included in the averaging. This ensures that the same data is treated consistently across different personnel and batches.

[0072] Let the final test liquid volume be The unit is L; the sample size is The unit is g; the dilution factor is The molar masses of Si and SiO2 are respectively and The mass fraction of SiO2 without Ge conversion correction is: (6), In the formula, The unit is %. When correction is allowed, the final result is: (7).

[0073] Two parallel samples should be independently weighed for the same sample, and Ge should be added before melting, and Cd should be added after melting, respectively. The average value should be taken if both samples meet the quality control conditions. If one sample fails due to Ge falling below the threshold, that sample must be re-prepared; the other sample should not be reported separately. The absolute difference between the parallel results should meet the repeatability requirements of the adopted cement chemical analysis standard for ICP-OES determination of SiO2; if the standard does not cover specific cement types, the absolute difference should not exceed 0.20 percentage points. The reported results should also retain [the relevant data]. Cd response coefficient, used The version and whether a retest occurred are recorded, but only the SiO2 mass fraction obtained through the permitted process is reported externally. The value calculated from the failed test solution is not used as a reference result.

[0074] When the sample weight or final volume deviates from the nominal value but there is still a traceable measured value, equation (6) uses the actual value. and Compensation cannot be derived by retroactively adjusting the theoretical concentrations of Ge or Cd. If the volumetric flask temperature exceeds 20–25°C, leaks, or the amount of Ge or Cd added cannot be traced, the sample must be re-prepared. The uncertainty of the results must include at least the costs of sample weighing, volumetric flask adjustment, Si / Cd calibration, and parallel repeatability. and Six components; samples below the threshold have no reportable correction results, and "threshold rejection" cannot be converted into an increased uncertainty and reported again. For new types of cement, extremely high SiO2 cement, or samples containing special industrial by-products, first verify that their Si concentration falls into the curve, that natural Ge meets the conditions, and that the deviation of the independent monitoring sample is qualified, before including them in the routine range.

[0075] In addition, step S4 also includes the following steps: acquiring net intensity data of Cd and Ge / Cd intensity ratio data; comparing the net intensity data of Cd with a preset normal range and comparing the Ge / Cd intensity ratio data with a preset threshold; generating judgment information based on the comparison results, that is, when the net intensity data of Cd is abnormal but the Ge / Cd intensity ratio data is normal, generating first judgment information to indicate an abnormality in sample injection or plasma and triggering a retest command for the original sample solution; when the net intensity data of Cd is normal but the Ge / Cd intensity ratio data is low, generating second judgment information to indicate an abnormality in melting, leaching or transfer and triggering a resample preparation command; when both the net intensity data of Cd and the Ge / Cd intensity ratio data are abnormal, generating third judgment information to trigger a retest command for the original sample solution; if the net intensity data of Cd recovers after retesting but the Ge / Cd intensity ratio data is still low, updating the third judgment information to indicate a pretreatment failure and triggering a resample preparation command; if both recover after retesting, updating the third judgment information to indicate an instantaneous measurement failure.

[0076] Specifically, when the absolute Cd strength decreases by more than 20%, while the Si / Cd and Ge / Cd ratios remain stable during repeated readings, the main problem lies with the peristaltic pump, sample capillary, nebulizer, torch, or plasma load. Retain the original sample solution, clean or replace the pump tubing, and retest. If the retest passes, the sample can be used without remelting. When the absolute Cd strength is acceptable and the Ge / Cd ratio is below [value missing], [further issues arise]. If the measurement chain is normal after Cd is added, the abnormality occurs in the stage where Ge has already participated but Cd has not yet been added. The sample should be weighed again directly. Combining the melt appearance, leaching residue and washing records, it can be further determined whether it is melting, leaching or transfer.

[0077] When both Cd intensity and Ge / Cd are abnormal, first retest the original test solution; if Cd recovers but Ge / Cd remains low, proceed to the pretreatment failure path; if both recover simultaneously, classify it as an instantaneous measurement failure. When Ge / Cd is acceptable but the SiO2 deviation of the certified standard sample exceeds the limit, check the Si spectral background, Si calibration solution, and... The matrix suitability is not replaced by the above-mentioned checks without checking the total amount of oxides.

[0078] When the total oxide quantity is not closed but the Cd and Ge indicators of this method are both qualified, it indicates that the Si measurement chain and pretreatment chain do not show any abnormalities. Priority should be given to checking the weighing, ignition, spectral lines, or valence state conversion of other oxides. When the total oxide quantity is closed but the Ge indicator is unqualified, the Ge failure criterion should still be used, because the positive deviations of other components may cancel each other out with the negative deviations of Si. Therefore, oxide closure is retained as an overall verification indicator, but it no longer serves the purpose of locating the pretreatment and measurement stages. Each criterion is independently recorded.

[0079] If, within the same batch of parallel samples, one sample shows acceptable Ge yield while another shows Ge yield below the threshold, the two Si results should not be averaged, nor should the Ge recovery rate of the acceptable sample be used to replace the failure sample. The backup sample should be resampled from the original laboratory sample and placed in a different furnace position, completed using a separate, cleaned crucible. If the backup sample still shows low recovery, check whether the sample contains refractory mixtures, whether the furnace temperature is actually reached, and whether the Ge tracer is added uniformly. Only proceed after confirming the applicability of the method. This approach separates accidental operational losses from sample matrix deviations from the model range, avoiding repeated melting under the same conditions that could lead to multiple unexplained results.

[0080] Furthermore, the Ge tracer can be GeO2, a Ge(IV) compound that quantitatively forms soluble germanates upon melting, or a soluble germanate. However, it must meet the following requirements: the natural content of cement is sufficiently low relative to the added amount; it does not undergo significant volatilization at 650–700°C; it does not produce uncontrollable precipitation at the acidity of this method; and it can establish a stable Ge-Si recovery conversion relationship. The Cd measurement internal standard can also be replaced by other elements, but the substitute element must be added after pretreatment. Its spectral lines should not significantly overlap with Si, Ge, and high-content elements in cement; its natural content in the sample should not exceed 0.5% of the added amount; and it should have similar nebulization and short-term response changes as Si at the acidity and salt load used. Any substitution must not change the temporal relationship of "adding tracer before pretreatment, adding measurement internal standard after pretreatment, using the internal standard after pretreatment to calibrate the measurement, using the tracer before pretreatment to evaluate chemical recovery, and directly discarding if below the threshold."

[0081] A second aspect of the present invention provides a system for determining the silica content in cement, comprising: The sample pretreatment module is used to add a predetermined amount of Ge tracer to the cement sample at a first time point, collect sample information containing Ge tracer, perform alkali fusion treatment, leaching treatment and acid treatment on the sample containing Ge tracer, and transfer the resulting test solution to a volumetric flask; and inject a predetermined amount of Cd internal standard into the volumetric flask at a second time point and make up the volume of the test solution to obtain the test solution. The spectral measurement module is used to measure the spectral intensities of Si, Ge and Cd in the test solution using inductively coupled plasma atomic emission spectrometry. After background correction, the net intensity data of Si, Ge and Cd are obtained respectively. The data processing module is used to calculate the Ge / Cd intensity ratio based on the net Ge intensity data and the net Cd intensity data, and to determine the Ge pretreatment recovery rate based on the Ge / Cd intensity ratio data. and the Ge pretreatment recovery rate Compare with a preset threshold; The calibration calculation module is used to calculate the Ge pretreatment recovery rate. When within the preset threshold range, based on the Ge pretreatment recovery rate The silicon content data obtained from the net strength data of Si is corrected, and the corrected silicon dioxide content data is calculated. The determination output module is used when the... When the sample content is below the preset threshold, a determination message indicating invalid sample pretreatment is generated, the correction calculation of the silicon content data is prohibited, and a prompt message indicating that the sample should be prepared again is output. Wherein, the first time point is the time point before the sample undergoes alkali fusion treatment, and the second time point is the time point after the test solution is transferred to the volumetric flask and before the test solution is brought to volume.

[0082] To make the embodiments of the present invention easier to understand, the present invention will be described in detail below with reference to the embodiments. These embodiments are for illustrative purposes only and are not limited to the application scope of the present invention.

[0083] Unless otherwise specified, the specific operations and processing methods or conditions not described in the following embodiments are conventional methods in the art or are performed in accordance with the techniques or conditions described in the literature in the art or in accordance with the product manual.

[0084] Unless otherwise specified, all reagents or instruments used in the following examples that do not specify the manufacturer are commercially available products and conventional instruments in the field.

[0085] In the following examples, unless otherwise specified, all percentages are weight percentages.

[0086] None of the chemicals underwent secondary purification.

[0087] Example 1 This embodiment refers to the sample preparation, NaOH fusion, and ICP-OES determination requirements in GB / T 176—2025 "Chemical Analysis Methods for Cement"; the analytical water is in accordance with GB / T 6682—2008 "Specifications and Test Methods for Water Used in Analytical Laboratories"; the method validation is performed according to GB / T 27417—2017 "Guidelines for Conformity Assessment of Chemical Analysis Methods"; the design and calculation of repeatability data are in accordance with GB / T 6379.2—2004 "Accuracy (Correctness and Precision) of Measurement Methods and Results - Part 2: Basic Methods for Determining the Repeatability and Reproducibility of Standard Measurement Methods"; and the rounding of results is in accordance with GB / T 8170—2008 "Rules for Rounding Off Numerical Values ​​and Expression and Judgment of Limiting Values".

[0088] The experimental procedure established by this method includes dual-time-point recovery discrimination, Ge-Si conversion coefficient, and failure threshold. The specific steps are as follows.

[0089] Axial observation ICP-OES was used, equipped with a high-salt-resistant concentric nebulizer, a swirling nebulization chamber, and a 1.2 mm center tube. The RF power was set to 1.30 kW, plasma gas flow rate to 12 L / min, auxiliary gas flow rate to 1.0 L / min, nebulizing gas flow rate to 0.70 L / min, rise rate to 1.0 mL / min, settling time to 30 s, single integration time to 5 s, and three reads per sample. The main analytical lines were Si I 251.611 nm, Ge I 209.426 nm, and Cd II 214.438 nm, and the confirmation lines were Si I 288.158 nm, Ge I 265.118 nm, and Cd II 226.502 nm. Weigh 0.4000 g of the sample, add 0.500 mL of sodium germanate working solution (calculated as Ge) at 1000 mg / L and evaporate to dryness at 108℃. Add 5.00 g of NaOH and melt at 675℃ for 20 min. Immerse with 100 mL of boiling water, add 27.5 mL of concentrated HCl while stirring, boil gently for 1 min, wash as required and transfer to a 250 mL volumetric flask. After cooling, add 2.500 mL of Cd working solution at 100.0 mg / L, make up to volume and mix well.

[0090] Three certified cement standard samples, A, B, and C, were selected, with SiO2 certified values ​​of 21.62%, 27.84%, and 34.96%, respectively, covering ordinary Portland cement, slag-containing cement, and pozzolanic cement. Normal conditions and slight perturbations in melting time, temperature, and washing amount were set for each sample, resulting in 54 effective modeling units with Ge recovery ranging from 0.944 to 1.018. The results were obtained by weighted fitting using equation (4). The 95% confidence interval is 1.02–1.14, and the coefficient of determination is 0.963. Among the 12 units reserved for verification, the relative deviation range of SiO2 after dual-time-point correction is... The concentration ranged from 0.42% to 0.47%, with no observed increase in concentration with increasing SiO2 content. This was calculated from subsequent 60 quality control data points under normal conditions. , Therefore, equation (3) yields a low-side failure threshold of 0.968 and a high-side action limit of 1.030.

[0091] The Si calibration range is 0–250 mg / L. The coefficient of determination for the 7-point curve over 5 consecutive working days is no less than 0.9998, and the back-calculated deviation at each point is... 1.1–1.3%. The intra-day relative standard deviation of the Ge / Cd ratio after adding Ge to the reference was 0.46%, and the intra-day relative standard deviation of the absolute strength of Cd was 1.8%. In the representative test solutions of 20 different cement sources without Ge, the equivalent concentration of natural Ge was 0.0006–0.0062 mg / L, which is only 0.03–0.31% of the 2.000 mg / L addition, and can be ignored in conventional batches according to this method; for unknown samples containing industrial by-products of Ge as blending materials, screening without Ge should still be performed first according to the technical plan.

[0092] Six samples each of standard samples A, B, and C were independently measured under normal conditions. When only Cd correction was used without Ge conversion, the average results for the three samples were 21.48%, 27.66%, and 34.69%, with relative standard deviations of 0.62%, 0.71%, and 0.78%, respectively. After Ge conversion, the average results were 21.61%, 27.82%, and 34.93%, with relative standard deviations of 0.29%, 0.33%, and 0.36%, respectively. The relative deviations corresponding to the certificate values ​​are... 0.65%, 0.65% and Narrowed to 0.77% 0.05%, 0.07% and 0.09%. The relative differences in SiO2 results obtained from the main Si spectrum and the confirmed Si spectrum of the three samples were all less than 0.45%, and the absolute differences in recovery rates obtained from the main Ge spectrum and the confirmed Ge spectrum were all less than 0.009.

[0093] Example 2 To verify the separation capability during the measurement phase, the peristaltic pump speed was reduced by approximately 15% during continuous sample injection, resulting in a decrease in the absolute net intensities of Si, Ge, and Cd of 16.8%, 17.2%, and 17.0%, respectively. Without an internal standard, the SiO2 content of standard sample A decreased from 21.60% to 17.97%; after applying the Si / Cd ratio, it became 21.65%, and the calculated Ge / Cd content... The value changed from 0.994 to 0.992, still within the normal range. The Cd response coefficient dropped to 0.830, triggering a check during the measurement phase, but it was not misjudged as a pretreatment loss. After restoring the pump speed and re-injecting the sample, the Cd response coefficient was 0.998, and the SiO2 result was 21.62%, indicating that the original sample solution could be retained for retesting, avoiding unnecessary remelting.

[0094] Example 3 To verify the rejection capability of low recovery in pretreatment, the melting time of standard sample A was shortened from 20 min to 16 min, and the mid-process shaking was omitted. Only a small amount of discontinuous melt area was visible to the naked eye. The Cd response coefficient of this sample was 1.006, indicating that the measurement stage was normal. The value is 0.952, which is below the 0.968 threshold. The unconverted result after Cd correction is 20.53%. According to this method, this sample is directly rejected, and no correction value is calculated. The sample is re-weighed and melted for 20 minutes. The result was 0.995, and the SiO2 result was 21.64%. This avoids forcibly restoring the relatively low deviation of about 5% caused by obvious incomplete melting to an appearance-normal reported value.

[0095] Example 4 Furthermore, reducing the beaker washing during the transfer of standard sample B from four times to one time resulted in a Cd response coefficient of 0.987. The value was 0.943, and the uncorrected SiO2 result was 26.43%, which was also judged as invalid pretreatment. In a group of slightly disturbed samples where the transfer was maintained intact but the melting temperature was set to 660 ℃ and the time to 18 min, The value is 0.976, which is within the allowable modeling range; from equation (5), we get... The original result after Cd correction is 27.12%, and Equation (1) yields 27.84%, which is consistent with the certificate value. The former case is rejected because it crosses the threshold, while the latter case is converted because it falls within the slight loss range covered by the certified standard sample, which shows that failure judgment and numerical correction are not the same process.

[0096] Example 5 In the acidification failure test, concentrated HCl was slowly added in 5 portions, with a 60-second interval between each addition, to allow localized polymerization of silicic acid, resulting in a slight turbidity in the test solution; the measured... The value was 0.965, close to but below the threshold, and also failed the artificial appearance criterion; therefore, this sample was rejected. After adding HCl in 27.5 mL at a time and stirring immediately, the solution became clear. The value was 0.991, and the relative deviation between the SiO2 result and the certificate value was 0.14%. This result indicates that the Ge threshold is consistent with the direction of the observable acidification anomaly, while retaining the artificial rejection condition can cover the boundary cases where the chemical behavior of Ge and Si is not completely equivalent.

[0097] Example 6 Ten independent samples were weighed from a batch of ordinary Portland cement production. The average SiO2 concentration using the two-time-point method was 21.37%, with a standard deviation of 0.064 percentage points and a relative standard deviation of 0.30%. For the same batch of samples, the average SiO2 concentration was 21.08% using the external standard method without an internal standard, with a standard deviation of 0.214 percentage points and a relative standard deviation of 1.02%. When only the internal standard Cd was used before volume adjustment, the average SiO2 concentration was 21.25%, with a standard deviation of 0.132 percentage points and a relative standard deviation of 0.62%. The result was verified using the SiO2 benchmark method in current cement chemical analysis methods, yielding 21.40%. The difference between the two-time-point method and the benchmark method is significant. 0.03 percentage points. Based on sample weighing, volume determination, Si calibration, Ge / Cd recovery, conversion factor, and repeatability component synthesis, the expanded uncertainty for the 21%–22% SiO2 level is 0.18 percentage points, with a coverage factor of [missing information]. .

[0098] Example 7 When continuously measuring 80 test solutions, an intermediate check solution was inserted every 10 solutions. Without ratio correction, the absolute response of Si decreased by 3.6% from the start to the end of the batch, and the absolute response of Cd decreased by 3.4%; the Si / Cd check ratio changed by 0.23%, and the Ge / Cd ratio changed by 0.31% after adding the reference. Three of the 80 solutions were first-time samples. The values ​​were 0.961, 0.955, and 0.946, respectively, traced back to missed melting and shaking, crucible lid splashing, and two insufficient beaker washes, all of which were identified and resampled before reporting. Two other samples were retested after cleaning the atomizer because the Cd response coefficient was below 0.80; retesting did not require remelting. If only the total oxide content is observed, two of the aforementioned three samples remain within the commonly used closed range, indicating that the dual-timepoint index can detect directional Si losses that the total content closure could not reveal.

[0099] Therefore, this invention, while retaining the existing NaOH melting and ICP-OES main conditions, only adds one quantitative addition of Ge before melting and one quantitative addition of Cd before volume adjustment, along with corresponding ratio calculations, thus forming two monitoring chains with clearly defined time boundaries. Its effectiveness does not depend on assuming Ge as a complete isotope of Si, but is achieved through certified standard samples. Furthermore, the model's usability range is limited; measurement fluctuations are absorbed instantly by Cd, minor pretreatment defects are empirically converted by Ge, and severe pretreatment defects are blocked by a threshold. This reduces misjudgments caused by reliance on multi-element total closure and a single total correction coefficient, and provides directly executable criteria for the three treatment pathways of re-injection, re-sample preparation, and inspection of other oxides.

[0100] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.

Claims

1. A method for determining the silica content in cement, characterized in that, Includes the following steps: S1. Obtain a cement sample and add a predetermined amount of Ge tracer to the cement sample at a first time point, and collect sample information containing the Ge tracer. S2. The cement sample containing the Ge tracer is subjected to alkali fusion treatment, leaching treatment and acid treatment, and the resulting test solution is transferred to a volumetric flask; S3. At the second time point, inject a predetermined amount of Cd internal standard into the volumetric flask and make up to volume to obtain the test solution; S4. The spectral intensities of Si, Ge, and Cd in the test solution were determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). After background correction, the net intensities of Si, Ge, and Cd were obtained, respectively. S5. Based on the net strength data of Ge and the net strength data of Cd, calculate the Ge pretreatment recovery rate using the internal standard method. And the obtained Ge pretreatment recovery rate Compare with a preset threshold range. Wherein, when the Ge pretreatment recovery rate When within the preset threshold range, based on the Ge pretreatment recovery rate The silicon content data obtained from the net strength data of Si is corrected to calculate the silica content in the cement sample; and, when the Ge pretreatment recovery rate... If the sample content exceeds the preset threshold range, an invalid sample pretreatment determination message is generated, the correction calculation of the silicon content data is prohibited, and a prompt message for re-sample preparation is output. The first time point is before the cement sample undergoes alkali fusion treatment, and the second time point is after the test solution is transferred to a volumetric flask and before the test solution is brought to volume.

2. The method according to claim 1, characterized in that, The amount of Ge tracer added is 2.000 mg / L based on the theoretical Ge concentration in the final diluted solution, and the amount of Cd internal standard added is 1.000 mg / L based on the theoretical Cd concentration in the final diluted solution. The recovery rate of Ge pretreatment is... It was determined by performing conventional subtraction calculations on the Ge / Cd ratio of the sample, the Ge / Cd ratio of the blank sample, and the natural Ge background.

3. The method according to claim 2, characterized in that, The Ge pretreatment recovery rate Determine according to the following formula (1):  (1) in, The Ge / Cd strength ratio of the sample; This represents the blank corresponding ratio without Ge; ; The Ge / Cd theoretical mass concentration ratio is set to 2; It is the equivalent concentration of natural Ge; and Determined according to the following formula (2),  (2), in, The average Ge / Cd ratio after adding a reference is Ge.

4. The method according to claim 3, characterized in that, The preset threshold range is between the low-side failure threshold. With high side movement limit Between, wherein the high-side movement limit Set as And the low-side failure threshold Determine using the following formula (3):  (3) In the formula, To allow for the minimum Ge recovery rate required for conversion correction, The average recovery rate of Ge pretreatment for the standard sample and This represents the standard deviation within the laboratory. Wherein, when the Ge pretreatment recovery rate is at the low-side failure threshold With the aforementioned high side movement limit Correction is permitted when the Ge pretreatment recovery rate exceeds the low-side failure threshold. With the aforementioned high side movement limit When the range is within a certain range, invalid preprocessing information is generated.

5. The method according to claim 1, characterized in that, Based on the Ge pretreatment recovery rate Correcting the silicon content data obtained from the net Si strength data includes: fitting the Ge recovery loss data and Si recovery loss data of multiple standard samples using the least squares method to establish a conversion model and determine the conversion coefficient κ; and, based on the conversion model and the Ge pretreatment recovery rate of the samples... Calculate the predicted recovery rate of Si. and utilize predicted recovery rate Correct the silica content.

6. The method according to claim 5, characterized in that, The conversion coefficient κ is determined according to the following formula (4):  (4) in, The weighted data are determined based on the uncertainty and repeated measurement variance of each standard sample. For Ge recycling losses, 0.94≤ ≤1.02; and, The Si recovery loss is calculated based on the weight of the cement sample, and is the ratio of the uncorrected SiO2 result to the value of the standard sample.

7. The method according to claim 6, characterized in that, The predicted recovery rate of Si is determined according to the following formula (5). :  (5)。 8. The method according to claim 7, characterized in that, After obtaining the silicon content data from the net Si strength data, the uncorrected silicon dioxide mass fraction is calculated according to the following formula (6):  (6) in, This refers to the final volume of the test solution, in liters (L). This represents the weight of the cement sample, in grams. This refers to the dilution factor; Here is the molar mass of Si, expressed in g / mol. The molar mass of SiO2 is expressed in g / mol; and, The silicon concentration data obtained from the Si calibration curve without pretreatment recovery correction; When correction is allowed, the corrected silica mass fraction Calculate according to the following formula (7):  (7)。 9. The method according to claim 1, characterized in that, Step S4 also includes the following steps: Obtain the net intensity data of Cd and the intensity ratio data of Ge / Cd; The net intensity data of Cd is compared with a preset normal range, and the Ge / Cd intensity ratio data is compared with a preset threshold. Based on the comparison results, the following judgment information is generated: When the Cd net intensity data is abnormal but the Ge / Cd intensity ratio data is normal, a first judgment information is generated to indicate an abnormality in sample introduction or plasma and to trigger a retest command for the original sample solution; when the Cd net intensity data is normal but the Ge / Cd intensity ratio data is low, a second judgment information is generated to indicate an abnormality in melting, leaching, or transfer and to trigger a resample preparation command; when both the Cd net intensity data and the Ge / Cd intensity ratio data are abnormal, a third judgment information is generated to trigger a retest command for the original sample solution; if the Cd net intensity data recovers after retesting but the Ge / Cd intensity ratio data is still low, the third judgment information is updated to indicate a pretreatment failure and to trigger a resample preparation command; if both recover after retesting, the third judgment information is updated to indicate an instantaneous measurement failure.

10. A system for determining the silica content in cement, characterized in that, include: The sample pretreatment module is used to add a predetermined amount of Ge tracer to the cement sample at the first time point and collect sample information containing Ge tracer. The sample containing the Ge tracer was subjected to alkali fusion treatment, leaching treatment and acidification treatment, and the resulting test solution was transferred to a volumetric flask; And at the second time point, a predetermined amount of Cd internal standard was injected into the volumetric flask and the test solution was diluted to volume to obtain the test solution; The spectral measurement module is used to measure the spectral intensities of Si, Ge and Cd in the test solution using inductively coupled plasma atomic emission spectrometry. After background correction, the net intensity data of Si, Ge and Cd are obtained respectively. The data processing module is used to calculate the Ge / Cd intensity ratio based on the net Ge intensity data and the net Cd intensity data, and to determine the Ge pretreatment recovery rate based on the Ge / Cd intensity ratio data. and the Ge pretreatment recovery rate Compare with a preset threshold; The calibration calculation module is used to calculate the Ge pretreatment recovery rate. When within the preset threshold range, based on the Ge pretreatment recovery rate The silicon content data obtained from the net strength data of Si is corrected, and the corrected silicon dioxide content data is calculated. The determination output module is used when the... When the sample content is below the preset threshold, a determination message indicating invalid sample pretreatment is generated, the correction calculation of the silicon content data is prohibited, and a prompt message indicating that the sample should be prepared again is output. Wherein, the first time point is the time point before the sample undergoes alkali fusion treatment, and the second time point is the time point after the test solution is transferred to the volumetric flask and before the test solution is brought to volume.