Analyzing method and device of lithium ion battery, and electronic equipment

By performing initial tomographic scanning, cyclic charge-discharge testing, and accelerated calorimetry analysis on lithium-ion batteries, combined with multi-parameter monitoring, the problem of full-process risk analysis of foreign matter defects in lithium-ion batteries during manufacturing was solved, achieving accurate classification and high-accuracy detection of battery safety risks.

CN123136397APending Publication Date: 2026-11-20EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611451280.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, the safety performance threats to lithium-ion batteries caused by the introduction of foreign objects during the manufacturing process have not been effectively identified, and there is a lack of risk analysis for foreign object defect cells from the beginning of service to the end of their life, resulting in low accuracy of battery safety risk detection.

Method used

By performing initial tomography, cyclic charge-discharge testing, accelerated calorimetry, and secondary tomography on lithium-ion batteries, combined with multi-parameter monitoring, the service life of lithium-ion batteries with foreign matter defects is classified, and a graded assessment is performed based on characteristic parameters to identify latent defects and improve the accuracy of safety risk prediction.

Benefits of technology

It enables precise risk classification of lithium-ion batteries throughout their entire life cycle, significantly improving the accuracy of battery safety risk detection. It can identify latent defects that cannot be detected by static screening, ensuring battery safety and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123136397A_ABST
    Figure CN123136397A_ABST
Patent Text Reader

Abstract

The application provides an analysis method and device of a lithium ion battery and electronic equipment, and relates to the technical field of battery safety evaluation. The method comprises the following steps: performing initial tomography on a lithium ion battery cell that has been assembled; performing a cyclic charge-discharge test on the lithium ion battery cell with an implanted foreign object to obtain a charge-discharge test result; after a target cycle number is reached, performing secondary tomography on the lithium ion battery cell and performing a comparison and analysis of the scanning results to determine the morphology change characteristics of the foreign object position; performing an accelerated calorimetric analysis on the lithium ion battery cell to obtain the thermal runaway critical temperature and kinetic parameters of the lithium ion battery cell; dividing the service process of the foreign object type defect lithium ion battery cell; and based on the characteristic parameters of each service stage, grading the thermal runaway risk of the lithium ion battery cell. The technical problem of low battery safety risk detection accuracy caused by static screening analysis of battery defect identification in the related art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery safety assessment technology, and more specifically, to an analysis method and apparatus for lithium-ion batteries, as well as an electronic device. Background Technology

[0002] With the transformation of the global energy structure and the increasing awareness of environmental protection, the new energy vehicle industry has developed rapidly. Lithium-ion batteries (LIBs), as the core component of power battery packs in new energy vehicles, are directly related to the safety and reliability of public property and the sustainable development of the industry. Various defects can occur during the manufacturing process of lithium-ion batteries, mainly including electrode defects, separator defects, assembly process defects, liquid injection and encapsulation defects, and formation and aging defects. Among these, the introduction of foreign objects during the assembly process poses a significant threat to the safety performance of the battery cell. Foreign objects remaining inside the cell can easily puncture the separator, causing direct contact between the positive and negative electrodes, leading to internal short circuits, and subsequently thermal runaway, fire, or even explosion.

[0003] In related technologies, the analysis and detection of battery defects, including micropore defects in the outer packaging of pouch batteries, focus on retrospective analysis of post-manufacturing causes. They do not address the electrochemical performance evolution and thermal runaway risk analysis caused by foreign objects inside the cell during long-term service. Furthermore, the market share of prismatic / cylindrical steel / aluminum-cased batteries is currently higher, limiting applicability. Simultaneously, these technologies largely concentrate on static screening during the manufacturing stage or microscopic analysis at the material level, lacking comprehensive analysis of foreign object-defective cells throughout their entire service life, from initial use to the end of their lifespan. This makes it difficult to quantify the cumulative effect of foreign objects on battery safety risks at different cycle stages, potentially leading to low accuracy in battery safety risk detection. Summary of the Invention

[0004] The main objective of this invention is to provide an analysis method, apparatus, and electronic device for lithium-ion batteries, in order to solve the technical problem that static screening analysis during battery defect identification in related technologies can easily lead to low accuracy in detecting battery safety risks.

[0005] To achieve the above objectives, according to one aspect of the present invention, an analysis method for lithium-ion batteries is provided, comprising: performing an initial tomographic scan on an assembled lithium-ion cell to obtain initial cell scan results; performing a cyclic charge-discharge test on a lithium-ion cell with implanted foreign matter under a preset constant temperature environment to obtain charge-discharge test results; performing a secondary tomographic scan on the lithium-ion cell after reaching a target number of cycles, and comparing and analyzing the secondary cell scan results with the initial cell scan results to determine the morphological change characteristics of the foreign matter location; performing accelerated calorimetry analysis on the lithium-ion cell that has reached the target number of cycles to obtain the critical temperature and kinetic parameters of thermal runaway of the lithium-ion cell; based on the integrated charge-discharge test results, the morphological change characteristics of the foreign matter location, and the critical temperature and kinetic parameters of thermal runaway, classifying the service process of the lithium-ion cell with foreign matter defects, and classifying and assessing the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0006] Optionally, the step of performing an initial tomographic scan on the assembled lithium-ion cell to obtain the initial cell scan result includes: obtaining the positions of the positive and negative electrode plates and the separator of the cell structure to be assembled, and obtaining metal solder particles of a first preset size and positive or negative electrode fragments of a second preset size to be implanted; in the stacking process, implanting the metal solder particles and the positive or negative electrode fragments between adjacent electrode plates at a first preset position, or, in the winding process, implanting the metal solder particles and the positive or negative electrode fragments between spirally wound electrode plates at a second preset position; completing all cell assembly processes according to standard processes, and performing an initial tomographic scan on the packaged lithium-ion cell to obtain the initial cell scan result, wherein the initial cell scan result includes at least: the three-dimensional spatial position and morphological distribution of foreign matter.

[0007] Optionally, the steps of performing cyclic charge-discharge tests on a lithium-ion battery cell with an implanted foreign object under a preset constant temperature environment to obtain charge-discharge test results include: activating a constant temperature environment control device, a programmable charge-discharge device, a self-discharge tester, a DC internal resistance tester, and an electrochemical workstation; using the constant temperature environment control device to control the lithium-ion battery cell to be in a preset constant temperature environment; using the programmable charge-discharge device to charge the lithium-ion battery cell at 1.0C to 4.2V, then charging it at a constant current and constant voltage of 0.05C to the cutoff current of 0.05C, and discharging it at a constant current of 1C to 2.5V, completing one charge-discharge cycle; controlling the lithium-ion battery cell to complete a predetermined number of charge-discharge cycles; at the end of each predetermined number of cycles, using the self-discharge tester to perform a self-discharge rate measurement, using the DC internal resistance tester to perform a DC internal resistance measurement, and using the electrochemical workstation to perform an electrochemical impedance spectroscopy measurement, to obtain charge-discharge test results including self-discharge rate data, DC internal resistance change curves, and electrochemical impedance spectroscopy spectra.

[0008] Optionally, after reaching the target number of cycle cycles, a second tomographic scan is performed on the lithium-ion cell, and the results of the second cell scan are compared and analyzed with the initial cell scan results to determine the morphological change characteristics of the foreign matter location. This step includes: after reaching the target number of cycle cycles, performing a second tomographic scan on the lithium-ion cell to obtain a three-dimensional image containing the location, morphology, and electrode structure of the foreign matter inside the lithium-ion cell, thus obtaining the second cell scan result; comparing and analyzing the second cell scan result with the initial cell scan result to analyze the area where the foreign matter is located, the electrode surface around the foreign matter, the condition of the separator, and lithium deposits in the lithium-ion cell to determine the morphological change characteristics of the foreign matter location.

[0009] Optionally, the step of performing accelerated calorimetry analysis on lithium-ion cells that have reached the target number of cycles to obtain the critical temperature and kinetic parameters of thermal runaway of lithium-ion cells includes: calling an accelerated calorimeter, placing the lithium-ion cell in the vacuum chamber of the accelerated calorimeter, heating it at a preset heating rate, recording the self-generated heat initiation temperature, thermal runaway initiation temperature, pressure relief temperature, maximum temperature, time corresponding to each temperature, and the mass change between the cell mass before and after the test under adiabatic conditions, to obtain the critical temperature and kinetic parameters of thermal runaway of lithium-ion cells.

[0010] Optionally, the steps of dividing the service process of a lithium-ion cell with foreign matter defects and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage include: dividing the service process of the lithium-ion cell into multiple service stages according to the evolution trend of the cell voltage with the number of cycles, wherein the multiple service stages include: voltage stabilization stage, voltage jump stage, voltage difference stage, and cell swelling stage, and each service stage includes voltage characteristics, internal resistance characteristics, lithium plating characteristics, appearance characteristics, and thermal runaway risk level; and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0011] Optionally, the steps of dividing the service process of a lithium-ion cell with foreign object defects and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage include: dividing the service process of the lithium-ion cell into multiple service stages according to the trend of DC internal resistance change, wherein the multiple service stages include: a normal internal resistance stage, a slightly fluctuating but recoverable internal resistance stage, a slightly increased but unrecoverable internal resistance stage, and a significantly increased internal resistance stage; and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0012] Optionally, the steps of dividing the service process of a lithium-ion cell with foreign matter defects and classifying and assessing the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage include: dividing the service process of the lithium-ion cell into multiple service stages according to the changes in lithium plating characteristics, wherein the multiple service stages include: a stage with a small amount of lithium plating around the foreign matter, a stage with severe lithium plating on the negative electrode at the foreign matter, a stage with a foreign matter diffusion trend, and a stage with severe lithium plating on the electrode sheet around the foreign matter; and classifying and assessing the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0013] According to another aspect of the present invention, an analysis apparatus for a lithium-ion battery is provided, comprising: a foreign matter implantation unit for performing an initial tomographic scan on an assembled lithium-ion cell to obtain an initial cell scan result; a cycle charge-discharge unit for performing a cycle charge-discharge test on the lithium-ion cell with the implanted foreign matter under a preset constant temperature environment to obtain a charge-discharge test result; a cell foreign matter scan comparison and analysis unit for performing a secondary tomographic scan on the lithium-ion cell after reaching a target number of cycles, and comparing and analyzing the secondary cell scan result with the initial cell scan result to determine the morphological change characteristics of the foreign matter location; a thermal runaway analysis unit for performing accelerated calorimetry analysis on the lithium-ion cell after reaching the target number of cycles to obtain the critical thermal runaway temperature and kinetic parameters of the lithium-ion cell; and a grading and evaluation unit for classifying the service process of the lithium-ion cell with foreign matter defects based on the integrated charge-discharge test results, the morphological change characteristics of the foreign matter location, and the critical thermal runaway temperature and kinetic parameters, and classifying and evaluating the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0014] According to another aspect of the present invention, an electronic device is provided, comprising one or more processors and a memory, the memory being used to store one or more programs, wherein, when the one or more programs are executed by the one or more processors, the one or more processors cause the one or more processors to implement the analysis method for lithium-ion batteries as described in any of the preceding claims.

[0015] By applying the technical solution of this invention, a predetermined number of cyclic tests can be conducted under constant temperature conditions to simulate the actual working conditions of a battery from the early stage of service to the end of its life. By capturing the trend of parameter evolution over time (such as the slow increase in self-discharge rate and the staged jump in internal resistance), latent defects that cannot be detected by static screening can be identified, thereby significantly improving the accuracy of predicting later safety risks. Based on experimental data, the life cycle of foreign matter defective lithium-ion batteries is divided into multiple service stages, and the battery can be located to a specific risk stage, achieving accurate risk classification. Through long-cycle cyclic testing, multi-parameter joint monitoring, and multi-stage risk classification strategies, the detection accuracy of safety risks of foreign matter defective lithium-ion batteries is improved, thereby solving the technical problem in related technologies where static screening analysis during battery defect identification easily leads to low accuracy in battery safety risk detection. Attached Figure Description

[0016] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0017] Figure 1This is a flowchart of an optional analysis method for lithium-ion batteries according to an embodiment of the present invention;

[0018] Figure 2 This is a schematic diagram illustrating the implantation of foreign objects during the assembly of battery cells according to an embodiment of the present invention;

[0019] Figure 3 This is a schematic diagram illustrating an optional division of lithium-ion battery service stages according to an embodiment of the present invention; and

[0020] Figure 4 This is a schematic diagram of an analysis device for a lithium-ion battery according to the present invention. Detailed Implementation

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0023] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps set forth in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.

[0024] To facilitate understanding of the present invention by those skilled in the art, some terms or nouns involved in the various embodiments of the present invention are explained below:

[0025] Computed Tomography (CT) is a non-destructive testing technique used to observe the morphology and structural changes of foreign objects inside a battery cell.

[0026] Direct Current Resistance (DCR) is a parameter that reflects a battery's ability to impede current under DC load and is used to assess battery aging and failure status.

[0027] Electrochemical impedance spectroscopy (EIS) is an AC impedance measurement technique used to analyze the internal impedance composition and reaction mechanism of a battery.

[0028] An adiabatic accelerated calorimeter (ARC) is an electrothermal performance testing device used to measure thermal runaway characteristic parameters of batteries, such as the self-generated heat initiation temperature.

[0029] The self-heating onset temperature, the temperature at which a violent exothermic reaction begins to occur inside the battery, is a key indicator for assessing the risk of thermal runaway.

[0030] The solid electrolyte interphase (SEI) is a passivation film formed on the surface of the negative electrode. It has a significant impact on battery performance and lifespan. Foreign matter can cause it to form unevenly or break down.

[0031] The following embodiments of the present invention can be applied to lithium-ion battery manufacturing quality control, battery failure analysis, and new energy vehicle battery safety assessment scenarios. For example, defective cells in power battery production lines can be screened and graded, especially cells containing metallic foreign objects can be classified into risk levels to intercept potential safety hazards; or they can be applied to the remaining life and safety assessment of aftermarket or retired battery packs, by monitoring characteristic parameters such as voltage, internal resistance, and self-discharge to determine whether there is a risk of micro-short circuit or lithium plating inside the battery due to foreign objects.

[0032] Figure 1 This is a flowchart of an optional analysis method for a lithium-ion battery according to an embodiment of the present invention, such as... Figure 1 As shown, the analysis method for the lithium-ion battery includes the following steps S102 to S105. The present invention will be described in detail below with reference to each implementation step.

[0033] Step S101: Perform an initial tomographic scan on the assembled lithium-ion cell to obtain the initial cell scan results.

[0034] Optionally, the step of performing an initial tomographic scan on the assembled lithium-ion cell to obtain the initial cell scan results includes: obtaining the positions of the positive and negative electrode plates and the separator of the cell structure to be assembled, and obtaining metal solder particles of a first preset size and positive or negative electrode fragments of a second preset size to be implanted; in the stacking process, implanting the metal solder particles and positive or negative electrode fragments between adjacent electrode plates at a first preset position, or in the winding process, implanting the metal solder particles and positive or negative electrode fragments between spirally wound electrode plates at a second preset position; completing all cell assembly processes according to standard processes, and performing an initial tomographic scan on the packaged lithium-ion cell to obtain the initial cell scan results, wherein the initial cell scan results include at least: the three-dimensional spatial position and morphological distribution of foreign matter.

[0035] Specifically, when obtaining metal slag particles of a first preset size and positive or negative electrode fragments of a second preset size to be implanted, the first preset size can be Cu / Al slag particles with a diameter of 200-1000 μm, and the second preset size can be positive or negative electrode fragments with an area of ​​1.0-1.0-2.0 cm².

[0036] Specifically, the battery cell type implanted in this invention can include stacked cells or wound cells. In the stacking process, metal solder slag particles and positive or negative electrode fragments are implanted between adjacent electrodes at a first preset position, thereby forming controllable foreign object defects inside the cell. Alternatively, in the winding process, metal solder slag particles, positive or negative electrode fragments are implanted between spirally wound electrodes at a second preset position. All cell assembly processes are completed according to standard procedures, and an initial tomographic scan is performed on the packaged lithium-ion cell to obtain initial cell scan results. The initial cell scan results at least include the three-dimensional spatial location and morphological distribution of the foreign objects, which helps to establish baseline data for foreign object defects.

[0037] Then, by precisely controlling the size and location of the implanted foreign object, manufacturing defects of different sources and types can be simulated, which helps to improve the universality and specificity of subsequent defect analysis methods.

[0038] Step S102: Perform a cyclic charge-discharge test on the lithium-ion battery cell with the implanted foreign object under a preset constant temperature environment to obtain the charge-discharge test results.

[0039] Optionally, the steps of performing cyclic charge-discharge tests on a lithium-ion battery cell with an implanted foreign object under a preset constant temperature environment to obtain charge-discharge test results include: activating a constant temperature environment control device, a programmable charge-discharge device, a self-discharge tester, a DC internal resistance tester, and an electrochemical workstation; using the constant temperature environment control device to control the lithium-ion battery cell to be in a preset constant temperature environment; using the programmable charge-discharge device to charge the lithium-ion battery cell at 1.0C to 4.2V, then charging it at a constant current and constant voltage of 0.05C to the cutoff current of 0.05C, and discharging it at a constant current of 1C to 2.5V, completing one charge-discharge cycle; controlling the lithium-ion battery cell to complete a predetermined number of charge-discharge cycles; at the end of each predetermined number of cycles, using the self-discharge tester to perform a self-discharge rate measurement, using the DC internal resistance tester to perform a DC internal resistance measurement, and using the electrochemical workstation to perform an electrochemical impedance spectroscopy measurement, to obtain charge-discharge test results including self-discharge rate data, DC internal resistance change curves, and electrochemical impedance spectroscopy.

[0040] This embodiment simulates the performance evolution of a battery during its service life by conducting cyclic charge-discharge tests on a lithium-ion battery cell with implanted foreign objects under a preset constant temperature environment. Specifically, various devices can be used to control the lithium-ion battery cell to a preset constant temperature environment, such as 45°C, through a constant temperature environment control device. This helps accelerate the evolution of internal side reactions and defects in the battery, thereby observing characteristic changes that would only appear after long-term cycling in a shorter period of time. Using a programmable charge-discharge device to complete a predetermined number of charge-discharge cycles on the lithium-ion battery cell, such as 500 cycles, helps simulate the battery's full life cycle operating conditions from the beginning of its service life to the end of its life, fully revealing problems such as lithium plating and micro-short circuits caused by foreign object defects. At the end of each predetermined number of cycles, for example, every 50 cycles...

[0041] Self-discharge rate measurement was performed using a self-discharge tester, DC internal resistance measurement was performed using a DC internal resistance tester, and electrochemical impedance spectroscopy (EIS) measurement was performed using an electrochemical workstation. The resulting charge-discharge test results include self-discharge rate data, DC internal resistance variation curves, and EIS spectra. By periodically performing self-discharge, DC internal resistance, and EIS tests, the dynamic changes in the battery's internal state with increasing cycle count can be captured. Specifically, self-discharge rate data helps identify the presence of micro-short circuits or severe side reactions caused by foreign matter; the DC internal resistance variation curve helps reflect the evolution of the battery's overall impedance with aging or defect deterioration; and the EIS spectra help to analyze the specific compositional changes of ohmic impedance, charge transfer impedance, and diffusion impedance, thereby distinguishing performance degradation caused by different mechanisms.

[0042] Step S103: After reaching the target number of cycles, a second tomographic scan is performed on the lithium-ion cell, and the results of the second cell scan are compared and analyzed with the initial cell scan results to determine the morphological change characteristics of the foreign object location.

[0043] Optionally, after reaching the target number of cycle cycles, a second tomographic scan is performed on the lithium-ion cell, and the results of the second cell scan are compared and analyzed with the initial cell scan results to determine the morphological change characteristics of the foreign matter location. This step includes: after reaching the target number of cycle cycles, performing a second tomographic scan on the lithium-ion cell to obtain a three-dimensional image containing the location, morphology, and electrode structure of the foreign matter inside the lithium-ion cell, thus obtaining the second cell scan results; comparing and analyzing the second cell scan results with the initial cell scan results to analyze the area where the foreign matter is located in the lithium-ion cell, the electrode surface around the foreign matter, the condition of the separator damage, and lithium deposition, in order to determine the morphological change characteristics of the foreign matter location.

[0044] Specifically, after reaching the target number of cycling cycles, a secondary tomographic scan can be performed on the lithium-ion cell to obtain a three-dimensional image containing the location, morphology, and electrode structure of foreign matter inside the lithium-ion cell, thus obtaining the secondary cell scan results. This secondary tomographic scan utilizes computed tomography (CT) technology, which can non-destructively reveal the microstructural state of the cell after long-term cycling. Comparing the secondary cell scan results with the initial cell scan results allows for analysis of the region containing foreign matter, the electrode surface surrounding the foreign matter, the condition of the separator, and lithium deposits within the lithium-ion cell. This analysis determines the morphological changes in the location of the foreign matter, facilitating a direct observation of whether the foreign matter has shifted during cycling, whether it has punctured the separator, and whether localized lithium deposition or electrode deformation has occurred around the foreign matter. By comparing the initial state with the post-cycling state, the degree of physical damage caused by the foreign matter to the internal structure of the cell can be quantified.

[0045] Furthermore, analyzing the electrode surface surrounding the foreign object can identify whether severe lithium plating exists around it, revealing the structural characteristics of the battery's evolution from a stable voltage stage to a voltage jump stage or a voltage difference stage. Analyzing separator damage can determine whether the foreign object caused localized thinning or rupture of the separator, thus assessing the physical basis for internal short circuits. Analyzing lithium deposits allows observation of the process of lithium plating spreading from a small amount around the foreign object to severe lithium plating on multiple electrode plates, helping to categorize the cell's condition into specific risk rating stages.

[0046] Step S104: Perform accelerated calorimetry analysis on the lithium-ion battery cell that has reached the target number of cycles to obtain the key temperature and kinetic parameters of thermal runaway of the lithium-ion battery cell.

[0047] Optionally, the step of performing accelerated calorimetry analysis on lithium-ion cells that have reached the target number of cycles to obtain the critical temperature and kinetic parameters of thermal runaway of lithium-ion cells includes: calling an accelerated calorimeter, placing the lithium-ion cell in the vacuum chamber of the accelerated calorimeter, heating it at a preset heating rate, recording the self-generated heat initiation temperature, thermal runaway initiation temperature, pressure relief temperature, maximum temperature, time corresponding to each temperature, and the mass change between the cell mass before and after the test under adiabatic conditions, to obtain the critical temperature and kinetic parameters of thermal runaway of lithium-ion cells.

[0048] Accelerated calorimetry can simulate the exothermic behavior of internal chemical reactions in batteries under extreme thermal environments under adiabatic conditions. By recording the self-heating initiation temperature, thermal runaway initiation temperature, pressure relief temperature, maximum temperature, and corresponding time for each temperature of lithium-ion cells under adiabatic conditions, as well as the mass change between the cell mass before and after the test, the key thermal runaway temperature and kinetic parameters of lithium-ion cells can be obtained. This helps to quantify the thermal stability of foreign-defective batteries after cycle aging. By comparing the thermal parameters of normal cells and defective cells, the impact of increased side reactions or lithium plating caused by foreign matter on the battery thermal runaway threshold can be identified.

[0049] Among these parameters, a decrease in the self-generated heat initiation temperature (T0) helps reflect the activity level of early side reactions inside the battery (such as SEI film decomposition or electrolyte oxidation); changes in the thermal runaway initiation temperature (T1) help assess the ease with which the battery undergoes a violent exothermic reaction; and the pressure relief temperature (T2) helps determine the timing of the battery safety valve opening, reflecting the internal gas generation rate and pressure accumulation. Recording the time corresponding to each temperature helps analyze reaction kinetic characteristics, and the changes in mass before and after the test help assess the degree of electrolyte evaporation or gas release during the test. These parameters together constitute an important basis for assessing the risk of thermal runaway in the battery cell, helping to correlate the cell state with thermal safety performance, thereby assisting in determining the risk stage of the battery cell.

[0050] Step S105: Based on the integrated charge and discharge test results, the morphological change characteristics of the foreign object location, the key temperature and kinetic parameters of thermal runaway, the service process of the lithium-ion cell with foreign object defects is divided, and the thermal runaway risk of the lithium-ion cell is graded and assessed based on the characteristic parameters of each service stage.

[0051] Specifically, this study integrates charge-discharge test results such as self-discharge rate, DC internal resistance, and electrochemical impedance spectroscopy, combined with morphological changes such as lithium plating around foreign matter and separator state obtained from tomographic scanning, and thermal safety parameters such as self-heating initiation temperature and thermal runaway temperature obtained from accelerated calorimetry. By comparing the evolution of these thermal safety parameters during cycling, the service life of foreign matter-type defective lithium-ion cells is divided into four stages. This helps to establish a complete evolution map of defective batteries from the initial to the end stage, overcoming the limitations of single-parameter evaluation, and thus achieving dynamic monitoring of the battery's safety status throughout its entire life cycle.

[0052] By applying the technical solution of this invention, a predetermined number of cyclic tests can be conducted under constant temperature conditions to simulate the actual working conditions of a battery from the early stage of service to the end of its life. By capturing the trend of parameter evolution over time (such as the slow increase in self-discharge rate and the staged jump in internal resistance), latent defects that cannot be detected by static screening can be identified, thereby significantly improving the accuracy of predicting later safety risks. Based on experimental data, the life cycle of foreign matter defective lithium-ion batteries is divided into multiple service stages, and the battery can be located to a specific risk stage, achieving accurate risk classification. Through long-cycle cyclic testing, multi-parameter joint monitoring, and multi-stage risk classification strategies, the detection accuracy of safety risks of foreign matter defective lithium-ion batteries is improved, thereby solving the technical problem in related technologies where static screening analysis during battery defect identification easily leads to low accuracy in battery safety risk detection.

[0053] Optionally, the steps of dividing the service process of a lithium-ion cell with foreign matter defects and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage include: dividing the service process of the lithium-ion cell into multiple service stages according to the evolution trend of the cell voltage with the number of cycles, wherein the multiple service stages include: voltage stabilization stage, voltage jump stage, voltage difference stage, and cell swelling stage, and each service stage includes voltage characteristics, internal resistance characteristics, lithium plating characteristics, appearance characteristics, and thermal runaway risk level; and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0054] Optionally, the steps of dividing the service process of a lithium-ion cell with foreign object defects and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage include: dividing the service process of the lithium-ion cell into multiple service stages according to the trend of DC internal resistance change, wherein the multiple service stages include: normal internal resistance stage, slight internal resistance jump but recoverable stage, slight internal resistance increase but unrecoverable stage, and significant internal resistance increase stage; and classifying the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0055] Optionally, the steps of dividing the service process of a lithium-ion cell with foreign matter defects and classifying and assessing the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage include: dividing the service process of the lithium-ion cell into multiple service stages based on changes in lithium plating characteristics, wherein the multiple service stages include: a stage with a small amount of lithium plating around the foreign matter, a stage with severe lithium plating on the negative electrode at the foreign matter, a stage with a foreign matter diffusion trend, and a stage with severe lithium plating on the electrode sheet around the foreign matter; and classifying and assessing the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0056] In this embodiment, the stages can be divided into voltage stability stage, voltage jump stage, voltage difference stage, and cell swelling stage based on voltage performance; the stages can be divided into almost unchanged, slight swelling, and obvious swelling based on appearance changes; the stages can be divided into normal internal resistance, slight jump in internal resistance but recoverable, slight increase in internal resistance but unrecoverable, and obvious increase in internal resistance based on internal resistance changes; the stages can be divided into almost equal, slight decrease, and further decrease based on the change in self-generated heat initiation temperature T1; the stages can be divided into small amount of lithium plating around foreign matter, severe lithium plating on the negative electrode at the foreign matter, severe lithium plating on the negative electrode at the foreign matter with a tendency to spread to more locations, and severe lithium plating on several electrode sheets around the foreign matter based on the above characteristic combinations; based on the above characteristic combinations, the thermal runaway risk is divided into four levels: low, low-medium, medium-high, and high. Furthermore, during the voltage stability phase, the characteristics are almost no abnormal voltage, normal internal resistance, a small amount of lithium plating, and T1 is almost constant, with a low risk rating. During the voltage jump phase, the characteristics are slight voltage jumps that can be recovered, slight internal resistance jumps that can be recovered, severe lithium plating on the negative electrode at the foreign object, and a slight decrease in T1, with a low to medium risk rating. During the differential voltage phase, the characteristics are irrecoverable voltage jumps, a slight but irrecoverable increase in internal resistance, severe lithium plating on the negative electrode at the foreign object with a diffusion trend, and a further decrease in T1, with a medium to high risk rating. During the cell swelling phase, the characteristics are significant differential voltage, significantly increased internal resistance, severe lithium plating on several electrode plates around the foreign object, and significant cell swelling, with a high risk rating.

[0057] As can be seen from the above description, the above embodiments of the present invention achieve the following technical effects: a multi-dimensional feature correlation model based on voltage, internal resistance, self-discharge, CT morphology and thermal safety parameters (such as T1, T0) is established, which can improve the accuracy of identification and classification of thermal runaway risk of foreign-type defective batteries.

[0058] The present invention will now be described with reference to a specific embodiment.

[0059] The purpose of this invention is to provide a method for analyzing foreign-type defective lithium-ion cells using characteristic parameters, and to divide foreign-type defective lithium-ion cells into stages from the early stage of service to the end of their life.

[0060] Step 1: In the lamination process, Cu / Al welding slag particles with a diameter of 200-1000 μm and an area of ​​1.0 μm are... 1.0-1.0 A 2.0 cm² positive electrode sheet is implanted into the stacked battery cell, and then assembled into the battery cell according to the normal process and subjected to CT testing.

[0061] Figure 2 This is a schematic diagram illustrating the implantation of foreign objects during the assembly of battery cells according to an embodiment of the present invention, such as... Figure 2 As shown, during the cell stacking process on the assembly table, metal solder slag particles and positive / negative electrode plates can be implanted into the stacked cells.

[0062] Step 2: Charge the lithium-ion battery at 1.0-0.05C and 1C at 45℃ for 500 cycles. Perform self-discharge, DCR, and EIS tests every 50 cycles.

[0063] Step 3: Perform CT testing on the cycled battery cells, observe the morphology of the foreign object locations, and disassemble and analyze the battery cells.

[0064] Step 4: Perform ARC and other electro-thermal performance tests on the cycled cells.

[0065] The specific data in Table 1 below illustrates the thermal runaway data of lithium-ion cells with foreign object defects and normal cells.

[0066] Table 1

[0067]

[0068] Step 5: Based on the experimental test results, foreign body defect LIBs are divided into four stages from the beginning of service to the end of their life, and a risk rating is given for each stage.

[0069] Figure 3 This is a schematic diagram illustrating an optional division of lithium-ion battery service stages according to an embodiment of the present invention, such as... Figure 3 As shown, foreign object defect LIBs are divided into four stages from the beginning of service to the end of their life: voltage stabilization stage, voltage jump stage, voltage difference stage, and cell swelling stage.

[0070] Based on the above stage division, the risk of thermal runaway of lithium-ion cells under different stages is assessed. Among them, the risk of thermal runaway of lithium-ion cells under the voltage stability stage is assessed as low. During the cycle process, its behavior is no different from that of normal cells, and the appearance of the cells is also no different. Its cell characteristics are a small amount of lithium plating around foreign matter, fewer side reactions, unchanged internal resistance, no micro-short circuits, and almost no expansion.

[0071] The risk assessment of thermal runaway of lithium-ion cells during the voltage jump stage is low to medium. During the cycle, it is characterized by severe lithium plating around foreign matter, increased side reactions inside the cell, a slight decrease in the cell's self-generated heat temperature (T1), and micro-short circuits inside the cell that can be recovered, but the cell's internal resistance remains unchanged and it hardly expands.

[0072] The risk assessment of thermal runaway during the differential pressure stage is medium to high. During the cycle, it is characterized by severe lithium plating around foreign matter and a tendency to spread to more locations, continued increase of side reactions inside the cell, further decrease of T1, irreversible micro-shortage inside the cell, and increase in cell internal resistance and slight expansion.

[0073] The risk of thermal runaway during the cell swelling stage is assessed as high. During the cycle, it manifests as severe lithium plating on several electrode plates around the foreign matter, continued increase in internal side reactions of the cell, further decrease in T1, the possibility of internal short circuits in the cell at any time, and a sharp increase in the internal resistance of the cell, which is in an expansion state.

[0074] Figure 4 This is a schematic diagram of an analysis device for a lithium-ion battery according to the present invention, as shown below. Figure 4 As shown, the analysis device for the lithium-ion battery includes: a foreign object implantation unit 41, a cycle charge-discharge unit 42, a cell foreign object scanning and comparison analysis unit 43, a thermal runaway analysis unit 44, and a grading and evaluation unit 45.

[0075] Among them, the foreign body implantation unit 41 is used to perform an initial tomographic scan on the assembled lithium-ion battery cell to obtain the initial battery cell scan results.

[0076] The cyclic charge-discharge unit 42 is used to perform cyclic charge-discharge tests on lithium-ion cells with implanted foreign objects under a preset constant temperature environment to obtain charge-discharge test results.

[0077] The foreign object scanning and comparison analysis unit 43 is used to perform a secondary tomographic scan on the lithium-ion cell after reaching the target number of cycles, and compare and analyze the secondary cell scan results with the initial cell scan results to determine the morphological change characteristics of the foreign object location.

[0078] The thermal runaway analysis unit 44 is used to perform accelerated calorimetry analysis on lithium-ion cells that have reached the target number of cycles, and to obtain the key thermal runaway temperature and kinetic parameters of the lithium-ion cells.

[0079] The grading and assessment unit 45 is used to classify the service process of lithium-ion cells with foreign object defects based on integrated charge and discharge test results, morphological change characteristics of foreign object locations, key thermal runaway temperatures and kinetic parameters, and to classify and assess the thermal runaway risk of lithium-ion cells based on the characteristic parameters of each service stage.

[0080] Optionally, the foreign object implantation unit includes: a cell structure acquisition module, used to acquire the positions of the positive and negative electrode plates and the separator of the cell structure to be assembled, and to acquire metal solder slag particles of a first preset size and positive or negative electrode fragments of a second preset size to be implanted; a foreign object implantation module, used to implant the metal solder slag particles and positive or negative electrode fragments between adjacent electrode plates at a first preset position during the stacking process; and a scanning module, used to complete all cell assembly processes according to standard processes, and to perform an initial tomographic scan on the packaged lithium-ion cell to obtain an initial cell scan result, wherein the initial cell scan result includes at least the three-dimensional spatial position and morphological distribution of the foreign object.

[0081] Optionally, the cyclic charge-discharge unit includes: a device invocation module for invoking a constant temperature environment control device, a programmable charge-discharge device, a self-discharge tester, a DC internal resistance tester, and an electrochemical workstation; a constant temperature control module for controlling the lithium-ion cell to be in a preset constant temperature environment using the constant temperature environment control device; a charge-discharge control module for applying 1.0C to charge the lithium-ion cell to 4.2V using the programmable charge-discharge device, then charging it at a constant current and constant voltage of 0.05C to the cutoff current of 0.05C, and discharging it at a constant current of 1C to 2.5V, completing one charge-discharge cycle; a charge-discharge cycle control module for controlling the lithium-ion cell to complete a predetermined number of charge-discharge cycles; and a parameter measurement module for performing self-discharge rate measurement using the self-discharge tester, DC internal resistance measurement using the DC internal resistance tester, and electrochemical impedance spectroscopy measurement using the electrochemical workstation at the end of each predetermined number of cycles, to obtain charge-discharge test results including self-discharge rate data, DC internal resistance change curves, and electrochemical impedance spectroscopy spectra.

[0082] Optionally, the foreign matter scanning and comparison analysis unit for the battery cell includes: a secondary scanning module, used to perform a secondary tomographic scan on the lithium-ion battery cell after reaching the target number of cycles, to obtain a three-dimensional image containing the location, morphology, and electrode structure of foreign matter inside the lithium-ion battery cell, and to obtain the secondary battery cell scanning result; and a scanning result comparison and analysis module, used to compare and analyze the secondary battery cell scanning result with the initial battery cell scanning result, and to analyze the area where the foreign matter is located in the lithium-ion battery cell, the electrode surface around the foreign matter, the condition of the separator damage, and lithium deposition, so as to determine the morphological change characteristics of the foreign matter location.

[0083] Optionally, the thermal runaway analysis unit includes a calorimeter calling module, used to call an accelerated calorimeter, place the lithium-ion cell in the vacuum chamber of the accelerated calorimeter, perform heating treatment at a preset heating rate, record the self-generated heat initiation temperature, thermal runaway initiation temperature, pressure relief temperature, maximum temperature, corresponding time for each temperature, and mass change value between the cell mass before and after the test under adiabatic conditions, and obtain the key thermal runaway temperature and kinetic parameters of the lithium-ion cell.

[0084] Optionally, the grading and evaluation unit includes: a first division module, used to divide the service process of the lithium-ion cell into multiple service stages based on the evolution trend of the cell voltage with the number of cycles, wherein the multiple service stages include: voltage stabilization stage, voltage jump stage, voltage difference stage and cell swelling stage, and each service stage includes voltage characteristics, internal resistance characteristics, lithium plating characteristics, appearance characteristics and thermal runaway risk level; and a first grading and evaluation module, used to grade and evaluate the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0085] Optionally, the grading and evaluation unit further includes: a second division module, used to divide the service process of the lithium-ion cell into multiple service stages based on the trend of DC internal resistance change, wherein the multiple service stages include: normal internal resistance stage, slight internal resistance jump but recoverable stage, slight internal resistance increase but unrecoverable stage, and significant internal resistance increase stage; and a second grading and evaluation module, used to grade and evaluate the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0086] Optionally, the grading and evaluation unit further includes: a third division module, used to divide the service process of the lithium-ion cell into multiple service stages based on changes in lithium plating characteristics, wherein the multiple service stages include: a stage with a small amount of lithium plating around foreign matter, a stage with severe lithium plating on the negative electrode at the location of foreign matter, a stage with a foreign matter diffusion trend, and a stage with severe lithium plating on the electrode around foreign matter; and a third grading and evaluation module, used to grade and evaluate the thermal runaway risk of the lithium-ion cell based on the characteristic parameters of each service stage.

[0087] According to another aspect of the present invention, an electronic device is provided, comprising one or more processors and a memory, the memory being used to store one or more programs, wherein when the one or more programs are executed by the one or more processors, the one or more processors cause the one or more processors to implement the analysis method of the lithium-ion battery of any of the above.

[0088] As can be seen from the above description, the above embodiments of the present invention achieve the following technical effects: realize dynamic risk assessment of foreign object defect batteries throughout their entire life cycle from manufacturing source to service, and overcome the shortcomings of traditional static screening methods that cannot predict long-term safety risks.

[0089] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects: providing a quantitative risk rating standard (low, low-medium, medium-high, high), which helps to optimize the battery production process, reduce the incidence of safety accidents, and improve the safety of the cascade utilization of battery resources.

[0090] In the description of this invention, it should be understood that the orientation or positional relationship indicated by directional terms such as "front, back, up, down, left, right", "horizontal, vertical, horizontal" and "top, bottom" is generally based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing this invention and simplifying the description. Unless otherwise stated, these directional terms do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on the scope of protection of this invention; the directional terms "inner" and "outer" refer to the inner and outer contours relative to the outline of each component itself.

[0091] For ease of description, spatial relative terms such as "above," "on top of," "on the upper surface of," "above," etc., are used herein to describe the spatial positional relationship of a device or feature as shown in the figures to other devices or features. It should be understood that spatial relative terms are intended to encompass different orientations in use or operation beyond the orientation of the device as described in the figures. For example, if the device in the figures were inverted, a device described as "above" or "on top of" other devices or structures would subsequently be positioned as "below" or "under" other devices or structures. Thus, the exemplary term "above" can include both "above" and "below." The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used herein will be interpreted accordingly.

[0092] Furthermore, it should be noted that the use of terms such as "first" and "second" to define components is merely for the purpose of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore should not be construed as limiting the scope of protection of this invention.

[0093] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An analytical method for lithium-ion batteries, characterized in that, include: An initial tomographic scan was performed on the assembled lithium-ion battery cell to obtain the initial cell scan results; The lithium-ion battery cell with the implanted foreign object was subjected to cyclic charge-discharge test under a preset constant temperature environment, and the charge-discharge test results were obtained. After reaching the target number of cycles, a second tomographic scan is performed on the lithium-ion cell, and the results of the second cell scan are compared and analyzed with the initial cell scan results to determine the morphological change characteristics of the foreign object location. Accelerated calorimetry analysis was performed on lithium-ion cells that reached the target number of cycles to obtain the key thermal runaway temperature and kinetic parameters of the lithium-ion cells. Based on the integrated charge and discharge test results, the morphological change characteristics of the foreign object location, and the key thermal runaway temperature and kinetic parameters, the service process of the foreign object defect lithium-ion cell is divided, and the thermal runaway risk of the lithium-ion cell is graded and assessed based on the characteristic parameters of each service stage.

2. The analytical method for lithium-ion batteries according to claim 1, characterized in that, The steps for performing an initial tomographic scan on the assembled lithium-ion battery cell to obtain the initial cell scan results include: The positions of the positive and negative electrode plates and the separator of the battery cell structure to be assembled are obtained, and the metal slag particles of the first preset size and the positive or negative electrode plate fragments of the second preset size to be implanted are obtained. In the stacking process, the metal welding slag particles and the positive or negative electrode fragments are implanted between adjacent electrodes at a first preset position; or, in the winding process, the metal welding slag particles and the positive or negative electrode fragments are implanted between spirally wound electrodes at a second preset position. All cell assembly processes are completed according to standard procedures, and an initial tomographic scan is performed on the packaged lithium-ion cell to obtain the initial cell scan results. The initial cell scan results include at least the three-dimensional spatial location and morphological distribution of foreign objects.

3. The analytical method for lithium-ion batteries according to claim 1, characterized in that, The steps for conducting cyclic charge-discharge tests on lithium-ion cells with implanted foreign objects under a preset constant temperature environment to obtain the charge-discharge test results include: It utilizes a constant temperature environment control device, a programmable charge and discharge device, a self-discharge tester, a DC internal resistance tester, and an electrochemical workstation; The constant temperature environment control device is used to control the lithium-ion battery cell to be in a preset constant temperature environment. The programmable charging and discharging device is used to charge the lithium-ion cell to 4.2V at 1.0C, then charge it to the cutoff current of 0.05C at a constant current and constant voltage, and then discharge it to 2.5V at a constant current of 1C to complete one charge-discharge cycle. Control the lithium-ion battery cell to complete a predetermined number of charge-discharge cycles; At the end of each predetermined number of cycles, the self-discharge rate is measured using the self-discharge tester, the DC internal resistance is measured using the DC internal resistance tester, and the electrochemical impedance spectroscopy is measured using the electrochemical workstation, to obtain charge-discharge test results including self-discharge rate data, DC internal resistance change curves, and electrochemical impedance spectroscopy.

4. The analytical method for lithium-ion batteries according to claim 1, characterized in that, After reaching the target number of cycle times, a second tomographic scan is performed on the lithium-ion cell, and the results of the second cell scan are compared and analyzed with the initial cell scan results to determine the morphological changes of the foreign object location. This includes the following steps: Once the target number of cycles is reached, a second tomographic scan is performed on the lithium-ion cell to obtain a three-dimensional image containing the location, morphology, and electrode structure of foreign matter inside the lithium-ion cell, thus obtaining the second cell scan result. The secondary cell scanning results are compared and analyzed with the initial cell scanning results to analyze the area where foreign matter is located in the lithium-ion cell, the surface of the electrode around the foreign matter, the damage to the separator, and the lithium deposits, so as to determine the morphological changes of the foreign matter location.

5. The analytical method for lithium-ion batteries according to claim 1, characterized in that, The steps for performing accelerated calorimetry analysis on lithium-ion cells that have reached the target number of cycles to obtain the key temperatures and kinetic parameters of thermal runaway in lithium-ion cells include: Using an accelerated calorimeter, the lithium-ion cell is placed inside the vacuum chamber of the accelerated calorimeter and heated at a preset heating rate. The self-heating initiation temperature, thermal runaway initiation temperature, pressure relief temperature, maximum temperature, and corresponding time for each temperature of the lithium-ion cell under adiabatic conditions are recorded, as well as the mass change between the cell mass before and after the test. This yields the key thermal runaway temperature and kinetic parameters of the lithium-ion cell.

6. The analytical method for lithium-ion batteries according to claim 1, characterized in that, The steps for classifying the service life of lithium-ion cells with foreign object defects and assessing the thermal runaway risk of lithium-ion cells based on the characteristic parameters of each service stage include: Based on the evolution trend of cell voltage with the number of cycles, the service process of the lithium-ion cell is divided into multiple service stages, including: voltage stabilization stage, voltage jump stage, voltage difference stage and cell swelling stage. Each service stage includes voltage characteristics, internal resistance characteristics, lithium plating characteristics, appearance characteristics and thermal runaway risk level. The thermal runaway risk of the lithium-ion battery cell is classified and assessed based on the characteristic parameters of each service stage.

7. The analytical method for lithium-ion batteries according to claim 1, characterized in that, The steps for classifying the service life of lithium-ion cells with foreign object defects and assessing the thermal runaway risk of lithium-ion cells based on the characteristic parameters of each service stage include: Based on the trend of DC internal resistance change, the service process of the lithium-ion battery cell is divided into multiple service stages, including: normal internal resistance stage, slight internal resistance jump but recoverable stage, slight internal resistance increase but unrecoverable stage, and significant internal resistance increase stage. The thermal runaway risk of the lithium-ion battery cell is classified and assessed based on the characteristic parameters of each service stage.

8. The analytical method for lithium-ion batteries according to claim 1, characterized in that, The steps for classifying the service life of lithium-ion cells with foreign object defects and assessing the thermal runaway risk of lithium-ion cells based on the characteristic parameters of each service stage include: Based on the changes in lithium plating characteristics, the service process of the lithium-ion battery cell is divided into multiple service stages, including: a small amount of lithium plating around foreign matter, a severe lithium plating stage on the negative electrode at the foreign matter, a foreign matter diffusion trend stage, and a severe lithium plating stage on the electrode around foreign matter. The thermal runaway risk of the lithium-ion battery cell is classified and assessed based on the characteristic parameters of each service stage.

9. An analytical apparatus for lithium-ion batteries, characterized in that, include: The foreign body implantation unit is used to perform an initial tomographic scan on the assembled lithium-ion battery cell to obtain the initial battery cell scan results. The cyclic charge-discharge unit is used to perform cyclic charge-discharge tests on lithium-ion cells with implanted foreign objects under a preset constant temperature environment to obtain charge-discharge test results. The foreign object scanning and comparison analysis unit is used to perform a secondary tomographic scan on the lithium-ion cell after reaching the target number of cycles, and compare and analyze the secondary cell scan results with the initial cell scan results to determine the morphological change characteristics of the foreign object location. The thermal runaway analysis unit is used to perform accelerated calorimetry analysis on lithium-ion cells that have reached the target number of cycles, and to obtain the key thermal runaway temperature and kinetic parameters of the lithium-ion cells. The grading and assessment unit is used to classify the service process of lithium-ion cells with foreign object defects based on the integrated charge and discharge test results, the morphological change characteristics of the foreign object location, and the key temperature and kinetic parameters of thermal runaway, and to grade and assess the thermal runaway risk of the lithium-ion cells based on the characteristic parameters of each service stage.

10. An electronic device, characterized in that, It includes one or more processors and a memory, the memory being used to store one or more programs, wherein when the one or more programs are executed by the one or more processors, the one or more processors cause the one or more processors to implement the analysis method for lithium-ion batteries according to any one of claims 1 to 8.