A method for the off-line preparation of a birefringent optical fiber

By scanning the drawn pre-formed optical fiber along the fiber axial direction with a CO₂ laser, a birefringent structure is generated offline, which solves the problems of high cost and non-adjustability in the traditional birefringent fiber fabrication and achieves flexible control and stable fabrication.

CN123136801APending Publication Date: 2026-11-20SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611087235.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional birefringent optical fibers are expensive to manufacture and their birefringence is not adjustable. Existing technologies have failed to enable flexible customization of the size and type of birefringence according to the application scenario.

Method used

A CO₂ laser is used to scan a pre-drawn fiber with photosensitive and thermally stressed properties along the fiber axis. A permanent birefringent structure is generated in the fiber doping region by offline writing. The writing path, power, scanning speed and pulse frequency of the laser are controlled to achieve diverse birefringent properties.

Benefits of technology

It achieves low-cost, flexible control of birefringence size and type, is suitable for different application fields, improves energy utilization, avoids fiber surface damage, and ensures the stability and consistency of the fabrication process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123136801A_ABST
    Figure CN123136801A_ABST
Patent Text Reader

Abstract

The application discloses a kind of offline preparation controllable birefringence structure optical fiber method, and the preform optical fiber with doped region has uniform photosensitivity and thermal stress characteristics, and permanent birefringence structure is generated in the doped region of optical fiber by laser along the axial scanning of optical fiber offline engraving.The size and distribution of optical fiber birefringence are offline regulated by the engraving path, power, scanning speed and pulse frequency of laser.The thermal expansion coefficient of doped region is greater than the thermal expansion coefficient of pure quartz, and the glass transition temperature is lower than the glass transition temperature of pure quartz.The application uses photoelectric detector to monitor scattered light intensity in real time and dynamically adjusts laser parameters to avoid optical fiber damage, and places optical fiber in a temperature and humidity controllable environment to stabilize stress distribution.The application does not need to redesign preform rod structure and perform drawing preparation process, has the advantages of low cost, adjustable parameters, flexible preparation, etc., and can be widely applied in optical fiber sensing, polarization control and optical communication fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of fiber optics and laser processing technology, specifically to a method for offline inscription of controllable birefringent structures in prefabricated optical fibers with photosensitivity and thermal stress characteristics using a laser. Background Technology

[0002] Birefringent fibers have important applications in fiber optic sensing, polarization control, and optical communication. Traditional polarization-maintaining fibers are classified into linear birefringent fibers, circular birefringent fibers, and elliptical birefringent fibers based on their birefringence type. Linear birefringent fibers achieve birefringence by introducing stress regions (such as panda-shaped or bowtie-shaped) into the preform; circular birefringent fibers achieve birefringence by online twisting of the preform; and elliptical birefringent fibers generate birefringence through the synergistic effect of an elliptical core and a stress region. However, traditional methods are complex, costly, and the magnitude of birefringence is fixed after fiber drawing, making flexible control difficult.

[0003] In recent years, CO2 laser post-processing technology has been used to control the internal stress of optical fibers. CO2 lasers are low-cost, have stable power, and high processing efficiency. Their 10.6 μm wavelength is strongly absorbed by quartz, serving as a surface heat source. This heat conduction generates a temperature gradient within the fiber, inducing thermal stress and refractive index modulation. Existing technologies include methods for writing long-period fiber gratings using CO2 lasers, as well as techniques for fabricating fiber gratings using unilateral or symmetrical CO2 laser irradiation. However, current technologies primarily focus on fiber grating fabrication and have not systematically studied how to control the distribution and type of birefringence in optical fibers using different CO2 laser writing paths, nor have they achieved the goal of flexibly customizing the size and type of birefringence according to application scenarios. Summary of the Invention

[0004] The purpose of this invention is to provide a method for offline fabrication of controllable birefringent optical fibers. This method utilizes pre-drawn optical fibers with photosensitivity and thermal stress characteristics, and performs offline writing along the fiber axis using a CO2 laser. This generates a permanent birefringent structure in the fiber's doped regions, solving the problems of high fabrication cost and untunable birefringence in existing birefringent optical fibers. Furthermore, this invention allows for the selection of different writing paths and laser parameters according to different application fields (such as fiber optic sensing, polarization control, and optical communication), achieving diverse birefringent properties.

[0005] The technical solution of this invention: A method for offline fabrication of controllable birefringent optical fibers is disclosed. The pre-drawn optical fiber has doped regions with uniform photosensitivity and thermal stress characteristics. Offline writing is performed by scanning along the fiber axis with a laser to generate a permanent birefringent structure in the doped regions of the optical fiber.

[0006] The size and distribution of fiber birefringence can be controlled offline by the laser marking path, power, scanning speed and pulse frequency.

[0007] The cladding of the prefabricated optical fiber contains doped regions, the coefficient of thermal expansion of which is greater than that of pure silica and the glass transition temperature is lower than that of pure silica.

[0008] The prefabricated optical fiber consists of an outer cladding, an inner cladding, a transition layer, and a core, from the outside in. The outer cladding is made of pure silica, and the inner cladding is made of boron-doped silica. The inner cladding is sensitive to the thermal response of lasers and has a higher coefficient of thermal expansion than the outer cladding.

[0009] By aligning a CO2 laser with an optical fiber and moving the CO2 laser in a straight or helical motion relative to the fiber axis, the thermal stress generated by the laser produces permanent birefringence in the doped regions inside the fiber.

[0010] After completing one inscription, restore the initial position of the optical fiber and laser, adjust the initial angle of the optical fiber, and then inscribe again to achieve multiple straight lines or multiple spiral lines.

[0011] Each birefringent structure can be inscribed using either a slow inscription method or a fast inscription method: Slow-speed writing method: The laser moves relatively slowly relative to the optical fiber, completing one writing step in one scan. This results in a greater heat penetration depth, allowing sufficient time for heat to conduct into the fiber's interior, leading to a more uniform temperature distribution across the cross-section and a symmetrical stress field, making it suitable for the fabrication of polarization-maintaining fibers.

[0012] Rapid writing method: The laser moves relatively fast relative to the optical fiber, and multiple scans along the same path complete one writing operation. In this method, the heat penetration depth is small, and heat is mainly concentrated near the fiber surface, forming a steep temperature gradient. Multiple scans are needed to accumulate heat and gradually bring the inner cladding to its glass transition temperature. Rapid writing is suitable for devices requiring strong unilateral birefringence or localized stress.

[0013] The invention also includes an online monitoring step: a photodetector is used to monitor the intensity of scattered light on the surface of the optical fiber in real time during the laser writing process. When the intensity of scattered light exceeds a preset threshold, the control system dynamically adjusts the laser power, scanning speed or optical fiber movement speed to avoid excessive damage to the optical fiber, thereby achieving stable and continuous offline fabrication of controllable birefringent optical fiber.

[0014] The present invention also includes a temperature and humidity control step: during and after the writing process, the optical fiber is placed in an environment with stable and controllable temperature and humidity, and the stress distribution is stabilized in a normal temperature and low humidity environment to prevent residual stress release and ensure the long-term stability of the birefringent structure.

[0015] The beneficial effects of this invention are: 1. This invention uses pre-drawn optical fibers for offline writing, eliminating the need for redesigning the pre-drawn structure and preparing the fiber. The size and type of birefringence can be customized according to the needs of the scenario, enabling mass production and rapid manufacturing.

[0016] 2. By utilizing prefabricated optical fibers with photosensitive and thermally stressed properties, the coefficient of thermal expansion of the doped region is greater than that of pure quartz and the glass transition temperature is lower than that of pure quartz, which enables selective heating, improves energy utilization, reduces the required laser power, and helps avoid damage to the optical fiber surface.

[0017] 3. By adjusting the laser marking path (straight or spiral, single or multiple channels), power, scanning speed, and pulse frequency, the size and distribution of birefringence can be flexibly controlled, making it suitable for different polarization control requirements and applications in sensing, communication, and other fields.

[0018] 4. The choice between slow and fast writing modes provides process flexibility, allowing users to select the optimal parameters based on thermal penetration depth theory to meet the needs of different application scenarios.

[0019] 5. The use of a photodetector to monitor the intensity of scattered light in real time and dynamically adjust laser parameters can effectively avoid excessive damage to the optical fiber; combined with a temperature and humidity control system to stabilize stress distribution, the stability of the preparation process and the consistency of the product are ensured. Attached Figure Description

[0020] Figure 1 A schematic diagram of the structure of a prefabricated optical fiber with photosensitivity and thermal stress characteristics (taking boron-doped inner cladding optical fiber as an example). From the fiber surface to the core, it includes an outer cladding, an inner cladding, a transition layer, and a core.

[0021] Figure 2 : Schematic diagram of CO2 laser unilateral axial writing on an optical fiber. The red area represents the writing trajectory formed by the laser along the fiber axis; the local cross-section shows the 50μm laser action width, and the blue arrows represent scattered light.

[0022] Figure 3 Comparison of stress distribution on fiber cross sections caused by different marking paths: (a) single-sided linear marking, (b) double-sided linear marking, (c) four-sided linear marking, and (d) spiral marking.

[0023] Figure 4 : Schematic diagram of an optical fiber fixing and writing device under controllable temperature and humidity conditions, where ① is a temperature control unit, ② is a humidity control unit, ③ is a spring clip, ④ is a prefabricated optical fiber with photosensitivity and thermal stress characteristics, ⑤ is a rotation controller, and ⑥ is a sealed door. Detailed Implementation

[0024] Example 1: This invention provides a method for offline fabrication of controllable birefringent optical fibers: A pre-drawn optical fiber is used, with doped regions in its cladding. These doped regions exhibit uniform photosensitivity and thermal stress characteristics. Offline writing is performed by scanning along the fiber axial direction using a laser, generating a permanent birefringent structure in the doped regions. The coefficient of thermal expansion of the doped regions is greater than that of pure silica, and their glass transition temperature is lower than that of pure silica.

[0025] Figure 1 In a preferred embodiment of the present invention, the prefabricated optical fiber comprises, from the outside in, an outer cladding 1, an inner cladding 2, a transition layer 3, and a core 4. The outer cladding 1 is pure silica, and the inner cladding 2 is boron-doped silica. The inner cladding 2 is sensitive to the thermal response of laser light and has a higher coefficient of thermal expansion than the outer cladding 1. The boron doping concentration of the boron-doped inner cladding 2 is optimized to give it a higher coefficient of thermal expansion than pure silica and a lower glass transition temperature. This optical fiber structure allows the inner cladding 2 region to preferentially reach the plastic deformation temperature under unilateral CO2 laser irradiation, while the outer cladding 1 maintains structural integrity, thereby achieving selective stress introduction. Compared with ordinary optical fibers, optical fibers with photosensitivity and thermal stress characteristics can produce more significant birefringence under the same laser parameters and require lower laser power, which helps to avoid surface damage.

[0026] like Figure 4 The structure comprises: ① a temperature control unit, ② a humidity control unit, ③ a spring clip, ④ a prefabricated optical fiber with photosensitivity and thermal stress characteristics, ⑤ a rotation controller, and ⑥ a sealed door. In this invention, the size and distribution of the fiber's birefringence are controlled offline by the laser's marking path, power, scanning speed, and pulse frequency. Specifically: A CO2 laser is aligned with an optical fiber, and the laser moves linearly relative to the fiber axis. The thermal stress generated by the laser induces permanent birefringence in the doped regions inside the fiber. After completing one pass of writing, the initial positions of the fiber and laser are restored, the initial angle of the fiber is adjusted, and writing is performed again to achieve multi-pass linear writing.

[0027] Each birefringent structure can be inscribed using either a slow inscription method or a fast inscription method: Slow-speed writing method: The laser moves relatively slowly relative to the optical fiber, completing one writing step in one scan. This results in a greater heat penetration depth, allowing sufficient time for heat to conduct into the fiber's interior, leading to a more uniform temperature distribution across the cross-section and a symmetrical stress field, making it suitable for the fabrication of polarization-maintaining fibers.

[0028] Rapid writing method: The laser moves relatively fast relative to the optical fiber, and multiple scans along the same path complete one writing operation. In this method, the heat penetration depth is small, and heat is mainly concentrated near the fiber surface, forming a steep temperature gradient. Multiple scans are needed to accumulate heat and gradually bring the inner cladding to its glass transition temperature. Rapid writing is suitable for devices requiring strong unilateral birefringence or localized stress.

[0029] The invention also includes an online monitoring step: a photodetector is used to monitor the intensity of scattered light on the surface of the optical fiber in real time during the laser writing process. When the intensity of scattered light exceeds a preset threshold, the control system dynamically adjusts the laser power, scanning speed or optical fiber movement speed to avoid excessive damage to the optical fiber, thereby achieving stable and continuous offline fabrication of controllable birefringent optical fiber.

[0030] The present invention also includes a temperature and humidity control step: during and after the writing process, the optical fiber is placed in an environment with stable and controllable temperature and humidity, and the stress distribution is stabilized in a normal temperature and low humidity environment to prevent residual stress release and ensure the long-term stability of the birefringent structure.

[0031] Example 2: Fabrication of linear birefringent optical fiber by slow single-sided writing A pre-drawn optical fiber with photosensitivity and thermal stress characteristics (taking boron-doped inner-clad fiber as an example) is selected. From the outside in, it consists of outer cladding 1, inner cladding 2, transition layer 3, and core 4. Outer cladding 1 is pure silica, and inner cladding 2 is boron-doped silica. Inner cladding 2 is sensitive to the thermal response of CO2 laser and has a higher coefficient of thermal expansion than outer cladding 1. The fiber coating is removed, and the surface is cleaned. The fiber is fixed on a displacement platform, and axial prestress is applied. A CO2 laser is used, and a slow writing mode is set. The laser moves relatively slowly relative to the fiber, completing one writing step in one scan. The writing process is as follows: Figure 2 In the figure, the red area represents the writing trajectory along the fiber axis, and the green area represents the CO2 laser-affected area. The width of the affected area shown in the local cross-sectional view is approximately 50 μm. The CO2 laser is aligned with the fiber and moved linearly relative to the fiber axis, writing along one side of the fiber axis. Slow writing results in a greater thermal penetration depth, sufficient heat conduction, and uniform cross-sectional temperature. The thermal stress generated by the laser induces permanent linear birefringence in the doped regions inside the fiber. During the writing process, a photodetector monitors the intensity of scattered light on the fiber surface in real time. When the scattered light intensity exceeds a preset threshold, the control system dynamically adjusts the laser power, scanning speed, or fiber movement speed to avoid excessive damage to the fiber. After writing, the fiber is placed in a stable and controllable environment with controlled temperature and humidity to stabilize the stress distribution. After writing, the inner cladding reaches the glass transition temperature, forming a symmetrical stress field and resulting in uniform and stable linear birefringence. This structure is suitable for polarization-maintaining fibers, polarization controllers in fiber optic current sensors, etc.

[0032] Example 3: Rapid multi-channel linear writing fabrication of linear birefringent optical fibers The fiber parameters and preprocessing are the same as in Example 1. A CO2 laser is used, and a fast writing mode is set, with the laser moving relatively quickly relative to the fiber. The CO2 laser is aligned with the fiber, and it moves linearly relative to the fiber axis, writing along one side of the fiber axis. During fast writing, the heat penetration depth is small, and the temperature rise in a single scan is insufficient. Multiple scans along the same path are required to complete one writing pass, allowing the inner cladding to gradually reach the glass transition temperature. After completing one writing pass, the initial positions of the fiber and laser are restored, the initial angle of the fiber is adjusted, and writing is performed again to achieve multiple linear writing passes (e.g., ...). Figure 3 b. Double-sided engraving Figure 3 (e.g., four-sided writing). By adjusting the laser power, scanning speed, pulse frequency, and number of scans, the size and distribution of birefringence can be controlled. Rapid writing is suitable for devices requiring strong unilateral birefringence or localized stress, such as polarization controllers and high-precision localized stress sensors.

[0033] Example 4: Rapid spiral writing fabrication of non-twisted circular birefringent optical fiber The fiber parameters and preprocessing are the same as in Example 2. A CO2 laser is used, and a fast writing mode is set. The prefabricated fiber with photosensitivity and thermal stress characteristics is fixed on a rotation control platform. The laser moves at a constant speed along the fiber axis, while the fiber rotation control platform controls the fiber to rotate at a constant angular velocity, forming a helical scanning trajectory. By adjusting the laser power, scanning speed, pulse frequency, and number of scans, the thermal penetration depth is made comparable to the inner cladding depth, thereby generating a steep radial temperature gradient. During the fast helical writing process, due to the high scanning speed, the penetration depth is small in a single scan, requiring multiple scans to achieve heat accumulation. After each scan, the surface heat dissipates rapidly, while the inner cladding temperature gradually rises. After cooling, periodic non-twisted circular birefringence is formed inside the fiber. By controlling the left and right helical rotation of the circular birefringent fiber, linearly polarized light can be converted into circularly polarized light, which is suitable for circular polarizers and all-fiber current sensors in integrated optics.

[0034] Example 5: Offline fabrication of non-twisted elliptical birefringent fiber using helical path inscription Elliptical birefringent fiber is fabricated by offline writing along a helical path using a CO2 laser along the fiber axis, in a slow writing mode, and by introducing asymmetric stress during the writing process to produce non-torsional elliptical birefringence. Three different methods can be used to introduce asymmetric stress: 1) Periodic modulation of laser power. During the helical writing process, the laser power is changed at a fixed period (e.g., per helical revolution) to subject the optical fiber to non-uniform heat input in the circumferential direction. Specifically, the power is increased or decreased when the optical fiber rotates to a specific angle, resulting in an asymmetrical thermal stress distribution along the circumferential direction.

[0035] 2) Modulate the scanning speed or pulse frequency. While keeping the average power constant, synchronously change the scanning speed and pulse frequency to make the heat accumulation in different angular regions different, thereby generating an asymmetric stress field.

[0036] 3) Combining the periodic variation of fiber rotation angular velocity. During the helical writing process, the fiber rotation angular velocity varies periodically with the axial position, resulting in uneven pitch and thus introducing additional asymmetric stress.

[0037] By employing the above method, the inner cladding of the optical fiber is subjected to radial stresses of varying magnitudes in the circumferential direction, thereby generating differentiated refractive index changes along the fast and slow axes, achieving elliptic birefringence. The fabricated elliptic birefringent fiber simultaneously possesses both linear and circular birefringence components. The left-hand and right-hand rotation of the circular birefringent fiber can be controlled by adjusting the rotation direction, making it applicable to polarization mode dispersion compensation, ellipters, and distributed fiber optic sensing systems.

Claims

1. A method for offline fabrication of controllable birefringent optical fibers, characterized in that: The drawn pre-formed optical fiber has doped regions with uniform photosensitivity and thermal stress characteristics. Offline writing is performed by scanning along the fiber axis with a laser to generate a permanent birefringent structure in the doped regions of the optical fiber.

2. The method for offline fabrication of controllable birefringent optical fiber according to claim 1, characterized in that: The size and distribution of fiber birefringence can be controlled offline by the laser marking path, power, scanning speed and pulse frequency.

3. The method for offline fabrication of controllable birefringent optical fiber according to claim 1, characterized in that: The cladding of the prefabricated optical fiber contains doped regions, the coefficient of thermal expansion of which is greater than that of pure silica and the glass transition temperature is lower than that of pure silica.

4. The method for offline fabrication of controllable birefringent optical fiber according to claim 1, characterized in that: The prefabricated optical fiber consists of an outer cladding, an inner cladding, a transition layer, and a core, from the outside in. The outer cladding is made of pure silica, and the inner cladding is made of boron-doped silica. The inner cladding is sensitive to the thermal response of lasers and has a higher coefficient of thermal expansion than the outer cladding.

5. The method for offline fabrication of controllable birefringent optical fiber according to claim 1, characterized in that: A photodetector is used to monitor the intensity of scattered light on the fiber surface in real time during the laser writing process. When the intensity of scattered light exceeds a preset threshold, the control system dynamically adjusts the laser power, scanning speed, or fiber movement speed to avoid excessive damage to the fiber.

6. The method for offline fabrication of controllable birefringent optical fiber according to claim 1, characterized in that: During and after the inscription process, the optical fiber is placed in an environment with stable and controllable temperature and humidity to stabilize stress distribution in a normal temperature and low humidity environment.

7. The method for offline fabrication of controllable birefringent optical fiber according to claim 1, characterized in that: By aligning a CO2 laser with an optical fiber and moving the CO2 laser in a straight or helical motion relative to the fiber axis, the thermal stress generated by the laser produces permanent birefringence in the doped regions inside the fiber.

8. The method for offline fabrication of controllable birefringent optical fiber according to claim 7, characterized in that: After completing one inscription, restore the initial position of the optical fiber and laser, adjust the initial angle of the optical fiber, and then inscribe again to achieve multiple straight lines or multiple spiral lines.

9. The method for offline fabrication of controllable birefringent optical fibers according to any one of claims 1-7, characterized in that: Each birefringent structure is inscribed using a slow inscription method, where the laser moves relatively slowly relative to the optical fiber, and one inscription is completed in one scan path.

10. The method for offline fabrication of controllable birefringent optical fibers according to any one of claims 1-7, characterized in that: Each birefringent structure is written using a rapid writing method, where the laser moves at a relatively high speed relative to the optical fiber, and multiple identical scanning paths are used to complete one writing step.