Optical fiber and method for manufacturing the same

By using polymethylsilsesquioxane aerogel as the fiber core and combining it with an air cladding, the problems of slow sensitivity and response speed of traditional optical fibers are solved, realizing the integration of optical transmission and gas enrichment, improving the performance of gas sensors and reducing manufacturing costs.

CN123136802APending Publication Date: 2026-11-20WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611315845.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional optical fibers use silicon dioxide as the core, resulting in low sensitivity and slow response speed of gas sensors, making it difficult to achieve accurate detection of specific gases.

Method used

Using polymethylsilsesquioxane aerogel as the fiber core and combining it with an air cladding, optical fibers are fabricated using a capillary mold, achieving integrated optical transmission and gas enrichment, simplifying the structure and reducing costs.

Benefits of technology

It improves the sensitivity and response speed of the gas sensor, simplifies the fiber optic structure, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123136802A_ABST
    Figure CN123136802A_ABST
Patent Text Reader

Abstract

The application provides an optical fiber and a preparation method thereof. The optical fiber comprises a fiber core, a material of the fiber core is selected from polymethylsilsesquioxane aerogel materials, a refractive index of the fiber core is 1.02-1.04, and a single-point total pore volume of the fiber core is 1.1 cm 3 / g-1.2 cm 3 / g. The application uses polymethylsilsesquioxane aerogel materials as the fiber core, uses the suitable refractive index and the high total pore volume of the polymethylsilsesquioxane aerogel, integrally realizes the functions of optical transmission and gas enrichment, improves the sensitivity and response speed of a gas sensor using the optical fiber, omits the setting of a redundant coating or other structures for gas adsorption, simplifies the structure of the optical fiber, and reduces the manufacturing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optical fiber technology, and in particular to an optical fiber and its fabrication method. Background Technology

[0002] Traditional optical fibers use silica as the core. Due to the density of the material, gases cannot permeate it. As a result, when optical fibers are used in gas sensors, they can only rely on weak signals generated on the fiber surface or end face, leading to low sensitivity. Even with methods to increase gas adsorption, such as adding coatings or capillary structures to the fiber surface, gas molecules undergo adsorption-diffusion-desorption processes on the coating or capillary surface, resulting in slow response speeds and making it difficult to achieve accurate detection of specific target gases.

[0003] Therefore, there is an urgent need for an optical fiber and its fabrication method to solve the above-mentioned technical problems. Summary of the Invention

[0004] In view of this, the present invention proposes an optical fiber and its preparation method to solve the technical problem that existing optical fibers use silicon dioxide as the core, which cannot directly achieve gas adsorption, and thus the sensitivity and response speed are difficult to improve when applied to gas sensors.

[0005] The technical solution of this invention is implemented as follows: In a first aspect, the present invention provides an optical fiber, comprising: The fiber core is made of polymethylsilsesquioxane aerogel material; The refractive index of the fiber core is between 1.02 and 1.04, and the total pore volume at a single point in the fiber core is 1.1 cm. 3 / g to 1.21cm 3 / g.

[0006] In some embodiments, the optical fiber further includes a cladding that covers the surface of the fiber core, the cladding being air; The optical fiber has a numerical aperture of 0.21 to 0.27 and a fiber core optical loss per unit length of 1.37 dB / cm to 1.97 dB / cm.

[0007] In some embodiments, the specific surface area of ​​the fiber core is 360 m². 2 / g to 500m 2 / g, the average pore size of the fiber core is 10.2nm to 14nm.

[0008] Secondly, the present invention also provides a method for preparing an optical fiber, comprising: The silicon source, the first catalyst, and water undergo a first mixing treatment to obtain a hydrolysate; The hydrolysate is mixed with surfactant and water in a second process to obtain a first precursor solution; After the first precursor liquid is cooled, it is mixed with the second catalyst in a third process to obtain the second precursor liquid. The capillary mold is inserted into the second precursor liquid and undergoes gelation treatment to obtain a wet gel fiber core preform in the capillary mold. The wet gel fiber core preform is subjected to aging treatment to obtain a wet gel fiber core; The wet gel fiber core is subjected to supercritical carbon dioxide drying to obtain the optical fiber; The optical fiber is the optical fiber as described above.

[0009] In some embodiments, the inner diameter of the capillary mold is 0.3 mm to 3 mm, and the length of the capillary mold is 2 cm to 50 cm.

[0010] In some embodiments, the cooling process takes 20 to 40 seconds; The gelation treatment temperature is 20°C to 30°C, and the gelation treatment time is greater than or equal to 0.5 hours and less than or equal to 2 hours.

[0011] In some embodiments, the aging treatment temperature is 40°C to 80°C, and the aging treatment time is greater than or equal to 24 hours and less than 72 hours. The heating rate from the gelation treatment temperature to the aging treatment temperature is 0.5℃ / min to 2℃ / min.

[0012] In some embodiments, prior to the supercritical carbon dioxide drying process, the wet gel fiber core also undergoes a demolding process, which includes: After the capillary mold is cleaned, it is placed in water, and the wet gel fiber core is pushed out of the capillary mold using an ejector pin. The difference between the inner diameter of the capillary mold and the diameter of the ejector pin is greater than or equal to 0.1 mm and less than or equal to 0.2 mm.

[0013] In some embodiments, the step of obtaining the optical fiber by supercritical carbon dioxide drying of the wet gel fiber core includes: The wet gel fiber core is dried under supercritical carbon dioxide for a specified time under drying pressure and temperature to obtain the optical fiber. The drying pressure is 8 MPa to 9 MPa, the drying temperature is 35°C to 40°C, and the drying time is greater than or equal to 4 hours and less than or equal to 12 hours.

[0014] In some embodiments, the silicon source is selected from methyltrimethoxysilane, the first catalyst is selected from at least one of acetic acid and phosphoric acid, the surfactant is selected from Pluronic F127 type surfactant, and the second catalyst includes at least one of tetramethylammonium hydroxide and lithium hydroxide; The molar ratio of the first catalyst to the silicon source is (0.011-0.72):1000; In the hydrolysate, the concentration of the first catalyst is from 0.04 mmol / L to 4 mmol / L; In the first precursor solution, the concentration of the surfactant is from 0.06 g / mL to 0.094 g / mL; The molar ratio of tetramethylammonium hydroxide to the volume of the silicon source is (0.24 to 0.36) mmol:1 mL.

[0015] The optical fiber and its preparation method of the present invention have the following advantages over the prior art: by using polymethylsilsesquioxane aerogel material as the fiber core, and utilizing the suitable refractive index and high total pore volume of polymethylsilsesquioxane aerogel, the optical transmission and gas enrichment functions are integrated, which improves the sensitivity and response speed of the gas sensor using the optical fiber, while eliminating the need for additional coatings or other structures for gas adsorption, simplifying the structure of the optical fiber and reducing the manufacturing cost. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a schematic diagram of the apparatus used for gelation treatment in the optical fiber preparation method of the present invention; Figure 2 This is a schematic flowchart of the optical fiber fabrication method according to Embodiment 1 of the present invention; Figure 3 A first physical diagram of an optical fiber provided in Embodiment 1 of the present invention; Figure 4 A second physical diagram of the optical fiber provided in Embodiment 1 of the present invention; Figure 5 A physical diagram of the first type of optical fiber light guide provided in Embodiment 1 of the present invention; Figure 6 A physical diagram of a second type of optical fiber provided in Embodiment 1 of the present invention; Figure 7 A physical diagram of the third type of optical fiber provided in Embodiment 1 of the present invention. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] Currently, existing optical fibers use silicon dioxide as the core, which cannot directly adsorb gases, resulting in technical problems in improving sensitivity and response speed when optical fibers are used in gas sensors.

[0020] In a first aspect, the present invention provides an optical fiber, comprising: The fiber core is made of polymethylsilsesquioxane aerogel material; The refractive index of the fiber core is between 1.02 and 1.04, and the total pore volume at a single point in the fiber core is 1.1 cm. 3 / g to 1.21cm 3 / g.

[0021] The optical fiber provided in this application uses polymethylsilsesquioxane aerogel material as the core. By utilizing the suitable refractive index and high total pore volume of polymethylsilsesquioxane aerogel, it can achieve both optical transmission and gas enrichment functions in one integrated manner. This improves the sensitivity and response speed of gas sensors using this optical fiber, while eliminating the need for additional coatings or other structures for gas adsorption, simplifying the structure of the optical fiber and reducing manufacturing costs.

[0022] In some embodiments, the optical fiber has no additional coating, and the fiber core is in direct contact with air. That is, the optical fiber further includes a cladding that covers the surface of the fiber core, and the cladding is air.

[0023] In some embodiments, the refractive index of the fiber core can be 1.02, 1.025, 1.03, 1.035, 1.04, etc., which is beneficial to ensure that the refractive index difference between the fiber core and air is sufficient, thereby achieving the condition of stable total internal reflection, realizing long-distance light guiding, and controlling the reflection loss at the interface between the fiber core and air, extending the transmission distance of light in the fiber core, and reducing the difficulty of optical path coupling.

[0024] In some embodiments, the total pore volume at a single point in the fiber core can be 1.1 cm. 3 / g, 1.12cm 3 / g, 1.15cm 3 / g, 1.18cm 3 / g, 1.2cm 3 / g, 1.21cm 3 The presence of gases such as g / g facilitates the rapid entry of the target gas into the optical fiber when it is used in a gas sensor, enabling rapid enrichment of the target gas molecules, reducing the response time of the gas sensor, and improving the detection sensitivity of the gas sensor.

[0025] In some embodiments, the numerical aperture of the optical fiber is 0.21 to 0.27, for example, it can be 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, etc., which is beneficial to the transmission of light by the optical fiber and reduces the difficulty of optical path coupling of the optical fiber.

[0026] In some embodiments, the optical loss per unit length of the fiber core is from 1.37 dB / cm to 1.97 dB / cm, for example, it can be 1.37 dB / cm, 1.38 dB / cm, 1.4 dB / cm, 1.42 dB / cm, 1.45 dB / cm, 1.5 dB / cm, 1.6 dB / cm, 1.8 dB / cm, 1.97 dB / cm, etc. Lower optical loss is beneficial for maintaining sufficient signal strength after the optical signal has been transmitted over a long distance in the fiber core, which is beneficial for improving the sensitivity of gas sensors using the optical fiber.

[0027] In some embodiments, the specific surface area of ​​the fiber core is 360 m². 2 / g to 500m 2 / g, for example, can be 360m 2 / g、400m 2 / g、430m 2 / g、450m 2 / g、480m 2 / g、500m 2 / g, etc. The average pore size of the fiber core is 10.2nm to 14nm, for example, it can be 10.2nm, 10.5nm, 11nm, 12nm, 13nm, 14nm, etc. By controlling the specific surface area and average pore size of the fiber core within the above ranges, it is beneficial that when the optical fiber is used in a gas sensor, the gas to be measured can quickly enter the interior of the optical fiber, providing abundant adsorption sites, achieving sufficient enrichment of the gas molecules to be measured, reducing the response time of the gas sensor and improving the detection sensitivity of the gas sensor.

[0028] In some embodiments, the fiber core is constructed from polymethylsilsesquioxane to form a mesoscopic fibrous framework. The gas to be tested can diffuse freely from both ends or sidewalls of the optical fiber, thereby rapidly penetrating the entire interior of the optical fiber. The gas molecules to be tested are uniformly adsorbed on the surface of the mesoscopic fibrous framework of polymethylsilsesquioxane material, which also constitutes the light transmission carrier. At this time, the light transmission channel and the gas adsorption channel of the optical fiber completely overlap, and the fiber core undertakes the dual functions of light transmission and gas enrichment. The light signal propagation process is in full contact with the enriched gas molecules to be tested, effectively improving the enhancement effect of the measured signal (e.g., Raman spectral signal) and improving the detection sensitivity of the gas sensor using the optical fiber.

[0029] In some embodiments, the optical fiber is an integral structure, that is, the optical fiber is integrally formed from the polymethylsilsesquioxane aerogel material.

[0030] In some embodiments, the fiber core is cylindrical, i.e., the optical fiber is cylindrical. The diameter of the fiber core is 0.3 mm to 3 mm, i.e., the diameter of the optical fiber is 0.3 mm to 3 mm. For example, it can be 0.3 mm, 0.5 mm, 0.8 mm, 1 mm, 1.5 mm, 1.8 mm, 2 mm, 2.5 mm, 2.8 mm, 3 mm, etc. This helps to reduce problems such as fiber breakage during the manufacturing process due to the fiber core being too small, or low mechanical strength due to the diameter being too small, making wiring and assembly difficult in practical applications. At the same time, it also helps to avoid problems such as internal pore collapse and decreased light transmittance during the manufacturing process due to the fiber core being too large, which would affect the sensing performance of the sensor when the optical fiber is used in a gas sensor. Preferably, the diameter of the fiber core is 0.5 mm to 1 mm.

[0031] In some embodiments, the length of the fiber core is 2cm to 50cm, that is, the length of the optical fiber is 2cm to 50cm. For example, it can be 2cm, 3cm, 5cm, 6cm, 7cm, 8cm, 9cm, 10cm, 15cm, 20cm, 25cm, 30cm, 40cm, 50cm, etc. This facilitates the docking and assembly of the optical fiber with the optical path when the optical fiber is used in a gas sensor, while avoiding cracking problems caused by uneven stress distribution during the manufacturing process due to an excessively long fiber core. Preferably, the length of the fiber core is 2cm to 10cm.

[0032] In some embodiments, the polymethylsilsesquioxane surface inside the optical fiber has a large number of active sites, which can be loaded with active materials such as metal-organic frameworks (MOFs) and quantum dots to selectively capture and identify specific gases, thus facilitating its application in gas-selective optical fiber sensors.

[0033] Secondly, the present invention provides a method for preparing an optical fiber, comprising: S100, silicon source, first catalyst and water are mixed in a first process to obtain hydrolysate.

[0034] S200, The hydrolysate, surfactant, and water undergo a second mixing treatment to obtain a first precursor solution.

[0035] S300. After the first precursor liquid is cooled, it is mixed with the second catalyst in a third process to obtain the second precursor liquid.

[0036] S400, the capillary mold is inserted into the second precursor liquid, and after gelation treatment, a wet gel fiber core preform is obtained in the capillary mold.

[0037] S500. The wet gel fiber core preform is subjected to aging treatment to obtain a wet gel fiber core.

[0038] S600. The wet gel fiber core is subjected to supercritical carbon dioxide drying treatment to obtain the optical fiber.

[0039] The optical fiber is the optical fiber as described above.

[0040] The optical fiber fabrication method provided by this invention utilizes a capillary mold to directly obtain a cylindrical wet gel core preform, thereby integrally molding the optical fiber as described above. The obtained optical fiber uses polymethylsilsesquioxane aerogel material as the core. By utilizing the suitable refractive index and high total pore volume of polymethylsilsesquioxane aerogel, it can integrally realize the functions of light transmission and gas enrichment. This improves the sensitivity and response speed of gas sensors using this optical fiber, while eliminating the need for additional coatings or other structures for gas adsorption, simplifying the structure of the optical fiber and reducing manufacturing costs.

[0041] Furthermore, the optical fiber preparation method provided by the present invention utilizes the capillary force of the capillary mold to drive the filling of the second precursor liquid, eliminating the need for external pumping equipment. This method is simple to operate and facilitates uniform filling, which is beneficial for the efficient and continuous production of optical fibers.

[0042] In some embodiments, in step S100, the silicon source is selected from methyltrimethoxysilane, the first catalyst is selected from at least one of acetic acid and phosphoric acid, and the water is selected from at least one of deionized water, secondary water, pure water, and ultrapure water.

[0043] In some embodiments, in step S100, after the first catalyst is mixed with water to form an aqueous solution of the first catalyst, the aqueous solution of the first catalyst is mixed with the silicon source, and after the first mixing treatment, the hydrolysate is formed.

[0044] The reaction equation for the hydrolysis of the silicon source catalyzed by the first catalyst is shown in equation (1): (1).

[0045] In some embodiments, the molar ratio of the first catalyst to the silicon source is (0.011 to 0.72):1000, for example, it can be 0.011:1000, 0.012:1000, 0.1:1000, 0.5:1000, 0.72:1000, etc. By controlling the amount of the first catalyst added, sufficient hydrolysis of the silicon source can be achieved to form a suitable silanol oligomer, and excessive first catalyst can be avoided to inhibit the polycondensation of the silicon source.

[0046] In some embodiments, the concentration of the first catalyst in the hydrolysate is from 0.04 mmol / L to 4 mmol / L, for example, it can be 0.04 mmol / L, 0.05 mmol / L, 0.10 mmol / L, 2 mmol / L, 2.2 mmol / L, 2.5 mmol / L, 2.8 mmol / L, 3 mmol / L, etc. By controlling the concentration of the first catalyst, it is beneficial to control the hydrolysis rate of the silicon source and stably form suitable silanol oligomers.

[0047] In some embodiments, when the first catalyst is acetic acid, the concentration of the first catalyst in the hydrolysate is from 1.5 mmol / L to 4 mmol / L, for example, it can be 1.5 mmol / L, 2.5 mmol / L, 3 mmol / L, 3.5 mmol / L, 4 mmol / L, etc.

[0048] In some embodiments, when the first catalyst is phosphoric acid, the concentration of the first catalyst in the hydrolysate is from 0.04 mmol / L to 0.05 mmol / L, for example, it can be 0.04 mmol / L, 0.045 mmol / L, 0.05 mmol / L, etc.

[0049] In some embodiments, in step S100, the first mixing process can be stirring. The temperature of the first mixing process can be 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc., so that the first catalyst can catalyze the silicon source to undergo acid-catalyzed hydrolysis at a suitable temperature to form silanol oligomers, while avoiding excessively high temperatures that could lead to the formation of silanol polymers.

[0050] In some embodiments, in step S100, the first mixing process is stopped when the mixed solution of the silicon source, the first catalyst, and water becomes clear. The duration of the first mixing process can be from 12 minutes to 18 minutes, for example, 12 minutes, 15 minutes, 18 minutes, etc.

[0051] In some embodiments, in step S200, the surfactant is selected from Pluronic F127 type surfactant, which is a poly(ethylene oxide)-b-poly(propylene oxide)-b-poly(ethylene oxide) triblock copolymer. This surfactant is beneficial in assisting the silanol oligomers formed from the silicon source to form a cross-linked gel network with a mesoporous structure during the gelation treatment. In step S200, the addition of water helps control the concentration of the surfactant in the first precursor solution. The water can be selected from at least one of deionized water, deionized water, pure water, and ultrapure water.

[0052] In some embodiments, the mass ratio of the surfactant to the volume of the silicon source is (0.2 to 0.28) g:1 mL, for example, it can be 0.2 g:1 mL, 0.22 g:1 mL, 0.25 g:1 mL, 0.28 g:1 mL, etc., so as to assist the silanol oligomer formed by the silicon source in forming a cross-linked gel network with uniform pore size during the gelation treatment.

[0053] In some embodiments, the concentration of the surfactant in the first precursor solution is from 0.06 g / mL to 0.094 g / mL, for example, it can be 0.06 g / mL, 0.07 g / mL, 0.08 g / mL, 0.09 g / mL, 0.094 g / mL, etc., so as to assist the silanol oligomer formed by the silicon source in forming a cross-linked gel network with uniform pore size during the gelation treatment.

[0054] In some embodiments, the second mixing process can be stirring. The temperature of the second mixing process can be 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc., so that the surfactant can form a stable micelle template at a suitable temperature and adsorb the silanol oligomer.

[0055] In some embodiments, in step S200, the second mixing process is stopped when the mixture of the hydrolysate, surfactant, and water becomes clear. The duration of the second mixing process can be from 50 minutes to 70 minutes, for example, 50 minutes, 55 minutes, 60 minutes, 65 minutes, 70 minutes, etc.

[0056] In some embodiments, in step S300, the cooling treatment can be achieved by subjecting the first precursor liquid to an ice-water bath. The cooling treatment time can be greater than or equal to 30 minutes, for example, 30 minutes, 40 minutes, 50 minutes, 60 minutes, etc., to fully remove microbubbles in the first precursor liquid and prevent the accumulation of microbubbles in the capillary mold, which could form isolated pores or elongated cavities in the wet gel fiber core, affecting the gas adsorption performance of the obtained optical fiber and causing stress concentration, cracks, or even fiber breakage during the supercritical carbon dioxide drying process.

[0057] In some embodiments, the second catalyst includes at least one of tetramethylammonium hydroxide and lithium hydroxide. While neutralizing the first catalyst, the second catalyst adjusts the pH value of the second precursor solution to facilitate the polycondensation of the silanol oligomers formed by the silicon source, thereby forming a polymethylsilsesquioxane aerogel material with a mesoscopic fibrous skeleton.

[0058] The chemical equation for the formation of silanol oligomers from the silicon source by the second catalyst is shown in equation (2): (2).

[0059] In some embodiments, the molar ratio of the second catalyst to the volume of the silicon source is (0.24 to 0.36) mmol:1 mL, for example, 0.2 mmol:1 mL, 0.25 mmol:1 mL, 0.3 mmol:1 mL, etc. By controlling the amount of the second catalyst added, the pH value of the second precursor solution is adjusted within a suitable range while neutralizing the first catalyst, thereby facilitating the condensation polymerization of the silanol oligomers formed by the silicon source at a suitable rate, thereby forming a polymethylsilsesquioxane aerogel material with a mesoscopic fibrous framework. When too much of the second catalyst is added, it easily leads to dissolution-redeposition of the gel framework, resulting in structural coarsening and a significant reduction in the transparency of the resulting optical fiber; when too little of the second catalyst is added, it easily leads to phase separation, and the transparency of the resulting optical fiber is also significantly reduced.

[0060] In some embodiments, the second catalyst is added in the form of an aqueous solution, that is, after the second catalyst is configured as an aqueous solution of the second catalyst, it is mixed with the first precursor solution in a third mixing process to obtain the second precursor solution.

[0061] In some embodiments, the concentration of the aqueous solution of the second catalyst is 0.4 mol / L to 0.6 mol / L, for example, it can be 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, etc., which helps to avoid the problem of local over-concentration caused by direct mixing of the second catalyst and the first precursor solution, premature gelation in some areas, resulting in uneven fiber density and cracking in subsequent supercritical carbon dioxide drying treatment.

[0062] In some embodiments, the third mixing process can be stirring. The temperature of the third mixing process can be 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc., so as to appropriately delay the gelation time and facilitate the timely insertion of the capillary mold into the second precursor liquid.

[0063] In some embodiments, in step S200, the time for the third mixing process can be 20 to 40 seconds, for example, 20 seconds, 25 seconds, 30 seconds, 35 seconds, 40 seconds, etc., so as to achieve sufficient mixing of the second catalyst and the first precursor liquid, minimize the number of bubbles in the second precursor liquid, and allow sufficient time for the timely insertion of the capillary mold into the second precursor liquid and other operations before the gelation process.

[0064] In some embodiments, the inner diameter of the capillary mold is 0.3 mm to 3 mm, for example, it can be 0.3 mm, 0.5 mm, 0.8 mm, 1 mm, 1.5 mm, 1.8 mm, 2 mm, 2.5 mm, 2.8 mm, 3 mm, etc. This helps to reduce the problems of fiber breakage in subsequent preparation steps due to the small diameter of the prepared wet gel fiber core preform, or low mechanical strength due to the small diameter of the prepared optical fiber, making it difficult to wire and assemble in practical applications. At the same time, it also helps to avoid problems such as internal pore collapse and decreased light transmittance in subsequent preparation steps due to the large diameter of the prepared wet gel fiber core preform, which would affect the sensing performance of the sensor when the prepared optical fiber is used in a gas sensor.

[0065] In some embodiments, the length of the capillary mold is 2cm to 50cm, for example, it can be 2cm, 3cm, 5cm, 6cm, 7cm, 8cm, 9cm, 10cm, 15cm, 20cm, 25cm, 30cm, 40cm, 50cm, etc. This is beneficial for the optical fiber to be applied to the gas sensor, making it easier to connect and assemble with the optical path, while avoiding cracking caused by uneven stress distribution in the subsequent preparation process due to the excessive length of the prepared wet gel fiber core preform.

[0066] In some embodiments, the outer diameter of the capillary mold is 0.5 mm to 3.5 mm, for example, it can be 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, etc.

[0067] In some embodiments, the capillary mold is inserted into the second precursor liquid, and the capillary mold draws in the second precursor liquid using capillary action, thereby allowing the second precursor liquid to enter the capillary mold and undergo the gelation treatment within the capillary mold to obtain the wet gel fiber core preform.

[0068] In some embodiments, after the second precursor liquid enters the capillary mold, the container containing the second precursor liquid and the capillary mold is sealed to maintain a stable liquid phase environment during the gelation process. This avoids uneven solvent evaporation and the entry of outside air during the gelation process, which could lead to uneven concentration of the second precursor liquid in the capillary mold and premature gelation in some areas. This is beneficial for the wet gel fiber core preform to be uniformly formed along the length of the capillary mold, and avoids uneven internal pore distribution and local cracking of the wet gel fiber core preform during the forming process.

[0069] like Figure 1 As shown, in some embodiments, the capillary mold 10 is vertically inserted into the second precursor liquid. In the container 20 containing the second precursor liquid and the capillary mold 10, the volume of the second precursor liquid is 60% to 70% of the volume of the container 20, for example, 60%, 62%, 65%, 68%, 70%, etc. This ensures that the second precursor liquid in the container 20 can fully enter a sufficient number of the capillary molds 10, while avoiding overflow due to excessive volume of the second precursor liquid, which would affect the sealing of the container 20. That is, by controlling the volume of the second precursor liquid to 60% to 70% of the volume of the container 20, it is beneficial to form as many wet gel fiber core preforms as possible simultaneously, achieving full utilization of the second precursor liquid and improving the production efficiency of the optical fiber fabrication method.

[0070] In some embodiments, the gelation treatment temperature is 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc., so as to form a uniform primary gel skeleton with suitable cross-linking degree and fewer defects at a slower rate, and at the same time, it is more conducive to suppressing phase separation and improving the transparency and uniformity of the resulting optical fiber.

[0071] In some embodiments, the gelation treatment time is greater than or equal to 0.5 hours and less than or equal to 2 hours, for example, it can be 0.5 hours, 1 hour, 1.5 hours, 2 hours, etc., so as to allow the second precursor liquid to fully gel in the capillary mold, avoiding convection and bubbles in the capillary due to incomplete gelation of the second precursor liquid in the capillary, which would affect the gas adsorption performance of the resulting optical fiber and cause stress concentration, cracks, or even optical fiber breakage during the supercritical carbon dioxide drying process. Preferably, the gelation treatment time is greater than 1 hour and less than or equal to 2 hours, so as to allow the second precursor liquid to fully and uniformly gel in the capillary mold.

[0072] In some embodiments, when the temperature of the gelation treatment is increased to the temperature of the aging treatment, the heating rate is from 0.5℃ / min to 2℃ / min, for example, it can be 0.5℃ / min, 1℃ / min, 1.2℃ / min, 1.5℃ / min, 2℃ / min, etc., so as to ensure that the wet gel fiber core preform is heated stably, avoids the generation of bubbles in the capillary mold due to excessive heating, and helps to avoid local overheating caused by excessive heating, and avoids the loss of control of local polycondensation rate, thereby helping to avoid a decrease in the overall consistency of the obtained optical fiber.

[0073] In some embodiments, when the temperature of the gelation treatment is increased to the temperature of the aging treatment, the temperature can be increased to 40°C at a rate of 0.5°C / min to 2°C / min, and then increased to the temperature of the aging treatment at a rate of 0.5°C / min to 2°C / min, so as to fully avoid the generation of bubbles in the capillary mold.

[0074] In some embodiments, when the aging treatment temperature is greater than 60°C and less than or equal to 80°C, when the temperature of the gelation treatment is increased to the aging treatment temperature, the temperature is increased to 40°C at a heating rate of 0.5°C / min to 2°C / min, and then the temperature can be held at 40°C for 1 to 2 hours to further avoid the formation of bubbles.

[0075] In some embodiments, the capillary mold can be uniformly heated by means of a water bath, oil bath, etc., so that the primary gel in the capillary mold is heated evenly, the resulting wet gel fiber core has a uniform pore size distribution in the length direction, and cracks are avoided.

[0076] In some embodiments, uniform heating of the capillary mold can also be achieved by placing a heating rod inside the container containing the second precursor liquid and the capillary mold. For example, a heating copper rod can be inserted into the gel formed by the second precursor liquid outside the capillary mold.

[0077] In some embodiments, the aging treatment temperature is between 40°C and 80°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, etc., to promote the continued condensation reaction of unreacted silanol groups within the primary cross-linking network of the gel, enhancing the compactness of the cross-linking network, improving the elasticity of the obtained optical fiber, and simultaneously suppressing the shrinkage rate of the polymethylsilsesquioxane aerogel, appropriately increasing the specific surface area of ​​the obtained wet gel fiber core, so as to obtain an optical fiber with suitable total pore volume, specific surface area, and average pore size, reducing light scattering caused by pore inhomogeneity, and improving the transparency of the obtained optical fiber. Preferably, the aging treatment temperature is greater than or equal to 40°C and less than 60°C.

[0078] In some embodiments, the aging treatment time is greater than or equal to 24 hours and less than 72 hours to obtain a wet gel fiber core with suitable total pore volume, specific surface area, and average pore size. Preferably, the aging treatment time is greater than or equal to 24 hours and less than or equal to 36 hours.

[0079] In some embodiments, after the aging treatment is completed, the wet gel fiber core can be cooled to room temperature at a cooling rate of 0.5℃ / min to 2℃ / min (e.g., 0.5℃ / min, 1℃ / min, 1.5℃ / min, 2℃ / min, etc.).

[0080] In some embodiments, prior to the supercritical carbon dioxide drying process, the wet gel fiber core also undergoes a demolding process, which includes: After being cleaned, the capillary mold is placed in water, and the wet gel fiber core is pushed out of the capillary mold using an ejector pin.

[0081] The difference between the inner diameter of the capillary mold and the diameter of the ejector pin is greater than or equal to 0.1 mm and less than or equal to 0.2 mm.

[0082] In some embodiments, the cleaning process may be to remove gel adhering to the surface of the capillary mold underwater. The water used in the demolding process may be selected from at least one of deionized water, pure water, and ultrapure water.

[0083] In some embodiments, the difference between the inner diameter of the capillary mold and the diameter of the ejector pin can be 0.1 mm, 0.15 mm, 0.2 mm, etc., so as to facilitate the complete ejection of the wet gel fiber core while avoiding cracks, breaks or surface damage caused by insufficient contact area with the wet gel fiber core or uneven force on the end face of the wet gel fiber core.

[0084] In some embodiments, the capillary mold can be made of a material with low surface energy, low coefficient of friction, and that does not react with the second precursor liquid. For example, the capillary mold can be made of polytetrafluoroethylene.

[0085] In some embodiments, prior to the gelation treatment, the inner wall of the capillary mold may be pre-coated with a layer of silicone oil or paraffin wax to facilitate the demolding process. When the inner wall of the capillary mold is coated with paraffin wax, the paraffin wax can be melted by heating before the demolding process to facilitate the demolding process.

[0086] In some embodiments, the wet gel fiber core that has undergone the demolding treatment is further subjected to a solvent replacement treatment before the supercritical carbon dioxide drying treatment, the solvent replacement treatment comprising: The wet gel fiber core is subjected to solvent replacement treatment using gradient solvents, a second solvent, and a third solvent in sequence.

[0087] In some embodiments, the gradient solvent includes water and an organic solvent, wherein the water in the gradient solvent is selected from at least one of deionized water, pure water, and ultrapure water. The organic solvent is selected from at least one of methanol, ethanol, and isopropanol. The second solvent and the third solvent are each independently selected from at least one of methanol, ethanol, and isopropanol, wherein the second solvent is the same as the organic solvent, and the third solvent is different from the second solvent.

[0088] In some embodiments, the gradient solvent includes a first gradient sub-solvent with a water-to-organic solvent volume ratio of (95 to 90):(5 to 10), a second gradient sub-solvent of (85 to 70):(15 to 30), a third gradient sub-solvent of (65 to 50):(35 to 50), a fourth gradient sub-solvent of (15 to 30):(70 to 85), and a fifth gradient sub-solvent of (5 to 10):(90 to 95). The volume percentage of the organic solvent gradually increases from the first gradient sub-solvent to the fifth gradient sub-solvent.

[0089] In some embodiments, the displacement time of the wet gel fiber core in each gradient sub-solvent is greater than or equal to 12 hours to ensure sufficient solvent displacement and avoid liquid residue caused by incomplete solvent displacement during the supercritical carbon dioxide drying process. This residue can lead to capillary forces causing shrinkage and collapse, reducing the specific surface area of ​​the resulting optical fiber, or even causing cracking. When the diameter of the wet gel fiber core is greater than 0.5 mm and less than or equal to 3 mm, the displacement time of the wet gel fiber core in each gradient sub-solvent is greater than or equal to 14 hours.

[0090] In some embodiments, the second solvent is replaced more than or equal to 3 times, for example, 3, 5, 6, 8 times, etc. The third solvent is replaced more than or equal to 3 times, for example, 3, 5, 6, 8 times, etc. The replacement time of the wet gel fiber core in each of the second solvents is greater than or equal to 12 hours, and the replacement time of the wet gel fiber core in each of the third solvents is greater than or equal to 12 hours, to ensure sufficient solvent replacement and avoid liquid residue caused by incomplete solvent replacement during the supercritical carbon dioxide drying process, which could lead to capillary forces causing shrinkage and collapse, reducing the specific surface area of ​​the resulting optical fiber, or even causing cracking of the optical fiber. When the diameter of the wet gel fiber core is greater than 0.5 mm and less than or equal to 3 mm, the replacement time of the wet gel fiber core in each of the second solvents is greater than or equal to 14 hours, and the replacement time of the wet gel fiber core in each of the third solvents is greater than or equal to 14 hours.

[0091] In some embodiments, the temperature of the solvent replacement treatment is 20°C to 30°C, for example, it can be 20°C, 25°C, 30°C, etc.

[0092] In some embodiments, step S600 includes: S610. In supercritical carbon dioxide, the wet gel fiber core is dried under drying pressure and temperature for a certain time to obtain the optical fiber.

[0093] In some embodiments, the drying pressure is 8 MPa to 9 MPa, for example, 8 MPa, 8.5 MPa, 9 MPa, etc. The drying temperature is 35°C to 40°C, for example, 35°C, 36°C, 38°C, 40°C, etc.

[0094] In some embodiments, the drying time is greater than or equal to 4 hours and less than or equal to 12 hours, for example, it can be 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, etc. When the diameter of the wet gel fiber core is greater than or equal to 0.3 mm and less than or equal to 0.5 mm, the drying time can be 4 to 7 hours; when the diameter of the wet gel fiber core is greater than 0.5 mm and less than or equal to 3 mm, for every 0.5 mm increase in diameter, the drying time is increased by 1 to 2 hours based on the drying time for the diameter of the wet gel fiber core greater than or equal to 0.3 mm and less than or equal to 0.5 mm. When the diameter of the wet gel fiber core is greater than 0.5 mm and less than or equal to 3 mm, the drying time of the wet gel fiber core is greater than 7 hours and less than or equal to 12 hours.

[0095] In some embodiments, the supercritical carbon dioxide drying process is carried out in an autoclave. The pressurization rate to reach the drying pressure is 6500 psi / h to 7500 psi / h, for example, 6500 psi / h, 7000 psi / h, 7500 psi / h, etc. By controlling the pressurization rate, while ensuring equipment operating efficiency, the process of carbon dioxide entering the pores of the wet gel fiber core is made more gradual, avoiding the formation of violent pressure shocks and effectively protecting the integrity of the resulting optical fiber skeleton. If a higher pressurization rate is used for rapid pressurization, the high-speed carbon dioxide gas flow is prone to causing mechanical erosion damage to the wet gel fiber core; at the same time, the compression heat generated by rapid compression will cause uneven temperature distribution within the autoclave, which is not conducive to the uniform formation of a stable supercritical fluid environment within the autoclave.

[0096] In some embodiments, after the supercritical carbon dioxide drying process is completed, the depressurization rate is greater than 0 psi / h and less than or equal to 70 psi / h, for example, it can be 1 psi / h, 10 psi / h, 20 psi / h, 30 psi / h, 50 psi / h, 70 psi / h, etc. By controlling the depressurization rate, it is beneficial to balance the internal and external pressures of the optical fiber's pores during the depressurization process, thus protecting the optical fiber and preventing problems such as fiber breakage and pore structure collapse caused by excessive capillary force due to an excessively high depressurization rate.

[0097] The technical solution of the present invention will be further described in detail below with reference to specific embodiments.

[0098] Example 1 like Figure 1 As shown, the optical fiber fabrication method provided in this embodiment is as follows: (1) Mix 2.5 mL of methyltrimethoxysilane with 2.5 mL of 5 mM dilute acetic acid aqueous solution and stir continuously at room temperature for 15 minutes until the solution is clear, so that methyltrimethoxysilane undergoes acid-catalyzed hydrolysis to generate silanol oligomers and obtain hydrolysate.

[0099] (2) Add 0.55g of Pluronic F127 surfactant and 2.5mL of deionized water to the above hydrolysate, stir at room temperature for 1 hour until the solution is clear, and obtain the first precursor solution.

[0100] (3) After cooling the first precursor solution in an ice bath for 30 minutes, add 1.5 mL of 0.5 M strong base catalyst tetramethylammonium hydroxide aqueous solution, mix and stir for 20 s, insert the capillary mold into the sol, and use capillary effect to draw in the solution. Seal and gel at room temperature for 1 h. Then, use water bath heating to raise the temperature to 50 °C at a rate of 1.5 °C / min and continue aging for 24 hours to obtain a wet gel fiber core with a diameter of 1 mm and a length of 8 cm. Cool to room temperature at a rate of 1.2 °C / min.

[0101] (4) Place the capillary mold in deionized water, remove the gel from the surface of the capillary mold below the liquid surface, and place it in another layer of deionized water. Use an ejector pin with a diameter 0.15 mm smaller than the capillary mold to push the wet gel fiber core out of the capillary mold in the deionized water. At room temperature, place the wet gel fiber core sequentially in the first sub-gradient solvent, the second sub-gradient solvent, the third sub-gradient solvent, the fourth sub-gradient solvent, and the fifth sub-gradient solvent for solvent replacement. The volume ratio of deionized water to analytical grade methanol in the first sub-gradient solvent is 90:10, the volume ratio of deionized water to analytical grade methanol in the second sub-gradient solvent is 70:30, the volume ratio of deionized water to analytical grade methanol in the third sub-gradient solvent is 50:50, the volume ratio of deionized water to analytical grade methanol in the fourth sub-gradient solvent is 30:70, and the volume ratio of deionized water to analytical grade methanol in the fifth sub-gradient solvent is 10:90. The replacement time of the wet gel fiber core in each sub-gradient solvent is 12 hours. Subsequently, the wet gel fiber core was placed in analytical grade methanol at room temperature, with the methanol being replaced 5 times, and the replacement time for the wet gel fiber core in each batch of analytical grade methanol was 12 hours. Finally, the wet gel fiber core was placed in analytical grade isopropanol at room temperature, with the isopropanol being replaced 3 times, and the replacement time for the wet gel fiber core in each batch of analytical grade isopropanol was 12 hours.

[0102] (5) The wet gel fiber core was subjected to supercritical carbon dioxide drying to obtain optical fiber. The drying temperature was 38℃, the drying time was 10 hours, and the drying pressure was 9.3 MPa. The pressure increase rate to reach this drying pressure was 7000 psi / h. After the supercritical carbon dioxide drying was completed, the pressure was reduced to atmospheric pressure at a rate of 70 psi / h to obtain optical fiber. The actual optical fiber is shown in the figure. Figure 3 and Figure 4 As shown.

[0103] Example 2 This embodiment is similar to Embodiment 1, except that in step (3), 1.5 mL of 0.5 M strong base catalyst tetramethylammonium hydroxide aqueous solution is added, and after mixing and stirring for 30 s, the capillary mold is inserted into the sol.

[0104] Example 3 This embodiment is similar to Embodiment 1, except that in step (3), 1.5 mL of 0.5 M strong base catalyst tetramethylammonium hydroxide aqueous solution is added, and after mixing and stirring for 40 s, the capillary mold is inserted into the sol.

[0105] Example 4 This embodiment is similar to Embodiment 1, except that in step (3), the solution is drawn in by capillary action, sealed, and gelled at room temperature for 1 hour. Then, an oil bath heating method is used to raise the temperature to 40°C at a rate of 0.5°C / min. After aging for 24 hours, the temperature is lowered to room temperature at a rate of 0.4°C / min.

[0106] Example 5 This embodiment is similar to Embodiment 1, except that in step (3), the solution is drawn in by capillary action, sealed, and gelled at room temperature for 1 hour. Then, a water bath heating method is used, and a copper rod is inserted into the gel inside the container containing the capillary mold and outside the capillary mold. The temperature is increased to 80°C at a rate of 2°C / min. After aging for 24 hours, the temperature is reduced to room temperature at a rate of 2°C / min.

[0107] Example 6 The optical fiber fabrication method provided in this embodiment is as follows: (1) Mix 2.5 mL of methyltrimethoxysilane with 2.5 mL of 0.08 mM dilute phosphoric acid aqueous solution and stir continuously at 20 °C for 18 minutes until the solution is clear, so that methyltrimethoxysilane undergoes acid-catalyzed hydrolysis to generate silanol oligomers and obtain hydrolysate.

[0108] (2) Add 0.5g of Pluronic F127 surfactant and 2.5mL of deionized water to the above hydrolysate, stir at 20°C for 70 minutes until the solution is clear to obtain the first precursor solution.

[0109] (3) After cooling the first precursor solution in an ice bath for 40 minutes, add 1.5 mL of 0.4 M strong base catalyst tetramethylammonium hydroxide aqueous solution, mix and stir for 20 s, insert the capillary mold into the sol, and use capillary effect to draw in the solution. Seal and gel at room temperature for 1 h. Then, use water bath heating to raise the temperature to 50 °C at a rate of 2 °C / min and continue aging for 36 hours to obtain a wet gel fiber core with a diameter of 0.3 mm and a length of 2 cm. Cool to room temperature at a rate of 2 °C / min.

[0110] (4) Place the capillary mold in deionized water, remove the gel from the surface of the capillary mold below the liquid surface, and place it in another layer of deionized water. Use an ejector pin with a diameter 0.1 mm smaller than the capillary mold to push the wet gel fiber core out of the capillary mold in the deionized water. At 20°C, place the wet gel fiber core sequentially in the first, second, third, fourth, and fifth sub-gradient solvents for solvent replacement. The volume ratio of deionized water to analytical grade ethanol in the first sub-gradient solvent is 95:5, in the second sub-gradient solvent it is 85:15, in the third sub-gradient solvent it is 65:35, in the fourth sub-gradient solvent it is 30:70, and in the fifth sub-gradient solvent it is 5:95. The replacement time of the wet gel fiber core in each sub-gradient solvent is 12 hours. Subsequently, at 20°C, the wet gel fiber core was placed in analytical grade ethanol, with the ethanol being replaced 6 times, and the replacement time for the wet gel fiber core in each ethanol solution was 12 hours. Finally, at 20°C, the wet gel fiber core was placed in analytical grade methanol, with the methanol being replaced 4 times, and the replacement time for the wet gel fiber core in each methanol solution was 12 hours.

[0111] (5) The wet gel fiber core was subjected to supercritical carbon dioxide drying to obtain optical fiber. The drying temperature was 35℃, the drying time was 4 hours, the drying pressure was 9MPa, and the pressure increase rate to reach this drying pressure was 6500psi / h. After the supercritical carbon dioxide drying was completed, the pressure was reduced to atmospheric pressure at a rate of 50psi / h.

[0112] Example 7 (1) Mix 2.5 mL of methyltrimethoxysilane with 2.5 mL of 0.10 mM dilute phosphoric acid aqueous solution and stir continuously at 30 °C for 12 minutes until the solution is clear, so that methyltrimethoxysilane undergoes acid-catalyzed hydrolysis to generate silanol oligomers and obtain hydrolysate.

[0113] (2) Add 0.7g of Pluronic F127 surfactant and 2.5mL of deionized water to the above hydrolysate, stir at 30°C for 50 minutes until the solution is clear to obtain the first precursor solution.

[0114] (3) After cooling the first precursor solution in an ice bath for 45 minutes, add 1.5 mL of 0.6 M strong base catalyst tetramethylammonium hydroxide aqueous solution, mix and stir for 20 s, insert the capillary mold into the sol, and use capillary effect to draw in the solution. Seal and gel at room temperature for 1 h. Then use water bath heating to raise the temperature to 50 °C at a rate of 2 °C / min and continue aging for 48 hours to obtain a wet gel fiber core with a diameter of 3 mm and a length of 50 cm. Cool to room temperature at a rate of 2 °C / min.

[0115] (4) Place the capillary mold in deionized water, remove the gel from the surface of the capillary mold below the liquid surface, and place it in another layer of deionized water. Use an ejector pin with a diameter 0.2 mm smaller than the capillary mold to push the wet gel fiber core out of the capillary mold in the deionized water. At 30°C, place the wet gel fiber core sequentially in the first, second, third, fourth, and fifth sub-gradient solvents for solvent replacement. The volume ratio of deionized water to analytical grade methanol in the first sub-gradient solvent is 95:5, in the second sub-gradient solvent it is 80:20, in the third sub-gradient solvent it is 60:40, in the fourth sub-gradient solvent it is 20:80, and in the fifth sub-gradient solvent it is 8:92. The replacement time of the wet gel fiber core in each sub-gradient solvent is 14 hours. Subsequently, at 30°C, the wet gel fiber core was placed in analytical grade methanol, with the methanol being replaced 5 times, and the replacement time for the wet gel fiber core in each batch of analytical grade methanol was 14 hours. Finally, at 30°C, the wet gel fiber core was placed in analytical grade ethanol, with the ethanol being replaced 3 times, and the replacement time for the wet gel fiber core in each batch of analytical grade ethanol was 14 hours.

[0116] (5) The wet gel fiber core was subjected to supercritical carbon dioxide drying to obtain optical fiber. The drying temperature was 40℃, the drying time was 12 hours, the drying pressure was 8MPa, and the pressure increase rate to reach this drying pressure was 7500psi / h. After the supercritical carbon dioxide drying was completed, the pressure was reduced to atmospheric pressure at a rate of 40psi / h.

[0117] Comparative Example 1 This comparative example is similar to Example 1, except that in step (3), 1.5 mL of 0.5 M strong base catalyst tetramethylammonium hydroxide aqueous solution is added, and after mixing and stirring for 10 s, the capillary mold is inserted into the sol.

[0118] Comparative Example 2 This comparative example is similar to Example 1, except that in step (3), 1.5 mL of 0.5 M strong base catalyst tetramethylammonium hydroxide aqueous solution is added, and after mixing and stirring for 1 minute, the capillary mold is inserted into the sol.

[0119] Comparative Example 3 This comparative example is similar to Example 1, except that in step (3), the heating method of the electric heating plate is used to raise the temperature to 50°C at a rate of 2°C / min, and continue aging for 24 hours.

[0120] Comparative Example 4 This comparative example is similar to Example 1, except that in step (3), the solution is drawn in by capillary action, sealed, and gelled at room temperature for 1 hour. Then, the temperature is increased to 50°C at a rate of 5°C / min and aged for 24 hours. Finally, the temperature is decreased to room temperature at a rate of 5°C / min.

[0121] The optical fibers obtained in the above embodiments and comparative examples were tested for performance in terms of refractive index, visible light transmittance, optical loss per unit length, specific surface area, total aperture volume at a single point, and average aperture. The results are shown in Table 1.

[0122] The method for testing refractive index is as follows: When a 532nm monochromatic light is shone on the side of the optical fiber, the refractive index is calculated using the minimum deviation angle method according to the formula shown in equation (3), where A is the aerogel angle between the incident ray and the outgoing optical fiber. Minimum deviation angle: (3).

[0123] The numerical aperture calculation method is shown in equation (4): (4).

[0124] Since the optical fibers obtained in the embodiments and comparative examples have no solid cladding and the outer medium is air, with an air refractive index n2=1.0003, the air refractive index and the refractive index of the optical fiber measured by the method described above are substituted into the formula shown above as n1 to obtain the numerical aperture of the optical fiber.

[0125] The method for testing optical loss per unit length is as follows: Fix one end of the fiber of length L1 to the output port of the laser, keep the incident light power constant, align the other end of the aerogel fiber with the optical power meter probe, and record the optical power meter reading P1 at this time; keep the light source position and input power unchanged, precisely cut off 1.5cm of length so that the remaining length of the aerogel fiber becomes L2, keep the incident end of the aerogel fiber exactly the same as the first measurement, and record the optical power P2 at this time; calculate the optical loss per unit length according to formula (5): (5).

[0126] Specific surface area, total pore volume at a single point, and average pore size were obtained using the nitrogen adsorption-desorption (BET) method. The BET testing procedure was as follows: equal amounts of optical fiber samples were pretreated under vacuum at 120℃ for 6 hours to remove adsorbed water vapor and impurities from the sample pores. A 77K nitrogen adsorption-desorption analyzer was used to quantitatively test the pore structure. Specific surface area was calculated using the BET model, and pore size distribution and average pore size were calculated using the BJH model.

[0127] Table 1 Performance test results of optical fibers in the examples and comparative examples

[0128] like Figure 3 and Figure 4 As shown, the optical fiber obtained in Example 1 has high visible light transmittance and is intact with no penetrating macroscopic cracks. Figure 4 , Figures 6 to 7 As shown, the optical fiber obtained in Example 1 has good bending resistance, and at the same time, as Figures 5 to 7 As shown, the optical fiber obtained in Example 1 has good light guiding performance.

[0129] As shown in Table 1, the results of Examples 1 to 3, Comparative Example 1 and Comparative Example 2 indicate that after adding the strong base catalyst tetramethylammonium hydroxide aqueous solution (second catalyst), the mixing and stirring time is controlled to be 20 to 40 seconds. This achieves thorough mixing of the second catalyst and the first precursor liquid while reducing the number of bubbles in the second precursor liquid, thereby effectively improving the performance of the obtained optical fiber in terms of gas adsorption and light transmission. This is more conducive to obtaining optical fibers with higher specific surface area, higher total pore volume at a single point, more suitable average aperture, more suitable refractive index and lower optical loss.

[0130] As can be seen from the results in Table 1 of Examples 1, 4 to 5 and Comparative Example 3, using a more uniform heating method such as a water bath or oil bath during the process of heating from the temperature of gelation treatment to the temperature of aging treatment is more conducive to reducing the generation of bubbles during the heating process, thereby making it more conducive to obtaining optical fibers with higher specific surface area, higher total pore volume at a single point, more suitable average pore size, more suitable refractive index and lower optical loss.

[0131] As can be seen from the results in Table 1 of Example 1 and Comparative Example 4, during the process of heating from the temperature of gelation treatment to the temperature of aging treatment, the excessively rapid heating rate is prone to cause uneven heating, resulting in local overheating, which leads to the uncontrolled local condensation rate of the gel. The polymethylsilsesquioxane skeleton of the obtained optical fiber is uneven, which leads to a significant decrease in the performance of the obtained optical fiber in terms of gas adsorption and optical transmission.

[0132] As can be seen from the results in Table 1 of Examples 1 to 7, the optical fiber prepared by the optical fiber preparation method proposed in this invention, using polymethylsilsesquioxane aerogel material as the fiber core, has a high specific surface area, a high total pore volume at a single point, a suitable average pore size, a suitable refractive index, and low optical loss. It integrates optical transmission and gas enrichment functions, improves the sensitivity and response speed of gas sensors using this optical fiber, and eliminates the need for additional coatings or other structures used for gas adsorption, simplifying the structure of the optical fiber and reducing manufacturing costs.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An optical fiber, characterized in that, include: The fiber core is made of polymethylsilsesquioxane aerogel material; The refractive index of the fiber core is between 1.02 and 1.04, and the total pore volume at a single point in the fiber core is 1.1 cm. 3 / g to 1.21cm 3 / g.

2. The optical fiber as described in claim 1, characterized in that, The optical fiber further includes a cladding layer, which covers the surface of the fiber core, and the cladding layer is air; The optical fiber has a numerical aperture of 0.21 to 0.27 and a fiber core optical loss per unit length of 1.37 dB / cm to 1.97 dB / cm.

3. The optical fiber as described in any one of claims 1 or 2, characterized in that, The specific surface area of ​​the fiber core is 360m². 2 / g to 500m 2 / g, the average pore size of the fiber core is 10.2nm to 14nm.

4. A method for fabricating an optical fiber, characterized in that, include: The silicon source, the first catalyst, and water undergo a first mixing treatment to obtain a hydrolysate; The hydrolysate is mixed with surfactant and water in a second process to obtain a first precursor solution; After the first precursor liquid is cooled, it is mixed with the second catalyst in a third process to obtain the second precursor liquid. The capillary mold is inserted into the second precursor liquid and undergoes gelation treatment to obtain a wet gel fiber core preform in the capillary mold. The wet gel fiber core preform is subjected to aging treatment to obtain a wet gel fiber core; The wet gel fiber core is subjected to supercritical carbon dioxide drying to obtain the optical fiber; The optical fiber is the optical fiber as described in any one of claims 1 to 3.

5. The method for preparing optical fiber as described in claim 4, characterized in that, The inner diameter of the capillary mold is 0.3 mm to 3 mm, and the length of the capillary mold is 2 cm to 50 cm.

6. The method for preparing optical fiber as described in claim 4, characterized in that, The cooling process takes 20 to 40 seconds. The gelation treatment temperature is 20°C to 30°C, and the gelation treatment time is greater than or equal to 0.5 hours and less than or equal to 2 hours.

7. The method for preparing optical fiber as described in claim 4, characterized in that, The aging treatment temperature is 40°C to 80°C, and the aging treatment time is greater than or equal to 24 hours and less than 72 hours. The heating rate from the gelation treatment temperature to the aging treatment temperature is 0.5℃ / min to 2℃ / min.

8. The method for preparing optical fiber as described in claim 4, characterized in that, Prior to the supercritical carbon dioxide drying process, the wet gel fiber core also undergoes a demolding process, which includes: After the capillary mold is cleaned, it is placed in water, and the wet gel fiber core is pushed out of the capillary mold using an ejector pin. The difference between the inner diameter of the capillary mold and the diameter of the ejector pin is greater than or equal to 0.1 mm and less than or equal to 0.2 mm.

9. The method for preparing optical fiber as described in claim 4, characterized in that, The step of obtaining the optical fiber by subjecting the wet gel fiber core to supercritical carbon dioxide drying includes: The wet gel fiber core is dried under supercritical carbon dioxide for a specified time under drying pressure and temperature to obtain the optical fiber. The drying pressure is 8 MPa to 9 MPa, the drying temperature is 35°C to 40°C, and the drying time is greater than or equal to 4 hours and less than or equal to 12 hours.

10. The method for preparing optical fiber as described in claim 4, characterized in that, The silicon source is selected from methyltrimethoxysilane, the first catalyst is selected from at least one of acetic acid and phosphoric acid, the surfactant is selected from Pluronic F127 type surfactant, and the second catalyst includes at least one of tetramethylammonium hydroxide and lithium hydroxide. The molar ratio of the first catalyst to the silicon source is (0.011-0.72):1000; In the hydrolysate, the concentration of the first catalyst is from 0.04 mmol / L to 4 mmol / L; In the first precursor solution, the concentration of the surfactant is from 0.06 g / mL to 0.094 g / mL; The ratio of the amount of the second catalyst to the volume of the silicon source is (0.24 to 0.36) mmol:1 mL.