Light coupling structure of an LED array and a fiber array and method of manufacturing the same

By setting opaque isolation sidewalls in the bottom silicon layer of SOI wafers to separate the optical transmission channels of LED arrays and fiber arrays, the stray light crosstalk problem is solved, and efficient optical coupling and thermal management are achieved.

CN123136831APending Publication Date: 2026-11-20上海曜感科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611348671.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing optical coupling structures of LED arrays and fiber arrays, stray light cannot be effectively suppressed, optical crosstalk between adjacent channels is severe, and there is a lack of end-to-end optical isolation and physical isolation structures.

Method used

An opaque isolation sidewall is set in the bottom silicon of the SOI wafer, extending from the gap between the light-emitting units to the upper surface of the bottom silicon, separating the light transmission channel into independent sub-channels, and filling the isolation sidewall with thermally conductive metal material to achieve full-process optical isolation and thermal management.

Benefits of technology

It achieves end-to-end optical isolation from the light source to the optical fiber, controls crosstalk between adjacent channels to below -40dB, reduces thermal crosstalk, and improves optical coupling efficiency and heat dissipation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123136831A_ABST
    Figure CN123136831A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of optoelectronic packaging, and particularly relates to an LED array and optical fiber array optical coupling structure and a manufacturing method thereof. The structure comprises: an SOI wafer, a light fiber lead-in groove array is arranged in the top layer silicon of the SOI wafer, the light fiber lead-in groove array is used for accommodating optical fibers, and a light-proof isolation side wall array is arranged in the bottom layer silicon; an LED array core particle comprises a plurality of light emitting units, is bonded to the bottom layer silicon lower surface of the SOI wafer, and the light emitting direction of each light emitting unit is towards the SOI wafer; and the light-proof isolation side wall array extends longitudinally from the area between adjacent light emitting units to the upper surface of the bottom layer silicon. According to the application, the light-proof isolation side wall extending from the area between adjacent light emitting units to the upper surface of the bottom layer silicon of the SOI wafer is arranged in the bottom layer silicon of the SOI wafer, the light transmission channel between each light emitting unit and the optical fiber is divided into independent sub-channels, full-path light isolation from the light source to the optical fiber is realized, and light crosstalk between channels is fundamentally inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optoelectronic packaging, specifically to an optical coupling structure for an LED array and an optical fiber array, and its manufacturing method. Background Technology

[0002] The optical coupling structure of LED arrays and fiber optic arrays is widely used in optical communication, optical interconnection and other fields. In the optical transmitter module, multiple LED light-emitting units are arranged in an array, and the emitted light from each light-emitting unit needs to be coupled to the corresponding optical fiber to achieve multi-channel parallel optical transmission. With the continuous increase in channel density and data rate, the problem of optical crosstalk between adjacent channels has become increasingly prominent. Specifically, a portion of the emitted light with a large divergence angle (usually greater than 60°) from the light-emitting unit enters the optical fiber of the adjacent channel, resulting in signal crosstalk and a decrease in signal-to-noise ratio, becoming one of the key factors restricting system performance.

[0003] Existing technologies include bonding LED array chips to silicon wafers and forming fiber guide grooves within the silicon wafer to accommodate the optical fiber. For example, some solutions integrate the LED array chips and driver chips and bond them integrally to the silicon wafer. Furthermore, beam-shaping structures such as V-shaped reflectors and microlenses are fabricated on the bottom layer of the silicon wafer. This beam-shaping compresses the large divergence angle of the LED's emitted light, thereby improving fiber coupling efficiency. While this approach improves optical coupling performance to some extent, it still has shortcomings in suppressing optical crosstalk between adjacent channels. (1) The beam shaping structure can only compress the main lobe divergence angle of the emitted light, but it cannot effectively suppress the large-angle stray light emitted from the LED sidewall, as well as the stray light that deviates from the main optical path after multiple reflections. These stray lights propagate laterally inside the silicon wafer and are prone to entering the optical fibers of adjacent channels to form crosstalk.

[0004] (2) The beam shaping structure is located at the bottom layer of the silicon wafer and only focuses the beam near the fiber receiver, failing to achieve full optical path control from the LED light-emitting unit to the fiber receiver. Stray light has sufficient space to diffuse laterally during its propagation from the LED light output port to the beam shaping structure.

[0005] (3) There is no effective physical isolation structure between adjacent channels. The light transmission areas of each channel are interconnected inside the silicon wafer, which cannot fundamentally block the cross-channel propagation path of stray light.

[0006] To address the above problems, this invention provides an optical coupling structure for an LED array and an optical fiber array, and a method for manufacturing the same. Summary of the Invention

[0007] This invention aims to overcome the problems in existing optical coupling structures for LED arrays and fiber optic arrays, such as the inability of surface light-blocking structures to effectively intercept stray light inside the silicon substrate, and the inability to achieve end-to-end optical isolation due to only localized installations. It provides an optical coupling structure for LED arrays and fiber optic arrays and its manufacturing method. This invention achieves end-to-end optical isolation from the light source to the optical fiber by setting opaque isolation sidewalls extending from the gaps between light-emitting units to the upper surface of the bottom silicon layer of the SOI wafer. The crosstalk between adjacent channels can be controlled below -40dB.

[0008] To address the above problems, this invention provides an optical coupling structure for an LED array and an optical fiber array, comprising: SOI wafers have an array of fiber optic inlet grooves in the top silicon layer to accommodate optical fibers, and an array of opaque isolation sidewalls in the bottom silicon layer. The LED array chip includes multiple light-emitting units, which are bonded to the bottom silicon surface of the SOI wafer, and the light emission direction of each light-emitting unit is towards the SOI wafer; An opaque isolation sidewall array extends longitudinally from the region between adjacent light-emitting units to the upper surface of the underlying silicon, dividing the light transmission channel between each light-emitting unit and each optical fiber guide groove into multiple independent sub-channels. An optical fiber array is disposed in the optical fiber guide groove array, with the optical receiving end of each optical fiber located at the end of each sub-channel; The emitted light from each of the light-emitting units is transmitted in the corresponding sub-channel and enters the corresponding optical fiber through the corresponding optical fiber guide groove.

[0009] Optionally, an isolation groove is provided between adjacent light-emitting units, at least a portion of the opaque isolation sidewall is filled in the isolation groove, and the isolation groove penetrates at least a portion of the thickness of the LED array chip, for providing electrical and optical isolation between adjacent light-emitting units.

[0010] Optionally, at least a portion of the opaque isolation sidewall is made of a thermally conductive metal material, and the opaque isolation sidewall extends upward from the bottom silicon of the SOI wafer to the gap between adjacent light-emitting units, for conducting the heat generated by the adjacent light-emitting units along the opaque isolation sidewall to the SOI wafer.

[0011] Optionally, the thermally conductive metal material is copper, tungsten, nickel, aluminum, silver, gold, or an alloy thereof.

[0012] Optionally, an optical waveguide layer or an anti-reflection film layer is provided on the inner wall surface of each of the sub-channels. The optical waveguide layer or anti-reflection film layer is used to restrict the emitted light of each of the light-emitting units within each of the sub-channels, so that the emitted light propagates to the corresponding optical fiber.

[0013] A method for manufacturing an optical coupling structure between an LED array and an optical fiber array includes the following steps: An SOI wafer is provided, wherein the SOI wafer comprises, from bottom to top, a bottom silicon layer, a buried oxide layer and a top silicon layer; An array of fiber guide grooves is formed in the top silicon layer of the SOI wafer by an etching process; An array of isolation sidewall mounting grooves is formed in the bottom silicon of the SOI wafer by an etching process, which extends from the top surface of the bottom silicon of the SOI wafer in a direction away from the optical fiber guide groove array. The isolation sidewall mounting groove is filled with opaque material to form an opaque isolation sidewall array. The opaque isolation sidewall extends from the area between adjacent light-emitting units to the bottom silicon surface of the SOI wafer, dividing the light transmission channel between each light-emitting unit and each optical fiber guide groove into multiple independent sub-channels. An LED array chip is provided, comprising multiple light-emitting units. The LED array chip is bonded to the lower surface of the underlying silicon. Using the opaque isolation sidewall as an alignment reference, each light-emitting unit is located at the entrance of each sub-channel, and the light emission direction of each light-emitting unit is towards the SOI wafer. The fiber array is placed into the fiber guide groove array, so that the optical receiving end of each fiber is located at the end of each sub-channel and is aligned and coupled with the emitted light path of each light-emitting unit.

[0014] Optionally, after forming the opaque isolation sidewall array, the method further includes: A high-reflectivity coating is deposited on the inner wall surface of the mounting groove of the isolation sidewall, so that the high-reflectivity coating covers the two oppositely arranged sidewall surfaces of the opaque isolation sidewall facing each of the sub-channels, and the high-reflectivity coating is used to reflect stray light incident on the sidewall surface back into the sub-channel.

[0015] Optionally, the step of filling the mounting groove of the isolation sidewall with an opaque material includes: An opaque material layer is deposited on the surface of the SOI wafer, and the opaque material layer fills the mounting groove of the isolation sidewall. The opaque material layer on the surface of the SOI wafer is removed by chemical mechanical polishing or etching back, leaving only the opaque material in the mounting groove of the isolation sidewall to form the opaque isolation sidewall.

[0016] Optionally, the step of filling the mounting groove of the isolation sidewall with an opaque material includes: A seed layer is formed on the inner wall of the mounting groove in the isolation sidewall and on the surface of the SOI wafer; Photoresist is spin-coated onto the seed layer, and the mounting groove area of ​​the isolation sidewall is exposed by photolithography. Selectively electroplat or chemically plate opaque metal material into the mounting groove of the isolation sidewall to fill the mounting groove of the isolation sidewall; Remove the photoresist and the exposed seed layer.

[0017] Optionally, the step of forming the array of mounting slots for the isolation sidewall includes: Using the buried oxide layer of the SOI wafer as the etching stop layer, wet etching is used to etch the isolation sidewall mounting trench array in the bottom silicon layer and to form the fiber guide trench in the top silicon layer; the etching depth of the deep reactive ion etching is consistent with the depth of the fiber guide trench. A reflective layer is deposited on the surface of the fiber guide groove and the isolation sidewall mounting groove using a deposition process.

[0018] The present invention has at least the following beneficial effects: 1. This solution establishes an opaque isolation sidewall in the bottom silicon of the SOI wafer, extending longitudinally from the region between adjacent light-emitting units to the upper surface of the bottom silicon of the SOI wafer. This isolation sidewall penetrates the buried oxide layer in the thickness direction and is embedded in the bottom region of the top silicon layer. In the horizontal direction, it extends from directly below the gap between LED array chips to the silicon wall between adjacent grooves. This divides the optical transmission channel between each light-emitting unit and each optical fiber guide groove into multiple independent sub-channels, achieving end-to-end optical channel isolation from the light source to the optical fiber. Stray light is directly intercepted in the lateral propagation path, and crosstalk between adjacent channels can be controlled below -40dB. This fundamentally solves the problem that existing surface light-blocking structures cannot effectively suppress stray light crosstalk inside the silicon body.

[0019] 2. This solution uses the buried oxide layer of the SOI wafer as an etching stop layer and employs deep reactive ion etching to form an array of isolation sidewall mounting trenches in the underlying silicon. Utilizing the high selectivity of the buried oxide layer during the etching process, etching automatically stops when the buried oxide layer is reached, achieving precise control of the etching depth. The depth of each mounting trench is consistent with good consistency, with an error of less than ±0.5μm. This avoids the problem of mounting trenches penetrating the SOI wafer due to over-etching. At the same time, the buried oxide layer also acts as a barrier layer when filling with opaque materials, preventing the filling material from leaking to the back side of the SOI wafer.

[0020] 3. This solution achieves planarization by filling the mounting slots of the isolation sidewalls with opaque material and then performing chemical mechanical polishing. This results in a flatness of less than 100nm on the top surface of the isolation sidewalls across the entire wafer. This flat top surface of the sidewalls serves directly as the passive alignment reference surface for LED array chip mounting, enabling the alignment accuracy between the light-emitting unit and the sub-channel entrance to reach ±1μm. This eliminates the need for additional alignment marks or active alignment steps, simplifying the packaging process and avoiding the accumulation of alignment errors caused by multiple mounting operations in traditional processes.

[0021] 4. This solution deposits a high-reflectivity coating on the inner wall surface of the mounting groove in the isolation sidewall, so that the high-reflectivity coating covers the two oppositely arranged sidewall surfaces of the isolation sidewall facing each sub-channel. This reflects stray light incident on the sidewall surface back into the sub-channel to continue propagating in the direction of the optical fiber, so that stray light that would otherwise be absorbed by the isolation sidewall can be recovered and reused. While maintaining the crosstalk suppression effect, it further improves the optical coupling efficiency of each channel.

[0022] 5. This solution uses at least a portion of the isolation sidewall as a thermally conductive metal material, extending the isolation sidewall upwards from the bottom silicon of the SOI wafer to the gap between adjacent light-emitting units. The lower end forms thermal contact with the bottom silicon, and the upper end forms thermal contact with the light-emitting unit. The heat generated by the light-emitting unit is transferred to the metal body through the upper end of the isolation sidewall, then conducted to the bottom silicon through the lower end, and dissipated through conduction to the heat dissipation substrate below. This allows the isolation sidewall to achieve optical isolation between channels while also serving as a lateral heat dissipation channel, avoiding thermal crosstalk caused by lateral heat diffusion between light-emitting units, increasing the heat dissipation area, and reducing the junction temperature of the light-emitting unit. Attached Figure Description

[0023] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 This is a schematic diagram of the structure of Embodiment 1 of the present invention; Figure 2 This is a schematic diagram of the etched fiber guide groove array in Embodiment 2 of the present invention; Figure 3 This is a schematic diagram of the etched isolation sidewall mounting groove array in Embodiment 2 of the present invention; Figure 4 This is a schematic diagram of the structure in Embodiment 2 of the present invention, in which LED array chips are bonded to SOI wafers.

[0025] Icon labels: 10 - SOI wafer; 11 - Bottom silicon; 12 - Buried oxide layer; 13 - Top silicon; 20 - LED array chip; 21 - Light-emitting unit; 30 - Opaque isolation sidewall array; 40 - Fiber optic guide groove array; 50 - Sub-channel; 60 - Isolation groove; 70 - Isolation sidewall mounting groove. Detailed Implementation

[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It is to be understood that the specific embodiments described herein are merely illustrative of the invention and not intended to limit it. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention.

[0027] In the description of this invention, it should be understood that the terms "center", "longitudinal", "lateral", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0028] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0029] Example 1

[0030] like Figure 1 As shown, this embodiment provides an optical coupling structure for an LED array and an optical fiber array, including: SOI wafer 10 has an optical fiber guide groove array 40 in its top silicon 13 for accommodating optical fibers, and an opaque isolation sidewall array 30 in its bottom silicon 11. LED array chip 20 includes multiple light-emitting units 21, which are bonded to the lower surface of the bottom silicon 11 of the SOI wafer 10, and the light emission direction of each light-emitting unit 21 is towards the SOI wafer 10. The opaque isolation sidewall array 30 extends longitudinally from the area between adjacent light-emitting units 21 to the upper surface of the bottom silicon 11 of the SOI wafer 10, dividing the optical transmission channel between each light-emitting unit 21 and each optical fiber guide groove into multiple independent sub-channels 50. An optical fiber array is disposed in the optical fiber guide groove array 40, with the optical receiving end of each optical fiber located at the end of each sub-channel 50. The emitted light from each of the light-emitting units 21 is transmitted in the corresponding sub-channel 50 and enters the corresponding optical fiber through the corresponding optical fiber guide groove.

[0031] like Figure 1 As shown, the SOI wafer 10 comprises, from bottom to top, a bottom silicon layer 11, a buried oxide layer 12, and a top silicon layer 13. An optical fiber guide groove array 40 is disposed in the top silicon layer 13 of the SOI wafer 10.

[0032] The fiber guide groove array 40 consists of multiple V-shaped or U-shaped grooves arranged side by side along the horizontal direction, with a center-to-center spacing of 250 μm between adjacent grooves. Each fiber guide groove extends downward from the upper surface of the top silicon layer 13 to a depth of 130 μm to 145 μm, and is used to accommodate the individual optical fibers in the fiber array. The groove has a trapezoidal cross-section, with a top width of 130 μm to 160 μm, a bottom width of 100 μm to 125 μm, and an angle of less than 5° between the sidewalls and the vertical direction.

[0033] In this embodiment, the depth of the fiber guide groove is 135 μm, the top width is 145 μm, and the bottom width is 110 μm.

[0034] An opaque isolation sidewall array 30 is disposed in the bottom silicon 11 of the SOI wafer 10. This opaque isolation sidewall array 30 extends longitudinally from the region between adjacent light-emitting units 21 to the upper surface of the bottom silicon 11 of the SOI wafer 10. That is, the isolation sidewalls penetrate the buried oxide layer 12 in the thickness direction of the SOI wafer 10 and are embedded in the bottom region of the top silicon 13. Horizontally, they extend from directly below the gap between adjacent light-emitting units 21 of the LED array chip 20 to the silicon wall between adjacent grooves in the fiber guide groove array 40. The width of the isolation sidewalls is 5 μm to 30 μm.

[0035] Through this extended structure, the isolation sidewall divides the optical transmission channel between each light-emitting unit 21 and each optical fiber guide groove into multiple independent sub-channels 50. Each sub-channel 50 starts from the light-emitting port of the corresponding light-emitting unit 21, passes through the interior of the SOI wafer 10, and reaches the optical receiving end face of the optical fiber in the corresponding optical fiber guide groove. In other words, each sub-channel 50 is confined by the isolation sidewall in the lateral direction and extends from the LED light-emitting unit 21 to the optical fiber receiving end in the longitudinal direction, forming a complete and independent optical transmission path.

[0036] By setting the opaque isolation sidewall array 30 as a bulk structure located inside the bottom silicon 11 and extending from the gap of the LED array chip 20 to the lower surface of the bottom silicon 11 of the SOI wafer 10, stray light is directly intercepted on the lateral propagation path, and crosstalk between adjacent channels can be controlled below -40dB, thereby solving the problem that existing surface light-blocking structures cannot effectively suppress stray light crosstalk inside the silicon bulk.

[0037] The LED array chip 20 comprises multiple light-emitting units 21, each fabricated based on a gallium nitride-on-silicon (GaN-on-Si) epitaxial wafer, emitting blue light at a wavelength of 450 nm in the visible or near-infrared band. Each light-emitting unit 21 has a P-electrode and an N-electrode, which are used for electrical connection to an external driving circuit to inject current into the light-emitting unit 21. The electrode material is a Ti / Au stack. The LED array chip 20 is bonded to the lower surface of the bottom silicon 11 of the SOI wafer 10 via a bonding layer, and the light emission direction of each light-emitting unit 21 faces the SOI wafer 10, i.e., downward light emission.

[0038] The fiber optic array is disposed in the fiber optic guide groove array 40, and the optical receiving end of each fiber is located at the end of each sub-channel 50. The fiber is a multimode fiber or a single-mode fiber.

[0039] Optical transmission process: The downward-emitted light beams from each light-emitting unit 21 enter their respective sub-channels 50, propagate vertically downwards within the sub-channels 50, pass through the top silicon layer 13 and the buried oxide layer 12 to reach the area between the opaque isolation sidewalls in the bottom silicon layer 11, and finally enter the optical receiving end face of the optical fiber in the corresponding optical fiber guide groove. Since adjacent sub-channels 50 are completely separated by opaque isolation sidewalls, the emitted light from each light-emitting unit 21 will not laterally interfere with adjacent channels.

[0040] In this embodiment, the width of the isolation sidewall is preferably 15 μm, and the height is matched with the total thickness of the SOI wafer 10 along the thickness direction of the SOI wafer 10.

[0041] In another embodiment, such as Figure 1As shown, an isolation groove 60 is provided between adjacent light-emitting units 21. The isolation groove 60 extends downward from the upper surface of the LED array chip 20, penetrating the P-type layer, quantum well active layer, and N-type layer of the epitaxial layer, with a depth of 5μm~10μm and a width of 10μm~20μm. The opaque isolation sidewall protrudes from the upper surface of the top silicon 13 of the SOI wafer 10 in a direction away from the SOI wafer 10, with a height of 10μm~100μm, preferably 20μm, and the protruding part is embedded in the isolation groove 60.

[0042] Specifically, the isolation trench 60 physically separates the PN junctions of adjacent light-emitting units 21, preventing carriers from laterally diffusing between adjacent light-emitting units 21, thus achieving electrical isolation. The protruding portion of the isolation sidewall fills the isolation trench 60, forming a continuous opaque physical barrier between adjacent light-emitting units 21, achieving optical isolation. Simultaneously, the protruding portion, after being embedded in the isolation trench 60, forms a mechanical interlock, enhancing the bonding strength between the LED array chip 20 and the SOI wafer 10. Thus, the isolation sidewall and the isolation trench 60 simultaneously achieve electrical isolation, optical isolation, and bonding enhancement functions in the same structure.

[0043] In another embodiment, at least a portion of the opaque insulating sidewall is made of a thermally conductive metal material. The thermally conductive metal material is selected from copper, tungsten, nickel, aluminum, silver, gold, or alloys thereof.

[0044] Copper possesses excellent thermal conductivity, with a thermal conductivity of approximately 400 W / (m·K), and is readily available for electroplating. Tungsten's coefficient of thermal expansion, approximately 4.5 ppm / K, is close to that of silicon (approximately 2.6 ppm / K), effectively reducing thermal stress. Nickel exhibits good corrosion resistance and compatibility with electroless plating processes. Aluminum offers advantages in low density and cost, making it suitable for lightweight applications. Silver boasts the highest thermal conductivity, approximately 429 W / (m·K), making it suitable for high power density applications. Gold offers excellent corrosion resistance and chemical stability, making it suitable for high-reliability applications. Copper-tungsten alloys combine the high thermal conductivity of copper with the low thermal expansion of tungsten. These thermally conductive metals can be selected as single metals or alloys.

[0045] Specifically, the isolation sidewall extends upward from the bottom silicon 11 of the SOI wafer 10 into the gap between adjacent light-emitting units 21. The lower end of the isolation sidewall extends into the interior of the bottom silicon 11 of the SOI wafer 10, forming thermal contact with the bottom silicon 11; the upper end of the isolation sidewall extends into the gap between adjacent light-emitting units 21 of the LED array chip 20, forming thermal contact with the sidewall or bottom of the light-emitting unit 21. The thermal contact is either direct physical contact or indirect contact through a thermally conductive medium layer.

[0046] When the light-emitting unit 21 is working, the heat it generates is transferred to the metal body of the isolation sidewall through the upper end of the isolation sidewall, and then conducted to the bottom silicon 11 of the SOI wafer 10 through the lower end of the isolation sidewall, and then dissipated by the heat dissipation substrate below through the bottom silicon 11.

[0047] In this structure, the isolation sidewalls not only achieve optical isolation between channels but also serve as lateral heat dissipation channels between adjacent light-emitting units 21. On one hand, the high thermal conductivity of the thermally conductive metal material allows the heat generated by adjacent light-emitting units 21 to be quickly dissipated, avoiding thermal crosstalk caused by lateral heat diffusion between light-emitting units 21. That is, the heat generated by light-emitting unit 21 diffuses to adjacent light-emitting units 21, causing their temperature to rise, emission wavelength to redshift, and light extraction efficiency to decrease. On the other hand, the isolation sidewalls extend vertically, with their lower ends in large-area contact with the underlying silicon 11, providing an additional path for heat to be conducted directly downwards from inside the LED chip. Compared to the traditional solution of only dissipating heat downwards through the substrate of the LED array chip 20, this increases the lateral heat dissipation channel, significantly increases the heat dissipation area, and further reduces the junction temperature of the light-emitting unit 21.

[0048] In another embodiment, an optical waveguide layer or an anti-reflection film layer is disposed on the inner wall surface of each of the sub-channels 50. The optical waveguide layer or anti-reflection film layer is continuously disposed along the longitudinal extension direction of the sub-channel 50, covering the entire inner wall surface of the sub-channel 50, that is, covering the sidewall of the top silicon 13, the surface of the buried oxide layer 12, and the sidewall of the bottom silicon 11 of the SOI wafer 10.

[0049] The optical waveguide layer is a transparent dielectric layer with a refractive index greater than that of the silicon material in the SOI wafer 10, forming a waveguide structure on the inner wall of the sub-channel 50. The anti-reflection coating layer is a distributed Bragg mirror, composed of alternating layers of high-refractive-index and low-refractive-index materials.

[0050] When the light beam propagates within the sub-channel 50 and reaches its inner wall, the waveguide layer ensures total internal reflection, causing the beam to be reflected back into the sub-channel 50 to continue propagating. The anti-reflection coating layer, through interference reflection of multiple layers, reflects the light beam incident on the inner wall of the sub-channel 50 back into the sub-channel 50. Thus, the waveguide layer or anti-reflection coating layer confines the light beam to propagation within the sub-channel 50, preventing lateral leakage through the sidewalls of the sub-channel 50 to adjacent channels, thereby reducing optical transmission loss and further suppressing inter-channel crosstalk.

[0051] Example 2

[0052] This embodiment provides a method for manufacturing an optical coupling structure between an LED array and an optical fiber array, including the following steps: like Figure 2As shown, an SOI wafer 10 is provided, which includes, from bottom to top, a bottom silicon layer 11, a buried oxide layer 12 and a top silicon layer 13. An optical fiber guide groove array 40 is formed in the top silicon 13 of the SOI wafer 10 by an etching process; Specifically, a hard mask layer is deposited on the top silicon 13 of the SOI wafer 10, and the pattern of the fiber guide groove array 40 is defined by photolithography. Using the patterned hard mask as the etching mask, deep reactive ion etching is performed on the top silicon 13, and the buried oxide layer 12 is used as the etching stop layer. The etching automatically stops when the buried oxide layer 12 is reached, thereby forming the fiber guide groove array 40. The remaining hard mask is removed, and the surface is cleaned and dried. In this step, the cross-section of the fiber guide groove is trapezoidal, with a top width of 145 μm, a bottom width of 115 μm, and an angle of less than 3° between the sidewalls and the vertical direction.

[0053] An array of isolation sidewall mounting grooves is formed in the bottom silicon 11 of the SOI wafer 10 by an etching process, which extends from the upper surface of the bottom silicon 11 of the SOI wafer 10 in a direction away from the optical fiber guide groove array 40. Specifically, such as Figure 3 As shown, the SOI wafer 10 is flipped so that its back side faces upward. Using a double-sided photolithography process, with the pattern of the front fiber guide groove array 40 as the alignment mark, back-side alignment exposure is performed on the back side of the underlying silicon 11 to define the pattern of the isolation sidewall mounting groove array.

[0054] The isolation sidewall mounting slot 70 extends from the upper surface of the bottom silicon 11 in a direction away from the fiber guide groove array 40. The width of the mounting slot is 15 μm, and the length extends from the end of the fiber guide groove to the edge of the SOI wafer 10. The center distance between adjacent mounting slots is 250 μm.

[0055] Deep reactive ion etching (DRIE) was used to etch from the back side of the bottom silicon 11, with an etching depth of approximately 365 μm, which is the total thickness of the SOI wafer 10 minus the remaining thickness of the fiber guide groove in the top silicon 13. Due to the large etching depth, a high aspect ratio etching process was used to form an array of isolation sidewall mounting trenches that extends from the bottom silicon 11 to the bottom of the top silicon 13. The angle between the sidewalls of the mounting trenches and the vertical direction is less than 5°.

[0056] The isolation sidewall mounting groove 70 is filled with opaque material to form an opaque isolation sidewall array. The opaque isolation sidewall extends from the area between adjacent light-emitting units 21 to the upper surface of the bottom silicon 11 of the SOI wafer 10, dividing the light transmission channel between each light-emitting unit 21 and each optical fiber guide groove into multiple independent sub-channels 50. Specifically, an opaque material layer is deposited on the entire surface of the SOI wafer 10 and inside the mounting groove of the isolation sidewalls. In this embodiment, the opaque material is a carbon black-doped polymer, such as carbon black-doped polyimide or SU-8, with a carbon black doping concentration of 5% to 15% (weight percentage), resulting in a light transmittance of <1%. The deposition method is spin coating or spray coating, ensuring that the material fully fills the interior of the mounting groove.

[0057] Excess opaque material on the surface of SOI wafer 10, the upper surface of top silicon 13, and the back of bottom silicon 11 is removed by chemical mechanical polishing (CMP), leaving only the opaque material inside the isolation sidewall mounting grooves to form an opaque isolation sidewall array 30. The CMP endpoint is the surface layer of SOI wafer 10, and the surface roughness Ra after polishing is <2nm.

[0058] The isolation sidewall array extends longitudinally from the region between adjacent light-emitting units 21 to the upper surface of the bottom silicon 11 of the SOI wafer 10, dividing the optical transmission channel between each light-emitting unit 21 and each optical fiber guide groove into multiple independent sub-channels 50.

[0059] An LED array chip 20 is provided, comprising a plurality of light-emitting units 21. The LED array chip 20 is bonded to the lower surface of the underlying silicon 11. With the opaque isolation sidewall as the alignment reference, each light-emitting unit 21 is located at the entrance of each sub-channel 50, and the light emission direction of each light-emitting unit 21 is towards the SOI wafer 10. Specifically, such as Figure 4 As shown, an LED array chip 20 is provided, comprising 12 light-emitting units 21 arranged in a one-dimensional linear array. The center-to-center distance between adjacent light-emitting units 21 is 250 μm, consistent with the center-to-center distance of the isolation sidewall array. Each light-emitting unit 21 is fabricated based on a GaN-on-Si epitaxial wafer, emits light at a wavelength of 450 nm, and has independent P-electrode and N-electrode.

[0060] A bonding dielectric layer, such as benzocyclobutene, with a thickness of 3 μm is spin-coated on the side of the bottom silicon 11 of the SOI wafer 10 away from the buried oxide layer 12. The LED array chip 20 is placed on top of the front side of the SOI wafer 10, with the top surface of the opaque isolation sidewall as the passive alignment reference plane. Each light-emitting unit 21 of the LED array chip 20 is aligned with the entrance of each sub-channel 50 one by one using a chip mounting device, and the gap between adjacent light-emitting units 21 is aligned with the extension direction of the isolation sidewall.

[0061] After alignment, the bonding medium layer is cured by thermo-press bonding, fixing the LED array chip 20 to the surface of the SOI wafer 10. After bonding, the light emission direction of each light-emitting unit 21 is towards the SOI wafer 10 (light emission downward), and each light-emitting unit 21 is located at the entrance of each sub-channel 50.

[0062] The fiber array is placed into the fiber guide groove array 40, so that the optical receiving end of each fiber is located at the end of each sub-channel 50 and is aligned and coupled with the output optical path of each light-emitting unit 21.

[0063] Specifically, a ribbon fiber array is provided, comprising 12 multimode fibers with a cladding diameter of 125 μm and a center-to-center distance of 250 μm between adjacent fibers, which matches the center-to-center distance of the fiber guide groove array 40.

[0064] The fiber array is placed one by one into the fiber guide groove array 40. The bottom of the fiber contacts the bottom of the groove, and the top of the fiber is about 3~5μm lower than the upper surface of the SOI wafer 10.

[0065] Since the angle between the sidewall of the fiber guide groove and the vertical direction is less than 3°, the fiber is precisely positioned in both the lateral and depth directions after it is inserted. The optical receiving end of each fiber is located at the end of each sub-channel 50 and is automatically aligned and coupled with the output optical path of each light-emitting unit 21.

[0066] The fiber guide groove is filled with UV-curable adhesive with a refractive index of 1.51, which matches the refractive index of the fiber cladding. The adhesive is then cured by irradiation with a UV lamp with a wavelength of 365nm and a power of 50mW / cm² for 60 seconds, thus fixing the fiber array in the groove.

[0067] Through the above manufacturing method, the isolation sidewall starts from the gap of the LED light-emitting unit 21 and extends all the way to the optical fiber receiving end face, realizing full-path optical isolation from the light source to the optical fiber, and the crosstalk between adjacent channels can be controlled below -40dB. At the same time, the method uses the buried oxide layer 12 of SOI wafer 10 as the etching stop layer, realizing precise control of etching depth, good consistency of depth of each mounting groove, and an error of less than ±0.5μm; the planarized top surface of the isolation sidewall is used as the passive alignment reference surface for mounting LED array chip 20, so that the alignment accuracy between the light-emitting unit 21 and the entrance of the sub-channel 50 can reach ±1μm, without active alignment; the sidewall of the optical fiber guide groove is used to precisely limit the optical fiber, so that the optical receiving end of the optical fiber is automatically located at the end of the sub-channel 50 and aligned and coupled with the output optical path of the light-emitting unit 21, achieving stable coupling efficiency without active alignment, and significantly reducing packaging costs. In addition, the double-sided photolithography process ensures that the mounting groove pattern on the back side and the groove pattern on the front side are precisely aligned in the vertical direction, guaranteeing the vertical continuity of the optical path from the LED light outlet to the fiber end face; the low-temperature bonding process avoids the adverse effects of high temperature on LED luminous efficiency; the entire manufacturing method is compatible with CMOS process and is suitable for wafer-level mass production.

[0068] Example 3

[0069] The difference between this embodiment and Embodiment 2 is that, after the step of forming the opaque isolation sidewall array 30, a high-reflectivity coating is deposited on the inner wall surface of the isolation sidewall mounting groove.

[0070] Specifically, after filling the isolation sidewall mounting groove with opaque material to form an opaque isolation sidewall array 30, a high-reflectivity coating is deposited on the inner wall surface of the isolation sidewall mounting groove by magnetron sputtering or electron beam evaporation. Then, the sidewall area of ​​the isolation sidewall mounting groove is protected by photolithography, and the high-reflectivity coating material in the bottom and opening areas of the isolation sidewall mounting groove is removed by etching, leaving the high-reflectivity coating only on the two oppositely arranged sidewall surfaces of the isolation sidewall, so that the high-reflectivity coating covers the two oppositely arranged sidewall surfaces of the opaque isolation sidewall facing each of the sub-channels 50.

[0071] The high-reflectivity coating is either a metallic reflective layer or a dielectric reflective layer. Specifically, the metallic reflective layer is selected from any one of a titanium / gold stack, a silver layer, or an aluminum layer. In the titanium / gold stack, the titanium layer has a thickness of 20 nm, the gold layer has a thickness of 300 nm, the silver layer has a thickness of 200 nm and a reflectivity greater than 95%, and the aluminum layer has a thickness of 300 nm and a reflectivity greater than 90%. The dielectric reflective layer is a silicon dioxide / titanium dioxide distributed Bragg mirror with a reflectivity greater than 98%.

[0072] When stray light emitted from an adjacent light-emitting unit 21 is incident at a large angle onto the inner surface of the isolation sidewall, the high-reflectivity coating reflects the stray light back into the sub-channel 50, allowing it to continue propagating along the sub-channel 50 towards the optical fiber. Thus, the high-reflectivity coating recovers and reuses a portion of the stray light that would otherwise be absorbed by the isolation sidewall, further improving the optical coupling efficiency of each channel while maintaining crosstalk suppression.

[0073] Example 4

[0074] The difference between this embodiment and Embodiment 2 lies in the specific implementation method of filling the installation groove of the isolation sidewall with opaque material.

[0075] Specifically, an opaque material layer is deposited on the entire surface of SOI wafer 10, including the top surface of top silicon 13, the back surface of bottom silicon 11, the interior of the fiber guide groove, and the interior of the isolation sidewall mounting groove. The opaque material can be one of the following options: Option 1: Spin-coat a carbon black-doped polyimide precursor solution at a concentration of 10 wt% at 3000 rpm, then heat to 80°C, 150°C, and 300°C in stages for curing to form a cured opaque polyimide layer. The polyimide shrinks by 15%–20% during curing, requiring 1–2 additional spin-coats to ensure the mounting groove is fully filled.

[0076] Option 2: Employ copper electroplating. First, sputter a titanium / copper seed layer onto the inner wall of the mounting tank on the isolation sidewall, with the titanium layer being 20nm thick and the copper layer 200nm thick. Immerse the SOI wafer 10 as the cathode in the electroplating solution, which consists of 200g / L copper sulfate pentahydrate, 60g / L sulfuric acid, and 50ppm chloride ions. The current density is 2A / dm², and the electroplating time is approximately 30 minutes, allowing the copper to completely fill the mounting tank.

[0077] Option 3: Low-pressure chemical vapor deposition is used to deposit phosphorus-doped polycrystalline silicon at a deposition temperature of 620°C, a silane flow rate of 100 sccm, a phosphine doping flow rate of 10 sccm, and a deposition time of approximately 4 hours, so that the polycrystalline silicon completely fills the mounting tank and covers the surface.

[0078] After deposition, chemical mechanical polishing (CMP) is used to remove the opaque material layer on the surface of SOI wafer 10, leaving only the opaque material within the isolation sidewall mounting grooves. CMP is performed using an IC1000 polishing pad and a colloidal silica or copper polishing slurry. The polishing pressure is 3 psi, the polishing disc speed is 100 rpm, and polishing continues until all excess material is removed, exposing the top surface of silicon 13 and the back surface of silicon 11 on SOI wafer 10. After CMP, the opaque material within the isolation sidewall mounting grooves is flush with the surface of SOI wafer 10, forming opaque isolation sidewalls.

[0079] For polymer materials, micro-depressions may appear on the top of the isolation sidewalls after chemical mechanical polishing, with a depth of 0.5 μm to 2 μm. A thin-layer deposition and etchback process can be performed after chemical mechanical polishing to fill the depressed areas and ensure a flat top surface of the isolation sidewalls.

[0080] In this embodiment, chemical mechanical polishing (CMP) enables global planarization of the top surface of the isolation sidewalls, achieving a flatness of less than 100 nm across the entire wafer. The flat top surface of the sidewalls can directly serve as a passive alignment reference surface for subsequent LED array chip mounting, ensuring an alignment accuracy of ±1 μm between the light-emitting unit 21 and the entrance of the sub-channel 50. This eliminates the need for additional alignment marks or active alignment steps, simplifying the packaging process. Furthermore, this embodiment provides three optional options: polymer filling, metal filling, and polysilicon filling, allowing for flexible selection of filling materials based on different application requirements, demonstrating strong adaptability. For micro-dimpling issues that may occur after polymer CMP, thin-layer deposition and etch-back are used for filling, further ensuring the flatness and alignment accuracy of the top surface of the sidewalls. In addition, CMP is a global planarization process, capable of simultaneously planarizing all isolation sidewalls across the entire wafer, ensuring good height consistency among sidewalls and guaranteeing the consistency of the light transmission path for each channel.

[0081] Example 5

[0082] The difference between this embodiment and Embodiment 2 lies in the specific implementation method of filling the installation groove of the isolation sidewall with opaque material.

[0083] Specifically, a seed layer is first sputtered onto the entire surface of SOI wafer 10, including the inner wall of the isolation sidewall mounting trench, the upper surface of the top silicon 13, the back surface of the bottom silicon 11, and the interior of the fiber guide groove. The seed layer is a titanium / copper stack, with a titanium layer thickness of 20 nm as an adhesion layer and a copper layer thickness of 200 nm as an electroplating conductive layer. Then, photoresist is spin-coated onto the seed layer, and the seed layer in the isolation sidewall mounting trench area is exposed using photolithography. The seed layer in other areas is covered and protected by photoresist. For the double-sided structure of SOI wafer 10, photolithography is performed separately on the front side to expose the mounting trench entrance in the top silicon 13 area and on the back side to expose the mounting trench entrance in the bottom silicon 11 area, or the entire area penetrating the mounting trench can be exposed at once.

[0084] Next, the SOI wafer 10 is immersed in an electroplating solution or a chemical plating solution, and an opaque metal material is selectively electroplated or chemically plated into the isolation sidewall mounting groove to fill the groove. Specifically, one of the following methods can be adopted: Option 1: The electroplating solution consists of 200 g / L copper sulfate pentahydrate, 60 g / L sulfuric acid, and 50 ppm chloride ions, with polyethylene glycol and thiourea added as additives. The current density is 2~5 A / dm², and the electroplating time is adjusted according to the depth and width of the mounting tank to ensure that the mounting tank is completely filled with copper. Because the seed layer outside the mounting tank area is covered by photoresist, copper is deposited only in the exposed mounting tank area, achieving selective filling.

[0085] Option 2: The chemical plating solution consists of 30 g / L nickel sulfate hexahydrate, 30 g / L sodium hypophosphite, and 20 g / L sodium citrate, with a pH of 8-9 and a temperature of 80°C. The deposition rate is 5-10 μm / hour, and the deposition time is adjusted according to the size of the installation tank.

[0086] After filling, the photoresist is removed with acetone to expose the seed layer in the protected area. Then, wet etching is used to selectively remove the seed layer, first using a copper etchant to remove the copper layer, and then using diluted hydrofluoric acid to remove the titanium layer. During etching, the filler metal in the mounting groove has a significant thickness because it completely fills the groove, and is therefore not completely removed by the thin-layer etchant, thus remaining intact. Ultimately, only the metal filler remains in the mounting groove of the isolation sidewall, forming a metal isolation sidewall.

[0087] In this embodiment, selective electroplating or electroless plating processes deposit metal only within the mounting tank area, eliminating the need for subsequent chemical mechanical polishing (CMP) steps and avoiding surface scratches and particle contamination issues that may arise from CMP. Simultaneously, the metal isolation sidewalls not only possess excellent opacity, enabling optical isolation between channels, but also exhibit high thermal conductivity, serving as heat dissipation channels to conduct heat generated by the light-emitting unit 21 downwards to the underlying silicon 11 of the SOI wafer 10, achieving the dual functions of optical isolation and heat dissipation. Furthermore, selective electroplating or electroless plating processes are compatible with semiconductor back-end processes, suitable for wafer-level mass production, and the metal material can be either electroplated copper or electrolessly plated nickel, allowing for flexible selection based on actual needs.

[0088] Example 6

[0089] The difference between this embodiment and embodiment two is that wet etching is used to simultaneously form fiber guide grooves in the top silicon 13 and an array of isolation sidewall mounting grooves in the bottom silicon 11.

[0090] Specifically, an SOI wafer 10 with a (100) crystal plane orientation is provided. Etching masks are formed on the front and back sides of the SOI wafer 10, respectively. The front mask defines the pattern of the fiber guide groove array 40, and the back mask defines the pattern of the isolation sidewall mounting groove array. A double-sided lithography machine is used to align the front and back patterns, so that the back mounting groove pattern and the front groove pattern are precisely aligned in the vertical direction, with an alignment accuracy of ±2μm.

[0091] The SOI wafer 10 with a double-sided mask was immersed in a 30% potassium hydroxide solution at a temperature of 80°C for approximately 3 hours. Since potassium hydroxide has selective etching characteristics for the silicon (100) and (111) crystal planes with an etching rate ratio of approximately 100:1, V-grooves were simultaneously formed in the front window of the top silicon 13 and the back window of the bottom silicon 11. Among them, the front V-shaped groove is etched downward from the upper surface of the top silicon 13 to form a fiber guide groove with a V-shaped cross section. The sidewall of the groove is a (111) crystal plane with an angle of 54.74° with the upper surface and a depth of 125μm~145μm. The back V-shaped groove is etched upward from the back of the bottom silicon 11 to form an isolation sidewall mounting groove with a V-shaped cross section. The sidewall of the mounting groove has an angle of 54.74° with the back surface and a depth of approximately the total thickness of the SOI wafer 10 minus the depth of the fiber guide groove in the top silicon 13 minus the thickness of the buried oxide layer 12. That is, the tip of the mounting groove just reaches the position of the buried oxide layer 12.

[0092] After etching, a reflective layer is simultaneously deposited on the surface of the fiber guide groove and the surface of the isolation sidewall mounting groove using a deposition process. The reflective layer material is a titanium / gold stack, with a titanium layer thickness of 20 nm and a gold layer thickness of 300 nm. During deposition, due to the inclined surface characteristics of the V-groove, the reflective layer can uniformly cover the inclined sidewall of the groove. The above filling step is completed before bonding the LED array chips to ensure that the LED array chips are not affected by the filling process (such as high-temperature deposition or electroplating annealing) during subsequent bonding.

[0093] After depositing the reflective layer, the mounting groove of the isolation sidewall is filled with opaque material to form an opaque isolation sidewall.

[0094] In this embodiment, anisotropic wet etching with potassium hydroxide is used to simultaneously form the front fiber guide groove and the back isolation sidewall mounting groove, completing both structures in a single etching process. This method is simple and low-cost. The V-shaped groove formed by wet etching has a smooth (111) crystal plane bevel, naturally forming a high-reflectivity surface without the need for additional surface polishing or roughness control. After the reflective layer is deposited, the V-shaped bevel of the fiber guide groove becomes a high-reflectivity surface, which can be used for fiber positioning and optical path reflection shaping. After the reflective layer is deposited on the V-shaped bevel of the isolation sidewall mounting groove, it becomes an isolation sidewall with a high-reflectivity inner wall. In addition, the V-shaped cross-section isolation sidewall has a geometric feature of being wide at the top and narrow at the bottom, which can provide a larger optical isolation area near the LED emitting surface and leave more space for the optical path near the fiber end.

[0095] The above description is merely an embodiment of this application and does not limit the patent scope of this application. Any equivalent structural or procedural transformations made using the content of this application's specification and drawings, such as the combination of technical features between embodiments, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of this application.

Claims

1. An optical coupling structure for an LED array and an optical fiber array, characterized in that, include: SOI wafers have an array of fiber optic inlet grooves in the top silicon layer to accommodate optical fibers, and an array of opaque isolation sidewalls in the bottom silicon layer. The LED array chip includes multiple light-emitting units, which are bonded to the bottom silicon surface of the SOI wafer, and the light emission direction of each light-emitting unit is towards the SOI wafer; An opaque isolation sidewall array extends longitudinally from the region between adjacent light-emitting units to the upper surface of the underlying silicon, dividing the light transmission channel between each light-emitting unit and each optical fiber guide groove into multiple independent sub-channels. An optical fiber array is disposed in the optical fiber guide groove array, with the optical receiving end of each optical fiber located at the end of each sub-channel; The emitted light from each of the light-emitting units is transmitted in the corresponding sub-channel and enters the corresponding optical fiber through the corresponding optical fiber guide groove.

2. The optical coupling structure of the LED array and the fiber optic array as described in claim 1, characterized in that, An isolation groove is provided between adjacent light-emitting units, and at least a portion of the opaque isolation sidewall is filled in the isolation groove. The isolation groove penetrates at least a portion of the thickness of the LED array chip to provide electrical and optical isolation between adjacent light-emitting units.

3. The optical coupling structure of the LED array and the fiber optic array as described in claim 1, characterized in that, At least a portion of the opaque isolation sidewall is made of a thermally conductive metal material. The opaque isolation sidewall extends upward from the bottom silicon layer of the SOI wafer to the gap between adjacent light-emitting units, and is used to conduct the heat generated by the adjacent light-emitting units along the opaque isolation sidewall to the SOI wafer.

4. The optical coupling structure of the LED array and the fiber optic array as described in claim 3, characterized in that, The thermally conductive metal material is copper, tungsten, nickel, aluminum, silver, gold, or an alloy thereof.

5. The optical coupling structure of the LED array and the fiber optic array as described in claim 1, characterized in that, Each of the sub-channels has an optical waveguide layer or an anti-reflection film layer on its inner wall surface. The optical waveguide layer or anti-reflection film layer is used to restrict the emitted light from each of the light-emitting units within each of the sub-channels, so that the emitted light propagates to the corresponding optical fiber.

6. A method for manufacturing an optical coupling structure of an LED array and an optical fiber array, characterized in that, Includes the following steps: An SOI wafer is provided, wherein the SOI wafer comprises, from bottom to top, a bottom silicon layer, a buried oxide layer and a top silicon layer; An array of fiber guide grooves is formed in the top silicon layer of the SOI wafer by an etching process; An array of isolation sidewall mounting grooves is formed in the bottom silicon of the SOI wafer by an etching process, which extends from the top surface of the bottom silicon of the SOI wafer in a direction away from the optical fiber guide groove array. The isolation sidewall mounting groove is filled with opaque material to form an opaque isolation sidewall array. The opaque isolation sidewall extends from the area between adjacent light-emitting units to the bottom silicon surface of the SOI wafer, dividing the light transmission channel between each light-emitting unit and each optical fiber guide groove into multiple independent sub-channels. An LED array chip is provided, comprising multiple light-emitting units. The LED array chip is bonded to the lower surface of the underlying silicon. Using the opaque isolation sidewall as an alignment reference, each light-emitting unit is located at the entrance of each sub-channel, and the light emission direction of each light-emitting unit is towards the SOI wafer. The fiber array is placed into the fiber guide groove array, so that the optical receiving end of each fiber is located at the end of each sub-channel and is aligned and coupled with the emitted light path of each light-emitting unit.

7. The manufacturing method as described in claim 6, characterized in that, After the step of forming the opaque isolation sidewall array, the method further includes: A high-reflectivity coating is deposited on the inner wall surface of the mounting groove of the isolation sidewall, so that the high-reflectivity coating covers the two oppositely arranged sidewall surfaces of the opaque isolation sidewall facing each of the sub-channels, and the high-reflectivity coating is used to reflect stray light incident on the sidewall surface back into the sub-channel.

8. The manufacturing method as described in claim 6, characterized in that, The step of filling the mounting groove of the isolation sidewall with an opaque material includes: An opaque material layer is deposited on the surface of the SOI wafer, and the opaque material layer fills the mounting groove of the isolation sidewall. The opaque material layer on the surface of the SOI wafer is removed by chemical mechanical polishing or etching back, leaving only the opaque material in the mounting groove of the isolation sidewall to form the opaque isolation sidewall.

9. The manufacturing method as described in claim 6, characterized in that, The step of filling the mounting groove of the isolation sidewall with an opaque material includes: A seed layer is formed on the inner wall of the mounting groove in the isolation sidewall and on the surface of the SOI wafer; Photoresist is spin-coated onto the seed layer, and the mounting groove area of ​​the isolation sidewall is exposed by photolithography. Selectively electroplat or chemically plate opaque metal material into the mounting groove of the isolation sidewall to fill the mounting groove of the isolation sidewall; Remove the photoresist and the exposed seed layer.

10. The manufacturing method as described in claim 6, characterized in that, The steps for forming the array of mounting slots for the isolation sidewall include: Using the buried oxide layer of the SOI wafer as the etching stop layer, wet etching is used to etch the isolation sidewall mounting trench array in the bottom silicon layer and to form the fiber guide trench in the top silicon layer; the etching depth of the deep reactive ion etching is consistent with the depth of the fiber guide trench. A reflective layer is deposited on the surface of the fiber guide groove and the isolation sidewall mounting groove using a deposition process.