A weather-resistant light-adjusting film with edge waterproof packaging and a preparation process thereof

By using a double-layer sealant structure with inner and outer channels and in-situ grown ZIF-8 nanocrystals, the problems of curved surface bonding and edge waterproofing of dimming films are solved, achieving high strength, self-healing weather resistance and waterproofing, and extending the service life of dimming films.

CN123136930APending Publication Date: 2026-11-20SHANGHAI ASTRACE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611329945.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing dimming films face challenges in curved surface lamination and edge waterproofing. During curved surface lamination, the film is prone to warping, and the edge sealing structure is prone to failure, resulting in a decline in dimming function and a shortened service life.

Method used

The system employs a dual-layer sealant structure with inner and outer layers. The inner sealant adheres tightly to the edge of the dimming film body, while the outer sealant comprises in-situ grown ZIF-8 nanocrystals and a polymer matrix. These layers are chemically anchored through zinc-imidazolium coordination bonds. Combined with a heating-setting-cooling process to fix the curvature, the sealant achieves high strength and self-healing capabilities.

Benefits of technology

It significantly improves the curved surface adaptability and waterproof performance of the dimming film, extends its service life, reduces water vapor permeability, and has self-healing ability, while also improving the tensile strength and toughness of the sealant.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123136930A_ABST
    Figure CN123136930A_ABST
Patent Text Reader

Abstract

The application discloses a kind of edge waterproof encapsulation weather-resistant light modulation film and preparation process thereof, belong to light modulation film technical field.The weather-resistant light modulation film includes curved light modulation film main body and edge waterproof sealing structure, by inner / outer double-layer chemical anchoring sealing structure barrier water vapor invasion and delamination, with heating-setting-cooling process eliminates curved surface bonding stress, utilize in situ growth ZIF-8 nanocrystal realizes the systematic improvement of sealing glue mechanics and barrier property, and with the aid of zinc-imidazole dynamic coordination bond gives sealing glue self-repairing ability, so that light modulation film has long-term weather-resistant reliability under curved surface bonding state, effectively prolongs service life.The application solves the problem of light modulation film curved surface bonding wrinkle and edge water vapor invasion, has excellent curved surface adaptability, mechanical property, barrier property and self-repairing ability, is suitable for vehicle-mounted awning, building curtain wall and other high weather-resistant scenes, effectively prolongs the service life of light modulation film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of dimming film technology, and in particular to a weather-resistant dimming film with edge waterproofing and its preparation process. Background Technology

[0002] Polymer dispersed liquid crystal (PDLC) dimming films, as an electronically controlled smart light valve material, are widely used in building curtain walls, automotive sunroofs, smart windows, and other fields because they can quickly switch between transparent and hazy states. A typical dimming film consists of two transparent conductive substrate layers and a dimming functional layer sandwiched between them, such as a PDLC layer or an electrochromic layer. Its edge sealing performance directly determines the service life and reliability of the device.

[0003] As dimming films expand into applications such as vehicle sunroofs and curved building curtain walls, curved surface bonding and edge waterproofing have become two major technical bottlenecks in the weather resistance of dimming films.

[0004] Regarding curved surface bonding, when existing flat dimming films are directly attached to hyperbolic glass, bulging and warping are very likely to occur at the edges because the film does not fit the curved surface.

[0005] In existing technologies, the membrane material is often softened by heating and then bonded to curved surfaces. However, the formed membrane is prone to shrinkage during subsequent processing and it is difficult to maintain the preset curvature stably.

[0006] Regarding edge waterproofing, the orientation of liquid crystal molecules in the dimming film is damaged after it gets damp, leading to a decline in dimming function or even rendering it unusable.

[0007] Existing edge sealing technologies mostly use a single layer of sealant, which has two shortcomings: Firstly, if a single-layer sealing structure has local defects, water vapor can travel directly to the functional layer along the defect channel. Secondly, traditional sealants are prone to aging and failure in outdoor environments such as high temperature and humidity and ultraviolet radiation, resulting in decreased bonding strength and delamination at the edges.

[0008] Furthermore, the insufficient adhesion reliability between the sealant and the dimming film substrate, especially the transparent conductive layer, at the humid interface further exacerbates the risk of moisture penetration along the interface.

[0009] Therefore, there is an urgent need to develop a weather-resistant dimming film that combines surface adaptability with long-lasting waterproof sealing performance and its preparation process. Summary of the Invention

[0010] The purpose of this invention is to address the shortcomings of existing technologies by proposing an edge-waterproof encapsulated weather-resistant dimming film and its preparation process.

[0011] To achieve the above objectives, the present invention adopts the following technical solution: This invention first proposes a weather-resistant dimming film with edge waterproofing and encapsulation, comprising: The dimming film body has a curved structure and sequentially includes a first transparent conductive substrate layer, a dimming function layer, and a second transparent conductive substrate layer. An edge waterproof sealing structure is provided at the circumferential edge of the dimming film body, including an inner sealing layer and an outer sealing layer; The inner sealing layer is set close to the circumferential end face of the dimming film body and covers the circumferential edge of the dimming functional layer; The outer sealant layer is disposed outside the inner sealant layer, covers at least a portion of the outer surface of the inner sealant layer, and extends to the surface of the first transparent conductive substrate layer and / or the second transparent conductive substrate layer. The outer sealant layer contains in-situ grown ZIF-8 nanocrystals and a polymer matrix. The ZIF-8 nanocrystals are dispersed in the polymer matrix of the outer sealant layer through zinc-imidazolium coordination bonds. The curvature of the dimming film body is fixed by a heating-shaping-cooling process, and the curvature remains stable within a temperature range of room temperature to 85°C. Preferably, the outer sealant layer is prepared by the following method: Step 1: Preparation of polymer-based adhesive containing zinc nucleation sites: Zinc methacrylate and polyethylene glycol methyl ether methacrylate were dissolved in anhydrous methanol at a molar ratio of 0.3:0.7 to 0.2:0.8. Initiator A and catalyst A were added, and the reaction was carried out at 50-70°C for 12-36 hours under nitrogen protection. After purification by methanol precipitation and drying, ZnDMA-co-PEGMA copolymer was obtained. The zinc methacrylate (ZnDMA) units in the copolymer are covalently bonded to the polymer backbone, achieving Zn 2+ Uniform, localized distribution within the polymer matrix, eliminating the need for additional zinc salt diffusion and infiltration processes.

[0012] These pre-anchored Zn 2+ It can be directly used as a heterogeneous nucleation site for ZIF-8, which greatly reduces the crystallization nucleation energy barrier. Therefore, ZIF-8 nucleation can be triggered under room temperature conditions, and nanocrystal growth can be completed in 2-6 hours. The PEGMA segments in the copolymer have a steric hindrance effect, which can limit the excessive growth of ZIF-8 crystals; at the same time, the density of nucleation sites can be controlled by adjusting the molar ratio of ZnDMA to PEGMA (0.3:0.7 to 0.2:0.8). ZnDMA-co-PEGMA copolymer was mixed with α,ω-dihydroxypolydimethylsiloxane, dimethyl silicone oil and fumed silica in a mass ratio of 5-15:100:10-20:5-15 and vacuum degassed to obtain the base adhesive component A containing zinc nucleation sites. Step 2: Preparation of ligand solution: 2-Methylimidazole was dissolved in anhydrous methanol to prepare a solution with a concentration of 0.5-2.0 mol / L, thus obtaining component B; Step 3: In-situ growth of ZIF-8 nanocrystals: Under nitrogen protection, component B is added to component A to control Zn. 2+ The molar ratio of 2-methylimidazole to Zn is 1:3 to 1:5, and the reaction is carried out with stirring at room temperature for 2-6 hours to allow 2-methylimidazole to react with Zn on the polymer chain. 2+ Coordination was performed to generate ZIF-8 nanocrystals in situ within the polymer matrix, yielding crude sealant. After the addition of 2-methylimidazole, the ligand molecules diffuse to the vicinity of the polymer chain and bind with the anchored Zn. 2+ Coordination occurs, preferentially forming Zn-imidazolium coordination units; as the ligands continue to bind, the coordination units gradually assemble into ZIF-8 crystal nuclei, which then grow into nanocrystals within the spatial confinement of the polymer chain.

[0013] Step 4: Cross-linking and curing: Add crosslinking agent, coupling agent and catalyst B to the crude sealant, stir evenly under vacuum and apply the sealant. Cure for 7-14 days at a temperature of 20-30℃ and a relative humidity of 45-65% to obtain the outer sealant layer. ZIF-8 itself can rapidly crystallize at room temperature under conditions of ligand excess, controlling Zn 2+ With a molar ratio of 1:3-5 to 2-methylimidazolium, it belongs to a typical ligand excess system, which can reduce the nucleation energy barrier and ensure that crystallization can be completed at room temperature; at the same time, the confinement effect of polymer chains avoids excessive grain growth, so that the reaction can reach a stable nanocrystal size within 2-6 hours without the need for high temperature hydrothermal conditions.

[0014] The content of ZIF-8 nanocrystals in the outer sealant layer is 0.7-1.3 wt%.

[0015] ZIF-8 nanocrystals themselves have high modulus and are uniformly distributed in the silicone sealant matrix as a rigid dispersed phase, which can effectively improve the tensile strength and deformation resistance of the sealant; at the same time, the coordination interface can efficiently transfer external forces to the nanocrystals, and the energy is absorbed by the nanocrystals through bearing and the plastic deformation of the matrix, which greatly improves the toughness.

[0016] Preferably, in step one: Initiator A is ethyl 2-bromoisobutyrate, and its dosage is 2-5% of the total molar amount of zinc methacrylate and polyethylene glycol methyl ether methacrylate; Catalyst A is a CuCl / PMDETA system, with a molar ratio of CuCl to PMDETA of 1:1, and the amount of catalyst used is 2-3 times the molar amount of initiator; In step four: The crosslinking agent is methyl tributanone oxime silane, and the amount used is 4-8% of the mass of α,ω-dihydroxypolydimethylsiloxane; The coupling agent is γ-aminopropyltriethoxysilane, and the amount used is 0.5-2% of the mass of α,ω-dihydroxypolydimethylsiloxane; The catalyst B is dibutyltin dilaurate, and its dosage is 0.1-0.5% of the mass of α,ω-dihydroxypolydimethylsiloxane.

[0017] Preferably, The viscosity of the α,ω-dihydroxypolydimethylsiloxane is 5000-8000 mPa·s; The viscosity of the dimethyl silicone oil is 100-350 mPa·s; The specific surface area of ​​the fumed silica is 150-200 m². 2 / g; The ZIF-8 nanocrystals have a particle size of 50-200 nm; The thickness of the outer sealant layer is 0.5-3.0 mm; The thickness of the inner sealant layer is 0.3-1.5 mm; The first transparent conductive substrate layer and the second transparent conductive substrate layer are ITO conductive films or transparent conductive films made of silver nanowires. The dimming functional layer is a polymer-dispersed liquid crystal layer or an electrochromic layer.

[0018] This invention also proposes a process for preparing the aforementioned edge-waterproof encapsulated weather-resistant dimming film, comprising the following steps: S1: Heat the dimming film body to soften it to a malleable state; S2: The heated and softened dimming film body is placed in a curved surface shaping mold for hot pressing and shaping, so that the dimming film body fits the curved surface of the mold cavity of the curved surface shaping mold, and a curved dimming film body with a preset curvature is obtained. S3: Cool the curved dimming film body to fix its curvature; S4: Apply inner sealant and outer sealant sequentially to the circumferential edge of the curved dimming film body after cooling and shaping to form an edge waterproof sealing structure, thus obtaining a weather-resistant dimming film with edge waterproof encapsulation.

[0019] Uniformly dispersed ZIF-8 nanocrystals can extend the penetration path of water vapor and corrosive media in sealant, creating a labyrinth barrier effect and significantly reducing water vapor permeability; at the same time, the hydrophobic porous structure of ZIF-8 itself can also block water molecule penetration.

[0020] Preferably, in step S1, the heat treatment temperature is 80-150°C, and the heating time is 5-30 minutes; In step S2, the hot pressing pressure is 0.1-1.0 MPa, the holding time is 5-20 minutes, and the setting temperature is 60-120℃. In S3, the cooling rate of the cooling process is 1-10℃ / min, and the final cooling temperature is 15-40℃.

[0021] Preferably, the curved surface shaping mold includes an upper mold and a lower mold, which form a mold cavity with a preset curved surface structure when the mold is closed; The upper mold and / or lower mold are provided with a temperature-controlled flow channel, which is connected to a heating medium source and a cooling medium source. In step S1, the dimming film body is heated by introducing a heating medium into the temperature control channel; In step S2, the molding temperature is maintained by a temperature-controlled flow channel under mold closing and pressure holding conditions; In step S3, rapid cooling is achieved by switching the flow of cooling medium into the temperature-controlled flow channel.

[0022] Preferably, in step S4, the inner sealant is applied by applying a first layer of sealant along the circumferential edge of the curved dimming film body, wherein the first layer of sealant at least covers the circumferential end face of the dimming functional layer. The outer sealant is applied as follows: after the inner sealant has cured, a second sealant is applied to the outside of the inner sealant. The second sealant covers at least a portion of the outer surface of the inner sealant and extends to the surface of the first transparent conductive substrate layer and / or the second transparent conductive substrate layer.

[0023] Preferably, step S5 is included after S4: bonding the curved dimming film body to the curved glass substrate, wherein the curvature of the curved glass substrate matches the curvature of the curved dimming film body. The bonding of the laminates is carried out under vacuum conditions, with a bonding temperature of 40-80℃, a bonding pressure of 0.2-0.8MPa, and a holding time of 10-60 minutes.

[0024] Preferably, the heating medium is hot oil or steam, and the temperature is 100-180℃; The cooling medium is cooling water or cooling gas, with a temperature of 5-25℃; The radius of curvature of the cavity of the curved surface shaping mold is 500-5000 mm; The curvature of the curved dimming film body changes by no more than 5% within a temperature range from room temperature to 85°C.

[0025] Compared with the prior art, the beneficial effects of the present invention are: 1. The inner sealant achieves direct physical isolation of the dimming layer end face with extremely low water vapor transmission rate; the microporous structure of ZIF-8 nanocrystals in the outer sealant creates a labyrinth effect, extending the water vapor diffusion path. The outer sealant forms a chemical anchor with the substrate surface through the zinc-imidazolium coordination bonds in the ZnDMA-co-PEGMA copolymer, preventing water molecules from competitively breaking the metal-ligand bonds, thus solving the delamination failure problem caused by water molecule interface substitution in traditional physical adhesives under humid and hot environments.

[0026] 2. The heating stage softens the dimming film to a plastic state, allowing the molecular chains to move. The hot-pressing stage reorients the molecular chains along the curved surface within the confined space of the mold. The cooling stage lowers the temperature at a controllable rate, fixing the oriented structure and achieving a permanent curvature precisely matched to the mold. The film already possesses the target curvature before lamination, preventing additional bending stress during bonding and effectively eliminating stress-induced blistering and delamination.

[0027] 3.Zn 2+ Fixed to the polymer backbone by chemical bonding, ZIF-8 nanocrystals nucleate and grow within the confined space of the polymer matrix, forming a continuous chemical bonding interface with the matrix rather than simple physical mixing, thus avoiding nanofiller agglomeration. ZIF-8 nanocrystals, acting as physical cross-linking nodes, are uniformly dispersed in the polymer network, while their rigid framework effectively constrains molecular chain movement, resulting in improved tensile strength and toughness of the sealant, while reducing water vapor permeability.

[0028] 4. ZIF-8 nanocrystals are connected to the polymer matrix via zinc-imidazolium coordination bonds, which are dynamically reversible non-covalent bonds. When microcracks develop in the sealant, the coordination bonds on the crack surface break, exposing active zinc ions and imidazolium groups; under mild heating conditions, the active groups re-coordinate, causing the crack to heal. This dynamic coordination bonding simultaneously endows the polymer network with stress relaxation capabilities, effectively dissipating internal stresses generated by heat dissipation cycles and mechanical impacts, maintaining the integrity of the sealing structure.

[0029] In summary, this invention uses an inner / outer double-layer chemical anchoring sealing structure to prevent moisture intrusion and delamination, eliminates curved surface bonding stress through a heating-shaping-cooling process, utilizes in-situ growth of ZIF-8 nanocrystals to systematically improve the mechanical and barrier properties of the sealant, and leverages the dynamic coordination bonds of zinc-imidazolium to endow the sealant with self-healing capabilities. This enables the dimming film to possess excellent long-term weather resistance and reliability in curved surface bonding, effectively extending its service life. Attached Figure Description

[0030] Figure 1 This is an SEM image of the crude sealant obtained in Example 1. Detailed Implementation

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0032] I. Basic Unified Preparation Parameters: 1. The main body of the dimming film has a uniform specification: Conductive substrate: transparent conductive film with silver nanowires; Dimming layer: Polymer-dispersed liquid crystal PDLC; Curvature radius of curved mold: 2000mm; Shaping process: heating at 120℃ / 15min, hot pressing at 0.5MPa / 10min, cooling rate at 5℃ / min to 25℃; Inner sealant: One-component epoxy sealant, uniform thickness 0.8mm; External sealant matrix: α,ω-dihydroxysiloxane (6000 mPa) s), dimethyl silicone oil (200mPa) s), Fumed silica (180m) 2 / g); Curing conditions: 23℃, 50% humidity, curing for 10 days; 2. Core evaluation indicators: Sealant mechanics: tensile strength (MPa), elongation at break (%), toughness (MJ / m) 3 ); Waterproof barrier: Water vapor transmission rate WVTR (g / (m)) 2 (24h) The lower the value, the better the waterproofing; Weather resistance: sealing failure rate (%) after xenon lamp aging for 1000 hours; failure criteria: edge water seepage, delamination. Self-healing efficiency: Strength recovery rate (%) after repair at 60℃ / 48h; Curved surface adaptability: Curvature change rate (%) after being placed at 85℃ for 500 hours, ≤5% is acceptable; Long-term damp heat stability: Edge debonding length (mm) after 500 hours of damp heat at 85℃ / 85RH; II. Example: Example 1: ZnDMA:PEGMA molar ratio = 0.2:0.8, ATRP polymerization at 60℃ for 24h; Group A allocation ratio: ZnDMA-co-PEGMA:siloxane:silicone oil:fumed silica = 8:100:12:8; Component B, 2-methylimidazole concentration 1.0 mol / L, Zn 2+ :2-mIm=1:4, in situ growth at room temperature for 3 hours; Crosslinking agent, coupling agent, and catalyst B are added according to the standard of claim 2; The outer adhesive layer is 1.2 mm thick, and the average particle size of ZIF-8 is 60-90 nm.

[0033] Example 2: ZnDMA:PEGMA molar ratio = 0.25:0.75, ATRP polymerization at 60℃ for 24h; Group A allocation ratio: ZnDMA-co-PEGMA:siloxane:silicone oil:fumed silica = 10:100:15:10; Component B, 2-methylimidazole concentration 1.5 mol / L, Zn 2+ :2-mIm=1:4, in situ growth at room temperature for 4 hours; The outer adhesive layer is 1.5 mm thick, and the average particle size of ZIF-8 is 100-140 nm.

[0034] Example 3: ZnDMA:PEGMA molar ratio = 0.3:0.7, ATRP polymerization at 60℃ for 24h; Group A allocation ratio: ZnDMA-co-PEGMA:siloxane:silicone oil:fumed silica = 14:100:18:14; Component B, 2-methylimidazole concentration 2.0 mol / L, Zn 2+ :2-mIm=1:5, in situ growth at room temperature for 6 hours; The outer adhesive layer is 2.0 mm thick, and the average particle size of ZIF-8 is 150-200 nm.

[0035] III. The following six sets of comparative examples were also set up: Comparative Example 1: Pure silicone sealant: without ZnDMA copolymer precursor, without 2-methylimidazolium ligand, only direct cross-linking and curing of the silicone matrix, without nanocrystal reinforcement.

[0036] Comparative Example 2: Physically blended ZIF-8 silicone sealant: In-situ growth was not used; commercially available ZIF-8 nanopowder (particle size 120nm) was directly purchased and mechanically mixed into the silicone matrix. The ZIF-8 addition amount was 5wt%, and the remaining matrix and curing conditions were the same as in Example 2.

[0037] Comparative Example 3: Zn ion crosslinking only, no ZIF-8 crystallization: Component A only added Zn(acac)2, without adding 2-methylimidazole, no ZIF-8 crystals were formed, relying solely on free Zn 2+It is weakly crosslinked with imidazole, and the other ratios are the same as in Example 2.

[0038] Comparative Example 4: Imidazole-free side-chain polymer substrate: comonomer replaced with MMA-co-PEGMA, no Zn metal nucleation sites, and an equal amount of Zn added. 2+ With 2-mIm, uniform ZIF-8 cannot be generated in situ, and only a small amount of free crystals agglomerate.

[0039] Comparative Example 5: High-temperature solvothermal in-situ growth of ZIF-8: After mixing the ZnDMA-co-PEGMA matrix and ligand, ZIF-8 was grown in situ by solvothermal reaction at 80°C for 4 hours. The remaining ratios and loadings were completely consistent with those in Example 2.

[0040] Comparative Example 6: Single-channel sealing structure: Only 0.8mm inner epoxy sealant is applied, all outer sealing layers are eliminated, and the curved dimming film is directly encapsulated.

[0041] Performance testing: Table 1. Performance test results of dimming films in each experimental group Data Analysis: for Figure 1 The dark continuous phase is the polymer matrix, and the bright white particles are the ZIF-8 phase. The surface of the polymer matrix has a small number of micropores and uneven structures. ZIF-8 does not exist in the form of monodisperse nanocrystals, but is dispersed in the matrix as micron-sized aggregates. The overall distribution is relatively uniform, but there is obvious nanocrystal aggregation. The aggregates are independent of each other and do not form a continuous filler network. Unlike the typical ZIF-8 morphology, the polymer chains penetrate into the outer framework of the ZIF-8 crystals, causing the regular cubic structure to have blurred boundaries.

[0042] Comparative Example 1 served as a blank control group for pure silicone sealant without ZIF-8. The key variable between the two was whether in-situ grown ZIF-8 nanocrystals were introduced into the sealant matrix. A comparison between Example 1 and Comparative Example 1 revealed that: Performance data show that Example 1 achieves a comprehensive improvement in overall performance compared to the pure silicone system: tensile strength increased from 1.10 MPa to 1.42 MPa, an increase of 29.1%; fracture toughness increased from 11.6 MJ / m 3 Increased to 18.2 MJ / m 3 The increase was 56.9%; the water vapor transmission rate increased from 22.5 g / (m²). 2 The concentration decreased to 12.8 g / (m²) over 24 hours. 2 (24h), waterproof barrier performance improved by 43.1%; the sealing failure rate after 1000h xenon lamp aging decreased from 18.3% to 8.6%, and weather resistance stability was significantly optimized; the self-healing efficiency at 60℃ / 48h increased from 32% to 82%.

[0043] Rigid ZIF-8 nanocrystals can disperse external loads and construct a labyrinthine moisture barrier path, simultaneously achieving mechanical enhancement and barrier improvement. Furthermore, the zinc-imidazolium dynamic coordination bonds introduced during the in-situ growth process endow the system with self-healing capabilities for microcracks, delaying seal failure. This comparison demonstrates that in-situ growth of ZIF-8 nanocrystals in silicone sealants can simultaneously achieve comprehensive modification of mechanical, waterproof, weather-resistant, and self-healing properties.

[0044] Comparative Example 2 represents the existing mainstream physical blending ZIF-8 modified silicone sealant solution (ZIF-8 addition amount 5wt%). The core variables of both are the introduction method and addition amount of ZIF-8. Their overall performance is at the same level, but each has its own advantages and disadvantages in specific dimensions. A comparison between Example 1 and Comparative Example 2 reveals the following: In terms of weather resistance, the sealing failure rate of Example 1 after 1000 hours of xenon lamp aging was 8.6%, while that of Comparative Example 2 was 9.0%. The in-situ growth scheme showed better weather resistance stability. The in-situ generated ZIF-8 formed a coordination bond interface with the polymer matrix, eliminating the two-phase void defects of the blended system and delaying the intrusion of aging media such as water vapor and ultraviolet light. In terms of mechanical properties, both had their advantages and disadvantages. Comparative Example 2, due to its higher ZIF-8 content, had a slightly higher tensile strength (1.53 MPa) than Example 1 (1.42 MPa). However, Example 1 had a more uniform interfacial bonding, and its elongation at break (415%) was much higher than that of Comparative Example 2 (310%), while its toughness (18.2 MJ / m) was also significantly higher. 3 Comparison Example 2 (16.3 MJ / m 3 The initial water vapor transmission rate of Comparative Example 2 was improved by 11.7%, resulting in better adaptability to curved surfaces; in terms of waterproofing and self-healing performance, the initial water vapor transmission rate of Comparative Example 2 was 10.0 g / (m 2 (24h) is slightly better than Example 1 (12.8g / (m) 2 However, the self-healing efficiency of Example 1 (82%) was significantly higher than that of Comparative Example 2 (68%), and its long-term sealing reliability was more outstanding. This comparison proves that the in-situ growth ZIF-8 technology of this solution can achieve a comprehensive level comparable to existing blending technologies with a lower filling amount, while achieving a slight improvement in weather resistance, and is more advantageous in curved surface adaptation and long-term service scenarios.

[0045] Comparative Example 3 only introduced free zinc ions for coordination crosslinking, without adding 2-methylimidazole to generate complete ZIF-8 crystals. The core variable between the two examples is whether a ZIF-8 crystalline phase structure is formed in the sealant system. A comparison between Example 1 and Comparative Example 3 shows that: Comparative Example 3, lacking the ZIF-8 crystalline phase, showed a significant decline in several properties: tensile strength decreased to 1.24 MPa and toughness decreased to 13.8 MJ / m. 3 All were lower than in Example 1; the water vapor transmission rate increased to 16.4 g / (m²). 2 The failure rate of the xenon lamp increased to 14.7% after 24 hours and 1000 hours, with a significant decrease in waterproof and weather-resistant performance; the self-healing efficiency was only 73%, lower than the 82% in Example 1. The mechanism lies in the free Zn... 2+ The formation of only weak, non-uniform ionic crosslinking points is insufficient to provide the load-bearing reinforcement and labyrinth barrier effect of rigid ZIF-8 nanocrystals. Furthermore, the limited number of coordination sites for free zinc ions results in a weaker dynamic reversible effect compared to the abundant unsaturated zinc sites on the ZIF-8 crystal surface. This comparison demonstrates that the formation of complete ZIF-8 nanocrystals is a necessary condition for achieving mechanical reinforcement, barrier enhancement, and weather resistance optimization in sealants; relying solely on free zinc ion crosslinking cannot achieve the desired modification effect.

[0046] Comparative Example 4 replaced the ZnDMA-co-PEGMA copolymer containing pre-anchored zinc nucleation sites. Without polymer chain-anchored zinc coordination sites, ZIF-8 was generated solely through the reaction of free zinc salt with 2-methylimidazole. The core variable between the two examples is whether the polymer matrix provides in-situ nucleation anchoring sites. A comparison between Example 1 and Comparative Example 4 reveals that: Performance data shows that Comparative Example 4, lacking nucleation anchors, exhibits a comprehensive decline in overall performance: tensile strength 1.31 MPa, toughness 14.5 MJ / m. 3 All were lower than in Example 1; water vapor transmission rate was 14.9 g / (m²). 2 The failure rate of the ZIF-8 crystals (24h) and the xenon lamp failure rate (13.5%) were both higher than those in Example 1; the self-healing efficiency was only 61%, far lower than the 82% in Example 1. The mechanism is that without pre-anchored nucleation sites, ZIF-8 crystals are prone to agglomeration and cannot be uniformly dispersed in the matrix, easily forming interface defects and stress concentration points. Simultaneously, ZIF-8 lacks a chemically bonded interface with the polymer matrix, resulting in low stress transfer efficiency and a significant reduction in the number of dynamic coordination sites that can play a role. This comparison demonstrates that the pre-anchored zinc nucleation sites provided by the ZnDMA-co-PEGMA copolymer are the core foundation for ensuring uniform dispersion of ZIF-8 and forming a strong bonding interface, determining the quality of the ZIF-8 modification effect.

[0047] Comparative Example 5 used a high-temperature solvothermal method to grow ZIF-8 in situ at 80℃, with the variable being the reaction temperature for in-situ growth of ZIF-8. A comparison between Example 1 and Comparative Example 5 shows that: The two materials have similar mechanical properties, but their long-term stability and process compatibility differ significantly: the tensile strength (1.69 MPa) of Comparative Example 5 is slightly higher than that of Example 1, but its elongation at break is only 275%, far lower than the 415% of Example 1, indicating a significant decrease in flexibility; the failure rate after 1000 hours of xenon lamp aging is 9.0%, slightly worse than the 8.6% of Example 1; the debonding length at 85℃ / 500 hours of wet heat is 1.9 mm, higher than the 1.6 mm of Example 1. High-temperature reactions can lead to premature degradation and abnormal cross-linking of some silicone prepolymers, damaging the ductility and aging resistance of the matrix; at the same time, ZIF-8 grains are prone to overgrowth under high-temperature conditions, resulting in decreased dispersion uniformity. In addition, the high-temperature growth process is not suitable for pre-formed curved dimming films, easily causing thermal deformation and excessive curvature of the film. This comparison demonstrates that the room temperature in-situ growth process, while ensuring the modification effect, also has better ductility, weather resistance, and adaptability to curved surface processes. It avoids damage to the sealing substrate and the main body of the dimming film caused by high temperature, and is more suitable for the encapsulation requirements of curved dimming films.

[0048] Comparative Example 6 uses a traditional single-stage epoxy sealing structure without an outer flexible sealing layer containing ZIF-8. The core difference between the two is the edge sealing structure. A comparison between Example 1 and Comparative Example 6 reveals that: The performance of the single-pass epoxy solution is clearly polarized and cannot meet the application requirements of curved dimming films: In terms of short-term static performance, the initial water vapor transmission rate of Comparative Example 6 is 7.2 g / (m²). 2 The epoxy resin exhibited a 24-hour elongation at break (slightly better than Example 1), but its elongation at break was only 85%, indicating extreme brittleness. Under long-term curved surface conditions, the debonding length of Comparative Example 6 at 85℃ / 500h reached 3.8mm, significantly higher than the 1.6mm of Example 1. The failure rate under 1000h xenon lamp aging reached 16.8%, nearly twice that of Example 1. Furthermore, the epoxy system lacks dynamic coordination bonds and self-healing capabilities, making it unable to self-repair microcracks and prone to developing into water seepage channels. This comparison demonstrates that the dual-seal structure of inner epoxy and outer ZIF-8 modified silicone can balance waterproof sealing with adaptability to curved surface deformation, solving the problems of high brittleness and easy cracking failure of traditional single-seal epoxy seals on curved surfaces. It is more suitable for long-term reliable encapsulation of curved dimming films.

[0049] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A weather-resistant dimming film with edge waterproofing and sealing, characterized in that, include: The dimming film body has a curved structure and sequentially includes a first transparent conductive substrate layer, a dimming function layer, and a second transparent conductive substrate layer. An edge waterproof sealing structure is provided at the circumferential edge of the dimming film body, including an inner sealing layer and an outer sealing layer; The inner sealing layer is set close to the circumferential end face of the dimming film body and covers the circumferential edge of the dimming functional layer; The outer sealant layer is disposed outside the inner sealant layer, covers at least a portion of the outer surface of the inner sealant layer, and extends to the surface of the first transparent conductive substrate layer and / or the second transparent conductive substrate layer. The outer sealant layer contains in-situ grown ZIF-8 nanocrystals and a polymer matrix. The ZIF-8 nanocrystals are dispersed in the polymer matrix of the outer sealant layer through zinc-imidazolium coordination bonds. The curvature of the dimming film body is fixed by a heating-shaping-cooling process, and the curvature remains stable within a temperature range of room temperature to 85°C.

2. The weather-resistant dimming film with edge waterproofing encapsulation according to claim 1, characterized in that, The outer sealant layer is prepared by the following method: Step 1: Preparation of polymer-based adhesive containing zinc nucleation sites: Zinc methacrylate and polyethylene glycol methyl ether methacrylate were dissolved in anhydrous methanol at a molar ratio of 0.3:0.7 to 0.2:0.

8. Initiator A and catalyst A were added, and the reaction was carried out at 50-70°C for 12-36 hours under nitrogen protection. After purification by methanol precipitation and drying, ZnDMA-co-PEGMA copolymer was obtained. ZnDMA-co-PEGMA copolymer was mixed with α,ω-dihydroxypolydimethylsiloxane, dimethyl silicone oil and fumed silica in a mass ratio of 5-15:100:10-20:5-15 and vacuum degassed to obtain the base adhesive component A containing zinc nucleation sites. Step 2: Preparation of ligand solution: 2-Methylimidazole was dissolved in anhydrous methanol to prepare a solution with a concentration of 0.5-2.0 mol / L, thus obtaining component B; Step 3: In-situ growth of ZIF-8 nanocrystals: Under nitrogen protection, component B is added to component A to control Zn. 2+ The molar ratio of 2-methylimidazole to Zn is 1:3-5. The reaction is carried out with stirring at room temperature for 2-6 hours to allow 2-methylimidazole to react with Zn on the polymer chain. 2+ Coordination was performed to generate ZIF-8 nanocrystals in situ within the polymer matrix, yielding crude sealant. Step 4: Cross-linking and curing: Add crosslinking agent, coupling agent and catalyst B to the crude sealant, stir evenly under vacuum and apply the sealant. Cure for 7-14 days at a temperature of 20-25℃ and a relative humidity of 45-55% to obtain the outer sealant layer. The content of ZIF-8 nanocrystals in the outer sealant layer is 0.5-10wt%.

3. The edge-waterproof encapsulated weather-resistant dimming film according to claim 2, characterized in that, In step one: Initiator A is ethyl 2-bromoisobutyrate, and its dosage is 2-5% of the total molar amount of zinc methacrylate and polyethylene glycol methyl ether methacrylate; Catalyst A is a CuCl / PMDETA system, with a molar ratio of CuCl to PMDETA of 1:1, and the amount of catalyst used is 2-3 times the molar amount of initiator; In step four: The crosslinking agent is methyl tributanone oxime silane, and the amount used is 4-8% of the mass of α,ω-dihydroxypolydimethylsiloxane; The coupling agent is γ-aminopropyltriethoxysilane, and the amount used is 0.5-2% of the mass of α,ω-dihydroxypolydimethylsiloxane; The catalyst B is dibutyltin dilaurate, and its dosage is 0.1-0.5% of the mass of α,ω-dihydroxypolydimethylsiloxane.

4. The weather-resistant dimming film with edge waterproofing encapsulation according to claim 1, characterized in that, The viscosity of the α,ω-dihydroxypolydimethylsiloxane is 5000-8000 mPa·s; The viscosity of the dimethyl silicone oil is 100-350 mPa·s; The specific surface area of ​​the fumed silica is 150-200 m². 2 / g; The ZIF-8 nanocrystals have a particle size of 50-200 nm; The thickness of the outer sealant layer is 0.5-3.0 mm; The thickness of the inner sealant layer is 0.3-1.5 mm; The first transparent conductive substrate layer and the second transparent conductive substrate layer are ITO conductive films or transparent conductive films made of silver nanowires. The dimming functional layer is a polymer-dispersed liquid crystal layer or an electrochromic layer.

5. A process for preparing a weather-resistant dimming film with edge waterproofing as described in any one of claims 1-4, characterized in that, Includes the following steps: S1: Heat the dimming film body to soften it to a malleable state; S2: The heated and softened dimming film body is placed in a curved surface shaping mold for hot pressing and shaping, so that the dimming film body fits the curved surface of the mold cavity of the curved surface shaping mold, and a curved dimming film body with a preset curvature is obtained. S3: Cool the curved dimming film body to fix its curvature; S4: Apply inner sealant and outer sealant sequentially to the circumferential edge of the curved dimming film body after cooling and shaping to form an edge waterproof sealing structure, thus obtaining a weather-resistant dimming film with edge waterproof encapsulation.

6. The preparation process according to claim 5, characterized in that, In step S1, the heating temperature is 80-150℃ and the heating time is 5-30 minutes; In step S2, the hot pressing pressure is 0.1-1.0 MPa, the holding time is 5-20 minutes, and the setting temperature is 60-120℃. In S3, the cooling rate of the cooling process is 1-10℃ / min, and the final cooling temperature is 15-40℃.

7. The preparation process according to claim 5, characterized in that, The curved surface shaping mold includes an upper mold and a lower mold, which form a mold cavity with a preset curved surface structure when the mold is closed. The upper mold and / or lower mold are provided with a temperature-controlled flow channel, which is connected to a heating medium source and a cooling medium source. In step S1, the dimming film body is heated by introducing a heating medium into the temperature control channel; In step S2, the molding temperature is maintained by a temperature-controlled flow channel under mold closing and pressure holding conditions; In step S3, rapid cooling is achieved by switching the flow of cooling medium into the temperature-controlled flow channel.

8. The preparation process according to claim 5, characterized in that, In S4, the inner sealant is applied by applying a first layer of sealant along the circumferential edge of the curved dimming film body, and the first layer of sealant covers at least the circumferential end face of the dimming functional layer. The outer sealant is applied as follows: after the inner sealant has cured, a second sealant is applied to the outside of the inner sealant. The second sealant covers at least a portion of the outer surface of the inner sealant and extends to the surface of the first transparent conductive substrate layer and / or the second transparent conductive substrate layer.

9. The preparation process according to claim 5, characterized in that, Step S5 is included after S4: the curved dimming film body and the curved glass substrate are laminated together, wherein the curvature of the curved glass substrate matches the curvature of the curved dimming film body. The bonding of the laminates is carried out under vacuum conditions, with a bonding temperature of 40-80℃, a bonding pressure of 0.2-0.8MPa, and a holding time of 10-60 minutes.

10. The preparation process according to claim 7, characterized in that, The heating medium is hot oil or steam, and the temperature is 100-180℃; The cooling medium is cooling water or cooling gas, with a temperature of 5-25℃; The radius of curvature of the cavity of the curved surface shaping mold is 500-5000 mm; The curvature of the curved dimming film body changes by no more than 5% within a temperature range from room temperature to 85°C.