A self-supporting light control film and light control glass

By setting a self-supporting structure and a high-barrier seal at the edge of the dimming film, the "color frame" problem caused by edge stress concentration after the dimming glass is laminated is solved, achieving a long lifespan and stability of the dimming glass, and improving the product's appearance consistency and usage stability.

CN123136931APending Publication Date: 2026-11-20ZHEJIANG JINGYI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611479684.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The existing dimming glass has weak edges after lamination, which leads to stress concentration and causes the decomposition of nanoparticles at the edge of the dimming film, forming an obvious "color frame" phenomenon, affecting the aesthetics and service life.

Method used

A self-supporting structure is set at the edge of the dimming film. Through the support members of a specific width and thickness, the mechanical stress during the lamination process is absorbed and dissipated, preventing stress concentration at the edge of the dimming film. And through the high-barrier sealing members, external factors are prevented from corroding, forming a multi-layer composite sealing structure.

Benefits of technology

It significantly extends the service life of the dimming glass, improves operational stability, avoids the "color frame" phenomenon, and enhances the aesthetic quality and market competitiveness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123136931A_ABST
    Figure CN123136931A_ABST
Patent Text Reader

Abstract

This invention provides a self-supporting dimming film, comprising a first transparent substrate (1), a first transparent conductive layer (3), a light-controlling layer (5), a second transparent conductive layer (4), a second transparent substrate (2), and a support member (6) that wraps around the edge of the dimming film, which are stacked sequentially. The widths of the first transparent substrate (1), the first transparent conductive layer (3), and the light-controlling layer (5) are substantially the same, w1; the widths of the second transparent conductive layer (4) and the second transparent substrate (2) are substantially the same, w2; (w2 - w1) / 2 = d1; the d1 region is the overlap region between the light-controlling layer (5) and the second transparent conductive layer (4), i.e., the d1 region does not include the first transparent substrate (1), the first transparent conductive layer (3), and the light-controlling layer (5); the width of the support member (6) at the outer surface edge of the first transparent substrate (1) is d2; the width of the support member (6) extending from the surface edge of the second transparent conductive layer (4) towards the light-controlling layer (5) to the outside of the dimming film is d3; d1 and d2 are not less than 5. mm, d3 is not less than 2mm; the thickness h of the support (6) is 0.5 to 1.5 times the sum of the thicknesses of the first transparent substrate (1), the first transparent conductive layer (3), the light control layer (5), the second transparent conductive layer (4), and the second transparent substrate (2). This dimming film with edge support can effectively eliminate edge stress during the lamination of dimming glass and subsequent use, thereby suppressing the generation of the "color frame" phenomenon and significantly improving the service life and optical stability of dimming glass products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electronic light control materials, specifically to a self-supporting dimming film and dimming glass. Background Technology

[0002] A dimming film is an electronically controlled light-active film, primarily consisting of a light-controlling layer sandwiched between two transparent conductive films. When an electric field is applied, the arrangement or state of the materials in the light-controlling layer changes, thereby altering the light transmission characteristics of the device, such as switching from low to high transmittance, or vice versa. Through the action of the electric field, rapid transitions between the on and off states can be achieved. Based on different light-controlling mechanisms, dimming films can be classified into suspended particle dimming films, polymer-dispersed liquid crystal dimming films, and electrochemical reaction dimming films, among others. In practical applications, to prevent the influence of external environments on the performance of the dimming film, it is generally encapsulated within materials such as glass.

[0003] Smart glass, an encapsulation structure of a dimming film, is a smart building material with controllable light transmittance. It can quickly switch between transparent and opaque (foggy) states and is widely used in building curtain walls, hotel partitions, office spaces, and automotive sunroofs. Smart glass mainly includes polymer-dispersed liquid crystal (PDLC) smart glass, electrochromic (EC) glass, and suspended particle device (SPD) smart glass, among which PDLC smart glass is the most widely used due to its relatively mature technology and moderate cost. The core structure of PDLC smart glass involves laminating a PDLC dimming film between two layers of glass using an adhesive film (usually PVB or EVA film), forming a single piece through a high-temperature, high-pressure lamination process.

[0004] In practical applications, after long-term use or under specific environmental conditions, a distinct optical chromatic aberration band often appears around the edge of smart glass, differing significantly from the central area; this is known as a "color frame" (or "colored edge," "edge discoloration," or "edge transparent area"). This phenomenon severely impairs the appearance consistency of smart glass, reducing its aesthetic quality and market competitiveness. Compared to batch-to-batch color differences or macroscopic optical defects such as internal glass inhomogeneity, the "color frame" has a distinct regional limitation—its location is clearly defined at the glass edge, and its morphology manifests as a continuous or localized color band extending circumferentially along the smart glass, especially noticeable when observed in a dark (foggy or tinted) state. The formation mechanism of the "color frame" is complex, often involving interactions across multiple levels, including material mechanics, material chemistry, processing technology, and the usage environment, making it a long-standing technical challenge in the smart glass industry.

[0005] Through years of research, the applicant discovered that one cause of the "color frame" phenomenon is the slight decomposition of nanoparticles at the edge of the dimming film induced by external conditions, leading to a decrease in its function and a color difference between the edge and center of the dimming film, thus forming a "color frame." The inducing factor for the "color frame" is that the edge of the dimming glass is relatively thin after lamination, resulting in stress compression. This internal stress exacerbates the decomposition of nanoparticles and induces a tendency for the edge of the dimming film to loosen, leading to poor edge sealing. Currently, there is a lack of effective solutions to the "color frame" phenomenon based on these mechanisms.

[0006] Based on this research, the applicant has developed a self-supporting dimming film and dimming glass, which solves the problem of "color frame" caused by increased internal stress at the edge of the dimming film after lamination when using conventional dimming films to prepare suspended particle dimming glass, polymer dispersed liquid crystal dimming glass and electrochromic dimming glass. Summary of the Invention

[0007] This invention aims to solve the technical problem of "color frame" that occurs when using ordinary dimming films to prepare dimming glass in the prior art. This is because the edges of the dimming glass are relatively thin after lamination, leading to stress compression that exacerbates the decomposition of the dimming components in the film, resulting in a color frame. To address this, this invention provides a self-supporting dimming film. By employing a specific support structure around the dimming film, this invention effectively avoids internal stress at the edges of the film after the lamination process in preparing the dimming glass, fundamentally preventing the formation of a "color frame," significantly extending the service life of the dimming glass, and improving its operational stability.

[0008] In a first aspect, the present invention provides a self-supporting dimming film, comprising a first transparent substrate (1), a first transparent conductive layer (3), a light control layer (5), a second transparent conductive layer (4), a second transparent substrate (2), and a support member (6) that wraps around the edge of the dimming film.

[0009] Among them, the widths of the first transparent substrate (1), the first transparent conductive layer (3) and the light control layer (5) are basically the same, which is w1; the widths of the second transparent conductive layer (4) and the second transparent substrate (2) are basically the same, which is w2; (w2 - w1) / 2 = d1; the d1 region is the overlap region between the light control layer (5) and the second transparent conductive layer (4), that is, the d1 region does not include the first transparent substrate (1), the first transparent conductive layer (3) and the light control layer (5); the width of the support member (6) located at the outer edge of the first transparent substrate (1) is d2; the width of the support member (6) located at the surface edge of the second transparent conductive layer (4) facing the light control layer (5) and extending to the outside of the dimming film is d3; d1 and d2 are not less than 5 mm, and d3 is not less than 2 mm; the thickness h1 of the support member (6) is 0.5 to 1.5 times the sum of the thicknesses of the first transparent substrate (1), the first transparent conductive layer (3), the light control layer (5), the second transparent conductive layer (4) and the second transparent substrate (2).

[0010] Preferably, the widths d1 and d2 of the support member (6) range from 5 to 12 mm, the width d3 ranges from 2 to 5 mm, and the width h1 is 0.8 to 1.2 times the thickness of the dimming film.

[0011] In this invention, if the widths d1 and d2 of the support member (6) are greater than 12mm, it will not have an adverse effect on the dimming performance or on suppressing the "color frame" phenomenon. However, if d1 and d2 are too wide, it will affect the visible area of ​​the dimming glass.

[0012] Furthermore, a support assembly (6-1) is provided on the outer surface edge of the second transparent substrate (2), the width of which is located at the outer surface edge of the second transparent substrate (2) is d4, the width of which extends to the outside of the dimming film is d3, and d4 is less than or equal to d1.

[0013] Furthermore, the thickness h3 of the support component assembly (6-1) ranges from 0.05 to 0.5 mm.

[0014] Furthermore, h3 is 0.1–0.3 mm.

[0015] In this invention, the support member (6) and the support member assembly (6-1) are set with a width of d3 extending beyond the dimming film. The purpose of this is to achieve a better connection between the support member (6) and the support member assembly (6-1), forming a good support effect and a sealing structure.

[0016] Furthermore, the support member (6) wraps around the outer surface edge of the first transparent substrate (1), the side edge of the dimming film and the outer surface edge of the second transparent substrate (2), and the width of the support member (6) at the outer surface edge of the second transparent substrate (2) is d4, and d4 is less than or equal to d1.

[0017] Furthermore, the support member (6) is made of an elastic material with a loss factor tan δ of 0.1 to 2.0.

[0018] Furthermore, the support component assembly (6-1) is made of an elastic material with a loss factor tan δ of 0.1 to 2.0.

[0019] Furthermore, the loss factor tan δ is 0.1 to 1.0.

[0020] Furthermore, the loss factor tan δ is 0.2 to 0.5.

[0021] When the loss factor tan δ of the support member (6) or support member assembly (6-1) is within this range, it can effectively absorb and dissipate the mechanical stress generated during lamination and use, and the stress peak in the edge area can be significantly reduced, thereby avoiding the concentrated transmission of stress to the edge of the dimming film. If tan δ is too small, the material is close to rigid and cannot play a buffering and energy absorption role; if tan δ is too large, the material is too soft and is prone to over-compression deformation during high temperature and high pressure lamination, and cannot provide stable support in the thickness direction.

[0022] Furthermore, the elastic material includes at least one of butyl rubber, brominated butyl rubber, chlorinated butyl rubber, natural rubber, nitrile rubber, hydrogenated nitrile rubber, ethylene propylene diene monomer (EPDM) rubber, fluororubber, and silicone rubber.

[0023] Furthermore, the light control layer (5) is selected from at least one of the suspended particle light control layer, polymer dispersed liquid crystal light control layer, or electrochromic light control layer.

[0024] Furthermore, the light control layer (5) is selected from the suspended particle light control layer.

[0025] Furthermore, a sealing element (7) is provided on the inner side of the support member (6).

[0026] Furthermore, the coverage area of ​​the support member (6) is less than or equal to the coverage area of ​​the seal member (7).

[0027] Furthermore, the sealing element (7) is a barrier tape with a thickness h2 ranging from 0.02 to 0.5 mm.

[0028] Preferably, the range of h2 is 0.05 to 0.1 mm.

[0029] Furthermore, the material of the seal (7) is selected from high-barrier tape.

[0030] Furthermore, the water vapor transmission rate (WVTR) of the high-barrier tape is less than 0.5 g / (m²·d), and the oxygen transmission rate (OTR) is less than 5.0 cm³ / (m²·d·atm).

[0031] Preferably, the water vapor transmission rate (WVTR) is less than 0.4 g / (m²·d) and the oxygen transmission rate (OTR) is less than 4.5 cm³ / (m²·d·atm).

[0032] Furthermore, the high-barrier tape is selected from at least one of polyimide tape, polyester tape, Teflon tape, and aluminum foil tape.

[0033] A second aspect of the present invention provides a self-supporting dimming glass, comprising a first glass and a second glass stacked sequentially, and the aforementioned self-supporting dimming film disposed between the first glass and the second glass; a first interlayer is disposed between the first glass and the self-supporting dimming film, and / or a second interlayer is disposed between the second glass and the self-supporting dimming film.

[0034] Furthermore, the self-supporting dimming glass is laminated.

[0035] Furthermore, the temperature of the lamination process is 90~140℃, the pressure is 0.1~1.5MPa, and the time is 30~240 minutes.

[0036] In this invention, there are no special restrictions on the method of adhesive bonding; any conventional adhesive bonding method in the art is acceptable, such as bonding adhesive in a laminator, autoclave, or adhesive bonding box / furnace.

[0037] After lamination, the thickness difference between the layers is compressed, especially the thickness of the support component is significantly compressed. It is precisely because of this significant compression that the support component forms a good support structure.

[0038] Furthermore, the first glass and / or the second glass are selected from at least one of inorganic glass and organic glass.

[0039] Furthermore, there are no special restrictions on the type of inorganic glass. It can be any conventional transparent glass known to those skilled in the art. It can be ordinary glass or functional glass, such as UV blocking glass, IR blocking glass, Low-E glass, tempered glass or antibacterial glass, etc. It can also be selected from colored glass such as gray glass or brown glass.

[0040] Furthermore, there are no special restrictions on the type of plexiglass; any conventional transparent plexiglass known to those skilled in the art is acceptable. It can be PMMA board, PC board, or functional plexiglass, such as UV-blocking PC board, IR-blocking PC board, etc. It can also be selected from colored plexiglass such as gray plexiglass and brown plexiglass.

[0041] Furthermore, there are no special restrictions on the types of the first and second adhesive layers, and they can be selected from at least one of PVB film, EVA film, TPU film, SGP film, functional PVB film, functional EVA film, functional TPU film, functional SGP film, colored PVB film, colored EVA film, colored TPU film, and colored SGP film.

[0042] Through in-depth research, the inventors have recognized that the fundamental physical mechanism underlying the "color frame" in existing technologies lies in the softening and flow of the glass substrate and intermediate layer (PVB, etc.) during the high-temperature, high-pressure lamination process of smart glass. Because the modulus of the smart film (especially its functional layers, such as PDLC and SPD layers) differs from that of the surrounding adhesive layers, significant stress concentration occurs at the edges. This edge stress physically compresses the microstructure within the smart film; furthermore, this continuous compressive or shear stress acts as a catalyst for the decomposition of functional materials in the functional layers (such as suspended particles in SPD and electrochromic materials in EC), accelerating their failure. This manifests macroscopically as a difference in color or transparency, i.e., the "color frame."

[0043] Based on this understanding of the mechanism, this invention precisely incorporates an elastic support member with a specific width and thickness at the edge of the dimming film. This support member occupies the area that would otherwise be filled by a fluid adhesive layer (such as PVB) during the lamination process. As a pre-installed, somewhat rigid "shield," the support member's thickness is designed to be 0.5 to 1.5 times the thickness of the main body of the dimming film. During the lamination process, when the two layers of glass are pressed together under high temperature and pressure, the pressure is first applied to the support member. Because the support member uses a wear-resistant elastic material, it is neither completely rigid (avoiding crushing the glass) nor completely flexible (avoiding complete flattening). It undergoes controllable elastic deformation, thereby redistributing and absorbing the stress that would otherwise be directly concentrated on the edges of the multi-layered structure of the dimming film. This effectively reduces the direct stress compression on the edges of the light-controlling layer.

[0044] Localized stress can also reduce interfacial adhesion. In this invention, the support member surrounding the edge of the dimming film forms a tight physical barrier. Particularly in the preferred embodiment, a seal made of a high-barrier material is provided on the inner side of the support member; the two together constitute a high-strength, multi-layered composite sealing structure. This structure effectively prevents external moisture, oxygen, or other potentially corrosive small molecules (such as unreacted residual monomers and plasticizers in the PVB adhesive layer) from diffusing along the interfacial gaps to the center of the dimming film under high temperature and high pressure conditions. By eliminating these external inducing factors, the decomposition reaction of the functional materials in the light-control layer is suppressed at the source, thereby maintaining the consistency of performance between the edge and center areas of the dimming film.

[0045] The overlapping region design of this invention, where the second transparent substrate and the second transparent conductive layer are wider than the first transparent substrate, the first transparent conductive layer, and the light-controlling layer, forms a region with a width of d1. This region is a controllable weak interface. Under lamination pressure, this region preferentially undergoes slight relative slippage or deformation, acting as a built-in stress relief groove to effectively dissipate shear stress that might be transmitted to the edge of the light-controlling layer, further protecting the core functional layer. Furthermore, the overlapping region design can minimize the overall thickness of the dimming film while introducing a support function, which is beneficial for the stability of subsequent process conditions.

[0046] In summary, the self-supporting dimming film provided by this invention, by introducing a support body, offsets the edge stress generated during the lamination process of dimming glass, protects the active materials in the dimming film, avoids high-temperature decomposition, and thus avoids the formation of "color frames". It can significantly extend the service life and working stability of dimming glass, and has industrial application value and broad market prospects. Attached Figure Description

[0047] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. The accompanying drawings described below are merely embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.

[0048] Figure 1 This is a schematic diagram of the cross-sectional structure of the dimming film in Embodiment 1 of the present invention;

[0049] Figure 2 This is a schematic diagram of the cross-sectional structure of the dimming film in Embodiment 2 of the present invention;

[0050] Figure 3 This is a schematic diagram of the cross-sectional structure of the dimming film in Embodiment 3 of the present invention;

[0051] Figure 4 This is a schematic diagram of the cross-sectional structure of the dimming film in Embodiment 4 of the present invention;

[0052] Figure 5 This is a schematic diagram of the cross-sectional structure of the dimming film in Embodiment 5 of the present invention;

[0053] Figure 6 This is a schematic diagram of the cross-sectional structure of the dimming film in Embodiment 6 of the present invention;

[0054] Figure 7 A photograph of the color frame generated by the dimming glass in Comparative Example 1 provided by the present invention;

[0055] Wherein, 1 is a first transparent substrate, 2 is a second transparent substrate, 3 is a first transparent conductive layer, 4 is a second transparent conductive layer, 5 is a light-controlling layer, 6 is a support member, 6-1 is a support member assembly, 7 is a sealant, d1 is the width of the overlap area between the light-controlling layer and the second transparent conductive layer, d2 is the width of the support member at the edge of the outer surface of the first transparent substrate, d3 is the width of the support member extending beyond the outer surface of the dimming film, d4 is the width of the support member at the edge of the outer surface of the second transparent substrate, h1 is the thickness of the support member, h2 is the thickness of the sealant, and h3 is the thickness of the support member assembly. Detailed Implementation

[0056] This invention provides a dimming film and dimming glass with stable working performance and a significantly long lifespan.

[0057] In this invention, the concepts of the first transparent substrate, the second transparent substrate, the first transparent conductive layer, the second transparent conductive layer, the first glass, the second glass, the first interlayer, and the second interlayer only indicate the relative relationship between the two, and are not limiting conditions. They do not necessarily have to be a first and second relationship, but can also be an orientation relationship such as up, down, front, back, left, right, etc.

[0058] A support is a combination of support elements and / or support element assemblies.

[0059] In this invention, the width refers to the dimension of the component in the direction parallel to the surface of the dimming glass or dimming film, and the thickness refers to the dimension of the component in the direction perpendicular to the surface of the dimming glass or dimming film.

[0060] Loss factor tan δ test method: The loss factor tan δ is measured using a dynamic mechanical analyzer. The loss factor tan δ value in this invention is the value under the conditions of 30℃ and 1000Hz.

[0061] Oxygen and water vapor transmission rates were tested using a Labthink C401H instrument from Jinan Langguang Electromechanical Technology Co., Ltd., under conditions of 38℃ and 90%RH.

[0062] Measurement of the dimming stability performance ΔT of smart glass: When the smart glass is not powered, the visible light transmittance is recorded as Toff. When the smart glass is connected to the corresponding power supply, the visible light transmittance is recorded as Ton. Therefore, Δt = Ton - Toff. Different smart glasses have different power supplies. For example, suspended particle smart glass can generally be connected to 110V, 60Hz AC power, polymer-dispersed liquid crystal smart glass can generally be connected to 60V, 60Hz AC power, and electrochromic dimming glass can generally be connected to 3V DC power. Specific requirements depend on the product specifications. ΔT = (Δt after aging / Δt before aging) * 100%.

[0063] Evaluation of the "color banding" phenomenon: Accelerated aging tests were conducted in a 100℃ forced-air oven, once daily, until a "color banding" appeared. The dimming glass was switched to a dark state, and under a D65 standard light source and a 3000 LUX plane light source, the presence of a noticeable color banding at the edge of the dimming film was visually observed. The chromaticity data (L, a*, b*) of the edge and center areas of the dimming film in the dimming glass were measured using a HunterLab UltraScan VIS colorimeter. The ΔC between the edge and center areas was calculated as follows: ΔC = (Δa*...) 2 +Δb* 2 ) 1 / 2 When ΔC > 0.5 and the width of the colored frame is greater than 5mm, the time when the colored frame appears is recorded. The later the time when the colored frame appears, the better the performance.

[0064] To better illustrate the present invention, the following specific embodiments are provided.

[0065] Example 1: Preparation of self-supporting dimming film and dimming glass

[0066] A 480 × 480 mm suspended particle dimming film was used. Using a laser processing device, a 10 mm wide area was cut off along the edge of the dimming film from the first transparent substrate (1) of PET, the first transparent conductive layer (3) of ITO, and the suspended particle light-controlling layer (5), so that the width w1 is 460 mm and the width w2 is 480 mm. The calculated d1 = (w2-w1) / 2 = 10 mm is obtained. The thickness of the five-layer dimming film is 0.5 mm.

[0067] The material of the support (6) is chlorinated butyl rubber with a loss factor tan δ of 1.2; the thickness of the support (h1) is 0.75 mm; the width of the support covering the outer edge of the first transparent substrate (1) is d2 = 8 mm; the width of the support covering the overlapping area of ​​the second transparent conductive layer (4) and extending outward is d3 = 3 mm, as shown in Figure 1.

[0068] The support material (6) was applied to a predetermined area by manual bonding to obtain the self-supporting dimming film Example 1.

[0069] Fabrication of self-supporting dimming glass

[0070] The first glass, the first laminated layer, the self-supporting dimming film prepared above, the second laminated layer, and the second glass are stacked sequentially. Both the first and second glass are tempered glass with dimensions of 500mm × 500mm. Both the first and second laminated layers are PVB films.

[0071] The assembled laminated glass was placed in an autoclave for lamination under the following conditions: temperature 120℃, pressure 1.2 MPa, and holding time 120 minutes. After the process was completed, the temperature and pressure were slowly reduced to obtain self-supporting dimming glass, Example 1.

[0072] The obtained dimming glass did not exhibit the "color frame" phenomenon during the 100℃ aging test, and the dimming stability performance ΔT test results are shown in Table 2.

[0073] Example 2: Preparation of self-supporting dimming film and dimming glass

[0074] Similar to Example 1, except that another component, namely the support component (6-1), is provided, which covers the outer surface of the second transparent substrate (2), with a width d4 of 9 mm and a thickness h3 of 0.1 mm, resulting in Example 2 of the self-supporting dimming film, as shown in Figure 2. After lamination, Example 2 of the self-supporting dimming glass is obtained. The obtained dimming glass did not exhibit the "color frame" phenomenon in the 100℃ aging test, and its dimming stability performance ΔT test results are shown in Table 2.

[0075] Example 3: Preparation of self-supporting dimming film and dimming glass

[0076] Similar to Example 1, but the light-controlling layer (5) is an electrochromic layer (EC); the material of the support (6) is silicone rubber, the loss factor tan δ is 0.9, and the thickness is 0.65 mm; the support (6) covers the outer surface of the first transparent substrate (1), the entire side of the dimming film, and the outer surface of the second transparent substrate (2), with d1 being 10 mm, d2 being 8 mm, d3 being 0.65 mm (the thickness of the support (6)), and d4 being 8 mm, thus obtaining the self-supporting dimming film Example 3, as shown in Figure 3; the lamination process parameters are adjusted to 140℃, 0.8 MPa, and 60 minutes, thus obtaining the self-supporting dimming glass Example 3. The obtained dimming glass did not show the "color frame" phenomenon in the 100℃ aging test, and its dimming stability performance ΔT test results are shown in Table 2.

[0077] Example 4: Preparation of self-supporting dimming film and dimming glass

[0078] Similar to Example 1, but the light control layer (5) is PDLC and the total thickness of the dimming film is 0.55 mm. The support (6) is made of EPDM rubber with a loss factor tanδ of 1.4, a thickness of 0.66 mm, d2 of 8 mm, and d3 of approximately 0. That is, the support (6) only wraps the first transparent substrate (1) and the sides and overlapping areas of the light control layer (5). A layer of polyimide tape is attached to the inside of the support (6) (near the dimming film body) as a sealant (7). The sealant (7) is 0.1 mm thick, with a water vapor transmission rate (WVTR) of 0.4 g / (m²·d) and an oxygen transmission rate (OTR) of 4.1 cm³ / (m²·d·atm). The sealant (7) completely wraps the sides of the dimming film and the outer surface of the second transparent substrate (2), thus obtaining the self-supporting dimming film Example 4, as shown in Figure 4. The lamination process involved a temperature of 120℃, a pressure of 1.0MPa, and a holding time of 120 minutes to obtain self-supporting dimming glass, Example 4. The resulting dimming glass did not exhibit a "color frame" phenomenon during the 100℃ aging test, and its dimming stability performance ΔT test results are shown in Table 2.

[0079] Example 5: Preparation of self-supporting dimming film and dimming glass

[0080] Similar to Example 2, but Teflon tape was used as a sealant (7) on the inner side of the support (6) (near the main body of the dimming film). Its water vapor transmission rate (WVTR) was 0.31 g / (m²·d), oxygen transmission rate (OTR) was 2.3 cm³ / (m²·d·atm), and the thickness of the sealant (7) was 0.3 mm. The sealant (7) wrapped the sides and overlapping area of ​​the first transparent substrate (1) and the light control layer (5), thus obtaining Example 5 of the self-supporting dimming film, as shown in Figure 5. After lamination, Example 5 of the self-supporting dimming glass was obtained. The obtained dimming glass did not show the "color frame" phenomenon in the 100℃ aging test, and the dimming stability performance ΔT test results are shown in Table 2.

[0081] Example 6: Preparation of self-supporting dimming film and dimming glass

[0082] Similar to Example 3, but the light control layer (5) is a polymer-dispersed liquid crystal layer with a thickness of 0.35 mm; the support member (6) is made of butyl rubber with a loss factor tanδ of 0.6, a thickness of 0.50 mm, d1 of 10 mm, d2 of 8 mm, d3 of 0.50 mm (the thickness of the support member (6)), and d4 of 8 mm; a layer of PET tape is attached to the inside of the support member (6) (near the main body of the dimming film) as a seal (7), with a water vapor transmission rate (WVTR) of 0.45 g / (m²·d) and an oxygen transmission rate (OTR) of 4.8 cm³ / (m²·d·atm), and the seal (7) has a thickness of 0.2 mm. The seal (7) completely covers the dimming film side of the outer surface of the first transparent substrate (1) and the outer surface of the second transparent substrate (2), thus obtaining the self-supporting dimming film Example 6, as shown in Figure 6. The lamination process parameters were adjusted to a temperature of 90℃, a pressure of 0.5MPa, and a holding time of 180 minutes, with the rest being the same as in Example 3, resulting in self-supporting dimming glass Example 6. The obtained dimming glass did not exhibit a "color frame" phenomenon during the 100℃ aging test, and its dimming stability performance ΔT test results are shown in Table 2.

[0083] Comparative Example 1

[0084] The process was basically the same as in Example 1, except that the support component (6) was not provided. Instead, a commercially available ordinary SPD dimming film (thickness 0.5 mm, size 480×480 mm) was directly placed between two layers of PVB film and glass for lamination. The process conditions were the same as in Example 1, resulting in Comparative Example 1 of dimming film and dimming glass. The obtained dimming glass showed obvious "color frame" phenomenon in the 100℃ aging test. The dimming stability performance ΔT test results are shown in Table 2.

[0085] Comparative Example 2

[0086] The results were basically the same as in Example 1, except that the thickness of the support (6) was 0.1 mm, and the other parameters remained unchanged, resulting in Comparative Example 2 of dimming film and dimming glass. The dimming glass obtained showed obvious "color frame" phenomenon in the 100℃ aging test, and the dimming stability performance ΔT test results are shown in Table 2.

[0087]

[0088] Table 1 lists the structural parameters of the dimming films prepared in Examples 1-6 and Comparative Examples 1-2.

[0089] To systematically verify the technical advantages of the self-supporting dimming film and its dimming glass provided by this invention, comparative tests were conducted on the dimming glass samples prepared in Examples 1-6 and Comparative Examples 1-2. The test items included initial dimming performance (ΔT), the time of occurrence of the "color frame" phenomenon after high-temperature accelerated aging, and ΔC. Specific results are summarized in Table 2.

[0090]

[0091] The performance test results of the above embodiments and comparative examples clearly show that the present invention can effectively eliminate the edge internal stress generated in the lamination process and service of the dimming glass by making the thickness and elastic parameters of the edge support (6) meet a specific matching relationship. Compared with conventional products, the edge color difference of the embodiments of the present invention is significantly reduced after accelerated aging test, proving that it can fundamentally suppress or delay the generation of "color frame" defects. Furthermore, when used with a high-barrier sealing element (7), the long-term optical stability is improved by a greater margin. In Examples 4 to 6, after 1500h aging, ΔT is greater than 90%. The dimming glass obtained after 1500h aging has ΔT greater than 90%. Although Comparative Example 2 also has a support, due to insufficient thickness design, it failed to form an effective support structure, so it still could not avoid the "color frame" phenomenon.

[0092] The descriptions of the above embodiments are merely illustrative of the methods and core ideas of the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A self-supporting dimming film, characterized in that, It includes a first transparent substrate (1), a first transparent conductive layer (3), a light control layer (5), a second transparent conductive layer (4), a second transparent substrate (2), and a support member (6) that wraps around the edge of the dimming film. Among them, the widths of the first transparent substrate (1), the first transparent conductive layer (3) and the light control layer (5) are basically the same, which is w1; the widths of the second transparent conductive layer (4) and the second transparent substrate (2) are basically the same, which is w2; (w2 - w1) / 2 = d1; the d1 region is the overlap region between the light control layer (5) and the second transparent conductive layer (4), that is, the d1 region does not include the first transparent substrate (1), the first transparent conductive layer (3) and the light control layer (5); the width of the support member (6) located at the outer edge of the first transparent substrate (1) is d2; the width of the support member (6) located at the surface edge of the second transparent conductive layer (4) facing the light control layer (5) and extending to the outside of the dimming film is d3; d1 and d2 are not less than 5 mm, and d3 is not less than 2 mm; the thickness h1 of the support member (6) is 0.5 to 1.5 times the sum of the thicknesses of the first transparent substrate (1), the first transparent conductive layer (3), the light control layer (5), the second transparent conductive layer (4) and the second transparent substrate (2).

2. The self-supporting dimming film according to claim 1, characterized in that, The outer surface edge of the second transparent substrate (2) is provided with a support component (6-1), the width of which is located at the outer surface edge of the second transparent substrate (2) is d4, the width of which extends to the outside of the dimming film is d3, and d4 is less than or equal to d1.

3. The self-supporting dimming film according to claim 1, characterized in that, The support member (6) wraps the outer edge of the first transparent substrate (1), the side of the dimming film and the outer edge of the second transparent substrate (2). The width of the support member (6) at the outer edge of the second transparent substrate (2) is d4, and d4 is less than or equal to d1.

4. The self-supporting dimming film according to claim 1, characterized in that, The support (6) is made of an elastic material with a loss factor tan δ of 0.1 to 2.

0.

5. The self-supporting dimming film according to claim 4, characterized in that, The elastic material includes at least one of butyl rubber, brominated butyl rubber, chlorinated butyl rubber, natural rubber, nitrile rubber, hydrogenated nitrile rubber, ethylene propylene diene monomer (EPDM) rubber, fluororubber, silicone rubber, and styrene-based thermoplastic elastomers.

6. The self-supporting dimming film according to claim 1, characterized in that, The light control layer (5) is selected from at least one of the suspended particle light control layer, polymer dispersed liquid crystal light control layer, or electrochromic light control layer.

7. The self-supporting dimming film according to claim 1, characterized in that, A sealing element (7) is provided on the inner side of the support member (6).

8. The self-supporting dimming film according to claim 7, characterized in that, The coverage area of ​​the support (6) is less than or equal to the coverage area of ​​the seal (7).

9. The self-supporting dimming film according to claim 7, characterized in that, The sealing element (7) is a barrier tape with a thickness h2 ranging from 0.02 to 0.5 mm.

10. The self-supporting dimming film according to claim 9, characterized in that, The barrier tape is selected from at least one of polyimide tape, polyester tape, Teflon tape, and aluminum foil tape.

11. A self-supporting dimming glass, characterized in that, It includes a first glass and a second glass stacked in sequence, and a self-supporting dimming film as described in any one of claims 1 to 10 disposed between the first glass and the second glass; a first interlayer is disposed between the first glass and the self-supporting dimming film, and / or a second interlayer is disposed between the second glass and the self-supporting dimming film.

12. The self-supporting dimming glass according to claim 11, characterized in that, The dimming glass needs to undergo an adhesive bonding process. The bonding process is carried out at a temperature of 90~140℃, a pressure of 0.1~1.5MPa, and a time of 30~240 minutes.