Low-hygroscopic positive photosensitive polyimide resin composition glue and preparation method and application thereof

By optimizing the composite resin system and components, the problems of moisture absorption and dielectric properties of positive photosensitive polyimide resin in high-frequency integrated circuit packaging were solved, achieving a synergistic effect of low-temperature curing, low moisture absorption, excellent photolithography processability, and high bonding strength.

CN123136958APending Publication Date: 2026-11-20BEIJING KEGUANG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611393817.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing positive photosensitive polyimide resin compositions suffer from high moisture absorption, deteriorated dielectric properties, insufficient photolithography resolution, and insufficient bonding strength in high-frequency integrated circuit packaging, making it difficult to simultaneously meet the requirements of low moisture absorption, low-temperature curing, high resolution, and high bonding strength.

Method used

By designing a composite resin system containing phenolic hydroxyl polyamide ester-1 and phenolic hydroxyl polyamide ester-2, hydrophobic aliphatic segments are introduced. The high reactivity of polyamide ester and the synergistic effect of the amide group of polyamide resin are utilized to optimize the components of photoacid generator, thermal crosslinker and sensitizer, forming a low moisture absorption positive photosensitive polyimide resin composition.

Benefits of technology

This technology achieves low moisture absorption in low-temperature curing resin films, reduces dielectric constant and dielectric loss, improves photolithography processability and copper bonding strength, and meets the requirements of multilayer metal wiring in high-frequency integrated circuit packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_11
    Figure SMS_11
  • Figure SMS_12
    Figure SMS_12
Patent Text Reader

Abstract

The application belongs to the technical field of high polymer materials, and particularly relates to a low-humidity-absorption positive photosensitive polyimide resin glue solution and a preparation method and application thereof. By introducing a hydrophobic fatty chain segment into a resin main chain structure of a phenolic hydroxyl polyamide acid ester-1, the hydrophobicity of a positive photosensitive polyimide cured film is improved, the humidity absorption rate is reduced, and the dielectric constant and dielectric loss of the cured resin film are reduced. By compounding the phenolic hydroxyl polyamide acid ester-1 and a phenolic hydroxyl polyamide resin-2 to form a composite resin system, the high reactivity of the ester group of the polyamide acid ester at low temperature and the synergistic effect of the amide group of the polyamide resin are utilized, the problems of low-temperature curing of the positive photosensitive resin and high heat resistance, high photoetching resolution and high chemical resistance are solved, the synergistic technical effects of excellent photoetching process of the positive photosensitive polyimide and high copper surface adhesion are realized, and the multi-layer metal wiring manufacturing process requirements of radio frequency integrated circuit packaging can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials technology, specifically relating to a low moisture absorption positive photosensitive polyimide resin composition liquid, its preparation method and application. Background Technology

[0002] With the rapid development of 5G mobile communication technology and emerging industries such as artificial intelligence and the Internet of Things, the integration and complexity of high-frequency integrated circuits have increased dramatically. In advanced packaging technologies, especially in multilayer metal interconnect processes for wafer-level packaging (WLP) and panel-level packaging (PLP), interlayer dielectric insulating materials play a crucial role. To meet the demands of high-speed, low-distortion transmission of high-frequency signals, these materials must possess both extremely low dielectric constants and dielectric losses. However, the dielectric properties of polymer materials are extremely sensitive to their moisture content; adsorbed water molecules significantly increase the dielectric constant and loss factor. Therefore, endowing dielectric materials with ultra-low hygroscopic properties has become a key challenge in developing next-generation high-frequency packaging materials.

[0003] Currently, photosensitive polyimide (PSPI) resin is one of the most widely used materials in this field, especially low-temperature positive photosensitive polyimide (p-PSPI) that can be cured at ≤230℃, which has attracted much attention due to its high photolithographic precision and good process compatibility. However, existing low-temperature curing p-PSPI materials have revealed significant performance shortcomings in practical applications: on the one hand, the moisture absorption rate of traditional p-PSPI cured films is generally high, which leads to a sharp deterioration in their dielectric properties at high frequencies, failing to meet application requirements; on the other hand, the introduction of a large number of hydrophobic segments to reduce moisture absorption often impairs the material's photolithographic resolution, heat resistance, chemical resistance, and critical adhesion strength to the copper substrate.

[0004] To overcome these problems, the industry has proposed several solutions. For example, Tory Corporation of Japan disclosed a positive photosensitizing composition based on organosiloxane resin, which has excellent photosensitivity, but its resin backbone structure differs from that of polyimide, making it difficult to meet the comprehensive requirements of high heat resistance and high mechanical strength for encapsulation materials. The US-Japan joint venture HD Corporation proposed using a mixture of polybenzimidazole precursor and phenolic resin to improve solderability, but the complexity of its formulation and lithography resolution still have room for improvement. Furthermore, Hitachi Chemical DuPont Microsystems of Japan reported a polyimide precursor composition formed by the condensation polymerization of aromatic diester diacyl chloride and phenolic hydroxyl diamine. This approach focuses on chip surface protection but does not resolve the contradiction between low moisture absorption, high adhesion, and high resolution.

[0005] In summary, existing positive photosensitive resin compositions fail to simultaneously meet the stringent requirements of high-frequency integrated circuit packaging for interlayer dielectric materials: namely, achieving low-temperature curing (≤230°C), high resolution, high resistance to damp heat, and excellent adhesion strength to the copper interface while ensuring low moisture absorption. The mutual constraints among these properties constitute the core bottleneck hindering the development of high-density, high-frequency packaging technologies. Summary of the Invention

[0006] To address the aforementioned technical problems, this invention provides a low-moisture-absorbing positive photosensitive polyimide resin composition liquid, its preparation method, and its application. By designing a composite resin system with a specific structure and synergistically optimizing other components, this invention fundamentally resolves the aforementioned performance contradictions, thereby obtaining a low-moisture-absorbing interlayer dielectric material with excellent comprehensive performance suitable for advanced packaging of high-frequency integrated circuits.

[0007] This invention improves the hydrophobicity and reduces the moisture absorption rate of the p-PSPI cured film by introducing hydrophobic aliphatic segments into the main chain structure of a resin containing phenolic hydroxyl polyamate-1, thereby significantly reducing the dielectric constant and dielectric loss of the cured resin film. Simultaneously, by compounding phenolic hydroxyl polyamate-1 with phenolic hydroxyl polyamide resin-2 to form a composite resin system, the high reactivity of the arylate groups of the polyamate at low temperatures and the synergistic effect of the amide groups of the polyamide resin effectively solve the challenges of low-temperature curing and the interplay between high heat resistance, high photolithography resolution, and high chemical resistance in positive photosensitive resins. This achieves a synergistic effect of excellent photolithography processability and high copper adhesion for PSPI, meeting the requirements of multilayer metal wiring fabrication processes for RF integrated circuit packaging.

[0008] This invention is specifically achieved through the following technical solutions: The first objective of this invention is to provide a low-moisture-absorbing, positively photosensitive polyimide resin composition liquid, made from the following raw materials in parts by weight: (A) 100 parts of phenolic hydroxyl polyaminate resin-1 and phenolic hydroxyl polyaminate resin-2; wherein the weight ratio of phenolic hydroxyl polyaminate resin-1 to phenolic hydroxyl polyaminate resin-2 is 99:1 to 50:50.

[0009] (B) Photo-induced acid-producing agent; 3-40 parts; (C) Thermal crosslinking agent; 3-40 parts; (D) Thermally induced acid-producing agent; 0.1-20 parts; (E) Sensitive agent; 3-40 parts; (F) Organic solvent; (G) Tackifier; 3-40 parts.

[0010] The solid content in the positive photosensitive resin solution is 15 wt.%~45 wt.%, and the solution viscosity at room temperature is 500 mPa.s~4000 mPa.s.

[0011] The structural formula of hydroxyl-containing polyamic acid ester resin-1 is shown below: Where: m = 2~50; X1 is selected from one of the following structures: , n = 1 or 2; Y1 is selected from one of the following structures: , R1 is an aliphatic chain, preferably a straight-chain alkane containing C1 to C8, and E1 is a reactive end-capping group. The structural formula of phenolic hydroxyl polyamic acid ester resin-2 is shown below: Where: n = 2~50; X2 is selected from one of the following structures: ; Y2 is selected from one of the following structures: , R2 is an aliphatic chain, preferably a straight-chain alkane containing C1 to C8; E2 is a reactive end-capping group.

[0012] Preferably, the preparation method of the above-mentioned phenolic hydroxyl polyamate resin-1 includes the following steps: (1) Aromatic tetracarboxylic dianhydride-1 is reacted with fatty alcohols under heating conditions to generate aromatic diacid diesters; (2) Then, the generated aromatic diacid diester reacts with thionyl chloride to generate aromatic diester diacyl chloride; (3) Aromatic diester diacyl chloride and phenol-hydroxyl-containing aromatic diamine-1 are reacted in an organic solvent via a condensation reaction in the presence of a reactive end-capping agent to generate a phenol-hydroxyl-containing polyamic acid ester resin solution. The resin is precipitated in a poor solvent, separated, and thoroughly washed to obtain a solid resin. After heating and vacuum drying, phenol-hydroxyl-containing polyamic acid ester resin (PAE-1) is obtained, with a GPC molecular weight of 1.0 × 10⁻⁶. 4 Up to 3.0×10 4 .

[0013] The molar ratio of aromatic tetracarboxylic dianhydride-1, fatty alcohol, thionyl chloride and phenolic hydroxyl-containing aromatic diamine-1 is 1:2:2:1.

[0014] In the preparation method of phenolic hydroxyl polyaminate resin-1, the aromatic tetracarboxylic dianhydride-1 includes 2,2-bis(3,4-dicarboxylphenyl)propane dianhydride (1BCDA, 187-188). o C, Mw=332.21); 2,4-Bis(3,4-dicarboxylphenyl)-2,4-dimethylpentane dianhydride (2BMDA, 166-167) o C, Mw=486.32); 2,7-Bis(3,4-dicarboxylphenyl)-2,7-dimethyloctane dianhydride, 3BODA, 166-167 o C, Mw=486.32); 2,7-Bis(3,4-dicarboxylphenyl)-2,7-dimethyldodecane dianhydride (2,7-Bis(3,4-dicarboxylphenyl)-2,19-dimethyldodecane dianhydride, 4BDDA, 121-126 o C,598.41), 4,4'-Isopropylidenediphenyl bis(trimellitate)dianhydride, 5IPDA, mp192-193 o C, 576.36) and mixtures thereof in any proportion.

[0015] In the preparation method of phenolic hydroxyl polyaminate resin-1, the phenolic hydroxyl aromatic diamine-1 includes 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17), 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane (abbreviated as: 4-HFAP, Mw=366.17), 2,2-bis(3-amino-4-hydroxyphenyl)propane (abbreviated as: 3-BAPP, Mw=258.17), bis(4-amino-3-hydroxyphenyl)methane (abbreviated as: 4BAPP, Mw=258.17), and 2,2'-bis[N-(3-aminobenzoamide)-3-amino-4-hydroxyphenyl]hexafluoropropane (abbreviated as: 3HFHA, Mw=604.32), 2,2'-bis[N-(4-aminobenzoylamino)-3-amino-4-hydroxyphenyl]hexafluoropropane (abbreviated as: 4HFHA, Mw=604.32), 1,3-bis(3-aminopropyl)tetramethyldisiloxane (4MSiNA), 1,3-bis(3-aminopropyl)tetraphenyldisiloxane (4BSiNA), 1,3-bis(3-aminophenoxy)tetramethyldisiloxane (3M2SiA) and 1,3-bis(4-aminophenoxy)tetramethyldisiloxane (4MSiA) and mixtures thereof in any proportion.

[0016] In the preparation method of phenolic hydroxyl polyamic acid ester resin-1, the organic solvent includes N'N dimethylformamide, N'N dimethylacetamide, N-methyl-ε-caprolactam, N-methylpyrrolidone, γ-butyrolactone, ethyl lactate, 1,3-dimethyl-2-imidazolium ketone, dimethyl sulfoxide, dimethyl sulfone, tetramethylene sulfone, tetramethylurea, phenol, m-cresol, ethyl acetate, butyl acetate, sulfolane, p-cresol, 3-chlorophenol, 4-chlorophenol, tetrahydrofuran, ethyl 3-ethoxypropionate, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc., and mixtures thereof in any proportion.

[0017] In the preparation method of phenolic hydroxyl polyaminate resin-1, the reactive end-capping agent includes maleic anhydride, 4-aminobenzocyclobutene, 4-vinylaniline, norbornene, allylamine, 4-ethynylphthalic anhydride, 4-phenylethynylphthalic anhydride, 4-ethynylaniline, 3-ethynylaniline, 3-phenylethynylaniline, 4-phenylethynylaniline, 4-(4-aminophenylethynyl)phenylethynyl, 4-[(trimethylsilyl)ethynyl]aniline, 4-(4-amino-phenyl)-2-methyl-but-3-yn-2-ol, (E)-3-aminocinnamic acid, propargylamine, and mixtures thereof in any proportion.

[0018] In the preparation method of phenolic hydroxyl polyamide ester resin-1, unsuitable solvents include deionized water, methanol, ethanol, hexane, butyl cellosolve, toluene, and mixtures thereof in any proportion.

[0019] A preferred method for preparing phenolic hydroxyl polyamic acid ester resin-2 includes the following steps: (1) Aromatic tetracarboxylic dianhydride-2 is reacted with fatty alcohols under heating conditions to generate aromatic diacid diesters; (2) Then, the generated aromatic diacid diester reacts with thionyl chloride to generate aromatic diester diacyl chloride; (3) Aromatic diester diacyl chloride and phenol-hydroxyl-containing aromatic diamine-2 are subjected to a polycondensation reaction in an organic solvent in the presence of a reactive end-capping agent to generate a phenol-hydroxyl-containing polyamic acid ester resin solution. The resin was precipitated in a poor solvent, separated, and thoroughly washed to obtain a solid resin. After heating and vacuum drying, a phenolic hydroxyl polyaminate resin (PAE-2) was obtained, with a GPC molecular weight of 1.0 × 10⁻⁶. 4 Up to 3.0×10 4 .

[0020] The molar ratio of aromatic tetracarboxylic dianhydride-2, fatty alcohol, thionyl chloride and phenolic hydroxyl-containing aromatic diamine-2 is 1:2:2:1.

[0021] In the preparation method of phenolic hydroxyl polyamic acid ester resin-2, aromatic tetracarboxylic dianhydride-2 includes 2,3,2',3'-diphenyl ether tetracarboxylic dianhydride (abbreviated as: 23ODPA), 2,3',3,4'-diphenyl ether tetracarboxylic dianhydride (abbreviated as: 34ODPA), 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (abbreviated as: 44ODPA), and pyromellitic dianhydride (abbreviated as: PMDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (44BTDA), 2,3',3,4'-benzophenone tetracarboxylic dianhydride (34BTDA), 2,3',2,3'-benzophenone tetracarboxylic dianhydride (33BTDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (44BPDA), 2,3',3,4'-biphenyltetracarboxylic dianhydride (34BPDA), 2,3',2,3'-biphenyltetracarboxylic dianhydride (33BPDA), 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (44ODDA)|、2,3' 3,4'-Diphenyl ether tetracarboxylic dianhydride (34ODDA), 2,3',2,3'-Diphenyl ether tetracarboxylic dianhydride (33ODDA), 3,3',4,4'-Diphenyl sulfone tetracarboxylic dianhydride (44DSDA), 2,3',2,3'-Diphenyl sulfone tetracarboxylic dianhydride (33DSDA), 3,3',4,4'-Diphenyl sulfide tetracarboxylic dianhydride (44TDPA), 2,3',2,3'-Diphenyl sulfide tetracarboxylic dianhydride (TDPA), 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane (6FDA) and mixtures thereof in any proportion.

[0022] In the preparation method of phenolic hydroxyl polyaminate resin-2, the phenolic hydroxyl aromatic diamine-2 includes 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17), 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane (abbreviated as: 4-HFAP, Mw=366.17), 2,2-bis(3-amino-4-hydroxyphenyl)propane (abbreviated as: 3-BAPP, Mw=258.17), bis(4-amino-3-hydroxyphenyl)methane (abbreviated as: 4BAPP, Mw=258.17), and 2,2'-bis[N-(3-aminobenzoamide)-3-amino-4-hydroxyphenyl]hexafluoropropane (abbreviated as: 3HFHA, Mw=604.32), 2,2'-bis[N-(4-aminobenzoylamino)-3-amino-4-hydroxyphenyl]hexafluoropropane (abbreviated as: 4HFHA, Mw=604.32), 1,3-bis(3-aminopropyl)tetramethyldisiloxane (4MSiNA), 1,3-bis(3-aminopropyl)tetraphenyldisiloxane (4BSiNA), 1,3-bis(3-aminophenoxy)tetramethyldisiloxane (3M2SiA) and 1,3-bis(4-aminophenoxy)tetramethyldisiloxane (4MSiA) and mixtures thereof in any proportion.

[0023] In the preparation method of phenolic hydroxyl polyamic acid ester resin-2, the organic solvent includes N'N dimethylformamide, N'N dimethylacetamide, N-methyl-ε-caprolactam, N-methylpyrrolidone, γ-butyrolactone, ethyl lactate, 1,3-dimethyl-2-imidazolium ketone, dimethyl sulfoxide, dimethyl sulfone, tetramethylene sulfone, tetramethylurea, phenol, m-cresol, ethyl acetate, butyl acetate, sulfolane, p-cresol, 3-chlorophenol, 4-chlorophenol, tetrahydrofuran, ethyl 3-ethoxypropionate, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc., and mixtures thereof in any proportion.

[0024] In the preparation method of phenolic hydroxyl polyamic acid ester resin-2, the reactive end-capping agent includes maleic anhydride, 4-aminobenzocyclobutene, 4-vinylaniline, norbornene, allylamine, 4-ethynyl phthalic anhydride, 4-phenylethynyl phthalic anhydride, 4-ethynyl aniline, 3-ethynyl aniline, 3-phenylethynyl aniline, 4-phenylethynyl aniline, 4-(4-aminophenylethynyl)phenylethynyl, 4-[(trimethylsilyl)ethynyl]aniline, 4-(4-amino-phenyl)-2-methyl-but-3-yn-2-ol, (E)-3-aminocinnamic acid, propargylamine, and mixtures thereof in any proportion.

[0025] In the preparation method of phenolic hydroxyl polyamide ester resin-2, unsuitable solvents include deionized water, methanol, ethanol, hexane, butyl cellosolve, toluene, and mixtures thereof in any proportion.

[0026] Preferably, the photoacid-producing agents include ① diazonoquinone compounds, ② iodonium salt compounds, and ③ sulfonium salt compounds.

[0027] Considering the effects of inhibiting the solubility of the resin film in the unexposed area and the high solubility of the resin film in the exposed area, diazonaquinone compounds are preferred, including compounds (B1) generated by esterification of diazonaquinone sulfonic acid and polyhydroxy compounds; compounds (B2) generated by sulfonation of diazonaquinone sulfonic acid and polyamine compounds; and compounds (B3) generated by esterification and / or sulfonation of diazonaquinone sulfonic acid and polyhydroxy polyamine compounds. The proportion of diazonaquinone sulfonic acid substituted in the polyhydroxy polyamine compounds is 30% to 90%, preferably 50% to 90%. The diazonaquinone compounds include 1,2-diazonaphthoquinone-5-sulfonyl compounds and 1,2-diazonaphthoquinone-4-sulfonyl compounds, such as 2,3,4-trihydroxybenzophenone-1,2-diazonaphthoquinone-5-sulfonate. The polyhydroxy compounds mentioned include Bis-Z, BisP-EZ, BisP-AP, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, Methylenetris-FR-CR, BisRS-26X, and DML. -MBPC, DML-MBOC, DML-OCHP, DML-PCHP, DML-PC, DML-PTBP, DML-34X, DML-EP, DML-POP, Dimethylol-BisOC-P, DML-PFP, D ML-PSBP, DML-MTrisPC, TriML-P, TriML-35XL, TML-BP, TML-HQ, TML-PP-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP (The above are trade names, available from Honshu Chemical Industry Co., Ltd.) BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (the above are trade names, products of Asahi Organic Materials Co., Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, 2,3,4-trihydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, pyrogallol acetone resin, m-cresol resin, phenolic resin, etc.

[0028] The iodonium salts include bis(4-tert-butylphenyl)iodonium hexafluorophosphate, diphenyliodonium hexafluoroarsenate, diphenyliodonium hexafluorophosphate, 4-isopropyl-4'-methyldiphenyliodonium tetra(pentafluorophenyl)borate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nitrate, [4-(trifluoromethyl)phenyl](2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, and [3-(trifluoromethyl)phenyl](2,4,6-trimethyl)phenyl (4-trifluoromethyl)phenyl iodonium trifluoromethanesulfonate, [(4-trifluoromethyl)phenyl](2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, phenyl(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, phenyl[3-(trifluoromethyl)phenyl]iodonium trifluoromethanesulfonate, (4-nitrophenyl)(phenyl)iodonium trifluoromethanesulfonate, (4-tolyl)(2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, (3-tolyl) (2,4,6-Trimethylphenyl)iodonium trifluoromethanesulfonate, (2-Tolyl)(2,4,6-Trimethylphenyl)iodonium trifluoromethanesulfonate, 4-Isopropyl-4'-Methyldiphenyliodonium tetra(pentafluorophenyl)borate, [4-[(2-hydroxytetradecyl)oxy]phenyl]phenyliohexafluoroantimonate, (5-Fluoro-2-nitrophenyl)(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, diphenyliodonium hexafluorophosphate, Diphenyliodonium hexafluoroarsenate, (3,5-dichlorophenyl)(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, (3-bromophenyl)(trimethylmethyl)iodonium trifluoromethanesulfonate, [4-(bromomethyl)phenyl](2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, bis(2,4,6-trimethylpyridine)iodonium hexafluorophosphate, 4,4'-xylyliodonium hexafluorophosphate, and mixtures thereof in any proportion.

[0029] Sulfonium salts include 1,3-benzodithiopyrrole tetrafluoroborate, cyclopropyl diphenylsulfonium tetrafluoroborate, dimethyl(methylthio)sulfonium tetrafluoroborate, diphenyl(methyl)sulfonium tetrafluoroborate, (difluoromethyl)bis(2,5-dimethylphenyl)sulfonium tetrafluoroborate, 2-[4-(3-ethoxy-2-hydroxypropoxy)phenylcarbamoyl]ethyldimethylthio-p-toluenesulfonate, 4-hydroxyphenyldimethylsulfonium methanesulfonate, triphenylsulfonium tetrafluoroborate, tri(4-tolyl)sulfonium hexafluorophosphate, tri(4-tolyl)sulfonium trifluoromethanesulfonate, triethylsulfonium bis(trifluoromethylsulfonyl)imide, and mixtures thereof in any proportion.

[0030] Preferably, the thermal crosslinking agent (C) refers to a compound that can undergo a crosslinking reaction under heating conditions or under the action of Lewis acid, including compounds containing epoxy groups, compounds containing hydroxymethyl or alkoxymethyl groups, etc.

[0031] The compounds containing epoxy groups include any one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polymethyl (glycidyloxypropyl), and epoxy-containing organosilicon, more preferably 3,3'-[oxybismethylene]bis[3-ethyl]oxetane, 1,4-butanediol diglycidyl ether, 2,2-bis(4-epoxypropoxyphenyl)propane, 9,9-bis(4-epoxypropyloxy-3-tolyl)fluorene, 9,9-bis(4-epoxypropoxyphenyl)fluorene, and 1,3-bis[2-(7-oxabicyclo[4.1]].[0]Hept-3-yl)ethyl]-1,1,3,3-tetramethyldisiloxane, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, 1,2,7,8-diepoxyoctane, 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, triglycidyl isocyanurate, 4,4'-methylenebis(N,N-dicyclopropoxyaniline), neopentyl glycol diglycidyl ether, 2,2'-(2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl)bis(ethylene oxide), pentaerythritol diglycidyl ether, vinylcyclohexene diglycidyl ether, polyethylene glycol diglycidyl ether ( Polymerization degree 1-15), polypropylene glycol diglycidyl ether (polymerization degree 1-15), polydimethylsiloxane diglycidyl ether (polymerization degree 1-15), butanediol diglycidyl ether, diglycidyl aniline, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, 5,5-dimethyl-1,3-di(epoxyethylenemethyl)imidazolidine-2,4-dione, 2,2',2''-[methimide-tris(phenoxymethylene)]tris(epoxyethylene), 1,1,1-tris(4-hydroxyphenyl)ethyl triglycidyl ether, bis(2,3-epoxycyclopentyl) ether, 3 4-Epoxy-6-methylcyclohexylcarboxylic acid-3',4'-epoxy-6'-methylcyclohexyl methyl ester, vinylcyclohexene epoxy compound, 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, diisoprene diester, tetraphenylglycidyl ether ethane, triphenylglycidyl ether methane, triglycidyl-p-aminophenol, triglycidyl triisocyanate, tetraglycidyl diaminodiphenylmethane, tetraglycidyl dimethylbenzene diamine, or tetraglycidyl-1,3-diaminomethylcyclohexane; products with trade names can be listed as H P-850, HP-4032, HP-7200, HP-820, HP-4700, EXA-4710, HP-4770, EXA-859CRP, EXA-1514, EXA-4880, EXA-4850-150, EXA-4850-1000, EXA-4816, EXA-4822, BEO-60E, BPO-20E, HBE-100, DME-100, NC-3000, NC-6000 (Nippon Kayaku Co., Ltd.), and mixtures thereof in any proportion.

[0032] The compounds containing hydroxymethyl or alkoxymethyl groups include 46DMOC, 46DMOEP (trade names, manufactured by Asahi Organic Materials Co., Ltd.), DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DMLMBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DMLBisOC-P, DMOM-PC, DMOMPTBP, DMOM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML- pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP (the above are trade names, available from Honshu Chemical Industry Co., Ltd.), "NIKALAC" MX-290, "NIKALAC" MX-280, "NIKALAC" MX-270, "NIKALAC" MX-279, "NIKALAC" MW-100LM, "NIKALAC" MX-750LM (Sanwa Chemical Co., Ltd.), and mixtures thereof in any proportion.

[0033] Preferably, the thermogenic acid-producing agent (D) refers to a compound that can produce a strong acid upon heating, with a thermal decomposition initiation temperature of 150℃-250℃, such as alkyl sulfonic acids, perfluoroalkyl sulfonic acids or pyridinium salts of alkyl sulfonic acids, alkylpyridinium salts, diaryl iodine salts, di(alkylaryl)iodine salts, trialkyl sulfonium salts, dialkyl monoaryl sulfonium salts or diaryl monoalkyl iodine salts or ester compounds, including p-toluenesulfonic acid pyridinium salt, p-toluenesulfonic acid di(tert-butylphenyl)iodine salt, trimethyl sulfonium salt of trifluorobenzenesulfonic acid, diphenylmethyl sulfonium salt of trifluoromethanesulfonic acid, p-toluenesulfonic acid-2-methoxyethyl ester, and mixtures thereof in any proportion.

[0034] Preferably, the sensitizer (E) includes compounds containing phenolic hydroxyl, hydroxyl, or carboxyl groups, which can increase the solubility of the exposed portion in the developer, improve photosensitivity, and shorten the development time.

[0035] The compounds containing phenolic hydroxyl groups include Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, methylenetris-FR-CR, BisRS-26X (these are trade names, available from Honshu Chemical Industry Co., Ltd.), BIP-PC, BIR-PC, BIR-PTBP, BIR-BIPC- F (the above are trade names, obtained by Asahi Organic Materials Co., Ltd.), 2,2-bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 9,9-bis(4-hydroxyphenyl)fluorene, 4,4'-dihydroxydiphenylcyclohexane, 1,4-naphthodiol, 1,5-naphthodiol, 1,6-naphthodiol, 1,7-naphthodiol, 2,3-naphthodiol, 2,7-naphthodiol, 2,6-naphthodiol, bis(4-hydroxyphenyl) sulfide, spiro[fluorene-9,9'-xanthan]-3',6'-diol and mixtures thereof in any proportion.

[0036] The organic compounds containing hydroxyl groups refer to saturated or unsaturated fatty alcohols containing 2-16 carbons, including ethanol, n-propanol, isopropanol, n-butanol, tert-butanol, pentanol, n-hexanol, cyclopropylmethanol, cyclohexylmethanol, 4-methyl-1-cyclohexylmethanol, 3,4-dimethylcyclohexanol, 4-ethylcyclohexanol, 4-tert-butylcyclohexanol, heptanol, octanol, cyclooctanol, 1-cyclohexyl-1-pentanol, 3,5,5-trimethylcyclohexanol, norberyl. 2-methyl-2-methanol, cis-4-hepten-1-ol, cis-3-octen-1-ol, 2,7-octadienol, 2,4,4-methyl-2-pentanol, cyclohexylmethanol, cis-2-hexen-1-ol, n-hexanol, 1-hexadecyl alcohol, 2-ethyl-1-butanol, DL-2-methyl-1-butanol, isoamyl alcohol, 3-methyl-2-butanol, 4-methyl-2-pentanol, isobutanol, neopentanol, and mixtures thereof in any proportion.

[0037] The organic compounds containing carboxyl groups refer to carboxylic acid compounds containing 2 to 16 carbon atoms, including acetic acid, propionic acid, butyric acid, valeric acid, 2-methyl-4-pentenoic acid, 4-methyl-2-pentenoic acid, 2-methyl-2-pentenoic acid, 3-methyl-n-pentanoic acid, 4-methyln-pentanoic acid, 2-ethylbutyric acid, heptanoic acid, octanoic acid, n-nonanoic acid, isononanoic acid, n-decanoic acid, 2-heptenoic acid, 2-octenoic acid, 2-nonenoic acid, 2-decenoic acid, 10-undecenoic acid, p-methoxybenzoic acid, m-methylbenzoic acid, benzoic acid, mandelic acid, trans-2-hexenoic acid, 3,7-dimethyl-6-octanoic acid, sorbic acid, 3,5,5-trimethylhexanoic acid, lauric acid, myrcenoic acid, and mixtures thereof in any proportion.

[0038] Preferably, in the positive photosensitive resin composition adhesive, the organic solvent (F) refers to a compound that can dissolve components (A) to (E) to form a homogeneous solution, including N-methylpyrrolidone, N,N'-dimethylacetamide, N,N'-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, ethyl acetate, butyl acetate, n-propyl acetate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, etc., and mixtures thereof in any proportion.

[0039] Preferably, the tackifier (G) comprises γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyl ether oxypropyltrimethoxysilane, γ-glycidyl ether oxypropyltriethoxysilane, 3-methacryloyloxypropyldimethoxymethylsilane, 3-methacryloyloxypropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 2-cyanoethyltrimethoxysilane, 2-cyanoethyltriethoxysilane, 3-isocyanate-trimethoxysilane, 3-isocyanate-triethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptomethyltrimethoxysilane, 3- Mercaptomethyl dimethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, vinyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-(triethoxysilyl)propylsuccinic anhydride, 3-(m-aminophenoxy)trimethoxysilane, p-aminophenyltrimethoxysilane, aminophenyltrimethoxysilane, vinylmethyl diethoxysilane, vinyltriethoxysilane, 3-acetoxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-piperazinylpropylmethyldimethoxysilane, and mixtures thereof in any proportion.

[0040] The second objective of this invention is to provide a method for preparing a positive photosensitive resin composition liquid with low moisture absorption properties, comprising the following steps: In a Class 1000 cleanroom equipped with a yellow light source, 100 parts by weight of hydroxyl-containing polyamide resin (A) (phenolic hydroxyl polyamide ester resin-1 + phenolic hydroxyl polyamide ester resin-2), 3-40 parts by weight of photoacid-generating agent (B), 3-40 parts by weight of thermal crosslinking agent (C), 0.1-20 parts by weight of thermal acid-generating agent (D), 3-40 parts by weight of sensitizer (E), and 3-40 parts by weight of tackifier (G) were added in batches to an organic solvent (F) under stirring to form a homogeneous solution. After filtration, the solution was packaged to obtain a positive photosensitive resin solution with a solid content of 15 wt.%~45 wt.% and a solution viscosity of 500 mPa.s~4000 mPa.s at room temperature.

[0041] The third objective of this invention is to provide an application of the above-mentioned positive photosensitive resin composition liquid with low moisture absorption properties, suitable not only for the surface of 12-inch silicon wafers, but also for the fabrication of dielectric insulating films for multilayer metal interconnect circuits (RDLs) on large-area (600mm long x 600mm wide) glass substrates, wherein the photolithography patterning process includes: 1) Coating: The positive photosensitive resin liquid is spin-coated onto the wafer surface or inkjet printed onto a large-area glass substrate to form a liquid film of uniform thickness. 2) Pre-baking: at 80-150°C o Pre-baking is performed at C to form a semi-solid adhesive film; 3) Exposure: Ultraviolet light is used to expose the material through a photomask or photomask; 4) Development + Rinsing: Aqueous developer (2.38% TMAH) is used for development by spraying or immersion, followed by rinsing with ultrapure water to form a three-dimensional pattern; 5) Heat curing: The precursor resin three-dimensional pattern on the substrate surface is heat-cured and transformed into a high heat-resistant curable resin three-dimensional pattern; 6) A continuous conductive copper layer is formed on the surface of the resin three-dimensional pattern by electroplating copper; then, the continuous conductive copper layer is etched to form conductive copper lines by photolithography patterning process, completing one RDL process (1P1M); repeat the above process to form a second RDL process (2P2M) on its surface; continue to repeat the above process to form a third RDL process (3P3M).

[0042] Compared with the prior art, the present invention has the following beneficial effects: This invention improves the hydrophobicity and reduces the moisture absorption rate of p-PSPI cured films by introducing hydrophobic aliphatic segments into the main chain structure of a resin containing phenolic hydroxyl polyamate-1, thereby significantly reducing the dielectric constant and dielectric loss of the cured resin film. Simultaneously, by compounding phenolic hydroxyl polyamate-1 with phenolic hydroxyl polyamide resin-2 to form a composite resin system, the high reactivity of the ester groups of the polyamate at low temperatures and the synergistic effect of the amide groups of the polyamide resin effectively solve the challenges of low-temperature curing and the interplay between high heat resistance, high photolithography resolution, and high chemical resistance in positive photosensitive resins. This achieves a synergistic effect of excellent photolithography processability and high copper adhesion for PSPI, meeting the requirements of multilayer metal wiring fabrication processes for RF integrated circuit packaging.

[0043] The positive PSPI resin solution described in this invention has excellent photolithography processability. A liquid film with uniform thickness is formed on the surface of a 12-inch silicon wafer through spin coating. The resin three-dimensional pattern formed after photolithography processes such as pre-baking, exposure, and development has the characteristics of high resolution and controllable steepness. The resin film formed after low-temperature curing (≤230℃) has low moisture absorption (≤0.4%) and excellent comprehensive mechanical properties, resistance to damp heat, resistance to chemical corrosion, and copper surface adhesion. It is suitable for fabricating interlayer dielectric insulating films for multilayer metal interconnect structures of high-frequency integrated circuits. Detailed Implementation

[0044] To enable those skilled in the art to better understand and implement the technical solutions of the present invention, the present invention will be further described below with reference to specific embodiments. However, the embodiments are not intended to limit the present invention. Unless otherwise specified, the experimental methods and detection methods described in the following embodiments are conventional methods; unless otherwise specified, the reagents and materials are commercially available.

[0045] 1. Comprehensive performance evaluation method: The performance of the positive photosensitive resin liquid was evaluated using the following evaluation method: 1) Photolithography processability: A positive photosensitive resin liquid is spin-coated onto the surface of a 12-inch silicon wafer to form a liquid film of uniform thickness; at 100-110... o After baking at C for 1-3 minutes, place a mask on its surface and expose it with ultraviolet lamps (i and g lines); develop it with an aqueous developer (2.38% TMAH) by spraying or immersion, rinse with ultrapure water, and then heat-cur it in a nitrogen-protected oven at 150°C. o C / 1h, 200 o C / 1h, 230 o C / 1h) was used to obtain a stereolithographic pattern of cured resin with a thickness of 8.0 μm.

[0046] The photolithography processability is evaluated by observing the three-dimensional pattern under an optical microscope: if the thickness uniformity of the cured resin film (8.0 μm) after curing is ≤0.50%, the resolution of the photolithographic pattern (strip pattern and through-hole) is ≤5.0 µm, and the patterns are cleanly developed without any foreign matter residue, the photolithography processability is rated as "excellent"; if the thickness uniformity of the cured film is 0.51-0.99%, the resolution of the photolithographic pattern is ≤10.0 µm, and the patterns are cleanly developed without any foreign matter residue, the photolithography resolution is rated as "good"; if the thickness uniformity of the cured film is ≥1.0%, the resolution of the pattern is ≥15 µm, and the patterns are not cleanly developed with foreign matter residue, the photolithography resolution is rated as "poor".

[0047] 2) Hygroscopicity: The thermosetting resin film sample formed after high-temperature curing was cut into test samples of 6.5cm × 5.5cm size. After wiping the surface clean with ethanol, the samples were tested at 90°C. o Dry at C for 30 minutes, cool to room temperature and weigh to obtain W1; then, place it in a container at 24°C. oC. The sample was placed in a constant temperature and humidity chamber with a relative humidity of 85% for 24 hours. After wiping the surface of the test sample clean, it was weighed to obtain W2. The moisture absorption rate of the sample was (W2-W1) / W1×100%. The test result is the average of the test results of a set of 3 samples. If the moisture absorption rate of the prepared film is ≤0.60 wt.%, it is rated as "Excellent"; if the moisture absorption rate of the prepared film is 0.61-0.99 wt.%, it is rated as "Good"; if the moisture absorption rate of the prepared film is 1.0 wt.%, it is rated as "Poor".

[0048] 3) Chemical resistance: The photolithographic 3D pattern of the heat-cured resin was subjected to 100°C immersion in a caustic solution (1 wt.% potassium hydroxide + 39 wt.% 3-methoxy-3-methyl-1-butanol + 60 wt.% dimethyl sulfoxide (DMSO)). o After soaking in C for 1 hour, the film was washed with water and air-dried. The chemical resistance of the cured resin film was evaluated by measuring the change in film thickness and observing it under an optical microscope: if the thickness change of the cured resin film after soaking was within ±1% and no cracks or defects were produced, it was rated as "excellent"; if the thickness change of the cured resin film after soaking was within ±3% and no cracks or defects were produced, it was rated as "good"; if the thickness change of the cured resin film after soaking exceeded ±5% or cracks or defects were produced, it was rated as "poor".

[0049] 4) Moisture and heat resistance: A liquid film is formed by spin-coating a high-frequency, low-dielectric-loss positive photosensitive resin onto the surface of a 12-inch silicon wafer; 120 o After baking at C for 3 minutes, the surface was exposed to UV light (i and g lines) without a mask. It was then developed by spraying or immersion with an aqueous developer (2.38% TMAH), rinsed with ultrapure water, and cured in a nitrogen-protected oven at 150°C. o C / 1h, 200 o C / 1h, 230 o C / 1h), a cured resin film is formed on the substrate surface; the substrate is then placed in 120 o After steaming in a pressure cooker at C / 2 atm for 100 hours, it was then cooled to room temperature of -260°C. o C. Three thermal cycling shock tests; using FIB (fiber optic lithography), the longitudinal section of the copper-tin bumps covering the resin film was cut open, and the interface morphology between the copper-tin bumps and the resin film was observed using an optical microscope. If no cracking or voids were found at the interface between the copper-tin bumps and the cured resin, it was rated as "Excellent"; if a few cracks or voids were found at the interface between the copper-tin bumps and the cured resin, it was rated as "Good"; if many cracks or voids were found at the interface between the copper-tin bumps and the cured resin, it was rated as "Poor".

[0050] 5) Adhesion to copper surfaces: Positive photosensitive resin is spin-coated onto the surface of a 12-inch silicon wafer to form a uniformly thick film; at 100-110... o After baking at C for 1-3 minutes, expose the surface with ultraviolet lamps (i and g lines) without placing a mask; develop with aqueous developer (2.38% TMAH) by spraying or immersion, rinse with ultrapure water, and then heat-cur in a nitrogen-protected oven at 150°C. o C / 1h, 200 o C / 1h, 230 o A cured resin film with a thickness of 8.0 µm was obtained by (C / 1h). The adhesion between the film and copper was evaluated using a cross-cut test: "Excellent" was defined as 0 crosses peeled off per 100 crosses; "Good" was defined as 1-10 crosses peeled off per 100 crosses; and "Poor" was defined as more than 11 crosses peeled off per 100 crosses.

[0051] 6) Overall performance evaluation: If all indicators are "excellent", the overall performance evaluation is "excellent"; if one of the indicators is "good", the overall performance evaluation is "good"; if one of the indicators is "poor", the overall performance evaluation is "poor".

[0052] 2. Example of synthesis of phenolic hydroxyl resin The preparation of phenolic hydroxyl polyamic acid ester resin-1 is shown below: Resin Synthesis Example 1 In a 500 ml three-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and nitrogen protection device, add 33.22 g (0.10 mol.) of 2,2-bis(3,4-dicarboxyphenyl)propanetetracarboxylic dianhydride (abbreviated as: 1BCDA, 187-188). o 9.20 g (0.20 mol. Mw=46.02) of ethanol, 15.82 g (0.20 mol.) of pyridine and 129 g of N-methylpyrrolidone (NMP) were stirred at room temperature for 6 h to produce the corresponding diethyl aromatic diacid.

[0053] The above product was reacted with 23.79 g of SOCl2 at 0-10 °C for 2 h, and then at room temperature for 4 h to produce a diethyl diacyl chloride solution of 1 EBTA.

[0054] In a 1L three-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and nitrogen protection device, 36.62 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) and 158 g of NMP were added and stirred until dissolved to form a homogeneous transparent solution (3HFAP / NMP); the 33BPDA diethyl dichlorodimethyl ... 1.00 g of 1,3-bis(3-aminopropyl)tetramethyldisiloxane (4MSiNA) was added to phthalic anhydride and stirred for 1 h. The reaction solution was poured into 5 L of deionized water, the solid precipitated, filtered, and dried under vacuum to obtain primary polyamic acid ester resin (PAE-1-1). This solution was dissolved in tetrahydrofuran to form a solution, and residual metal or non-metal ions were removed by adsorption with anionic and cationic resins to obtain high-purity phenolic hydroxyl-containing polyamic acid ester resin solid (abbreviated as: PAE-1-1: 1BCDA-3HFAP).

[0055] Resin Synthesis Example 2 33.22 g (0.10 mol.) of 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride (abbreviated as: 1BCDA, 187-188) from the resin synthesis example 1 was used. o C, Mw=332.21) was replaced with 30.80 g (0.10 mol.) of 2,4-bis(3,4-dicarboxyphenyl)-2,4-dimethylpentane dianhydride (abbreviated as: 2BMDA, 166-167). o With C, Mw=308.02, and other parameters remaining the same, a high-purity solid polyamide ester resin containing phenolic hydroxyl groups was obtained (abbreviated as: PAE-1-2: 2BMDA-3HFAP).

[0056] Resin Synthesis Example 3 33.22 g (0.10 mol.) of 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride (abbreviated as: 1BCDA, 187-188) from the resin synthesis example 1 was used. o C, Mw=332.21) was replaced with 48.63 g (0.10 mol.) of 2,7-bis(3,4-dicarboxyphenyl)-2,7-dimethyloctane dianhydride (abbreviated as: 3BODA, 166-167). o With C, Mw=486.32, and other parameters remaining the same, a high-purity phenolic hydroxyl polyamide ester resin solid (abbreviated as: PAE-1-3: 3BODA-3HFAP) was obtained.

[0057] Resin Synthesis Example 4 33.22 g (0.10 mol.) of 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride (abbreviated as: 1BCDA, 187-188) from the resin synthesis example 1 was used. o C, Mw=332.21) was replaced with 59.84 g (0.10 mol.) of 2,7-bis(3,4-dicarboxyphenyl)-2,7-dimethyldodecane dianhydride (abbreviated as: 4BDDA, 121-126). o C, 598.41), otherwise identical, yielded a high-purity solid polyamide resin containing phenolic hydroxyl groups (abbreviated as: PAE-1-4: 4BDDA-3HFAP).

[0058] Resin Synthesis Example 5 33.22 g (0.10 mol.) of 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride (abbreviated as: 1BCDA, 187-188) from the resin synthesis example 1 was used. o C, Mw=332.21) was replaced with 57.64 g (0.10 mol.) bis(p-2)trimethoate-bisphenol A ester (abbreviated as: 5IPDA, mp192-193). o C, 576.36), otherwise the same, to obtain high-purity phenolic hydroxyl polyamide ester resin solid (abbreviation: PAE-1-5: 5IPDA-3HFAP).

[0059] Resin Synthesis Example 6 In Resin Synthesis Example 3, 36.62 g (0.10 mol.) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) was replaced with 36.62 g (0.10 mol.) 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane (abbreviated as: 4HFAP, Mw=366.17), while all other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyaminate resin solid (abbreviated as: PAE-1-6:3BODA-4HFAP).

[0060] Resin Synthesis Example 7 In Resin Synthesis Example 3, 36.62 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) was replaced with 60.43 g (0.10 mol.) of 2,2'-bis[N-(3-aminobenzoamide)-3-amino-4-hydroxyphenyl]hexafluoropropane (abbreviated as: 3HFHA, Mw=604.32), while all other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyaminate resin solid (abbreviated as: PAE-1-7:3BODA-3HFHA).

[0061] Resin Synthesis Example 8 In Resin Synthesis Example 3, 36.62 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) was replaced with 60.43 g (0.10 mol.) of 2,2'-bis[N-(3-aminobenzoamide)-4-amino-3-hydroxyphenyl]hexafluoropropane (abbreviated as: 4HFHA, Mw=604.32), while all other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyaminate resin solid (abbreviated as: PAE-1-8:3BODA-4HFHA).

[0062] Resin Synthesis Example 9 In Resin Synthesis Example 3, 36.62 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) was replaced with 25.82 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)propane (abbreviated as: 3HHAP, Mw=258.17), while all other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyamide ester resin solid (abbreviated as: PAE-1-9: 3BODA-3HHAP).

[0063] Resin Synthesis Example 10 In Resin Synthesis Example 3, 36.62 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) was replaced with 25.82 g (0.10 mol.) of 2,2-bis(4-amino-3-hydroxyphenyl)propane (abbreviated as: 4HHAP, Mw=258.17), while all other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyamide ester resin solid (abbreviated as: PAE-1-10: 3BODA-4HHAP).

[0064] The synthesis of phenolic hydroxyl polyamic acid ester resin-2 is shown below: Resin Synthesis Example 11 In a 500 ml three-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and nitrogen protection device, 31.02 g (0.10 mol.) of 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA), 9.20 g (0.20 mol.) of ethanol, 15.82 g (0.20 mol.) of pyridine, and 129 g of N-methylpyrrolidone (NMP) were added. The mixture was stirred at room temperature for 6 h to produce the corresponding diethyl aromatic diacid ester. The product was then reacted with 23.79 g of SOCl2 at 0-10 °C for 2 h, followed by a reaction at room temperature for 4 h to produce a solution of the corresponding 44ODPA diethyl diacid chloride.

[0065] In a 1L three-necked round-bottom flask equipped with a mechanical stirrer, thermometer, and nitrogen protection device, 36.62 g (0.10 mol.) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as: 3HFAP, Mw=366.17) and 158 g of NMP were added and stirred until dissolved to form a homogeneous transparent solution (3HFAP / NMP); the 44ODPA diethyl dichlorodimethyl ... 1.00 g of 1,3-bis(3-aminopropyl)tetramethyldisiloxane (4MSiNA) was added to phthalic anhydride and stirred for 1 h. The reaction solution was poured into 5 L of deionized water, the solid precipitated, filtered, and dried under vacuum to obtain primary polyamic acid ester resin (PAE-2-1). This solution was dissolved in tetrahydrofuran and subjected to adsorption by anionic and cationic resins to remove residual metal or non-metal ions, yielding high-purity phenolic hydroxyl-containing polyamic acid ester resin solid (abbreviated as: PAE-2-1: 44ODPA-3HFAP).

[0066] Resin Synthesis Example 12 In Resin Synthesis Example 11, 31.02 g (0.10 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA) was replaced with 31.02 g (0.10 mol.) 2,2,3',3'-diphenyl ether tetracarboxylic dianhydride (33ODPA), while other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyamide resin solid (abbreviated as: PAE-2-2:33ODPA-3HFAP).

[0067] Resin Synthesis Example 13 In Resin Synthesis Example 11, 31.02 g (0.10 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA) was replaced with 31.02 g (0.10 mol.) 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (34ODPA), while all other parameters remained the same, to obtain a high-purity phenolic hydroxyl polyamide resin solid (abbreviated as: PAE-2-3:34ODPA-3HFAP).

[0068] Resin Synthesis Example 14 In Resin Synthesis Example 11, 31.02 g (0.10 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA) was replaced with a mixture of 15.51 g (0.05 mol.) 2,2,3',3'-diphenyl ether tetracarboxylic dianhydride (33ODPA) and 15.51 g (0.05 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA), otherwise the same, to obtain a high-purity phenolic hydroxyl polyamide resin solid (abbreviated as: PAE-2-4:33ODPA / 44ODPA(1 / 1)-3HFAP).

[0069] Resin Synthesis Example 15 In Resin Synthesis Example 11, 31.02 g (0.10 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA) was replaced with a mixture of 15.51 g (0.05 mol.) 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (34ODPA) and 15.51 g (0.05 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA), otherwise the same, to obtain a high-purity phenolic hydroxyl polyamide resin solid (abbreviated as: PAE-2-5: 34ODPA / 44ODPA(1 / 1)-3HFAP).

[0070] Resin Synthesis Example 16 In Resin Synthesis Example 11, 31.02 g (0.10 mol.) 3,3,4',4'-diphenyl ether tetracarboxylic dianhydride (44ODPA) was replaced with a mixture of 15.51 g (0.05 mol.) 2,2,3',3'-diphenyl ether tetracarboxylic dianhydride (33ODPA) and 15.51 g (0.05 mol.) 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (34ODPA), otherwise the same, to obtain a high-purity phenolic hydroxyl polyamide resin solid (abbreviated as: PAE-2-6: 33ODPA / 34ODPA(1 / 1)-3HFAP).

[0071] 3. The preparation of the positive photosensitive resin solution is as follows: Example 1 In a cleanroom equipped with a yellow light, 50g of phenolic hydroxyl polyamide ester resin-1 (PAE-1-1) prepared in Resin Synthesis Example 1 and 50g of phenolic hydroxyl polyamide resin-2 (PAE-2-1) prepared in Resin Synthesis Example 11 were weighed and dissolved in 100g of γ-butyrolactone solvent to form a homogeneous solution. Then, 10g of 2,3,4-trihydroxybenzophenone-1,2-naphthoquinone-5-sulfonate (photoacid-generating agent), 5.0g of p-toluenesulfonic acid-2-methoxyethyl ester (thermal acid-generating agent), 5.0g of 2,2-bis(4-hydroxyphenyl)propane (sensitizer), 4.0g of 2,2-bis(4-epoxypropoxyphenyl)propane (thermal crosslinking agent), and 5.0g of γ-aminopropyltriethoxysilane (adhesive agent) were added sequentially, and the mixture was stirred at room temperature for 1 hour to obtain a positive resin composition solution. When the solid content is 35 wt.%, the solution viscosity is 1500 mPa·s.

[0072] The above-mentioned positive resin solution is uniformly coated onto the surface of a 12-inch silicon wafer or a large-area glass substrate using a spin coating process; at a temperature of 100-110°C... o After baking at C for 1-3 minutes, place a mask on its surface and expose it with ultraviolet lamps (i and g lines); spray develop it with a tetramethylammonium hydroxide alkaline aqueous solution (2.38% TMAH), rinse with deionized ultrapure water, and then heat-cur it in a nitrogen-protected forced-air oven (150°C). o C / 1h, 200 o C / 1h, 200 o (C / 1h) to obtain a stereolithographic pattern formed by a thermosetting resin film.

[0073] The prepared positive photosensitive resin solution was evaluated using the above-mentioned evaluation method. The evaluation results are as follows: ① Photolithography processability: film thickness uniformity is 0.45%, photolithography resolution is 4.5 μm, rated as "excellent"; ② Moisture absorption: 0.58%, rated as "excellent"; ③ Chemical corrosion resistance: film thickness change rate is 0.85%, no microcracks or defects were observed, rated as "excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result is 0 / 100, rated as "excellent"; ⑥ Comprehensive performance evaluation: all indicators are excellent, rated as "excellent".

[0074] Example 2 In Example 1, PAE-1-1 was replaced with PAE-1-2, while other aspects remained the same, to obtain a positive photosensitive resin solution. The performance of the positive photosensitive resin solution was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.48%, photolithography resolution was 4.6 μm, rated as "Excellent"; ② Moisture absorption: 0.55%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness change rate was 0.78%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0075] Example 3 PAE-1-1 in Example 1 was replaced with PAE-1-3, while other aspects remained the same, to obtain a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.47%, photolithography resolution was 4.5 μm, rated as "Excellent"; ② Moisture absorption: 0.55%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.83%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0076] Example 4 In Example 1, PAE-1-1 was replaced with PAE-1-4, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.49%, photolithography resolution was 4.3 μm, rated as "Excellent"; ② Moisture absorption: 0.54%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.76%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0077] Example 5 In Example 1, PAE-1-1 was replaced with PAE-1-5, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.55%, photolithography resolution was 7.3 μm, rated as "Good"; ② Moisture absorption: 0.58%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.77%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 8 / 100, rated as "Good"; ⑥ Comprehensive performance evaluation: two indicators were good, rated as "Good".

[0078] Comparative Example 1 PAE-2-1 was removed from Example 1, while all other parameters remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the aforementioned evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.46%, photolithography resolution was 4.6 μm, rated as "Excellent"; ② Moisture absorption: 0.82%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.72%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 12 / 100, rated as "Good"; ⑥ Comprehensive performance evaluation: all three indicators were "Good", rated as "Good".

[0079] Comparative Example 2 PAE-1-1 was removed from Example 1, while all other parameters remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 1.1%, photolithography resolution was 12.2 μm, rated as "poor"; ② Moisture absorption: 0.84%, rated as "excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.85%, no microcracks or defects were observed, rated as "excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 11 / 100, rated as "good"; ⑥ Overall performance evaluation: one indicator was poor, rated as "poor".

[0080] Table 1 Comparison of results from Examples 1-5 and Comparative Examples 1-2 Table 1 compares the effects of the different molecular structures of the PAE-1 series resins (PAE-1-1, 1-2, 1-3, 1-4, 1-5) containing aliphatic chain aromatic tetracarboxylic dianhydride monomers on the overall performance of the prepared positive photosensitive resins when the weight ratio of the PAE-1 series resins (PAE-1-1, 1-2, 1-3, 1-4, 1-5) in Examples 1-5 is 1:1. The results show that the mixed resin formed by combining PAE-1-1 or PAE-1-2, PAE-1-3, PAE-1-4 and PAE-2-1 in a 1:1 weight ratio, when thoroughly mixed with other components such as photoacidifiers, thermal crosslinking agents, and tackifiers, exhibits excellent overall performance, and its overall performance is rated as "excellent". The positive photosensitive resin solution prepared from a mixed resin formed by combining PAE-1-5 and PAE-2-1 in a 1:1 weight ratio exhibits poor resistance to damp heat, and its overall performance is rated as "good". In contrast, when either the phenolic hydroxyl polyaminate resin (PAE-1-1) or the phenolic hydroxyl polyaminate resin (PAE-2-1) is a single component, rather than a mixture of both, the overall performance of the prepared positive photosensitive resin solution is rated as "good or poor".

[0081] Example 6 PAE-1-1 in Example 1 was replaced with PAE-1-6, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.47%, photolithography resolution was 4.6 μm, rated as "Excellent"; ② Moisture absorption: 0.54%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.82%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0082] Example 7 In Example 1, PAE-1-1 was replaced with PAE-1-7, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.45%, photolithography resolution was 4.5 μm, rated as "Excellent"; ② Moisture absorption: 0.55%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.73%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0083] Example 8 In Example 1, PAE-1-1 was replaced with PAE-1-8, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.47%, photolithography resolution was 4.4 μm, rated as "Excellent"; ② Moisture absorption: 0.57%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.73%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0084] Example 9 In Example 1, PAE-1-1 was replaced with PAE-1-9, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.44%, photolithography resolution was 4.8 μm, rated as "Excellent"; ② Moisture absorption: 0.56%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.73%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0085] Example 10 In Example 1, PAE-1-1 was replaced with PAE-1-10, while other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.43%, photolithography resolution was 4.6 μm, rated as "Excellent"; ② Moisture absorption: 0.58%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.77%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: microcracks or defects were observed, rated as "Poor"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 8 / 100, rated as "Good"; ⑥ Overall performance evaluation: one indicator was poor, rated as "Poor".

[0086] Comparative Example 3 PAE-2-1 was removed from Example 8, while all other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 0.46%, photolithography resolution was 4.6 μm, rated as "Excellent"; ② Moisture absorption: 1.2%, rated as "Poor"; ③ Chemical corrosion resistance: film thickness variation rate was 0.74%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 12 / 100, rated as "Good"; ⑥ Overall performance evaluation: one indicator was poor, rated as "Poor".

[0087] Table 2 Comparison of results from Examples 6-10 and Comparative Example 3 Table 2 compares the effects of the different molecular structures of the aliphatic chain aromatic dianhydride monomers (4HFAP, 3HFHA, 4HFHA) in the PAE-1 series resins (PAE-1 or 1-7, 1-8, 1-9) on the overall performance of the prepared positive photosensitive resin when the weight ratio of the phenolic hydroxyl polyaminate resin-1 series resins (PAE-1-6 or 1-7, 1-8, 1-9) in Examples 6-10 is 1:1. The results show that the positive photosensitive resin solution formed by thoroughly mixing the mixed resin of PAE-1-6 or PAE-1-7, PAE-1-8, PAE-1-9 and PAE-2-1 in a 1:1 weight ratio with other components such as photoacidifiers, thermal crosslinking agents, thermal acidifiers, and tackifiers exhibits excellent overall performance, and its overall performance is rated as "excellent". The overall performance of the positive photosensitive resin solution prepared by combining PAE-1-10 and PAE-2-1 in a 1:1 weight ratio was rated as "poor". In contrast, when the phenolic hydroxyl polyaminate resin (PAE-1-8) was only a single component and did not form a mixed resin with PAE-2-1, the overall performance of the prepared positive photosensitive resin solution was also rated as "poor".

[0088] Example 11 In Example 2, PAE-2-1 was replaced with PAE-2-2, while other aspects remained the same, to obtain a positive photosensitive resin solution. The performance of the positive photosensitive resin solution was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.47%, photolithography resolution was 4.4 μm, rated as "Excellent"; ② Moisture absorption: 0.53%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness change rate was 0.82%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0089] Example 12 In Example 2, PAE-2-1 was replaced with PAE-2-3, while other aspects remained the same, to obtain a positive photosensitive resin solution. The performance of the positive photosensitive resin solution was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.45%, photolithography resolution was 4.5 μm, rated as "Excellent"; ② Moisture absorption: 0.56%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness change rate was 0.73%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0090] Example 13 In Example 2, PAE-2-1 was replaced with PAE-2-4, while other aspects remained the same, resulting in a positive photosensitive resin solution. The performance of the positive photosensitive resin solution was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.47%, photolithography resolution was 4.4 μm, rated as "Excellent"; ② Moisture absorption: 0.54%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness change rate was 0.73%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Copper adhesion: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0091] Example 14 In Example 2, PAE-2-1 was replaced with PAE-2-5, while other aspects remained the same, resulting in a positive photosensitive resin solution. The performance of the positive photosensitive resin solution was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.42%, photolithography resolution was 4.8 μm, rated as "Excellent"; ② Moisture absorption: 0.52%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness change rate was 0.73%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0092] Example 15 In Example 2, PAE-2-1 was replaced with PAE-2-6, while other aspects remained the same, resulting in a positive photosensitive resin solution. The performance of the positive photosensitive resin solution was evaluated using the above evaluation method. The evaluation results were as follows: ① Photolithography processability: film thickness uniformity was 0.43%, photolithography resolution was 4.5 μm, rated as "Excellent"; ② Moisture absorption: 0.48%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness change rate was 0.77%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: no microcracks or defects were observed, rated as "Excellent"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: all indicators were excellent, rated as "Excellent".

[0093] Comparative Example 4 PAE-1-2 was removed from Example 13, while all other aspects remained the same, resulting in a positive photosensitive resin solution. Its performance was evaluated using the above evaluation method, and the results were as follows: ① Photolithography processability: film thickness uniformity was 1.1%, photolithography resolution was 7.6 μm, rated as "Excellent"; ② Moisture absorption: 0.55%, rated as "Excellent"; ③ Chemical corrosion resistance: film thickness variation rate was 0.74%, no microcracks or defects were observed, rated as "Excellent"; ④ Damp heat resistance: a few microcracks or defects were observed, rated as "Good"; ⑤ Adhesion to copper surface: cross-cut adhesion test result was 0 / 100, rated as "Excellent"; ⑥ Comprehensive performance evaluation: two indicators were good, rated as "Good".

[0094] Table 3 Comparison of results from Examples 11-15 and Comparative Example 4 Table 3 compares the effects of different molecular structures of aromatic tetracarboxylic dianhydrides (33-ODPA, 34-ODPA, 44-ODPA, and their 1:1 weight ratio) on the overall performance of the prepared positive photosensitive resin when the weight ratio of PAE-2 series resins (PAE-2-2, 2-3, 2-4, 2-5, 2-6) in Examples 11-15 is 1:1. The results show that the mixed resin formed by thoroughly mixing PAE-2-1, 2-2, 2-3, PAE-2-4, PAE-2-5, PAE-2-6 with PAE-1-2 in a 1:1 weight ratio, along with other components such as photoacidifiers, thermal crosslinking agents, and tackifiers, exhibits excellent overall performance, and its overall performance is rated as "excellent". In comparison, when the phenolic hydroxyl polyamide resin (PAE-2-3) is only a single component, rather than a mixed resin formed with PAE-1-2, the overall performance of the prepared positive photosensitive resin solution is rated as "good".

[0095] This invention discloses a positive photosensitive resin composition liquid with low moisture absorption properties, its preparation method, and its application. The positive photosensitive resin composition liquid has high photolithographic resolution and excellent photolithographic processability. The liquid film formed after coating is subjected to pre-baking, exposure, development, rinsing, and heat curing (180-230°C). o C) High-quality three-dimensional photolithography patterns can be formed after the resin film is cured by heating. It has the characteristics of low moisture absorption, high resistance to damp heat, high resistance to chemical immersion, and high copper surface adhesion. It is suitable for multilayer metal interconnect wiring in advanced packaging of high-density integrated circuits.

[0096] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, it is intended to include any modifications and variations that fall within the scope of the claims and their equivalents.

Claims

1. A low-moisture-absorbing, positively photosensitive polyimide resin composition liquid, characterized in that, It is made from the following raw materials in parts by weight: The mixture comprises 100 parts of phenolic hydroxyl polyaminate resin-1 and 2; wherein the weight ratio of phenolic hydroxyl polyaminate resin-1 to 2 is 99:1 to 50:50; 3-40 parts of photoacid-generating agent, 3-40 parts of thermal crosslinking agent, 0.1-20 parts of thermal acid-generating agent, 3-40 parts of sensitizer, 3-40 parts of tackifier, and organic solvent; The solid content in the positive photosensitive resin solution is 15 wt.%~45 wt.%, and the solution viscosity at room temperature is 500 mPa.s~4000 mPa.s; The structural formula of hydroxyl-containing polyamic acid ester resin-1 is shown below: Where: m = 2~50; X1 is selected from one of the following structures: , n = 1 or 2; Y1 is selected from one of the following structures: , R1 is an aliphatic chain, and E1 is a reactive end-capping group. The structural formula of phenolic hydroxyl polyamic acid ester resin-2 is shown below: Where: n = 2~50; X2 is selected from one of the following structures: ; Y2 is selected from one of the following structures: , R2 is an aliphatic chain; E2 is a reactive end-capping group.

2. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 1, characterized in that, A method for preparing phenolic hydroxyl polyamic acid ester resin-1 includes the following steps: Aromatic tetracarboxylic dianhydride-1 is reacted with a fatty alcohol under heating conditions to generate aromatic diacid diester; The generated aromatic diacid diester reacts with thionyl chloride to form an aromatic diester diacyl chloride; Aromatic diester diacyl chloride and phenol-hydroxyl-containing aromatic diamine-1 are reacted in an organic solvent via a condensation reaction in the presence of a reactive end-capping agent to generate a phenol-hydroxyl-containing polyamic acid ester resin solution; the resin solution is then subjected to precipitation of solid resin in a poor solvent, followed by separation, washing, and drying to obtain phenol-hydroxyl-containing polyamic acid ester resin-1; Aromatic tetracarboxylic dianhydride-1 is one or more of the following: 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,4-bis(3,4-dicarboxyphenyl)-2,4-dimethylpentane dianhydride, 2,7-bis(3,4-dicarboxyphenyl)-2,7-dimethyloctane dianhydride, 2,7-bis(3,4-dicarboxyphenyl)-2,7-dimethyldodecane dianhydride, and bis(triphenyl)-bisphenol A ester. The molar ratio of aromatic tetracarboxylic dianhydride-1, fatty alcohol, thionyl chloride and phenolic hydroxyl-containing aromatic diamine-1 is 1:2:2:

1.

3. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 2, characterized in that, The phenolic hydroxyl aromatic diamine-1 is one or more of the following: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, bis(4-amino-3-hydroxyphenyl)methane, 2,2'-bis[N-(3-aminobenzoamido)-3-amino-4-hydroxyphenyl]hexafluoropropane, 2,2'-bis[N-(4-aminobenzoamide)-3-amino-4-hydroxyphenyl]hexafluoropropane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(3-aminopropyl)tetraphenyldisiloxane, 1,3-bis(3-aminophenoxy)tetramethyldisiloxane, and 1,3-bis(4-aminophenoxy)tetramethyldisiloxane.

4. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 1, characterized in that, A method for preparing phenolic hydroxyl polyamic acid ester resin-2 includes the following steps: Aromatic tetracarboxylic dianhydride-2 is reacted with fatty alcohols under heating conditions to generate aromatic diacid diesters; The generated aromatic diacid diester reacts with thionyl chloride to form an aromatic diester diacyl chloride; Aromatic diester diacyl chloride and phenol-hydroxyl-containing aromatic diamine-2 are reacted in an organic solvent in the presence of a reactive end-capping agent to generate a phenol-hydroxyl-containing polyamic acid ester resin solution. The resin solution was precipitated into solid resin in a poor solvent. After separation, washing and drying, phenolic hydroxyl polyamic acid ester resin-2 was obtained. Aromatic tetracarboxylic dianhydride-2 includes 2,3,2',3'-diphenyl ether tetracarboxylic dianhydride, 2,3',3,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,3',2,3'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, and 2,3',2,3'-biphenyltetracarboxylic dianhydride. One or more of the following: 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 2,3',3,4'-diphenyl ether tetracarboxylic dianhydride, 2,3',2,3'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 2,3',2,3'-diphenyl sulfone tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfide tetracarboxylic dianhydride, 2,3',2,3'-diphenyl sulfide tetracarboxylic dianhydride, and 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane; The molar ratio of aromatic tetracarboxylic dianhydride-2, fatty alcohol, thionyl chloride and phenolic hydroxyl-containing aromatic diamine-2 is 1:2:2:

1.

5. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 4, characterized in that, The phenolic hydroxyl aromatic diamine-2 is one or more of the following: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, bis(4-amino-3-hydroxyphenyl)methane, 2,2'-bis[N-(3-aminobenzoamido)-3-amino-4-hydroxyphenyl]hexafluoropropane, 2,2'-bis[N-(4-aminobenzoamide)-3-amino-4-hydroxyphenyl]hexafluoropropane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(3-aminopropyl)tetraphenyldisiloxane, 1,3-bis(3-aminophenoxy)tetramethyldisiloxane, and 1,3-bis(4-aminophenoxy)tetramethyldisiloxane.

6. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 1, characterized in that, Photoacid-producing agents are diazonoquinone compounds, iodonium salts, and sulfonium salts.

7. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 1, characterized in that, Thermal crosslinking agents are compounds containing epoxy groups, or compounds containing hydroxymethyl or alkoxymethyl groups.

8. The low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 1, characterized in that, Thermally induced acid-producing agents are compounds that can produce strong acids when heated, with a thermal decomposition initiation temperature of 150℃~250℃; sensitizers are compounds containing phenolic hydroxyl, hydroxyl, or carboxyl groups.

9. A method for preparing a low-moisture-absorbing, positively photosensitive polyimide resin composition liquid according to claim 1, characterized in that, Includes the following steps: Phenolic hydroxyl polyamide ester resin-1, phenolic hydroxyl polyamide ester resin-2, photoacid-generating agent, thermal crosslinking agent, thermal acid-generating agent, sensitizer, and tackifier were added in batches to an organic solvent under stirring to form a homogeneous solution; after filtration, the solution was packaged to obtain a positive photosensitive resin liquid with a solid content of 15 wt.%~45 wt.% and a solution viscosity of 500~4000 mPa.s at room temperature.

10. The application of the low moisture absorption positive photosensitive polyimide resin composition liquid according to claim 1 in the dielectric insulating material of multilayer metal interconnect circuits, characterized in that, The photolithography patterning process for a dielectric insulating film suitable for fabricating multilayer metal interconnect circuits on the surface of a 12-inch silicon wafer or a glass substrate includes: Coating: The positive photosensitive resin liquid of claim 1 is spin-coated on the surface of a wafer or inkjet printed on the surface of a glass substrate to form a liquid film of uniform thickness; Pre-baking: Pre-baking treatment is carried out at 80℃~150℃ to form a semi-solid film; Exposure: Ultraviolet light is used to expose the material through a photomask or photomask. Developing + rinsing: Water-based developing solution is used to develop the image by spraying or immersion, followed by rinsing with ultrapure water to form a three-dimensional pattern; Heat curing: The precursor resin three-dimensional pattern on the substrate surface is heat-cured and transformed into a high heat-resistant curable resin three-dimensional pattern; A continuous conductive copper layer is formed on the surface of the resin three-dimensional graphic through an electroplating copper process. Then, the continuous conductor copper layer is etched to form conductor copper lines by photolithography, completing one RDL process; repeating the above process, a second RDL process can be formed on its surface; continue repeating the above process to form a third RDL process.