Photolithographic method
By employing multi-stage drying processes and adjusting exposure energy, the problem of insufficient adhesion between the photoresist precursor layer and the silicon nitride substrate was solved, resulting in high-quality photolithography patterns, eliminating over-development and bottom residue, and improving the process effect of semiconductor manufacturing.
Patent Information
- Application Number
- CN202611348171.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-20
AI Technical Summary
In semiconductor manufacturing, insufficient adhesion between the photoresist precursor layer with a thickness exceeding 5 micrometers and the silicon nitride substrate leads to erosion of the pattern edges and residual substrate film at the bottom during the development process, affecting the quality of the photolithography pattern.
A multi-stage drying process is adopted, including a heating stage, a bonding stage, and a cooling stage. Si-OC covalent bonds are generated through chemical condensation reaction to enhance the interfacial bonding force. The high glass transition temperature is quickly locked in the cooling stage, and the exposure energy is adjusted to compensate for the development and dissolution value after densification in the bonding stage.
It effectively eliminates over-development defects and residual substrate film, improves the quality and precision of photolithography patterns, and ensures efficient production in semiconductor manufacturing.
Smart Images

Figure CN123136971A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of semiconductor manufacturing technology, and more particularly to a photolithography method. Background Technology
[0002] In semiconductor manufacturing processes, a photoresist precursor layer is typically first coated onto the substrate surface, then dried to transform it into a photoresist layer. This is followed by exposure and development to form the desired pattern. With the increasing integration of devices, the thickness of the photoresist precursor layer often needs to reach 5 micrometers or more.
[0003] However, the adhesion between the photoresist and the silicon nitride substrate is insufficient under low-temperature pre-baking. During the development process, the developer can easily seep into the interface, causing the edge of the pattern to be eroded, resulting in overdevelopment defects such as reduced linewidth, jagged edges, and excessive exposure of the substrate. Excessively high temperatures can cause the thick film to become overly dense, which can easily produce residual film at the bottom and affect subsequent processes.
[0004] Therefore, how to provide technical solutions to improve the quality of photolithography patterns has become an urgent technical problem to be solved. Summary of the Invention
[0005] In view of this, the present disclosure provides a photolithography method that can improve the quality of photolithographic patterns.
[0006] This disclosure provides a photolithography method, comprising: providing a substrate having a silicon nitride layer on its surface; coating a photoresist precursor layer on the silicon nitride layer, the thickness of the photoresist precursor layer being greater than or equal to 5 μm; and performing a multi-stage drying process on the photoresist precursor layer to obtain a photoresist layer, the multi-stage drying process comprising: a heating stage, heating from room temperature to a first temperature at a first heating rate and maintaining the temperature for a first time to allow the solvent in the photoresist precursor layer to evaporate; and a bonding stage, heating to a second temperature at a second heating rate greater than the first heating rate. A second temperature is maintained for a second time, the second temperature being selected from 110°C to 130°C, to cause the active functional groups in the photoresist precursor layer to undergo a chemical condensation reaction with the silicon nitride layer, thereby increasing the glass transition temperature of the photoresist precursor layer; during the cooling stage, the photoresist precursor layer is cooled to room temperature at a cooling rate of greater than or equal to 5°C / s; the photoresist layer is patterned by a first exposure energy, the first exposure energy being selected from 1.15 to 1.25 times the standard exposure energy; the exposed photoresist layer is then developed to obtain the photolithographic pattern.
[0007] Optionally, in the heating stage, the first heating rate is selected from 1.5℃ / s to 2.5℃ / s, the first temperature is selected from 90℃ to 100℃, and the first time is selected from 50 seconds to 70 seconds.
[0008] Optionally, in the bonding stage, the second heating rate is greater than or equal to 3°C / s, and the second time is selected from 20 seconds to 40 seconds.
[0009] Optionally, during the cooling stage, the substrate is purged and cooled using nitrogen gas at a temperature of 15°C to 20°C.
[0010] Optionally, the method for determining the first exposure energy includes: processing the test substrate using the same process as the coating and multi-stage drying process, and forming a photoresist layer on the silicon nitride layer of the test substrate; wherein the photoresist layer on the test substrate has the same material and thickness as the photoresist layer on the substrate; exposing the test substrate in different regions, wherein the exposure dose of each exposure region of the test substrate is different, and the exposure dose is based on the standard exposure energy and increases in a gradient of 2% to 5% of the standard exposure energy; developing the exposed test substrate; measuring the residual film thickness of the photoresist layer in each exposure region; wherein the first exposure energy is the minimum exposure dose among the exposure doses corresponding to the residual film thickness of the photoresist test layer being zero.
[0011] Optionally, the development process employs a spraying process, which includes: real-time monitoring of the photoresist layer thickness using a development endpoint detector and outputting the thickness change rate; in the initial stage of development, spraying the substrate surface with a first spraying flow rate to rinse the photoresist layer; when the absolute value of the thickness change rate drops below 20% of the absolute value of the average thickness change rate within the first 5 seconds after the development reaction begins, switching to a second spraying flow rate, where the second spraying flow rate is less than the first spraying flow rate; when the absolute value of the thickness change rate is less than or equal to 0.5 nm / s, determining that the development reaction has reached its endpoint, and immediately stopping development.
[0012] Optionally, the first spray flow rate is selected from 1.8 L / min to 2.2 L / min, and the second spray flow rate is selected from 0.8 L / min to 1.2 L / min.
[0013] Optionally, the active functional groups in the photoresist precursor layer include carboxyl groups and / or hydroxyl groups, and the silicon nitride layer on the substrate surface has silanol groups (Si-OH); the chemical condensation reaction is a dehydration condensation reaction between the active functional groups and the silanol groups to generate Si-OC covalent bonds, thereby upgrading the interfacial bonding between the photoresist precursor layer and the substrate from interfacial bonding mainly based on physical adsorption to interfacial bonding mainly based on chemical bonding.
[0014] Optionally, the coating thickness of the photoresist precursor layer is selected from 5 μm to 20 μm; the photoresist precursor layer is a positive photoresist or a negative photoresist.
[0015] Optionally, the interfacial bonding energy between the photoresist layer and the substrate is greater than or equal to 300 kJ / mol.
[0016] Compared with the prior art, the technical solution of the present disclosure has the following advantages: The photolithography method provided in this disclosure includes: providing a substrate with a silicon nitride layer on its surface; coating a photoresist precursor layer on the silicon nitride layer, the thickness of the photoresist precursor layer being greater than or equal to 5 μm; performing a multi-stage drying process on the photoresist precursor layer to obtain a photoresist layer, the multi-stage drying process including: a heating stage, heating from room temperature to a first temperature at a first heating rate and maintaining it for a first time; a bonding stage, heating to a second temperature at a second heating rate greater than the first heating rate and maintaining it for a second time, the second temperature being selected from 110°C to 130°C; a cooling stage, cooling the photoresist precursor layer to room temperature at a cooling rate greater than or equal to 5°C / s; patterning the photoresist layer with a first exposure energy, the first exposure energy being selected from 1.15 to 1.25 times the standard exposure energy; and developing the exposed photoresist layer to obtain a photolithographic pattern. The multi-stage drying process achieves uniform solvent escape from the thick film layer by layer during the heating stage to avoid bubbles and stress concentration. In the bonding stage, a heating of 110℃~130℃ triggers a dehydration condensation reaction between the active functional groups in the photoresist precursor and the silanol groups on the silicon nitride layer surface, generating Si-OC covalent bonds. This elevates interfacial bonding from physical adsorption to chemical bonding and simultaneously increases the glass transition temperature of the film. This enhances interfacial adhesion from both chemical bonding and physical barrier dimensions to eliminate over-development defects. Finally, a cooling stage with temperatures greater than [missing information]... Rapid cooling at 5°C / s locks in the high glass transition temperature and suppresses latent reactions after exposure to avoid linewidth drift. Simultaneously, the first exposure energy is set to 1.15 to 1.25 times the standard exposure energy to compensate for the increased development and dissolution values after densification during the bonding stage, thus thoroughly removing residual substrate film caused by high-temperature densification. Through the synergistic effect of the above-mentioned temperature rise and dissolution, high-temperature bonding, rapid cooling locking, and exposure compensation, the process defects of "overdevelopment" and "substrate film residue" of thick photoresist (≥5μm) on silicon nitride substrates are solved. Therefore, the described photolithography method can improve the quality of photolithographic patterns. Attached Figure Description
[0017] To more clearly illustrate the technical solutions of the embodiments disclosed in this specification, the drawings used in the description of the embodiments disclosed in this specification or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this specification. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1This is a schematic flowchart of a photolithography method according to an embodiment of the present disclosure. Detailed Implementation
[0019] The technical solutions described herein will be described in detail below with reference to specific embodiments and accompanying drawings. The embodiments described herein are specific implementations of this disclosure and are used to illustrate the concept of this disclosure. These descriptions are illustrative and exemplary and should not be construed as limiting the implementation methods or the scope of protection of this disclosure. In addition to the embodiments described herein, those skilled in the art can employ other obvious technical solutions based on the content disclosed in the claims and specification of this application. These technical solutions include those that make any obvious substitutions and modifications to the embodiments described herein.
[0020] It should be noted that the accompanying drawings in this embodiment are schematic diagrams used to illustrate the concept of this disclosure, and to schematically show the shape and interrelationship of each part. It should be understood that, in order to clearly show the structure of each component of this disclosure, the drawings are not drawn to the same scale, and the same reference numerals are used to indicate the same parts in the drawings.
[0021] As described in the background section, in semiconductor manufacturing processes, a photoresist precursor layer is typically first coated onto the substrate surface, then dried to transform it into a photoresist layer, followed by exposure and development to form the desired pattern. With the continuous increase in device integration, the thickness of the photoresist precursor layer often needs to reach 5 micrometers or more.
[0022] However, the adhesion between the photoresist and the silicon nitride substrate is insufficient under low-temperature pre-baking. During the development process, the developer can easily seep into the interface, causing the edge of the pattern to be eroded, resulting in overdevelopment defects such as reduced linewidth, jagged edges, and excessive exposure of the substrate. Excessively high temperatures can cause the thick film to become overly dense, which can easily produce residual film at the bottom and affect subsequent processes.
[0023] Therefore, how to provide technical solutions to improve the quality of photolithography patterns has become an urgent technical problem to be solved.
[0024] The photolithography method provided in this disclosure includes: providing a substrate with a silicon nitride layer on its surface; coating a photoresist precursor layer on the silicon nitride layer, the thickness of the photoresist precursor layer being greater than or equal to 5 μm; performing a multi-stage drying process on the photoresist precursor layer to obtain a photoresist layer, the multi-stage drying process including: a heating stage, heating from room temperature to a first temperature at a first heating rate and maintaining it for a first time; a bonding stage, heating to a second temperature at a second heating rate greater than the first heating rate and maintaining it for a second time, the second temperature being selected from 110°C to 130°C; a cooling stage, cooling the photoresist precursor layer to room temperature at a cooling rate greater than or equal to 5°C / s; patterning the photoresist layer with a first exposure energy, the first exposure energy being selected from 1.15 to 1.25 times the standard exposure energy; and developing the exposed photoresist layer to obtain a photolithographic pattern. The multi-stage drying process achieves uniform solvent escape from the thick film layer by layer during the heating stage to avoid bubbles and stress concentration. In the bonding stage, a heating of 110℃~130℃ triggers a dehydration condensation reaction between the active functional groups in the photoresist precursor and the silanol groups on the silicon nitride layer surface, generating Si-OC covalent bonds. This elevates interfacial bonding from physical adsorption to chemical bonding and simultaneously increases the glass transition temperature of the film. This enhances interfacial adhesion from both chemical bonding and physical barrier dimensions to eliminate over-development defects. Finally, a cooling stage with temperatures greater than [missing information]... Rapid cooling at 5°C / s locks in the high glass transition temperature and suppresses latent reactions after exposure to avoid linewidth drift. Simultaneously, the first exposure energy is set to 1.15 to 1.25 times the standard exposure energy to compensate for the increased development and dissolution values after densification during the bonding stage, thus thoroughly removing residual substrate film caused by high-temperature densification. Through the synergistic effect of the above-mentioned temperature rise and dissolution, high-temperature bonding, rapid cooling locking, and exposure compensation, the process defects of "overdevelopment" and "substrate film residue" of thick photoresist (≥5μm) on silicon nitride substrates are solved. Therefore, the described photolithography method can improve the quality of photolithographic patterns.
[0025] To make the above-described objects, features and advantages of this disclosure more apparent and understandable, the disclosure is illustrated below with reference to the accompanying drawings.
[0026] See Figure 1 , Figure 1 This is a schematic flowchart of a photolithography method according to an embodiment of the present disclosure. The method can perform the following steps S101 to S105.
[0027] Step S101: Provide a substrate having a silicon nitride layer on its surface.
[0028] Step S102: Coat a photoresist precursor layer on the silicon nitride layer, wherein the thickness of the photoresist precursor layer is greater than or equal to 5 μm.
[0029] Step S103: Perform a multi-stage drying process on the photoresist precursor layer to obtain a photoresist layer. The multi-stage drying process includes: a heating stage, heating from room temperature to a first temperature at a first heating rate and maintaining it for a first time to allow the solvent in the photoresist precursor layer to evaporate; a bonding stage, heating to a second temperature at a second heating rate greater than the first heating rate and maintaining it for a second time, the second temperature being selected from 110°C to 130°C to allow the active functional groups in the photoresist precursor layer to undergo a chemical condensation reaction with the silicon nitride layer and to increase the glass transition temperature of the photoresist precursor layer; and a cooling stage, cooling the photoresist precursor layer to room temperature at a cooling rate greater than or equal to 5°C / s.
[0030] Step S104: The photoresist layer is patterned by a first exposure energy, wherein the first exposure energy is selected from 1.15 to 1.25 times the standard exposure energy.
[0031] Step S105: Develop the exposed photoresist layer to obtain the photolithographic pattern.
[0032] It is understandable that photolithography methods may include more or fewer steps, and the order of the steps may be the same or different.
[0033] In step S101, a substrate is provided, the surface of which has a silicon nitride layer.
[0034] The substrate is used to provide a process platform for the formation of semiconductor structures.
[0035] The substrate can be any semiconductor substrate known in the art, including but not limited to silicon substrates (such as single-crystal silicon wafers), germanium-silicon substrates, silicon-on-insulator (SOI) substrates, and III-V compound semiconductor substrates (such as gallium arsenide and gallium nitride). The type and specific material of the substrate can be selected according to the type of semiconductor device being manufactured and the process requirements, and the present invention does not impose any particular limitation on this.
[0036] The substrate can be a semi-finished wafer with a device structure already formed, such as a substrate that has completed some front-end processes (e.g., shallow trench isolation, gate formation, source / drain implantation, etc.) or back-end processes (e.g., interconnect layer formation, dielectric layer deposition, etc.). Subsequently, a photoresist precursor layer needs to be coated on the silicon nitride layer on the substrate surface, and a patterned photoresist layer is formed through photolithography to achieve functions such as insulation isolation between devices, surface passivation protection, or stress buffering. The photolithography method provided by this invention is applicable to both photolithographic patterning processes on blank substrates and photolithographic patterning processes on substrates with pre-formed device structures.
[0037] The silicon nitride layer is disposed on the substrate surface and can be formed by methods such as chemical vapor deposition, plasma-enhanced chemical vapor deposition, or physical vapor deposition.
[0038] The silicon nitride layer can serve multiple functions in semiconductor devices. Due to its high dielectric constant, high density, and tunable stress, silicon nitride can be used as a passivation layer to protect the device structure from the intrusion of mobile ions, moisture, or other contaminants. It can also act as an insulating layer, providing electrical isolation between conductive layers. Furthermore, silicon nitride can serve as a substrate for subsequent polyimide photoresist coating, utilizing its interfacial properties with polyimide to achieve multilayer insulating or passivating structures in the device.
[0039] The silicon nitride layer can be a single-layer structure or part of a multi-layer composite structure.
[0040] The thickness of the silicon nitride layer can be selected according to the device design requirements, and the present invention does not impose any particular limitation on it.
[0041] In step S102, a photoresist precursor layer is coated on the silicon nitride layer, and the thickness of the photoresist precursor layer is greater than or equal to 5 μm.
[0042] The photoresist precursor layer can be coated using coating methods including, but not limited to, spin coating, slot die coating, spray coating, or screen printing, with spin coating being the most commonly used implementation method.
[0043] Specifically, a liquid photoresist precursor solution (i.e., photoresist composition) is applied to the surface of a silicon nitride layer, and a wet film of the target thickness is obtained by controlling coating parameters (such as spin coating speed, acceleration, coating amount, etc.). This film is then converted into a photoresist layer through subsequent drying. In one specific embodiment, a spin coating method is used, with the spin speed set to 500 rpm to 3000 rpm and the spin coating time set to 20 seconds to 60 seconds. Specific parameters can be adjusted according to the target film thickness and the solid content, viscosity, and other characteristics of the photoresist solution.
[0044] In some embodiments, the photoresist precursor solution typically comprises a photoresist resin, a solvent (such as N-methylpyrrolidone NMP, dimethylacetamide DMAc, γ-butyrolactone GBL, etc.), and optional additives such as photosensitizers, crosslinking agents, leveling agents, and surfactants.
[0045] In this embodiment, the photoresist precursor layer is made of positive phenolic resin photoresist.
[0046] Specifically, the photoresist precursor layer is a classic positive photolithography material system using linear phenolic resin (Novolac resin) as the film-forming framework and diazonaphthoquinone as the photosensitive active ingredient, supplemented with propylene glycol methyl ether acetate and / or propylene glycol methyl ether as solvents and appropriate amounts of polyhydroxy aromatic compounds and other performance-modifying additives. The linear phenolic resin can be prepared by addition condensation reaction of phenolic derivatives and aldehyde compounds under acid catalysis, giving the photoresist film good substrate adhesion, mechanical strength and etching resistance; the diazonaphthoquinone photosensitizer acts as a dissolution inhibitor before exposure, interacting with the phenolic resin to reduce its dissolution rate in alkaline developer.
[0047] In some embodiments, the photoresist precursor layer is primarily made of polyamic acid (PAA) or polyamic ester. As a precursor to polyimide, polyamic acid is typically soluble in organic solvents such as N-methylpyrrolidone (NMP) and dimethylacetamide (DMAc), and can be mixed with photosensitizers (such as diazonaphthoquinone DNQ), crosslinking agents, leveling agents, and other additives as needed to form positive or negative photosensitive polyimide (PSPI) precursor compositions. Furthermore, depending on different molecular structure designs, the precursor can also be other types such as polyamic acid ester (PAE) or polyisoimide (PII).
[0048] The thickness of the photoresist precursor layer is greater than or equal to 5 μm.
[0049] In this embodiment, the coating thickness of the photoresist precursor layer is selected from 5 μm to 20 μm.
[0050] In some embodiments, the thickness refers to the thickness of the photoresist precursor layer after initial leveling but before drying.
[0051] In some embodiments, the thickness is the dry film thickness of the photoresist layer that is finally formed after drying.
[0052] The thickness of 5 μm or more refers to a final film thickness of 5 μm or more after subsequent drying and conversion into a photoresist layer. This thickness range is applicable to semiconductor device structures that require thicker insulating layers, planarization layers, or stress buffer layers, such as power devices, MEMS devices, and redistribution layers (RDLs) in advanced packaging.
[0053] After coating is completed, the substrate coated with the photoresist precursor layer may undergo optional pre-bake or hold steps to promote the leveling and spreading of the coating liquid on the substrate surface. However, this step is not necessary for the present invention and may be performed or not performed according to actual process requirements.
[0054] In some embodiments, before coating the photoresist precursor layer, the silicon nitride layer on the substrate surface can be pretreated. This pretreatment includes, but is not limited to, oxygen plasma treatment, ultraviolet ozone treatment, or vapor phase substrate treatment using hexamethyldisilazane (HMDS). This can improve the interfacial wettability between the photoresist precursor layer and the silicon nitride layer, preventing bubbles or pinhole defects from forming during the coating process.
[0055] In some embodiments, the photoresist precursor layer is a positive photoresist or a negative photoresist. When the photoresist precursor layer is a positive photoresist, the solubility of the photoresist precursor in the exposed area increases in the developer, and it is removed after development. When the photoresist precursor layer is a negative photoresist, the photoresist precursor in the exposed area undergoes a cross-linking reaction, its solubility in the developer decreases, and it is retained after development. The photolithography method provided by this invention is applicable to both positive and negative photoresists.
[0056] In step S103, the photoresist precursor layer is subjected to a multi-stage drying process to obtain the photoresist layer.
[0057] The multi-stage drying process includes: a heating stage, a bonding stage, and a cooling stage.
[0058] During the heating phase, the temperature is increased from room temperature to a first temperature at a first heating rate and maintained for a first time to allow the solvent in the photoresist precursor layer to evaporate.
[0059] Specifically, the first heating rate is selected from 1.5℃ / s to 2.5℃ / s, the first temperature is selected from 90℃ to 100℃, and the first time is selected from 50 seconds to 70 seconds. The first heating rate is selected from 1.5℃ / s to 2.5℃ / s, which is sufficient to complete the heating within a reasonable time window, while preventing the solvent on the surface of the photoresist precursor layer from evaporating before the internal solvent due to excessively rapid heating, thus avoiding the formation of a dense "skin layer". This ensures that the solvent escapes uniformly layer by layer while also maintaining production efficiency.
[0060] The first temperature is selected from 90°C to 100°C. This temperature range is higher than the evaporation initiation temperature of most organic solvents in the photoresist precursor layer (such as N-methylpyrrolidone, with a boiling point of about 202°C; and dimethylacetamide, with a boiling point of about 165°C), which can provide sufficient thermal energy to drive solvent molecules to diffuse and evaporate from the interior of the film to the surface, while being lower than the temperature at which the photoresist precursor undergoes a significant imidization reaction (usually starting above 120°C), ensuring that the physical solvent removal process mainly occurs during the heating phase, without prematurely triggering chemical crosslinking or imidization reactions.
[0061] The first time interval is selected from 50 seconds to 70 seconds.
[0062] The first time, in conjunction with the first temperature and the first heating rate, is maintained for a sufficiently long time during the heating phase to ensure that most of the free solvent in the photoresist precursor layer with a thickness of 5 μm or more can be fully diffused to the surface and evaporated. At the same time, the film surface will not be excessively dry or unnecessary thermal history accumulation will occur due to excessive time. This ensures sufficient solvent removal, uniformity of film structure, and overall process efficiency.
[0063] In some embodiments, the heating method used in the heating stage may be hot plate heating, infrared heating, or convection oven heating.
[0064] The hot plate heating method is a preferred embodiment of the present invention due to its advantages such as fast heating response, precise temperature control, and ease of programmable heating. When using hot plate heating, the precise heating rate of 1.5℃ / s to 2.5℃ / s and the constant temperature control of 90℃ to 100℃ can be achieved through feedback control of the heating element and temperature sensor in the hot plate.
[0065] The heating stage process allows most of the free solvent inside the photoresist precursor layer to diffuse and evaporate layer by layer from the inside to the outside along the film thickness direction, making the film structure initially compact. This provides solvent-free interface contact conditions for the chemical condensation reaction in the subsequent bonding stage, while avoiding bubbles and stress concentration in the film caused by solvent residue, thus laying the structural foundation for subsequent high-precision patterning.
[0066] During the bonding stage, the temperature is raised to a second temperature at a second heating rate greater than the first heating rate and maintained for a second time. The second temperature is selected from 110°C to 130°C, so that the active functional groups in the photoresist precursor layer undergo a chemical condensation reaction with the silicon nitride layer, and the glass transition temperature of the photoresist precursor layer is increased.
[0067] The second heating rate is greater than the first heating rate.
[0068] In some embodiments, the second heating rate is greater than or equal to 3°C / s.
[0069] The second heating rate is selected to be greater than the first heating rate (i.e., greater than 1.5℃ / s to 2.5℃ / s), preferably greater than or equal to 3℃ / s. A faster heating rate aims to allow the photoresist precursor layer to quickly cross the temperature range where solvents evaporate in large quantities (90℃ to 100℃) and rapidly enter the activation temperature window (110℃ to 130℃) required for the chemical condensation reaction. This avoids unnecessary slow pre-crosslinking or thermal decomposition of the photosensitizer in the intermediate temperature range, ensuring that the photosensitivity of the photoresist remains unaffected. It also ensures rapid entry into the reaction temperature window while maintaining equipment controllability and film uniformity.
[0070] The second time is selected from 20 seconds to 40 seconds. The second time can avoid excessive thermal crosslinking or imidization reaction of the photoresist precursor layer at high temperature, thereby protecting the photosensitivity and development and dissolution properties of the photoresist; and ensure that the chemical condensation reaction at the interface can proceed fully, so that the active functional groups and the silanol groups on the surface of the silicon nitride layer form a sufficiently dense covalent bond, thereby increasing the interfacial bonding energy to above 300 kJ / mol, and thus achieving a balance between sufficient bonding and avoiding excessive crosslinking.
[0071] The second temperature is selected from 110°C to 130°C.
[0072] Specifically, the active functional groups in the photoresist precursor layer include carboxyl groups (-COOH) and / or hydroxyl groups (-OH), while the surface of the silicon nitride layer has silanol groups (Si-OH) under natural conditions or after plasma treatment. When the temperature reaches above 110°C, the active functional groups can obtain sufficient activation energy to overcome the energy barrier of the dehydration condensation reaction. A dehydration condensation reaction occurs between the carboxyl groups and silanol groups, or between the hydroxyl groups and silanol groups, generating Si-OC covalent bonds. The bond energy of this covalent bond is much higher than the van der Waals forces of physical adsorption, increasing the interfacial bonding energy between the photoresist precursor layer and the silicon nitride substrate from less than or equal to 10 kJ / mol (primarily due to physical adsorption) to greater than or equal to 300 kJ / mol (primarily due to chemical bonding). This second temperature triggers interfacial chemical bonding between the photoresist precursor layer and the silicon nitride layer, while simultaneously preventing thermal failure of the photoresist.
[0073] Furthermore, the bonding stage treatment at 110°C to 130°C significantly increases the glass transition temperature of the photoresist precursor layer. The glass transition temperature of the photoresist precursor layer is closely related to the mobility and free volume of its molecular chains. Within the temperature range of 110°C to 130°C, the molecular chains of the photoresist precursor layer gain sufficient kinetic energy, leading to further arrangement and entanglement between the chains. Combined with the thorough removal of the solvent, this reduces the free volume of the film and decreases the mobility of the molecular chain segments. When the temperature cools to room temperature, the glass transition temperature of the film is permanently increased to a level far exceeding the development temperature, making it difficult for developer molecules to penetrate into the interior of the film during development, thereby further suppressing overdevelopment from a physical barrier perspective.
[0074] Therefore, the bonding stage treatment at the second temperature achieves the dual effects of "enhancing interfacial bonding through chemical bonding" and "improving resistance to penetration through physical densification." At the chemical level, the interfacial bonding method is upgraded from physical adsorption to chemical bonding via Si-OC covalent bonds, fundamentally eliminating the path of developer penetration along the interface. At the physical level, by increasing the glass transition temperature, the film layer is in a dense glassy state at the developing temperature, making it difficult for developer molecules to penetrate longitudinally into the film layer, thereby inhibiting overdevelopment.
[0075] The progress of the chemical condensation reaction can be verified by measuring the interfacial binding energy.
[0076] In some embodiments, X-ray photoelectron spectroscopy (XPS) is used to characterize the interface before and after the bonding treatment: before treatment, characteristic peaks such as CC, CO, and Si-N / Si-O are mainly detected at the interface, indicating that there is only physical contact between the photoresist precursor layer and the silicon nitride layer; after the bonding stage treatment, a new Si-OC characteristic peak is detected at the interface, indicating that chemical covalent bonds have been formed at the interface. The presence and thickness of the chemically bonded layer can be further verified by analyzing the interface transition layer using angle-resolved XPS or high-resolution transmission electron microscopy combined with electron energy loss spectroscopy. Simultaneously, the interface binding energy can be quantitatively measured by scratch testing or four-point bending testing. The interface binding energy after the bonding stage treatment can reach over 300 kJ / mol, which is much higher than that of the untreated physisorption interface (≤10 kJ / mol).
[0077] The second heating rate, the second temperature, and the second time are interrelated. The second heating rate determines the speed at which the photoresist precursor layer enters the 110°C~130°C reaction window; the second temperature determines whether the interfacial chemical reaction can occur, as well as the rate and extent of the reaction; and the second time determines whether the reaction is sufficient but not excessive. These three factors work synergistically to ensure the full realization of interfacial chemical bonding and the effective protection of the photoresist's photosensitivity.
[0078] During the cooling phase, the photoresist precursor layer is cooled to room temperature at a cooling rate of 5°C / s or greater.
[0079] During the cooling stage, the substrate is purged and cooled using nitrogen gas at a temperature of 15°C to 20°C.
[0080] Specifically, the cooling rate is greater than or equal to 5°C / s, which rapidly lowers the temperature of the photoresist precursor layer to room temperature after the bonding stage. This physically locks the dense arrangement of molecular chains formed during the bonding stage and the increased glass transition temperature, preventing the glass transition temperature from dropping back due to the relaxation of molecular chains to a lower energy barrier state during slow cooling. The diffusion rate and reactivity of photoactive species (such as photoacids or free radicals) that may be generated after exposure at room temperature are suppressed by reducing the heat supply, thereby curbing latent reactions after exposure (i.e., the phenomenon that photoactive species continue to slowly diffuse and erode the edges of non-exposed areas during the waiting period after exposure).
[0081] During the cooling stage, nitrogen gas at a temperature of 15°C to 20°C is used to purge and cool the substrate. As an inert gas, nitrogen serves a dual function of cooling and atmosphere protection during purging. Firstly, the low-temperature nitrogen gas purges the substrate surface at a certain flow rate, removing heat from the photoresist precursor layer and the substrate through forced convection heat exchange, achieving rapid cooling. The nitrogen temperature is selected from 15°C to 20°C to prevent condensation on the substrate surface or photoresist precursor layer due to excessive temperature differences. Nitrogen purging can also quickly remove organic solvent vapors or byproducts (such as water vapor generated by dehydration condensation reactions) that may be released during the bonding stage from the substrate surface, preventing them from re-adsorbing or condensing on the photoresist precursor layer surface during cooling, thereby maintaining the cleanliness and chemical stability of the film surface.
[0082] In some embodiments, the flow rate of the nitrogen purging is selected from 50 L / min to 150 L / min, and the purging direction is inclined at an angle of 30° to 60° relative to the substrate surface to avoid physical impact or airflow turbulence on the film surface caused by vertical purging.
[0083] The chemical bonding state and dense film structure formed during the bonding stage are locked, and the glass transition temperature of the photoresist precursor layer is maintained at a high level, significantly suppressing the penetration rate of developer molecules in subsequent development processes. Therefore, the cooling stage ensures high fidelity of subsequent exposure patterns and consistency of development endpoints, making the exposed photolithographic pattern less sensitive to post-exposure waiting time, significantly improving the process tolerance window and mass production reliability.
[0084] After the photoresist precursor layer is subjected to multi-stage drying treatment, the organic solvent in the photoresist precursor layer is fully evaporated and removed, thereby forming a uniform, dense solid photoresist film with good adhesion on the substrate surface, namely the photoresist layer.
[0085] In some embodiments, after the photoresist precursor layer is dried in multiple stages, the linear phenolic resin and the diazonoquinone photosensitizer remain uniformly dispersed, and the diazonoquinone remains stable in its dissolution-inhibiting form. This results in the solid film exhibiting an extremely low dissolution rate in the tetramethylammonium hydroxide alkaline developer in the unexposed state (i.e., the developer does not erode the film at all). At the same time, the film has a uniform thickness, a smooth and defect-free surface, and sufficient mechanical strength and scratch resistance to support the high-precision pattern transfer in subsequent exposure processes.
[0086] In some embodiments, the photoresist layer is primarily made of polyimide (PI). Polyimide is a high-performance polymer material with excellent heat resistance, mechanical properties, electrical insulation properties, and chemical corrosion resistance, and is widely used as an insulating layer, buffer layer, or protective layer in semiconductor devices. Depending on the type of photosensitizer in the photoresist precursor components, the final polyimide photoresist can be positive (the exposed area is dissolved and removed in the developer) or negative (the exposed area is cross-linked, cured, and retained), both of which are suitable for the photolithography method described in this solution.
[0087] In step 104, the photoresist layer is patterned by a first exposure energy, which is selected from 1.15 to 1.25 times the standard exposure energy.
[0088] In existing technologies, exposure processes typically employ standard exposure energy for pattern exposure. This standard exposure energy is determined based on the current product's design rule and standard process specification. For example, it is determined by the minimum exposure dose required to achieve zero residual film thickness after exposure and development under low-temperature pre-baking conditions (80℃~100℃) based on the photoresist's photosensitivity curve, photoresist layer thickness, and target linewidth. After verification that it meets the pattern resolution requirements, it is fixed as the benchmark exposure dose for this process condition.
[0089] When the photoresist film thickness is greater than or equal to 5 μm, based on the standard exposure energy determined by the low-temperature pre-baking conditions, the photoresist layer in the exposed area is prone to complete dissolution after employing the multi-stage drying process of this invention (especially the densification process at 110℃~130℃). The bonding stage process densifies the photoresist precursor layer and increases the glass transition temperature. Simultaneously, a chemical condensation reaction occurs at the interface to generate Si-OC covalent bonds. These physical and chemical changes together significantly increase the dissolution threshold of the exposed area in the developer. If the original exposure method is still used, the concentration of photoactive species at the substrate interface is insufficient to allow the densified photoresist layer to overcome the increased dissolution value, resulting in residual substrate film at the bottom.
[0090] In this embodiment, the standard exposure energy is the minimum exposure dose corresponding to the point where the residual film thickness of the photoresist layer in the exposed area is zero after exposure to the photoresist layer under low-temperature pre-baking conditions of 80℃~100℃ and development. The minimum exposure dose is the reference exposure dose (standard exposure energy) used by photolithography engineers in existing low-temperature pre-baking processes, and can be determined based on the photosensitivity curve provided by the photoresist supplier and actual process verification.
[0091] In this embodiment, the first exposure energy is selected from 1.15 to 1.25 times the standard exposure energy. That is, compared with the standard exposure energy determined in the existing low-temperature pre-baking process, the present invention actively increases the exposure dose by 15% to 25%, thereby using a larger exposure energy. The determination of this multiple range is not an empirical and arbitrary increase, but is based on the quantitative measurement and precise compensation of the change in the development dissolution value after densification in the bonding stage.
[0092] In some embodiments, the method for determining the first exposure energy includes the following steps S1041 to S1044.
[0093] Step S1041: The test substrate is processed using the same process as the coating and multi-stage drying process to form a photoresist test layer on the silicon nitride layer of the test substrate; wherein the photoresist test layer on the test substrate has the same material and thickness as the photoresist layer on the substrate.
[0094] Step S1042: Expose the test substrate in different regions, wherein the exposure dose of each exposure region of the test substrate is different, and the exposure dose is based on the standard exposure energy and increases in a gradient of 2% to 5% of the standard exposure energy.
[0095] Step S1043: Develop the exposed test substrate.
[0096] Step S1044: Measure the residual film thickness of the photoresist test layer in each exposure area; wherein, the first exposure energy is the minimum exposure dose among all exposure doses corresponding to the residual film thickness of the photoresist test layer being zero.
[0097] Specifically, the test substrate is processed using the same process as the aforementioned coating and multi-stage drying treatment, forming a photoresist test layer on the silicon nitride layer of the test substrate. The test substrate can be a wafer from the same batch as the product substrate, or it can be a separate test wafer, as long as its surface has a silicon nitride layer. The photoresist test layer on the test substrate has the same material and thickness as the photoresist layer on the product substrate to ensure a reliable mapping of the measurement results to the product process.
[0098] In some embodiments, the test substrate is subjected to open-frame exposure, that is, the entire surface of the test substrate is exposed without using a mask, and the test substrate is divided into multiple exposure areas.
[0099] In some embodiments, the test substrate is divided into multiple exposure areas, with sufficient isolation spacing (preferably ≥5mm) between each area to avoid light crosstalk or scattered light interference between adjacent areas.
[0100] Different exposure doses are applied to each exposure area, with each exposure dose increasing in a gradient from 2% to 5% of the standard exposure energy, based on the standard exposure energy. For example, when the step size is set to 5% of the standard exposure energy, the exposure dose sequence is 0.80×E0, 0.85×E0, 0.90×E0, ..., 1.40×E0, where E0 is the standard exposure energy. Those skilled in the art can select an appropriate step size value within the range of 2% to 5% of the standard exposure energy based on the type of photoresist used, film thickness, and equipment conditions.
[0101] The exposed test substrate is then subjected to a development process. The development conditions (such as the type of developer, development temperature, and development time) are exactly the same as those in the product manufacturing process to ensure consistency between the measurement results and the actual production process.
[0102] After development, the residual film thickness of the photoresist test layer in each exposed area is measured using a film thickness gauge or scanning electron microscope (SEM). The minimum exposure dose among all exposure doses corresponding to a residual film thickness of zero (i.e., the photoresist test layer is completely removed and there is no residue on the silicon nitride layer surface) is determined as the first exposure energy.
[0103] If the residual film thickness of the photoresist test layer in all exposed areas is not zero, it indicates that the set exposure dose range is generally too low, and the upper dose limit needs to be increased for re-measurement; if the residual film thickness in all exposed areas is zero, it indicates that the set exposure dose range is generally too high, and the lower dose limit needs to be decreased for re-measurement. Experimental verification shows that the first exposure energy determined using the above method corresponds to a value range of 1.15 to 1.25 times the standard exposure energy.
[0104] In other embodiments, the above measurement method may also perform single-dose exposure on multiple test substrates (i.e., only one exposure dose is applied to each test substrate), rather than performing partitioned exposure on a single test substrate.
[0105] Specifically, multiple test substrates are prepared, each with the same photoresist layer material and thickness. Each substrate is exposed to a full surface using different exposure doses (based on the standard exposure energy, with increments of 2% to 5% of the standard exposure energy, increasing in a gradient). Subsequently, uniform development is performed, and the residual photoresist layer thickness on each substrate is measured. The minimum exposure dose corresponding to zero residual film thickness is determined as the first exposure energy. The measurement principle is exactly the same as the aforementioned zoned exposure method, and it achieves the same technical effect as this invention.
[0106] In step S105, the exposed photoresist layer is developed to obtain the photolithographic pattern.
[0107] The developing process employs a spraying technique, in which the developing solution is sprayed onto the photoresist layer on the substrate surface at a certain flow rate using a spraying device, in order to dissolve and remove the photoresist layer in the exposed areas (for positive photoresist).
[0108] In this embodiment, the developing endpoint detector is an online film thickness monitoring device based on the principle of optical interference, which includes a light source, a light receiver, and a signal processor.
[0109] Specifically, during the development process, a light source emits a detection beam towards the photoresist layer on the substrate surface. The beam is reflected at the upper surface of the photoresist layer and at the interface between the photoresist layer and the substrate, and the two reflected beams interfere. Since there is a definite functional relationship between the intensity of the reflected interference signal and the thickness of the photoresist layer, the photodetector converts the received reflected light signal into an electrical signal and transmits it to the signal processor. The signal processor calculates and outputs the current thickness of the photoresist layer in real time based on this functional relationship.
[0110] The film thickness change rate can be calculated as follows: The signal processor continuously acquires real-time film thickness data of the photoresist layer at a sampling frequency of not less than 10Hz. The difference in film thickness between two adjacent sampling times is divided by the sampling time interval, and the resulting value is the film thickness change rate at that time, in nm / s. The signal processor outputs this film thickness change rate to the main controller of the developing equipment in real time.
[0111] In the initial development stage, the substrate surface is sprayed with a first spray flow rate to wash away the photoresist layer in the exposed area.
[0112] The first spray flow rate is 1.8 L / min to 2.2 L / min. This larger flow rate is used to quickly wash away the photoresist layer that has undergone photochemical reaction after exposure from the substrate surface in the early stage of development, so as to avoid the accumulation of reaction products on the substrate surface and thus prevent the fresh developer from contacting the undissolved photoresist layer.
[0113] The main controller of the developing equipment compares the absolute value of the film thickness change rate received in real time with the absolute value of the average film thickness change rate within the first 5 seconds after the development reaction begins.
[0114] When the absolute value of the film thickness change rate drops to less than 20% of the absolute value of the average film thickness change rate in the first 5 seconds, it indicates that the development reaction rate has been significantly reduced and a large amount of photoresist layer has been removed. At this time, the second spray flow rate is switched to spray.
[0115] The second spray flow rate is less than the first spray flow rate.
[0116] The second spray flow rate is selected from 0.8L / min to 1.2L / min, and is used to remove residual trace amounts of photoresist layer in a gentle spraying manner during the later stage of development, avoiding damage to the exposed pattern structure caused by high-flow spraying, while reducing the consumption of developer.
[0117] When the absolute value of the film thickness change rate is less than or equal to 0.5 nm / s, the development reaction is determined to have reached its endpoint, and the main controller immediately issues a stop command to stop the development process.
[0118] Specifically, the 0.5 nm / s endpoint threshold is set according to the equipment noise level of the developing endpoint detector, and is usually taken as the film thickness change rate value corresponding to three times the standard deviation of the equipment noise signal.
[0119] During the development reaction, the photoresist layer continuously dissolves, the film thickness decreases, and the absolute value of the film thickness change rate remains at a high level. Once the photoresist layer in the exposed area is completely removed, the film thickness no longer changes significantly, and the absolute value of the film thickness change rate rapidly decreases and approaches zero. Therefore, using the threshold corresponding to an absolute value of the film thickness change rate being less than or equal to three times the standard deviation of the equipment noise as the criterion for the development endpoint can accurately capture the moment of development completion while effectively avoiding misjudgments caused by equipment noise.
[0120] In some embodiments, the developing endpoint detector employs a multi-channel fiber optic probe array to simultaneously monitor film thickness changes at different locations on the substrate surface through multiple detection channels. The arithmetic mean of the film thickness change rate data from each channel is used for endpoint determination, thereby eliminating measurement deviations caused by uneven local development and improving the reliability and accuracy of endpoint determination.
[0121] In other embodiments, in addition to the film thickness change rate, the optical signal intensity change rate of the developer can also be used as an auxiliary criterion. After the developer dissolves the photoresist layer, its transmittance or reflectance will change accordingly. By monitoring the optical signal intensity change rate of the developer, the endpoint determination result of the film thickness change rate can be verified, further improving the accuracy of the development endpoint determination. When both criteria indicate that development has reached the endpoint, the main controller issues a stop command.
[0122] By combining spraying processes with varying flow rates with development endpoint detection, precise control of the development process and accurate determination of the endpoint are achieved. In the initial stage of development, a high flow rate is used to rapidly remove the main adhesive layer to improve production efficiency. In the later stage of development, a low flow rate is used to meticulously remove residual adhesive layers to protect the pattern structure. Simultaneously, real-time film thickness monitoring accurately captures the development endpoint, ensuring both sufficient development (no substrate residue) and avoiding pattern damage caused by overdevelopment (no width reduction, no edge jaggedness), thereby significantly improving the quality and consistency of the photolithography pattern.
[0123] The foregoing describes several embodiments of the photolithography method. The optional methods described in each embodiment can be combined and cross-referenced without conflict, thereby extending to a variety of possible embodiments. These can all be considered as embodiments disclosed in this disclosure.
[0124] While the embodiments disclosed above are described in this application, this application is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of this application; therefore, the scope of protection of this application should be determined by the scope defined in the claims.
[0125] It should be understood that the term "and / or" in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the character " / " in this article indicates that the preceding and following related objects have an "or" relationship.
[0126] In the embodiments of this application, "multiple" refers to two or more.
[0127] The descriptions of "first," "second," etc., appearing in the embodiments of this application are for illustrative purposes and to distinguish the objects being described. They have no order and do not indicate any special limitation on the number of objects in the embodiments of this application. They cannot constitute any limitation on the embodiments of this application.
[0128] While the embodiments disclosed herein are as described above, this disclosure is not limited thereto. Any person skilled in the art can make various alterations and modifications without departing from the spirit and scope of this disclosure; therefore, the scope of protection of this disclosure should be determined by the scope defined in the claims.
Claims
1. A photolithography method, characterized in that, include: A substrate is provided, the surface of which has a silicon nitride layer; A photoresist precursor layer is coated on the silicon nitride layer, and the thickness of the photoresist precursor layer is greater than or equal to 5 μm; The photoresist precursor layer is subjected to a multi-stage drying process to obtain a photoresist layer. The multi-stage drying process includes: During the heating phase, the temperature is increased from room temperature to a first temperature at a first heating rate and maintained for a first time to allow the solvent in the photoresist precursor layer to evaporate. During the bonding stage, the temperature is raised to a second temperature at a second heating rate greater than the first heating rate and maintained for a second time. The second temperature is selected from 110°C to 130°C, so that the active functional groups in the photoresist precursor layer undergo a chemical condensation reaction with the silicon nitride layer and the glass transition temperature of the photoresist precursor layer is increased. During the cooling stage, the photoresist precursor layer is cooled to room temperature at a cooling rate of 5°C / s or higher. The photoresist layer is patterned using a first exposure energy, wherein the first exposure energy is selected from 1.15 to 1.25 times the standard exposure energy; The exposed photoresist layer is developed to obtain the photolithographic pattern.
2. The method according to claim 1, characterized in that, During the heating phase, the first heating rate is selected from 1.5℃ / s to 2.5℃ / s, the first temperature is selected from 90℃ to 100℃, and the first time is selected from 50 seconds to 70 seconds.
3. The method according to claim 1, characterized in that, During the bonding stage, the second heating rate is greater than or equal to 3°C / s, and the second time is selected from 20 seconds to 40 seconds.
4. The method according to claim 1, characterized in that, During the cooling stage, nitrogen gas at a temperature of 15°C to 20°C is used to purge and cool the substrate.
5. The method according to claim 1, characterized in that, The method for determining the first exposure energy includes: The test substrate is processed using the same process as the coating and multi-stage drying process, and a photoresist test layer is formed on the silicon nitride layer of the test substrate; wherein the photoresist test layer on the test substrate has the same material and thickness as the photoresist layer on the substrate; The test substrate is exposed in different regions, wherein the exposure dose of each exposure region of the test substrate is different, and the exposure dose is based on the standard exposure energy and increases in a gradient of 2% to 5% of the standard exposure energy. The exposed test substrate is then developed. Measure the residual film thickness of the photoresist test layer in each exposure area; Wherein, the first exposure energy is the minimum exposure dose among all exposure doses corresponding to the photoresist test layer residual film thickness being zero.
6. The method according to claim 1, characterized in that, The developing process employs a spraying process, which includes: The thickness of the photoresist layer is monitored in real time by a development endpoint detector, and the thickness change rate is output. In the initial stage of development, the substrate surface is sprayed with a first spray flow rate to rinse the photoresist layer. When the absolute value of the film thickness change rate drops to less than 20% of the absolute value of the average film thickness change rate within the first 5 seconds after the development reaction begins, the spraying is switched to the second spray flow rate, which is less than the first spray flow rate. When the absolute value of the film thickness change rate is less than or equal to 0.5 nm / s, the development reaction is determined to have reached its endpoint, and development is immediately stopped.
7. The method according to claim 6, characterized in that, The first spray flow rate is selected from 1.8 L / min to 2.2 L / min, and the second spray flow rate is selected from 0.8 L / min to 1.2 L / min.
8. The method according to claim 1, characterized in that, The active functional groups in the photoresist precursor layer include carboxyl groups and / or hydroxyl groups, and the silicon nitride layer on the substrate surface has silanol groups (Si-OH). The chemical condensation reaction is a dehydration condensation reaction between the active functional group and the silanol group, generating Si-OC covalent bonds, thereby upgrading the interfacial bonding between the photoresist precursor layer and the substrate from a physical adsorption-based interfacial bonding to a chemical bonding-based interfacial bonding.
9. The method according to claim 1, characterized in that, The coating thickness of the photoresist precursor layer is selected from 5 μm to 20 μm; The photoresist precursor layer is either a positive photoresist or a negative photoresist.