Photoresist stripping solution, method for preparing the same, and use thereof
By combining fatty amino alcohol ethers, polar solvents, and triazine metal corrosion inhibitors, the corrosion problem of traditional photoresist stripping solutions on metal films was solved, achieving efficient stripping and cleaning effects and improving the performance and stability of the photoresist stripping solution.
Patent Information
- Application Number
- CN202611468946.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional photoresist stripping solutions can easily lead to excessive corrosion of metal films under high-temperature conditions, and may leave residues that affect the quality of subsequent processes.
A compound system consisting of fatty amine alcohol ethers, polar solvents, and triazine metal corrosion inhibitors is adopted. The fatty amine alcohol ethers provide moderate alkaline fracture of the intramolecular/intermolecular bonds of the photoresist, the polar solvents enhance wettability and dispersibility, and the triazine corrosion inhibitors form a protective film at the metal interface. The synergistic effect achieves efficient stripping and metal corrosion inhibition.
It achieves efficient decomposition of photoresist, reduces the risk of corrosion to underlying metals such as copper and molybdenum, improves wettability and penetration, simplifies the types of raw materials, reduces batch fluctuation risk, and improves cleaning effect and metal compatibility.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] This invention relates to the field of photoresist stripping solution technology, and more specifically, to a photoresist stripping solution, its preparation method, and its application. Background Technology
[0002] Photolithography, a crucial process in semiconductor manufacturing and display device production, directly impacts the quality of the final product through the performance of its core material, photoresist. In the semiconductor industry, the manufacturing of integrated circuits (ICs) and very large-scale integrated circuits (VLSIs), as well as the production of image display devices such as liquid crystal displays (LCDs) and flat panel displays (PDPs), all rely on precise photolithography processes. After the photolithography process is complete, a stripping process is necessary to thoroughly remove any remaining photoresist; this step has a decisive influence on the quality of subsequent processing.
[0003] Traditional photoresist stripping solutions mainly consist of amine compounds and organic solvents, with added auxiliary components such as metal corrosion inhibitors. These stripping solutions act on photoresist under high-temperature conditions, aiming to ensure complete removal of photoresist residues, maintain good washability, and minimize corrosion of the underlying metal film. However, conventional organic amine stripping solutions have significant drawbacks in practical applications: firstly, their strong alkalinity can easily lead to excessive corrosion of the metal film; secondly, residues may remain during the cleaning process, causing quality problems in subsequent processes. These technical limitations necessitate the development of novel stripping solutions that simultaneously meet the triple requirements of efficient stripping, easy cleaning, and excellent metal protection.
[0004] In view of this, the present invention is proposed. Summary of the Invention
[0005] The purpose of this invention is to provide a photoresist stripping solution, its preparation method, and its application. The photoresist stripping solution provided by this invention has excellent decomposition ability for photoresist, while reducing the corrosion risk to metals such as copper and molybdenum.
[0006] This invention is implemented as follows: In a first aspect, the present invention provides a photoresist stripping solution, comprising, by weight percentage, 40wt%~79wt% fatty amino alcohol ether, 20wt%~59wt% polar solvent, and 0.5wt%~5wt% metal corrosion inhibitor; the chemical formula of the fatty amino alcohol ether is: .
[0007] In the above chemical formula, R1 is selected from any one of H, -OH, -CH2OH, -CH2CH2OH and C1~C3 chain alkyl groups; R2 is selected from any one of H, -OH, -CH2OH, -CH2CH2OH and C1~C3 chain alkyl groups; n is an integer from 2 to 4.
[0008] Secondly, the present invention provides a method for preparing a photoresist stripping solution as described in any of the foregoing embodiments, comprising mixing raw materials uniformly in a specified proportion.
[0009] Thirdly, the present invention provides an application of a photoresist stripping solution as described in any of the foregoing embodiments in a photoresist stripping process.
[0010] The present invention has the following beneficial effects: This invention provides a photoresist stripping solution, its preparation method, and its applications. By employing a fatty amine alcohol ether with a specific structure, this invention retains moderate alkalinity to break intramolecular / intermolecular bonds in the photoresist, while its alkalinity is weaker than traditional fatty amine and alcohol ether complex systems. This allows for efficient decomposition of the photoresist while inhibiting corrosion of underlying metals such as copper and molybdenum. This structure also imparts excellent wettability to the system, enhancing penetration and spreading capabilities into micro / nano structures, and improving the efficiency of residue removal during subsequent rinsing, thus improving the rinsing effect. The polar solvent synergistically enhances the photoresist swelling and product dispersion capabilities, ensuring effective exposure of the functional sites of the fatty amine alcohol ether; further, the probability of metal corrosion can be reduced by combining it with a metal corrosion inhibitor. The complementary and synergistic effects of these three components enable the stripping solution to possess efficient stripping, thorough cleaning, and excellent metal compatibility. Furthermore, the photoresist stripping solution system provided by this invention simplifies the types of raw materials, reduces formulation complexity and batch variation risks, and facilitates solvent recovery. It has outstanding practicality and industrial application value in the post-processing stage of photolithography processes in advanced semiconductor manufacturing and high-resolution display panels. Detailed Implementation
[0011] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0012] In a first aspect, the present invention provides a photoresist stripping solution, comprising, by weight percentage, 40wt%~79wt% fatty amino alcohol ether, 20wt%~59wt% polar solvent, and 0.5wt%~5wt% metal corrosion inhibitor; the chemical formula of the fatty amino alcohol ether is: .
[0013] In the above chemical formula, R1 is selected from any one of H, -OH, -CH2OH, -CH2CH2OH and C1~C3 chain alkyl groups; R2 is selected from any one of H, -OH, -CH2OH, -CH2CH2OH and C1~C3 chain alkyl groups; n is an integer from 2 to 4.
[0014] By employing aliphatic amino alcohol ethers with the aforementioned structure, the stripping performance of photoresist materials can be improved while simultaneously enhancing the wettability of the photoresist stripping solution. This, in turn, improves the rinsing ability of the photoresist stripping solution on the photoresist material and provides partial alkalinity to enhance the stripping effect. By compounding aliphatic amino alcohol ethers with polar solvents and triazine metal corrosion inhibitors, the resulting photoresist stripping solution can not only dissolve and clean the photoresist but also provide alkalinity to break down intramolecular or intermolecular bonds. Furthermore, this photoresist stripping solution exhibits corrosion stability against the underlying metal, demonstrating outstanding practicality and industrial application value in the post-processing stages of photolithography processes in advanced semiconductor manufacturing and high-resolution display panels.
[0015] In an optional embodiment, in the chemical formula of the fatty amino alcohol ether, R1 is selected from any one of H and C1~C3 chain alkyl groups; R2 is selected from any one of H and C1~C3 chain alkyl groups.
[0016] In the chemical formula of aliphatic amine alcohol ethers, the choice of R1 and R2 affects the basicity of the aliphatic amine alcohol ether. By selecting the above-mentioned R1 and R2 groups, compared with the existing photoresist stripping solutions that directly mix aliphatic amine compounds with alcohol ether compounds, the aliphatic amine alcohol ether selected in this invention has a weaker basicity, but is sufficient to decompose photoresist, and is easy to recycle, thus reducing the risk of corrosion to metals. By using aliphatic amine alcohol ethers in synergy with metal corrosion inhibitors, the anti-corrosion effect of the photoresist stripping solution can be further enhanced.
[0017] Preferably, in the photoresist stripping solution provided by the present invention, the amount of fatty amino alcohol ether added is greater than the amount of polar solvent added, so as to ensure that the photoresist stripping solution has sufficient photoresist stripping effect.
[0018] Preferably, the fatty amino alcohol ether is selected from any one of 2-[2-(dimethylamino)ethoxy]ethanol ((CH3)2N(CH2CH2O)2H), 2-(2-diethylaminoethoxy)ethanol ((CH3CH2)2N(CH2CH2O)2H), 2-[2-(methylamino)ethoxy]ethane-1-ol ((CH3)NH(CH2CH2O)2H) and diethylene glycolamine (NH2(CH2CH2O)2H).
[0019] By selecting the aforementioned fatty amine alcohol ethers, the peeling performance of photoresist materials can be improved, while simultaneously enhancing the wettability of the peeling solution composition and further improving the rinsing ability of photoresist materials, while also providing partial alkalinity to enhance the peeling effect. At the same time, the selection of fatty amine alcohol ethers simplifies the types of raw materials, reduces formulation complexity and batch variation risk, and facilitates solvent recovery.
[0020] In optional embodiments, the polar solvent includes at least one of dimethyl sulfoxide (DMSO), sulfolane (SL), N-methylformamide (NMF), N-methylacetamide (NMA), N-methylpyrrolidone (NMP), N-ethylpyrrolidone (NEP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N,N-dimethylpropionamide (DMPA).
[0021] By selecting the aforementioned polar solvents, not only can the gelled photoresist polymers be dissolved, but the mild alkalinity of the fatty amino alcohol ethers can also be synergistically utilized to promote the decomposition of photosensitive components in the photoresist and the dissociation of resin backbone segments. This also ensures the effective adsorption and film formation of triazine corrosion inhibitors at the metal interface, thereby achieving a dynamic balance between stripping efficiency, water rinsing residue control, and inhibition of underlying metal corrosion. After the photoresist stripping process is completed, the selection of these polar solvents also facilitates the removal of the photoresist stripping solution when rinsing the metal wiring structure with deionized water, ensuring product yield.
[0022] In optional embodiments, the metal corrosion inhibitor includes triazine-based metal corrosion inhibitors or triazole-based metal corrosion inhibitors, preferably triazine-based metal corrosion inhibitors. Compared with triazole-based metal corrosion inhibitors, triazine-based corrosion inhibitors are relatively cheaper and show less difference in corrosion inhibition effect on molybdenum and copper, resulting in a better overall corrosion inhibition effect.
[0023] Triazine metal corrosion inhibitors include at least one of 1,3,5-triazine, 2-amino-1,3,5-triazine, 6-methyl-1,3,5-triazine-2,4-diamine, 2,4,6-tris(pyridyl)triazine, and 2,4,6-triamino-1,3,5-triazine.
[0024] By selecting the above-mentioned triazine-based metal corrosion inhibitors, a dense heterocyclic coordination film can be directionally adsorbed at the metal interface in a fatty amine alcohol ether-polar solvent composite system, effectively blocking the erosion of metal grain boundaries and edges by alkaline components and residual organic matter in the stripping solution. This significantly inhibits side etching and undercut phenomena that occur during photoresist stripping, ensuring the geometric fidelity and electrical reliability of the metal wiring structure.
[0025] In an optional embodiment, the photoresist stripping solution comprises, by weight percentage, 40-79 wt% fatty amino alcohol ether, 20-59 wt% polar solvent, and 0.5-5 wt% triazine metal corrosion inhibitor.
[0026] By controlling the mass of each raw material within the aforementioned proportion range, a dynamic balance can be achieved between alkaline depolymerization capability, polymer dissolution capability, and interfacial corrosion inhibition capability. Specifically, the fatty amine alcohol ether provides appropriate alkalinity to break intramolecular / intermolecular bonds in the photoresist, the polar solvent ensures uniform dispersion and synergistically swells the stripping products, and the triazine corrosion inhibitor forms a highly effective adsorption protective film on the metal surface within this concentration window. Thus, the photoresist stripping solution provided by this invention simultaneously meets the process requirements of efficient stripping, thorough cleaning, and zero-damage corrosion.
[0027] In an optional embodiment, the mass percentage of fatty amino alcohol ether in the photoresist stripping solution is 40 wt% to 79 wt%. When the content of fatty amino alcohol ether is less than 40 wt%, it may lead to a decrease in the stripping and cleaning properties of the photoresist; when the content of fatty amino alcohol ether is greater than 79 wt%, corrosion or damage to the metal film layer in the metal wiring structure may occur.
[0028] For example, in the photoresist stripping solution provided by the present invention, the mass percentage of fatty amino alcohol ether in the photoresist stripping solution can be any value or a range formed by any two of the following: 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, or 79wt%.
[0029] Preferably, the mass percentage of the polar solvent in the photoresist stripping solution is 20wt% to 59wt%. When the content of the polar solvent is less than 20wt%, it may lead to a decrease in the stripping performance of the photoresist; when the content of the polar solvent is greater than 59wt%, the content of other components in the stripping solution will be relatively reduced, which may cause problems such as poor stripping performance and reduced cleanability of the photoresist.
[0030] For example, in the photoresist stripping solution provided by the present invention, the mass percentage of the polar solvent in the photoresist stripping solution can be any value or a range formed by any two values from 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, or 59wt%.
[0031] Preferably, the triazine-based metal corrosion inhibitor in the photoresist stripping solution is 0.5wt% to 5wt%. When the content of the triazine-based metal corrosion inhibitor is less than 0.5wt%, it may not be able to inhibit the corrosion of the metal film during the photoresist stripping process; when the content of the triazine-based metal corrosion inhibitor is greater than 5wt%, the photoresist stripping solution will severely adsorb the metal, resulting in a decrease in the stripping effect, more residue, and affecting the product yield.
[0032] For example, in the photoresist stripping solution provided by the present invention, the mass percentage of the triazine metal inhibitor in the photoresist stripping solution can be any value or a range formed by any two values from 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, or 5wt%.
[0033] In an optional embodiment, the solution comprises, by weight percentage, 50-65 wt% fatty amino alcohol ether, 33-49 wt% polar solvent, and 0.5-4.5 wt% triazine metal corrosion inhibitor, to ensure that the photoresist stripping solution has excellent alkaline depolymerization ability, polymer dissolution ability, and interface corrosion inhibition ability.
[0034] In an optional embodiment, the additives are also included, including at least one of antioxidants, defoamers, and stripping accelerators.
[0035] Preferably, the antioxidant can be selected from conventional antioxidants in the art, such as at least one of phenolic antioxidants, amine antioxidants, thiol antioxidants and phosphine antioxidants, as long as it can effectively prevent the oxidation of the metal film layer in the metal wiring structure.
[0036] Preferably, the defoamer can be a conventional defoamer in the art, such as a silicone-based defoamer, as long as it can remove air bubbles contained in the photoresist stripping solution. The silicone-based defoamer can be in the form of a solution, emulsion, self-emulsifying agent, or solid.
[0037] Preferably, the stripping accelerator can be, for example, a hydroxylamine compound, as long as it can effectively promote the depolymerization of the photoresist.
[0038] In optional embodiments, the content of the above-mentioned additives is not particularly limited and can be adjusted appropriately according to the purpose of addition. For example, the mass percentage of the above-mentioned additives in the photoresist stripping solution can be any range from 0.5wt% to 1wt%, 0.5wt% to 2wt%, 0.5wt% to 3wt%, 0.5wt% to 4wt%, or 0.5wt% to 5wt%.
[0039] Secondly, the present invention provides a method for preparing a photoresist stripping solution as described in any of the foregoing embodiments, comprising mixing raw materials uniformly in a specified proportion.
[0040] Thirdly, the present invention provides an application of a photoresist stripping solution as described in any of the foregoing embodiments in a photoresist stripping process.
[0041] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0042] Example 1 This embodiment provides a photoresist stripping solution, which, by mass percentage, comprises 45 wt% fatty amino alcohol ether, 53.5 wt% polar solvent, 1 wt% triazine metal corrosion inhibitor, and 0.5 wt% additives.
[0043] Among them, the fatty amino alcohol ether is 2-[2-(dimethylamino)ethoxy]ethanol ((CH3)2N(CH2CH2O)2H); the polar solvent is N-methylformamide (NMF); the triazine metal corrosion inhibitor is 6-methyl-1,3,5-triazine-2,4-diamine; and the additive is catechol (phenolic antioxidant).
[0044] This embodiment also provides a method for preparing the above-mentioned photoresist stripping solution, including mixing the raw materials evenly in proportion.
[0045] The following examples and comparative examples all provide a photoresist stripping solution and its preparation method, and the differences from Example 1 are shown in Table 1.
[0046] Table 1 Formulation of photoresist stripping solution
[0047] Experimental Example 1 The photoresist stripping solutions provided in Examples 1-22 and Comparative Examples 1-13 were subjected to performance tests, and the results are shown in Table 2.
[0048] Unless otherwise specified, the preparation method of the photoresist samples used in the following performance tests is as follows: A 10cm × 10cm glass substrate (thickness ≈ 0.5cm) is coated with a photoresist of approximately 1.2μm thickness using a spin coater, baked at 170℃ for 15 minutes, and then cut into 3cm × 3cm glass samples for later use. The photoresist includes phenolic resin and diazonoquinone, or other combinations commonly used in this technical field.
[0049] 1) The stripping performance test and evaluation method includes: taking 100g of the photoresist stripping solution provided in each example and comparative example, heating it to 60℃, immersing a 3cm×3cm glass sample in the photoresist stripping solution, observing the removal of photoresist using a metallographic microscope, and evaluating the stripping performance of the photoresist stripping solution based on the photoresist removal time. The specific evaluation criteria are as follows: ◎: Photoresist removal time < 10s; ○: Photoresist removal time is 10~30s; △: Photoresist removal time is 30~60s; ×: Photoresist removal time > 60s.
[0050] 2) The cleaning performance test and evaluation method includes: taking 100g of the photoresist stripping solution provided in each example and comparative example, and dissolving 1wt% of photoresist solid in each solution to simulate a high-load photoresist stripping solution system. Immersing a 3cm×3cm glass sample into the above-mentioned high-load photoresist stripping solution system, then rinsing with ultrapure water and drying with air to obtain the cleaned sample.
[0051] At 25°C, 2 μL of ultrapure water was dropped onto the surface of the cleaned sample, and the contact angle of the water droplet was measured using a contact angle meter to evaluate the cleaning performance of the photoresist stripping solution. The specific evaluation criteria are as follows: ◎: Water droplet contact angle < 40°; ○: The water droplet contact angle is 40°~50°; △: The water droplet contact angle is 51°~60°; ×: Water droplet contact angle > 60°.
[0052] 3) The corrosion stability test and evaluation method for the metal film includes: immersing the Cu / MoTi metal wiring film sample coated with photoresist into the photoresist stripping solution provided in the above examples and comparative examples, soaking at 60°C for 5 min, rinsing with ultrapure water for 1 min, and air drying for 1 min. The cross-sectional corrosion of the metal film is evaluated using scanning electron microscopy (SEM). Lateral corrosion and bottom notch conditions at at least 10 sites on the metal film sample are randomly observed to evaluate the corrosion stability of the metal film in the photoresist stripping solution. The specific evaluation criteria are as follows: ◎: The number of lateral corrosion sites plus bottom cut sites is ≤2; ○: The number of lateral corrosion + bottom cut sites is 3~5; △: The number of lateral corrosion and bottom cut sites is 6~9; ×: Lateral corrosion + number of bottom cut sites ≥ 10.
[0053] Table 2 Performance of Photoresist Stripping Solution
[0054] As shown in Table 2, in Comparative Example 1 without the addition of triazine metal corrosion inhibitors, the photoresist removal time of the obtained resist stripping solution was prolonged and the stripping ability was reduced; at the same time, the corrosion stability of the metal film was poor, and the product showed a large number of lateral corrosion and bottom cut phenomena.
[0055] As shown in Example 2 and Comparative Example 2, the amount of triazine-based metal corrosion inhibitor added in Comparative Example 2 was too low, only 0.2 wt%, resulting in poor corrosion stability of the photoresist stripping solution and a large amount of lateral corrosion and bottom cutting phenomena in the product. In Comparative Example 9, the amount of triazine-based metal corrosion inhibitor added was 0.4 wt%, slightly lower than the lower limit required by the present invention and slightly higher than Comparative Example 2. The corrosion stability of the obtained photoresist stripping solution was slightly better than that of Comparative Example 2, but still not as good as the corrosion stability of the embodiments of the present invention. In Comparative Example 13, the amount of triazine-based metal corrosion inhibitor added was also 0.4 wt%, and the amount of polar solvent added was increased. Although the corrosion stability was improved compared with Comparative Example 9, the stripping performance and cleaning performance were still significantly worse than those of the examples. This indicates that an amount of triazine-based metal corrosion inhibitor greater than or equal to 0.5 wt% is beneficial for balancing the stripping performance, cleaning performance and corrosion stability of the photoresist stripping solution.
[0056] Furthermore, in Comparative Example 5, the addition of both fatty amino alcohol ethers and triazine metal corrosion inhibitors was increased, resulting in a simultaneous deterioration in both the stripping performance and corrosion stability of the obtained photoresist stripping solution. This indicates that the addition amounts of fatty amino alcohol ethers and triazine metal corrosion inhibitors must be within the range defined by this invention to ensure excellent stripping performance and corrosion stability of the photoresist stripping solution. Increasing the amount of fatty amino alcohol ethers in pursuit of improved stripping performance and increasing the amount of triazine metal corrosion inhibitors in pursuit of improved corrosion stability not only fails to improve performance but also leads to a simultaneous deterioration in both the stripping performance and corrosion stability of the product due to the imbalance in the ratio of the photoresist stripping solution.
[0057] Comparative Example 11 increased the amount of triazine metal corrosion inhibitor while reducing the content of polar solvent. The resulting photoresist stripping solution had corrosion stability comparable to that of the Examples, but its stripping and cleaning performance were lower than those of Examples 19 and 20.
[0058] As illustrated by the above comparative examples 1, 2, 5, 9, 11 and 13, the amount of triazine metal corrosion inhibitor added has a significant impact on the corrosion stability of the photoresist stripping solution. At the same time, due to the change in the content of triazine metal corrosion inhibitor, the stripping performance and / or cleaning performance of the photoresist stripping solution will also be affected.
[0059] Furthermore, the excessively high polar solvent content in Comparative Example 3 resulted in a decrease in both its peeling and cleaning performance compared to the Example.
[0060] Furthermore, compared with the examples, the photoresist stripping solutions provided in Comparative Examples 4, 7 and 12 all exhibited a decrease in the content of fatty amine alcohol ethers and an excessive increase in the content of polar solvents, which led to a decrease in the stripping performance and / or cleaning performance of the photoresist stripping solutions. Meanwhile, Comparative Example 7 also had a decrease in corrosion stability compared to Comparative Examples 4 and 12 because the content of triazine metal corrosion inhibitor was slightly lower than that of Comparative Examples 4 and 12.
[0061] Compared with the examples, the photoresist stripping solutions provided in Comparative Examples 6, 8 and 10 all showed an increase in the content of fatty amine alcohol ethers and a decrease in the content of polar solvents, which led to a decrease in the stripping performance and corrosion stability of the photoresist stripping solutions; at the same time, Comparative Example 8 had a higher content of fatty amine alcohol ethers, so the cleaning performance of the photoresist stripping solution was also significantly worse.
[0062] As can be seen from the above comparative examples 3, 4, 6-8, 10 and 12, the content of fatty amine alcohol ethers and polar solvents needs to be within the range required by the present invention in order to ensure the triple improvement of the photoresist stripping solution's stripping performance, cleaning performance and metal corrosion stability.
[0063] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A photoresist stripping solution, characterized in that, By weight percentage, it includes 40wt%~79wt% fatty amino alcohol ethers, 20wt%~59wt% polar solvents, and 0.5wt%~5wt% metal corrosion inhibitors; The chemical formula of the fatty amino alcohol ether is: ; In the chemical formula, R1 is selected from any one of H, -OH, -CH2OH, -CH2CH2OH and C1~C3 chain alkyl groups; R2 is selected from any one of H, -OH, -CH2OH, -CH2CH2OH and C1~C3 chain alkyl groups; n is an integer from 2 to 4.
2. The photoresist stripping solution according to claim 1, characterized in that, In the chemical formula of the fatty amine alcohol ether, R1 is selected from any one of H and C1~C3 chain alkyl groups; R2 is selected from any one of H and C1~C3 chain alkyl groups.
3. The photoresist stripping solution according to claim 2, characterized in that, The fatty amino alcohol ethers include any one of (CH3)2N(CH2CH2O)2H, (CH3CH2)2N(CH2CH2O)2H, (CH3)NH(CH2CH2O)2H, and NH2(CH2CH2O)2H.
4. The photoresist stripping solution according to claim 1, characterized in that, The polar solvent includes at least one of dimethyl sulfoxide, sulfolane, N-methylformamide, N-methylacetamide, N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylpropionamide.
5. The photoresist stripping solution according to claim 1, characterized in that, The metal corrosion inhibitor includes triazine-based metal corrosion inhibitors, which include at least one of 1,3,5-triazine, 2-amino-1,3,5-triazine, 6-methyl-1,3,5-triazine-2,4-diamine, 2,4,6-tris(pyridyl)triazine, and 2,4,6-triamino-1,3,5-triazine.
6. The photoresist stripping solution according to claim 1, characterized in that, By mass percentage, it includes 50wt%~65wt% fatty amino alcohol ethers, 33wt%~49wt% polar solvents, and 0.5wt%~4.5wt% triazine metal corrosion inhibitors.
7. The photoresist stripping solution according to claim 1, characterized in that, It also includes additives, which include at least one of antioxidants, defoamers, and peeling promoters.
8. The photoresist stripping solution according to claim 7, characterized in that, The mass percentage of the additive in the photoresist stripping solution is 0.5~5 wt%.
9. A method for preparing a photoresist stripping solution as described in any one of claims 1 to 8, characterized in that, This includes mixing the raw materials evenly in a specific ratio.
10. The application of the photoresist stripping solution as described in any one of claims 1 to 8 in the photoresist stripping process.