A non-destructive extraction method of equivalent interface transport resistance of silicon heterojunction solar cell
By obtaining the current-voltage characteristic curves of silicon heterojunction solar cells in a dark environment, and using a dual-diode model and parameter calculations, the non-destructive extraction of the transfer resistance at the interface between TCO and μc-Si:H was achieved. This solves the problem of interface resistance characterization that cannot be performed quickly, with good repeatability and high process sensitivity in existing technologies, and has degradation location capability.
Patent Information
- Application Number
- CN202611646228.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies cannot perform rapid, repeatable, and highly sensitive non-destructive characterization of the interface transfer resistance between TCO and μc-Si:H in silicon heterojunction solar cells without damaging the cell structure, and cannot locate the contact degradation sites.
By applying a step-scanning current to a silicon heterojunction solar cell in a dark environment, the dark-state current-voltage characteristic curve is obtained. The total series resistance is fitted using a dual-diode model, and the equivalent interface transport resistance is calculated by combining geometric and material parameters, thus achieving non-destructive extraction.
It enables non-destructive testing of complete silicon heterojunction solar cells, which is fast, low-cost, and highly repeatable. It can distinguish between changes in metal grid resistance and heterojunction interface resistance, and has high sensitivity in detecting process differences and locating degradation.
Smart Images

Figure CN123139899A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrical characterization technology of solar cells, and in particular to a non-destructive method for extracting the equivalent interface transport resistance of silicon heterojunction solar cells. Background Technology
[0002] Silicon heterojunction (SHJ) solar cells consist of a stacked structure comprising a crystalline silicon substrate, an intrinsic amorphous silicon layer, a doped microcrystalline silicon (μc-Si:H) layer, a transparent conductive oxide (TCO) layer, and metal grid lines. With its high open-circuit voltage, low temperature coefficient, and excellent bifacial power generation capability, SHJ solar cells have become a crucial technology in the field of high-efficiency crystalline silicon photovoltaics, holding a global market share exceeding 8%. As conversion efficiency continues to improve, series resistance has become a major factor limiting fill factor and overall device performance. Among these factors, the interfacial contact characteristics between the TCO and μc-Si:H layers determine the tunneling and extraction efficiency of charge carriers, making it a critical factor affecting the cell's electrical performance. Therefore, rapid evaluation of interfacial transport characteristics is increasingly important for SHJ solar cell process optimization and industrial quality control.
[0003] Currently, the quantitative characterization of contact resistance mainly relies on two dedicated testing methods: the transfer length method (TLM) and the Cox-Strack technique.
[0004] TLM (Transient Photoresistivity) measures the relationship between total resistance and electrode spacing by fabricating electrodes with different spacings on a test structure and extracting the contact resistivity from the intercept using linear fitting (e.g., Lachenal et al., Energy Procedia, 2016, 92: 932-938). Its structural premise is that the current is confined within a single conductive layer. However, due to the pin structure of SHJ solar cells, current shunting occurs between the TCO (Transient Contact Oscillator) and the crystalline silicon substrate, making this premise difficult to meet; furthermore, electron contact and hole contact resistance require separate fabrication of n-type and p-type test structures, making simultaneous evaluation on a single complete cell impossible.
[0005] The Cox-Strack method inverts interface parameters by analyzing the current spread beneath circular electrodes of different diameters (e.g., Cox and Strack, Solid-State Electronics, 1967, 10: 1213-1218). This method relies on an approximate current diffusion model, which makes it difficult to distinguish between contact resistance and spread resistance for large-diameter electrodes, and its assumptions have not been fully verified.
[0006] The common structural drawback of the two methods mentioned above is that they both require surface etching, scribing, and specially designed test patterns or electrodes. These are destructive, offline laboratory characterization methods that cannot be directly applied to complete production line cells, failing to meet the requirements for real-time, non-destructive production line monitoring. While there have been improvements in recent years—for example, Zogbo et al. demonstrated through simulation and experiments that accurately measuring the contact resistance between the metal and TCO requires controlling the activation energy of a-Si:H within 0.6–1.4 eV to ensure the current is confined within the TCO layer (Sol. Energy Mater. Sol. Cells, 2024, 265: 112623); and Bhattacharya et al. used TLM to optimize the doping concentration and thickness of the a-Si:H(p) layer, reducing the hole contact resistivity to 432 Ω·cm. 2 (ACS Appl. Electron. Mater., 2025, 7: 4065-4074). However, these methods still rely on specialized test structures and are not suitable for the non-destructive characterization of complete industrial batteries.
[0007] Furthermore, existing methods cannot pinpoint the specific location of contact degradation at the process diagnostic level, such as the contact interface between the metal and TCO, the μc-Si:H / c-Si heterojunction region, and the TCO bulk resistance. In summary, current technologies lack a rapid, non-destructive method for characterizing interface transport resistance that does not require a dedicated test structure, can be directly applied to complete SHJ solar cells, combines repeatability and process sensitivity, and can locate the site of contact degradation. Summary of the Invention
[0008] The purpose of this invention is to provide a non-destructive extraction method for the equivalent interface transfer resistance of silicon heterojunction solar cells. By decomposing the series resistance based on the dark-state current-voltage characteristics, the equivalent interface transfer resistance between TCO and μc-Si:H can be extracted from an intact silicon heterojunction solar cell without damaging the cell or preparing a dedicated test structure. This method enables rapid, low-cost, and repeatable production-line level interface quality assessment, and can compare process differences and locate contact degradation sites, overcoming the shortcomings of methods such as TLM and Cox-Strack that require destructive sample preparation.
[0009] To achieve the above objectives, the present invention provides a non-destructive method for extracting the equivalent interface transport resistance of a silicon heterojunction solar cell, comprising the following steps: S1. Apply a step-scanning current to a complete silicon heterojunction solar cell in a dark environment and at a preset temperature to obtain the dark current-voltage characteristic curve. S2. Based on the dark-state current-voltage characteristic curve, the linear segment in which dV / d(lnI) is linearly related to the current I is determined using a dual-diode model. The slope is obtained by fitting the linear segment, and the slope is the total series resistance. S3. Obtain the geometric and material parameters of the complete silicon heterojunction solar cell, and use the pre-calibrated or empirical values as the contact resistivity between the metal and the TCO. Based on the geometric parameters, material parameters and the contact resistivity between the metal and the TCO, calculate the metal grid resistance, TCO lateral resistance, contact resistance between the metal and the TCO and silicon substrate resistance respectively. S4. Convert the total series resistance to the surface resistance of the total series resistance. Subtract the surface resistance of the metal gate resistance, the surface resistance of the TCO lateral resistance, the surface resistance of the contact resistance between the metal and the TCO, and the surface resistance of the silicon substrate from the surface resistance of the total series resistance to obtain the equivalent interface transfer resistance between the TCO and μc-Si:H.
[0010] Preferably, S1 specifically includes: S11. Place the complete silicon heterojunction solar cell in a dark environment, wherein the dark environment is a dark room, and set the preset temperature to 298.15K; S12. Set the scanning range of the step scanning current to 0 to 0.6A and the step size to 3mA; S13. Connect the complete silicon heterojunction solar cell using the four-wire (Kelvin) method, apply a step-scanning current to the complete silicon heterojunction solar cell in current source mode, and measure the corresponding voltage. S14. Perform S13 three times, take the average of the three measurement results, and obtain the dark-state current-voltage characteristic curve.
[0011] Preferably, S2 specifically includes: S21. In the forward bias region where the voltage is greater than 0.4V, the dark-state current-voltage characteristic curve satisfies the dual-diode model, which is as follows: ; in, For voltage, For current, It is a natural exponential function. This is the reverse saturation current corresponding to the diffusion current. This is the reverse saturation current corresponding to the composite current. and As an ideal factor, For series resistance, For parallel resistors, For electron charge, Boltzmann's constant, Thermodynamic temperature; Differentiating the dual-diode model in the forward bias region yields: ; in, This is the thermal voltage; dV / d(lnI) has a linear relationship with the current I. In the forward bias region, the data points of dV / d(lnI) and current I are calculated based on the dark-state current-voltage characteristic curve, and these data points constitute a linear segment. S22. Perform least squares fitting on the data points of the linear segment to obtain the slope, where the slope is the total series resistance, and the correlation coefficient of the least squares fitting is greater than or equal to 0.99.
[0012] Preferably, S3 specifically includes: S31. Obtain the geometric and material parameters of the complete silicon heterojunction solar cell. The geometric parameters include grid line size and fine grid spacing. The material parameters include TCO sheet resistance, grid line paste resistivity, silicon substrate resistivity and silicon wafer thickness. Use pre-calibrated or empirical values as the contact resistivity between the metal and TCO. S32. Calculate the resistance of the metal grid wire based on the grid wire size and the resistivity of the grid wire paste; S33. Calculate the TCO transverse resistance based on the TCO sheet resistance and fine grid spacing; S34. Calculate the contact resistance between the metal and the TCO based on the contact resistivity and total contact area between the metal and the TCO. S35. Calculate the silicon substrate resistance based on the silicon substrate resistivity and silicon wafer thickness; S36. The resistance of the metal gate line, the lateral resistance of the TCO, the contact resistance between the metal and the TCO, and the resistance of the silicon substrate are all represented as the surface ratio resistance.
[0013] Preferably, the calculation method for the metal gate resistance in S32 is as follows: The equivalent resistance of a single fine grid segment is: ; in, The equivalent resistance of a single fine grid segment. The resistivity of the grid line paste, For a single segment of fine grid length, For fine grid linewidth, For fine grid line height; The equivalent resistance is converted to the area ratio resistance based on the number of fine grid segments on the front and back sides: ; in, The surface resistivity of the metal grid line resistor. The number of fine grid segments on the front side. The number of fine grid segments on the back side. Battery area; The calculation method for the TCO transverse resistance in S33 is as follows: ; in, The surface resistance of the TCO transverse resistance. For TCO sheet resistors For fine gate pitch, n-plane TCO sheet resistors are used on the front side and p-plane TCO sheet resistors are used on the back side; The method for calculating the contact resistance between the metal and the TCO in S34 is as follows: ; in, The surface resistivity is the contact resistance between the metal and the TCO. The contact resistivity between the metal and the TCO. The total contact area is calculated separately for the front and back sides and then connected in series. The calculation method for the silicon substrate resistance in S35 is as follows: ; in, The surface resistivity is the resistance of the silicon substrate. The resistivity of the silicon substrate, This refers to the thickness of the silicon wafer.
[0014] Preferably, in S4, the equivalent interface transfer resistance between TCO and μc-Si:H is calculated using the following formula: ; in, The surface resistance is the area ratio of the equivalent interfacial transport resistance between TCO and μc-Si:H. The surface resistance is the area ratio of the total series resistance. The surface resistivity of the metal grid line resistor. The surface resistance of the TCO transverse resistance. The surface resistivity is the contact resistance between the metal and the TCO. The surface resistance of the silicon substrate is the surface resistance.
[0015] Preferably, the method further includes step S5, immersing the silicon heterojunction solar cell under test in a 10% wt flux solution for different durations, then removing and drying it, repeating steps S1 to S4, and independently monitoring the changes in the TCO sheet resistance, grid line paste resistivity and silicon substrate resistivity among the material parameters. When the relative changes in TCO sheet resistance, grid line paste resistivity and silicon substrate resistivity are all less than a preset percentage and the total series resistance increases, the degradation site is located at the contact interface between the metal and TCO.
[0016] Preferably, the method further includes S6, preparing a ring electrode structure on the TCO surface of the silicon heterojunction solar cell. The ring electrode structure has a solid circular electrode at its center and a square electrode on its periphery, forming a ring gap between the two electrodes. A small current is applied between the two electrodes to measure the total resistance, which is used to independently monitor the relative change trend of the contact resistance between the metal and the TCO, and cross-validate with the back-calculation results of S4 to S5.
[0017] Preferably, the pre-calibration value in S31 is obtained by random sampling and calibration of the TLM of the same batch of batteries, and the empirical value is a process empirical value.
[0018] Therefore, the present invention employs the above-mentioned non-destructive extraction method for the equivalent interface transport resistance of silicon heterojunction solar cells. Compared with the prior art, the beneficial technical effects achieved by the present invention are as follows: (1) Non-destructive and production line friendly: No special test structure or surface etching is required. Complete silicon heterojunction solar cells can be tested directly, overcoming the defects of destructive sample preparation methods such as TLM and Cox-Strack. The test only requires one dark state current-voltage characteristic test and a small number of geometric and material parameters, which is fast and low cost.
[0019] (2) Good repeatability: When the silver content of the silver paste is changed (25%, 30%, 36%) for batteries from the same manufacturer, the maximum deviation of the extracted equivalent interfacial transport resistance is only about 0.075 Ω·cm. 2 One-way ANOVA showed no statistically significant differences within the groups (first manufacturer: F(2,6)=2.06, p=0.21; second manufacturer: F(2,6)=3.79, p=0.086), indicating that the method can effectively distinguish between the changes in metal grid resistance and the changes in heterojunction interface resistance, and has strong self-consistency.
[0020] (3) Sensitive to process differences: Under the same printed electrode process conditions, the equivalent interfacial transport resistance of batteries from different manufacturers is 0.980 Ω·cm. 2 With 1.667 Ω·cm 2 The relative differences were approximately 70%; independent samples t-tests showed that the differences were extremely significant under the three silver contents (t values were -16.08, -26.50, and -20.10, respectively, and p < 0.001 for all three), indicating that the method has high sensitivity to TCO deposition quality and interface state changes.
[0021] (4) Degradation location capability: By cross-judging the total series resistance increment with the independent measurements of TCO sheet resistance, grid paste resistivity and silicon substrate resistivity, degradation can be located at the contact interface between the metal and TCO, and the trend is consistent with the change trend of the direct measurement method of the ring electrode; this is a capability that dedicated methods such as TLM and Cox-Strack do not have.
[0022] (5) Strong parameter robustness: When the contact resistivity between the back metal and TCO is 0.0034~0.0044 Ω·cm 2 When the range changes, the extracted equivalent interfacial transport resistance fluctuates by less than 0.02 Ω·cm. 2 When the resistivity of the silicon substrate varies within the range of 1.0 to 1.5 Ω·cm, the fluctuation is less than 0.008 Ω·cm. 2 This indicates that the method is not sensitive to non-dominant parameters and is suitable as a production line monitoring indicator.
[0023] (6) Applicability of dark-state testing: This method uses dark-state current-voltage characteristic testing, with relative comparison as the core objective, and can be used for process monitoring, difference assessment and degradation analysis.
[0024] (7) Single-sided TLM verification experiments show that the equivalent interface transfer resistance extracted in this invention (1.667 Ω·cm) 2 The measured contact resistance of the n-type TLM is greater than 0.549 Ω·cm. 2 ), and the difference between the two (approximately 1.118 Ω·cm) 2 This aligns with the physical expectation that the p-type transport resistance is higher than the n-type transport resistance, indicating that the decomposition results have a clear physical explanation and experimental verifiability.
[0025] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0026] Figure 1 This is a flowchart illustrating a non-destructive extraction method for the equivalent interface transport resistance of a silicon heterojunction solar cell according to the present invention. Figure 2 The present invention provides a schematic diagram of the dark-state current-voltage characteristic test of a solar cell and an equivalent circuit diagram of the series resistance decomposition. (a) is the schematic diagram of the dark-state current-voltage characteristic test of a solar cell, and (b) is the equivalent circuit diagram of the series resistance decomposition. Figure 3 This is a schematic diagram of the solar cell grid structure of the present invention; Figure 4 This is a schematic diagram of the dV / d(lnI)-I fitting of the present invention; Figure 5 The above are stacked bar charts of the resistance components of Examples 1 and 2 of the present invention under different silver contents, where (a) is Example 1 and (b) is Example 2; Figure 6 The above is a comparison chart of the first manufacturer and the second manufacturer under a silver content of 25% in the present invention, where (a) is a bar chart comparing each resistance component and (b) is a comparison curve of dark state current-voltage characteristics. Figure 7 The figures show the dark-state current-voltage characteristic curves under different flux immersion times in embodiments of the present invention, where (a) is the curve for the entire voltage range and (b) is a locally magnified curve for the high voltage region. Detailed Implementation
[0027] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments.
[0028] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] like Figure 1 As shown, a non-destructive method for extracting the equivalent interface transport resistance of a silicon heterojunction solar cell includes the following steps: S1. Apply a step-scanning current to a complete silicon heterojunction solar cell in a dark environment and at a preset temperature to obtain the dark current-voltage characteristic curve. S1 specifically includes: S11. Place the complete silicon heterojunction solar cell in a dark environment, which is a dark room, and set the preset temperature to 298.15K. S12. Set the scanning range of the step scanning current to 0 to 0.6A and the step size to 3mA; S13. Connect the complete silicon heterojunction solar cell using the four-wire (Kelvin) method, apply a step-scanning current to the complete silicon heterojunction solar cell in current source mode, and measure the corresponding voltage. S14. Perform S13 three times, take the average of the three measurement results, and obtain the dark-state current-voltage characteristic curve.
[0030] like Figure 2 As shown in (a), a complete silicon heterojunction solar cell is connected using a four-wire method: a pair of current lines apply a step-scanning current (0 to 0.6A, step size 3mA) to the cell in current source mode, and another pair of voltage lines measure the voltage across the cell to obtain the dark-state current-voltage characteristic curve. Figure 2 In (a), ITO is a specific material of TCO, and the metal grid line is Ag-Cu grid line.
[0031] S2. Based on the dark-state current-voltage characteristic curve, the linear segment in which dV / d(lnI) is linearly related to the current I is determined using a dual-diode model. The slope is obtained by fitting the linear segment, and the slope is the total series resistance. S2 specifically includes: S21. In the forward bias region where the voltage is greater than 0.4V, the dark-state current-voltage characteristic curve satisfies the dual-diode model, which is as follows: ; in, For voltage, For current, It is a natural exponential function. This is the reverse saturation current corresponding to the diffusion current. This is the reverse saturation current corresponding to the composite current. and As an ideal factor, For series resistance, For parallel resistors, For electron charge, Boltzmann's constant, Thermodynamic temperature; Differentiating the dual-diode model in the forward bias region yields: ; in, Let dV / d(lnI) be the thermal voltage; from the above formula, it can be seen that dV / d(lnI) has a linear relationship with the current I. In the forward bias region, the data points of dV / d(lnI) and current I are calculated based on the dark-state current-voltage characteristic curve, and the data points form a linear segment; S22. Perform least squares fitting on the data points of the linear segment to obtain the slope, which is the total series resistance. The correlation coefficient of the least squares fitting is greater than or equal to 0.99.
[0032] like Figure 4 As shown, the horizontal axis represents the current. The vertical axis is dV / d(lnI), and the data points are taken from the forward bias region (V>0.4V) and calculated from the dark-state I–V curve. Least squares fitting yields y=0.1664x+0.05(R²). 2 =0.9929), where y=dV / d(lnI), x=I. The slope of 0.1664Ω is the total series resistance, and the intercept of 0.058V corresponds to n2Vt.
[0033] S3. Obtain the geometric and material parameters of the complete silicon heterojunction solar cell, and use the pre-calibrated or empirical values as the contact resistivity between the metal and the TCO. Based on the geometric parameters, material parameters and the contact resistivity between the metal and the TCO, calculate the metal grid resistance, TCO lateral resistance, contact resistance between the metal and the TCO and silicon substrate resistance respectively. S3 specifically includes: S31. Obtain the geometric and material parameters of the complete silicon heterojunction solar cell. The geometric parameters include grid line size and fine grid spacing. The material parameters include TCO sheet resistance, grid line paste resistivity, silicon substrate resistivity and silicon wafer thickness. Use pre-calibrated or empirical values as the contact resistivity between the metal and TCO. The pre-calibrated values were obtained from TLM sampling and calibration of batteries from the same batch; the empirical values were process empirical values. According to the TLM measured results of this embodiment of the invention, the contact resistivity range between the metal and the TCO is 3.34 × 10⁻⁶. -3 ~ 4.70×10 -3 Ω·cm 2 (Among them, the n-type side is 4.41 × 10 -3 ~4.70×10 -3 Ω·cm 2 The p-type side is 3.34 × 10 -3 ~4.30×10 -3 Ω·cm 2 ).
[0034] S32. Calculate the resistance of the metal grid wire based on the grid wire size and the resistivity of the grid wire paste. The calculation method is as follows: The equivalent resistance of a single fine grid segment is: ; in, The equivalent resistance of a single fine grid segment. The resistivity of the grid line paste, For a single segment of fine grid length, For fine grid linewidth, For fine grid line height; such as Figure 3 As shown, S represents the fine grid spacing. Main grid width, The main gate length.
[0035] The equivalent resistance is converted to the area ratio resistance based on the number of fine grid segments on the front and back sides: ; in, The surface resistivity of the metal grid line resistor. The number of fine grid segments on the front side. The number of fine grid segments on the back side. Battery area; S33. Calculate the TCO lateral resistance based on the TCO sheet resistance and fine grid spacing: ; in, The surface resistance of the TCO transverse resistance. For TCO sheet resistors For fine gate pitch, n-plane TCO sheet resistors are used on the front side and p-plane TCO sheet resistors are used on the back side; S34. Calculate the contact resistance between the metal and the TCO based on the contact resistivity and the total contact area: ; in, The surface resistivity is the contact resistance between the metal and the TCO. The contact resistivity between the metal and the TCO. The total contact area is calculated separately for the front and back sides and then connected in series. S35. Calculate the silicon substrate resistance based on the silicon substrate resistivity and silicon wafer thickness: ; in, The surface resistivity is the resistance of the silicon substrate. The resistivity of the silicon substrate, This refers to the thickness of the silicon wafer.
[0036] S36. The resistance of the metal gate line, the lateral resistance of the TCO, the contact resistance between the metal and the TCO, and the resistance of the silicon substrate are all represented as the surface ratio resistance.
[0037] S4. Convert the total series resistance to the surface resistance of the total series resistance. The slope obtained from the fitting in S2 is the total series resistance. The unit is Ω. Multiply by battery area The surface resistance of the total series resistance is obtained. The unit is Ω·cm 2 Subtracting the surface resistance of the metal gate resistance, the surface resistance of the TCO lateral resistance, the surface resistance of the contact resistance between the metal and the TCO, and the surface resistance of the silicon substrate from the surface resistance of the total series resistance yields the equivalent interface transport resistance between the TCO and μc-Si:H. ; in, The surface resistance is the area ratio of the equivalent interfacial transport resistance between TCO and μc-Si:H. The surface resistance is the area ratio of the total series resistance. The surface resistivity of the metal grid line resistor. The surface resistance of the TCO transverse resistance. The surface resistivity is the contact resistance between the metal and the TCO. The surface resistance of the silicon substrate is the surface resistance.
[0038] like Figure 2As shown in (b), the metal gate line resistance, the contact resistance between the metal and the TCO, the lateral resistance of the TCO, the equivalent interface transfer resistance between the TCO and μc-Si:H(n), the silicon substrate resistance, and the equivalent interface transfer resistance between the TCO and μc-Si:H(p) are connected in series. The equivalent interface transfer resistance between TCO and μc-Si:H(n) is given. The equivalent interfacial transfer resistance between TCO and μc-Si:H(p) is the value of the series connection of the two components, which is the value in S4. ,Right now: ; This is a lumped parameter, not just referring to the single interface resistance between TCO and μc-Si:H, but encompassing the tunneling resistance of the a-Si:H(i) intrinsic layer, the TCO / μc-Si:H contact resistance, and the contribution of the a-Si:H(i) / c-Si heterojunction barrier. Because the a-Si:H(i) intrinsic layer is extremely thin (5~10nm), its tunneling resistance, TCO / μc-Si:H contact resistance, and a-Si:H(i) / c-Si heterojunction barrier cannot be distinguished individually in dark-state current-voltage decomposition; therefore, they are all included in the equivalent interface transport resistance. This parameter is suitable for relative comparisons and process monitoring, not for absolute quantification.
[0039] S5. The silicon heterojunction solar cell to be tested is immersed in a 10% wt flux solution for different durations and then dried. S1 to S4 are repeated. At the same time, the changes in the TCO sheet resistance, grid line paste resistivity and silicon substrate resistivity in the material parameters are independently monitored. When the relative changes in TCO sheet resistance, grid line paste resistivity and silicon substrate resistivity are all less than a preset percentage and the total series resistance increases, the degradation site is located at the contact interface between the metal and TCO. The preset percentage in this invention is 5%.
[0040] S6. A ring electrode structure is prepared on the TCO surface of a silicon heterojunction solar cell. The center of the ring electrode structure is a solid circular electrode, and the outer periphery is a square electrode. A ring gap is formed between the two electrodes. A small current is applied between the two electrodes to measure the total resistance. This is used to independently monitor the relative change trend of the contact resistance between the metal and the TCO, and cross-validate with the back-calculation results of S4 to S5.
[0041] The present invention will be further described below with reference to the embodiments. The silicon heterojunction solar cells used in the embodiments are all commercially available pre-fabricated silicon heterojunction substrates (210mm×105mm, with textured surface preparation, (i)a-Si:H layer, μc-Si:H layer and TCO layer deposition completed, but no metal electrodes printed), which are cut into 3.5cm×3.5cm pieces using a chip dicing machine; the device structure is: TCO / μc-Si:H(n) / (i)a-Si:H / nc-Si / (i)a-Si:H / μc-Si:H(p) / TCO. Fishbone-shaped double-sided metal grid lines were printed on both sides of the substrate using screen printing technology. The substrate was first sintered at 175℃ for 4 minutes, then at 195℃ for 30 minutes. The main grid width is 0.1 cm; the fine grid length is 1.5 cm on each side; the front fine grid spacing is 3.2 mm (11 fine grids), and the back spacing is 1.6 mm (20 fine grids); there are 22 fine grid segments on the front and 40 segments on the back; the cell area... =12.25cm 2 Silicon substrate resistivity =1.2Ω·cm, silicon wafer thickness =150μm.
[0042] Example 1 In this embodiment, the number of fine grid segments on the front side N1=22, and the number of fine grid segments on the back side N2=40. Fine grid line height ≈0.00166cm (n-side), 0.00164cm (p-side); grid line paste resistivity =6.67×10 -6 ~7.77×10 -6 Ω·cm (varying with silver content); contact resistivity between the metal and TCO Using the same batch of TLM sampling calibration values, the n-type side is 4.41 × 10⁻⁶. -3 ~4.70×10 -3 Ω·cm 2 The p-type side is 3.34 × 10 -3 ~4.30×10 -3 Ω·cm 2 The front (n-side) TCO sheet resistance is approximately 43.6 Ω / □, and the back (p-side) TCO sheet resistance is approximately 52.8 Ω / □.
[0043] Silicon heterojunction (SHJ) solar cells from the first manufacturer were used. Electrodes were printed using silver paste with silver content of 25%, 30%, and 36%, respectively, and the sintering process was the same (175℃ / 4min + 195℃ / 30min), with n=3 for each group. Dark-state current-voltage characteristics were tested in a dark room at 298K using a Keithley 2601B source meter in current source mode, using the four-wire (Kelvin) method, with a current range of 0~0.6A and a step size of 3mA. Each sample was measured three times and the average was taken. The resistance components were extracted according to steps S1~S4, and the results are shown in Table 1.
[0044] Table 1. Resistivity components (Ω·cm) for different silver contents from the first manufacturer. 2 (n=3, mean ± standard deviation):
[0045] Experimental results: Slight differences in the width and height of the fine gate under different silver contents lead to minor changes in the resistance of the metal gate lines, but the equivalent interface transfer resistance remains the same. It remained stable at 1.08-1.15 Ω·cm 2 Within the range, the maximum deviation is only about 0.06 Ω·cm. 2 One-way ANOVA showed no statistically significant differences within groups (F(2,6)=2.06, p=0.21). This indicates that the method can effectively distinguish between changes in metal gate resistance and changes in heterojunction interface resistance, and has good self-consistency and repeatability.
[0046] Example 2 In this embodiment, the number of fine grid segments on the front side N1=22, and the number of fine grid segments on the back side N2=40. The fine grid line height h≈0.00137cm (n-side) and 0.00139cm (p-side); the grid line resistivity ρ=6.67×10 -6 ~ 7.77×10 -6 Ω·cm (varying with silver content); contact resistivity between the metal and TCO Using the same batch of TLM sampling calibration values, the n-type side is 3.06 × 10⁻⁶. -3 ~3.10×10 -3 Ω·cm 2 The p-type side is 6.37 × 10 -3 ~6.75×10 -3 Ω·cm 2 The front (n-side) TCO sheet resistance is approximately 40.9 Ω / □, and the back (p-side) TCO sheet resistance is approximately 110 Ω / □.
[0047] Silicon heterojunction solar cells from the second manufacturer were used. Both cells from the first manufacturer in Example 1 were prepared using 25% silver paste and the same sintering conditions. The equivalent interfacial transport resistance between TCO and μc-Si:H was extracted using the same process. The results are shown in Table 2.
[0048] Table 2. Resistivity components (Ω·cm) for different silver contents from the second manufacturer. 2 (n=3, mean ± standard deviation):
[0049] Test results: At a silver content of 25%, the equivalent interfacial transport resistance of the second manufacturer was 1.667 Ω·cm. 2 ) compared to the first manufacturer (0.980Ω·cm) 2 The equivalent interfacial transport resistance (TCO) of the second manufacturer was approximately 70% higher than that of the first manufacturer (approximately 110 Ω / □), with the latter being significantly higher than the former (approximately 52 Ω / □). After deducting all components, the difference in interfacial transport was significant. Independent samples t-tests showed that at silver contents of 25%, 30%, and 36%, the equivalent interfacial transport resistance of the second manufacturer was significantly higher than that of the first manufacturer (t-values were -16.08, -25.50, and -20.10, respectively, p < 0.001).
[0050] The t-value for an independent samples t-test is calculated using the following formula: ; in , These are the average equivalent interface transfer resistances of the first and second manufacturers, respectively. , Standard deviation, .
[0051] This indicates that the method can effectively distinguish the interface differences caused by different process conditions (TCO deposition quality, μc-Si:H layer carrier transport characteristics, heterojunction interface transport barrier, etc.).
[0052] Figure 5 This is a stacked bar chart of the resistance components of Embodiments 1 and 2 of the present invention under different silver contents.
[0053] like Figure 6 As shown in (a), the equivalent interface transfer resistance of the second manufacturer is higher than that of the first manufacturer; Figure 6 As shown in (b), the second manufacturer has a smaller slope in the high bias region, corresponding to a higher total series resistance.
[0054] To further verify the technical effectiveness of the method of the present invention, the following verification experiments were conducted.
[0055] I. Contact Degradation Location Verification: Silicon heterojunction solar cells from the first manufacturer were immersed in a 10% wt flux solution for different durations (0, 2, 4, 6, 10 min), blotted dry with filter paper, and baked at 150℃ for 2 min. Dark-state current-voltage characteristics and resistivity decomposition were then performed. The total resistance (TCO) sheet resistance and grid size were measured independently before and after immersion.
[0056] Experimental results: (1) The sheet resistance of the p-side TCO decreased from 51.46 Ω / □ to 48.14 Ω / □ (a decrease of 6.4%) within 2 minutes of immersion, and the sheet resistance of the n-side TCO decreased from 40.68 Ω / □ to 39.26 Ω / □ (a decrease of 3.5%), after which it remained basically stable; the resistivity of the gate line paste remained almost unchanged within 0-10 minutes (relative change <2%). That is, the metal gate line resistance, the TCO lateral resistance, and the silicon substrate resistance can be considered to remain basically unchanged during the immersion process.
[0057] (2) According to the dark current-voltage characteristic curve, the dark current-voltage characteristic curves in the low voltage region almost overlap, indicating that the flux treatment did not cause significant changes in the junction-related transport behavior or bulk electrical characteristics in the silicon heterojunction structure; the curves in the high voltage region gradually separate with immersion time, indicating that the total series resistance gradually increases.
[0058] (3) Under the condition that the equivalent interface transfer resistance between TCO and μc-Si:H remains approximately constant (as evidenced by the overlap of curves in the low voltage region), the contact resistance between the metal and TCO can be inferred from the increase in the total series resistance, and its value is 0.182 Ω·cm. 2 Increased to 0.322 Ω·cm 2 .
[0059] (4) The resistance measured independently using the direct measurement method with ring electrodes (S6) is 0.389 Ω·cm. 2 Increased to 0.427 Ω·cm 2 In the ring electrode structure, the diameter of the solid circular electrode is 1 mm, the side length of the square electrode is 3 mm, the width of the ring gap is 0.35 mm, the electrode material is silver-coated copper paste, and the preparation method is screen printing. This trend is consistent with the trend of the reverse inference method, cross-confirming the degradation localization conclusion: the increase in series resistance caused by flux mainly originates from the gradual degradation of the contact interface between the metal and the TCO (possibly due to acidic components corroding the silver electrode and oxidizing the TCO, forming a high-resistance interface layer), rather than the silicon heterojunction or the TCO bulk resistance.
[0060] (5) Parameter sensitivity analysis: When the contact resistivity between the back metal and TCO In the range of 0.0034-0.0044 Ω·cm 2 When changing within the range, Fluctuation less than 0.02Ω·cm 2 When the resistivity of the silicon substrate When varying within the range of 1.0–1.5 Ω·cm, the fluctuation is less than 0.008 Ω·cm. 2 This indicates that the proposed method is insensitive to non-dominant parameters and has good robustness and engineering applicability.
[0061] Figure 7 The figures show the dark-state current-voltage characteristic curves of this invention under different flux immersion times. Figure 7 As shown in (a), the curves in the low-voltage region almost overlap, while the curves in the high-voltage region gradually separate with immersion time, indicating that the total series resistance gradually increases; as Figure 7 As shown in (b) in the figure, after local magnification of the high voltage region, the trend of the curves gradually separating with the soaking time becomes more obvious.
[0062] II. Verification aided by single-sided interface resistance: To further verify the physical rationality of the equivalent interface transport resistance extracted in this invention, a silicon heterojunction solar cell from the same batch as in Example 2 (but using pure silver electrodes) from a second manufacturer was selected. An ITO transparent conductive layer and silver electrodes were deposited on the μc-Si:H(n) layer surface on the back side (n-type side) of the cell using magnetron sputtering to prepare a test structure for the transmission line method (TLM). The thickness of the ITO transparent conductive layer was 105 nm, the thickness of the silver electrodes was approximately 220 nm, and the TLM electrode spacing was 0.4 mm–1.2 mm. The measured equivalent interface transport resistance on the n-type side was 0.549 Ω·cm. 2 .
[0063] In comparison, the total equivalent interfacial transport resistance extracted from the same batch of intact batteries using the method of this invention is: =1.667Ω·cm 2 (See Table 2). Since this total resistance is the series equivalent value of the heterojunction interfaces on the front and back sides (n-side and p-side), the equivalent interface transfer resistance of the p-type side (μc-Si:H(p) / TCO) can be deduced from this as approximately: ; This inverse value is physically reasonable and consistent with expectations—because hole mobility is lower than electron mobility, the transport barrier at the p-type μc-Si:H / TCO interface is typically higher than that on the n-type side, hence the p-side resistance (1.118 Ω·cm) is relatively low. 2 The value is greater than the measured value of the TLM on the n-side (0.549 Ω·cm). 2 The result is reasonable. Meanwhile, the measured value of the n-side TLM (0.549 Ω·cm) is... 2 The total interfacial resistance extracted in this invention is less than 1.667 Ω·cm. 2 This also conforms to the circuit logic that the total resistance is the sum of the two series connections.
[0064] This verification experiment shows that the lumped parameters extracted by this invention are highly consistent with the single-sided contact resistance measured by independent TLM experiments in terms of both numerical magnitude and physical trend, further confirming the reliability and interpretability of the decomposition method. Due to the complex fabrication process and poor repeatability of p-type side TLM test structures (p-type microcrystalline silicon doped layers are easily damaged by subsequent ITO sputtering), industrial implementation is generally difficult. This invention completely avoids this difficulty, requiring only a complete cell to obtain comprehensive information about both interfaces, highlighting its practical engineering value.
[0065] Therefore, this invention employs a non-destructive extraction method for the equivalent interface transport resistance of silicon heterojunction solar cells. This method requires no specialized testing structure and can directly test intact silicon heterojunction solar cells without damaging the cell, making it suitable for production line monitoring. The extracted equivalent interface transport resistance exhibits good repeatability, effectively distinguishing between changes in metal grid resistance and heterojunction interface resistance, and demonstrates high sensitivity to TCO deposition quality and interface state differences. Furthermore, by cross-referencing independent measurements with other resistance components, the location of contact degradation can be pinpointed. This method is insensitive to non-dominant parameters, yields stable and reliable results, and provides a rapid and low-cost characterization method for evaluating the interface quality of silicon heterojunction solar cells.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A non-destructive method for extracting the equivalent interface transport resistance of a silicon heterojunction solar cell, characterized in that, Includes the following steps: S1. Apply a step-scanning current to a complete silicon heterojunction solar cell in a dark environment and at a preset temperature to obtain the dark current-voltage characteristic curve. S2. Based on the dark-state current-voltage characteristic curve, the linear segment in which dV / d(lnI) is linearly related to the current I is determined using a dual-diode model. The slope is obtained by fitting the linear segment, and the slope is the total series resistance. S3. Obtain the geometric and material parameters of the complete silicon heterojunction solar cell, and use the pre-calibrated or empirical values as the contact resistivity between the metal and the TCO. Based on the geometric parameters, material parameters and the contact resistivity between the metal and the TCO, calculate the metal grid resistance, TCO lateral resistance, contact resistance between the metal and the TCO and silicon substrate resistance respectively. S4. Convert the total series resistance to the surface resistance of the total series resistance. Subtract the surface resistance of the metal gate resistance, the surface resistance of the TCO lateral resistance, the surface resistance of the contact resistance between the metal and the TCO, and the surface resistance of the silicon substrate from the surface resistance of the total series resistance to obtain the equivalent interface transfer resistance between the TCO and μc-Si:H.
2. The method according to claim 1, characterized in that, S1 specifically includes: S11. Place the complete silicon heterojunction solar cell in a dark environment, wherein the dark environment is a dark room, and set the preset temperature to 298.15K; S12. Set the scanning range of the step scanning current to 0 to 0.6A and the step size to 3mA; S13. Connect the complete silicon heterojunction solar cell using the four-wire method, apply a step-scanning current to the complete silicon heterojunction solar cell in current source mode, and measure the corresponding voltage. S14. Perform S13 three times, take the average of the three measurement results, and obtain the dark-state current-voltage characteristic curve.
3. The method according to claim 1, characterized in that, S2 specifically includes: S21. In the forward bias region where the voltage is greater than 0.4V, the dark-state current-voltage characteristic curve satisfies the dual-diode model, which is as follows: ; in, For voltage, For current, It is a natural exponential function. This is the reverse saturation current corresponding to the diffusion current. This is the reverse saturation current corresponding to the composite current. and As an ideal factor, For series resistance, For parallel resistors, For electron charge, Boltzmann's constant, Thermodynamic temperature; Differentiating the dual-diode model in the forward bias region yields: ; in, This is the thermal voltage; dV / d(lnI) has a linear relationship with the current I. In the forward bias region, the data points of dV / d(lnI) and current I are calculated based on the dark-state current-voltage characteristic curve, and these data points constitute a linear segment. S22. Perform least squares fitting on the data points of the linear segment to obtain the slope, where the slope is the total series resistance, and the correlation coefficient of the least squares fitting is greater than or equal to 0.
99.
4. The method according to claim 1, characterized in that, S3 specifically includes: S31. Obtain the geometric and material parameters of the complete silicon heterojunction solar cell. The geometric parameters include grid line size and fine grid spacing. The material parameters include TCO sheet resistance, grid line paste resistivity, silicon substrate resistivity and silicon wafer thickness. Use pre-calibrated or empirical values as the contact resistivity between the metal and TCO. S32. Calculate the resistance of the metal grid wire based on the grid wire size and the resistivity of the grid wire paste; S33. Calculate the TCO transverse resistance based on the TCO sheet resistance and fine grid spacing; S34. Calculate the contact resistance between the metal and the TCO based on the contact resistivity and total contact area between the metal and the TCO. S35. Calculate the silicon substrate resistance based on the silicon substrate resistivity and silicon wafer thickness; S36. The metal grid line resistance, TCO lateral resistance, contact resistance between the metal and TCO, and silicon substrate resistance are all uniformly expressed as surface ratio resistance.
5. The method according to claim 4, characterized in that, The calculation method for the metal grid line resistance in S32 is as follows: The equivalent resistance of a single fine grid segment is: ; in, The equivalent resistance of a single fine grid segment. The resistivity of the grid line paste, For a single segment of fine grid length, For fine grid linewidth, For fine grid line height; The equivalent resistance is converted to the area ratio resistance based on the number of fine grid segments on the front and back sides: ; in, The surface resistivity of the metal grid line resistor. The number of fine grid segments on the front side, The number of fine grid segments on the back side. Battery area; The calculation method for the TCO transverse resistance in S33 is as follows: ; in, The surface resistance of the TCO transverse resistance. For TCO sheet resistors For fine gate pitch, n-plane TCO sheet resistors are used on the front side and p-plane TCO sheet resistors are used on the back side; The method for calculating the contact resistance between the metal and the TCO in S34 is as follows: ; in, The surface resistivity is the contact resistance between the metal and the TCO. This refers to the contact resistivity between the metal and the TCO. The total contact area is calculated separately for the front and back sides and then connected in series. The calculation method for the silicon substrate resistance in S35 is as follows: ; in, The surface resistivity is the resistance of the silicon substrate. The resistivity of the silicon substrate, This refers to the thickness of the silicon wafer.
6. The method according to claim 1, characterized in that, In S4, the equivalent interfacial transfer resistance between TCO and μc-Si:H is calculated using the following formula: ; in, The surface resistance is the area ratio of the equivalent interfacial transport resistance between TCO and μc-Si:H. The surface resistance is the area ratio of the total series resistance. The surface resistivity of the metal grid line resistor. The surface resistance of the TCO transverse resistance. The surface resistivity is the contact resistance between the metal and the TCO. The surface resistance of the silicon substrate is the surface resistance.
7. The method according to claim 1, characterized in that, It also includes S5, immersing the silicon heterojunction solar cell under test in a 10% wt flux solution for different durations, then removing and drying it, repeating S1 to S4, and independently monitoring the changes in the TCO sheet resistance, grid line paste resistivity and silicon substrate resistivity among the material parameters. When the relative changes in TCO sheet resistance, grid line paste resistivity and silicon substrate resistivity are all less than the preset percentage and the total series resistance increases, the degradation site is located at the contact interface between the metal and TCO.
8. The method according to claim 7, characterized in that, It also includes S6, which involves preparing a ring electrode structure on the TCO surface of a silicon heterojunction solar cell. The ring electrode structure has a solid circular electrode at its center and a square electrode around it. A ring gap is formed between the two electrodes. A small current is applied between the two electrodes to measure the total resistance. This is used to independently monitor the relative change trend of the contact resistance between the metal and the TCO, and to cross-confirm with the back-calculation results of S4 to S5.
9. The method according to claim 4, characterized in that, The pre-calibration value mentioned in S31 is obtained by random sampling and calibration of the TLM of the same batch of batteries, and the empirical value is the process empirical value.