A process for preparing a litz wire and an on-line detection system thereof

By employing multi-stage gradual stranding and closed-loop control of monofilament tension, combined with an online detection system, the problems of uneven stranding and tension control in the preparation of Litz wire were solved, resulting in improved high-frequency performance and better consistency of finished products, while reducing high-frequency loss and raw material waste.

CN123143147APending Publication Date: 2026-11-20TONGLING JINGXUN SPECIAL ENAMELLED WIRE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611012315.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-08
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The existing Litz wire manufacturing process suffers from problems such as uneven stranding, inaccurate tension control, delayed detection, and uncontrollable end treatment, resulting in high high-frequency loss, poor product consistency, and serious waste of raw materials.

Method used

By employing a multi-stage gradual stranding structure, single-filament tension adaptive closed-loop control, and multi-sensor fusion online detection technology, stranding quality is improved, tension is precisely controlled, and full-process detection is achieved. Combined with the central control unit, a closed-loop quality control system is formed.

Benefits of technology

This has resulted in improved current distribution uniformity, reduced high-frequency losses, increased finished product qualification rate, reduced raw material waste, and improved production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143147A_ABST
    Figure CN123143147A_ABST
Patent Text Reader

Abstract

This invention relates to the field of Litz wire preparation and testing technology, and discloses a Litz wire preparation process and its online testing system. The preparation process includes: ultra-fine single-crystal copper gradient cooling drawing, four-layer nano-composite insulating coating, primary stranding pre-twisting, secondary complex stranding self-positioning, segmented heat setting, double-layer composite wrapping tape, and constant tension take-up. All single filaments are equipped with independent tension closed-loop control with an accuracy of ±1%. The pre-twisting angle is adapted to the wire diameter to ensure equal filament lengths. The online testing system is integrated into each process, including five major testing modules: single filament quality, stranding state, tension distribution, electrical performance, and appearance defects. A digital twin model is built in the central unit for real-time scoring and parameter adjustment feedback. This invention achieves a Litz wire current distribution uniformity of ≥95%, a 25%-35% reduction in 100kHz loss, and a first-pass yield of over 99.5%, solving the pain points of traditional processes such as insufficient positioning, tension loss control, and delayed testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of Litz wire preparation and detection technology, specifically to a Litz wire preparation process and its online detection system. Background Technology

[0002] Litz wire is a special electromagnetic wire designed specifically for high-frequency applications. Its core principle involves layering hundreds to thousands of insulated fine copper wires, each with a diameter much smaller than the skin depth, in a specific pattern. This forces the high-frequency current to be evenly distributed across the cross-section of each conductor, fundamentally suppressing high-frequency losses caused by the skin effect and proximity effect. In the 10kHz-1MHz frequency band, high-quality Litz wire can reduce high-frequency losses by 60%-85% compared to solid copper wire of the same cross-sectional area. It has become a core material for high-end equipment such as high-frequency transformers, wireless charging coils, new energy vehicle motors, aerospace power supplies, and induction heating equipment.

[0003] The existing manufacturing process for Litz wire mainly includes six steps: drawing, enameling, single stranding, double stranding, wrapping, and winding. The mainstream production technology has the following significant defects: First, the stranding process employs a constant pitch design, resulting in an inherent difference in the actual path lengths of the inner and outer monofilaments. The inner monofilaments are in a relaxed state for a long time, while the outer monofilaments are in a tensile state for a long time, with a tension difference between strands reaching 15%-25%. This causes severe uneven current distribution, and the actual high-frequency loss is 30%-50% higher than the theoretical value. At the same time, the traditional re-stranding process uses a two-stage structure of "first stranding and then re-stranding". During the re-stranding process, each sub-bundle undergoes relative torsion, and the position of the monofilaments inside the sub-bundle becomes fixed, making it impossible to achieve a true "repositioning" effect, and significantly reducing the ability to suppress proximity effects.

[0004] Second, the tension control adopts open-loop passive adjustment, which provides constant tension through mechanical dampers or magnetic powder brakes. It cannot respond to dynamic factors such as changes in the diameter of the pay-off reel, fluctuations in the diameter of the single wire, and fluctuations in the stranding speed. The tension fluctuation range of the single wire is usually more than ±20%. Excessive tension will cause the enameled insulation layer to be stretched and damaged, resulting in pinholes and electrical breakdown hazards; insufficient tension will cause the single wire to entangle and form internal structural defects.

[0005] Third, quality inspection heavily relies on manual offline sampling. During production, only the surface appearance can be observed with the naked eye. Key parameters such as stranding pitch, stranding angle, single filament tension distribution, and insulation integrity cannot be quantitatively detected online. This lag in inspection means that by the time defects are discovered, thousands of meters of substandard products have already been produced, resulting in significant waste of raw materials. Existing visual inspection systems, due to the helical motion characteristics of Litz wire, have a pitch measurement error exceeding 10% and cannot detect internal defects such as broken wires, hidden insulation damage, and short circuits between strands.

[0006] Fourth, the quality of end treatment and welding is uncontrollable. The multi-strand structure makes it easy for traditional wire stripping methods to cause single wire breakage or short circuit between strands. Improper control of hot air paint stripping temperature will damage the adjacent insulation layer. Uneven distribution of ultrasonic welding energy will lead to poor welding. The final product end contact resistance difference can reach an order of magnitude, which seriously affects the reliability of end application.

[0007] While some improvement solutions exist within the industry to address the aforementioned issues, such as the stress relief process for compressed Litz wire disclosed in Chinese patent CN202511418154 and the pre-bonded self-adhesive Litz wire preparation method disclosed in CN202511425320, these only optimize single processes and fail to address core pain points at the system level, such as insufficient stranding transposition, dynamic tension control, and multi-dimensional online detection. Furthermore, they lack an integrated and collaborative design between the preparation process and the detection system. Therefore, developing a Litz wire preparation process and its detection system that offers high stranding quality, precise tension control, comprehensive and real-time detection, and good finished product consistency has significant industrial value. Summary of the Invention

[0008] The purpose of this invention is to overcome the shortcomings of the prior art and provide a Litz wire manufacturing process and its detection system. Through three core technological innovations—multi-stage gradual stranding structure, single-filament tension adaptive closed-loop control, and multi-sensor fusion online detection—the high-frequency performance, production efficiency, and finished product qualification rate of Litz wire are simultaneously improved.

[0009] To achieve the above objectives, the present invention adopts the following technical solution: A process for preparing Litz wire includes the following steps: S1. Preparation of ultra-fine single crystal copper wire: Ultra-fine single crystal copper wire with a diameter of 0.03mm-0.15mm is prepared by continuous extrusion-multi-die drawing composite process of oxygen-free copper rod. Gradient temperature drawing oil is used for cooling during the drawing process. The die temperature gradually changes from 45℃ at the inlet to 30℃ at the outlet. The compression rate of each pass is controlled at 12%-15%. The drawing speed is 800-1200m / min. Online eddy current detection is used to remove surface microcracks and internal pore defects. S2. Nanocomposite insulating enamel coating: The ultra-fine copper wire is coated with four layers of composite insulation. The first layer is a 0.5μm-1μm thick polyurethane primer, the second layer is a 2μm-3μm thick polyesterimide intermediate varnish, the third layer is a 1μm-2μm thick polyamideimide topcoat, and the fourth layer is a 0.3μm-0.5μm thick self-lubricating nano coating. Each coating is cured in a segmented drying tunnel with an inlet temperature of 280℃, a middle section temperature of 350℃, and an outlet temperature of 320℃. The enamel coating line speed is 150-200m / min, and the online pinhole detector has a detection sensitivity of 1 pinhole per meter. S3. First-stage stranding and pre-twisting: Divide N strands of enameled monofilament into M sub-bundles, each sub-bundle containing n strands of monofilament, N=M×n, M=3-7, n=15-60. Each sub-bundle is first pre-twisted in the same direction, with a pre-twisting angle of 3°-8° / cm. Then, first-stage stranding is performed. The stranding pitch increases from the center of the sub-bundle to the outer layer in a gradient of 5%-10%. The stranding direction adopts SZ alternation, changing direction 1-2 times per meter. S4. Secondary Retwisting and Transposition: The M pre-twisted sub-bundles are subjected to secondary retwisting. During the retwisting process, each sub-bundle rotates in the opposite direction along its own axis. The ratio of its rotation speed to its revolution speed is 1:(M-1), achieving complete transposition between the sub-bundles. The retwisting pitch is 3-5 times the average pitch of the primary retwisting bundle, and the retwisting tension is 10%-15% higher than that of the primary retwisting bundle. S5. Heat setting and stress relief: After stranding, the Litz wire passes through a segmented heating and setting channel, where the temperature is linearly raised from 120°C to 180°C and held for 8-12 seconds. Then it enters the cooling zone and is forced to be cooled to room temperature to eliminate the internal stress generated during stranding. S6. Multi-layer composite wrapping tape: Double-layer overlapping wrapping tape of polyimide film and non-woven fabric is used, with a wrapping tape overlap rate of 45%-55% and a wrapping tape tension of 5-10N. The film tension and overlap rate are monitored online during the wrapping process. S7. Constant tension take-up and winding: Active constant tension take-up is adopted, and the take-up tension fluctuation is controlled within ±3%. The wire pitch adapts to the change of wire diameter. The inner diameter of the winding is 150-300mm, and the length of each winding is 1000-5000m.

[0010] Furthermore, in steps S3 and S4, all monofilaments pass through an independent tension closed-loop control unit. Each control unit includes a servo motor, a tension sensor, and a guide wheel assembly. The tension sensor detects the tension of the monofilament in real time with a feedback frequency of 1kHz. The servo motor adjusts the wire feeding speed in real time according to the tension deviation, with a tension control accuracy of ±1%.

[0011] Furthermore, the pre-twist angle in step S3 is adjusted according to the diameter of the monofilament. When the diameter of the monofilament is 0.03mm, the pre-twist angle is 8° / cm, and when the diameter of the monofilament is 0.15mm, the pre-twist angle is 3° / cm, to ensure that all monofilaments have the same length after twisting.

[0012] An online detection system for Leeds wire, integrated into key process nodes of the above-mentioned preparation process, includes: The monofilament quality inspection module is located at the exit of the enameling process and includes a laser diameter gauge, a pinhole detector, and an eddy current flaw detector. It can detect monofilament diameter tolerance, insulation layer pinholes, and conductor internal defects in real time, with a data sampling frequency of 10kHz. The stranding status detection module is located at the exit of the re-stranding process. It includes two sets of orthogonally arranged line array cameras and a structured light 3D scanner. The line array camera has a resolution of 4096 pixels and a scanning speed of 18000 lines / second. It calculates the stranding pitch, stranding angle, and uniformity of single filament arrangement through continuous image sequence analysis. The pitch measurement accuracy is ±0.1mm. The tension distribution detection module is installed on each filament pay-off frame. It includes a high-precision tension sensor with a sampling frequency of 1kHz. It monitors the tension value of all filaments in real time, constructs a tension distribution heat map, and identifies filaments with abnormal tension. The electrical performance testing module, located before the finished product is finished, includes a high-frequency impedance tester, an insulation resistance tester, and an inter-strand short-circuit tester. It adopts the non-contact electromagnetic coupling principle to test the AC impedance, quality factor Q value, and insulation resistance in the 10kHz-1MHz frequency band online. The testing speed is synchronized with the production line. The appearance defect detection module is set after the wrapping process. It includes a 360° surround vision inspection array consisting of 8 high-speed cameras, each covering a 45° field of view. It detects defects such as outer wrapping tape damage, poor overlap, exposed threads, and bulges, with a defect recognition accuracy of 0.1mm. The central control and data processing unit receives data from all inspection modules, establishes a digital twin model of the Leeds line quality, calculates the comprehensive quality score in real time, automatically alarms and marks the defect location when the quality exceeds the tolerance range, and simultaneously provides feedback to adjust process parameters.

[0013] Furthermore, the twisting state detection module adopts a spiral motion image decoupling algorithm to separate the axial motion and circumferential rotation of the Litz wire. It calculates the actual twisting pitch by matching feature points of adjacent frames, eliminating the effects of motion blur and viewpoint distortion, and the pitch measurement error is less than 2%.

[0014] Furthermore, the electrical performance testing module includes a standard impedance calibration unit that automatically calibrates once per hour to ensure long-term stability of test data and repeatability of high-frequency impedance testing within ±0.5%.

[0015] Furthermore, the central control unit employs machine learning algorithms to establish a quality prediction model based on historical data, identify process drift trends in advance, achieve preventative quality control, and increase the first-pass yield of finished products to over 99.5%.

[0016] Compared with the prior art, the present invention provides a process for preparing Litz wire and its online detection system, which has the following beneficial effects: 1. Multi-stage gradual twisting and active transposition technology fundamentally solves the problems of inter-strand length difference and uneven tension. All monofilaments achieve true spatial transposition, current distribution uniformity is improved to over 95%, high-frequency loss at 100kHz is reduced by 25%-35%, and Q value is improved by 15%-20%. 2. Single-filament independent tension closed-loop control, with tension control accuracy of ±1%, completely eliminates insulation layer damage and structural defects caused by tension fluctuations, reduces insulation layer pinhole rate by 90%, and controls DC resistance batch consistency deviation within ±0.5%; 3. A multi-dimensional online inspection system enables full-process quality monitoring from monofilament to finished product, with 100% inspection coverage and a defect detection rate of 99.8%, completely eliminating manual omissions and inspection delays, and reducing raw material waste by 80%. 4. The integrated design of process and testing allows for real-time feedback of testing data to adjust process parameters, forming a closed-loop quality control system. This increases production efficiency by 30% and raises the first-pass yield of finished products from 85% to over 99.5%. Attached Figure Description

[0017] Figure 1 This is a flowchart of the production process of the Litz line according to the present invention; Figure 2 This is a flowchart of the Litz line detection system of the present invention; Detailed Implementation

[0018] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0019] like Figure 1 As shown, the present invention discloses a process for preparing Litz wire, the specific implementation process of which is as follows: Example 1: Preparation of 0.1mm×400 strand Litz wire for high-frequency transformers This embodiment describes the fabrication of a high-performance Litz wire with a single wire diameter of 0.1 mm, a total of 400 strands, and suitable for 100 kHz high-frequency transformers. Specific process steps are as follows: S1. Preparation of Ultra-fine Single-Crystal Copper Wire: φ8mm oxygen-free copper rods with a purity of 99.995% and an oxygen content of less than 5ppm are selected. These are extruded into φ3mm copper billets using a continuous extrusion press, and then drawn through 13 passes using multiple dies to finally produce φ0.100±0.001mm ultra-fine single-crystal copper wires. Gradient temperature control is used during the drawing process: the die temperature for the first pass is 45℃, decreasing by 1℃ for each pass, with the final pass at 33℃. Water-soluble copper drawing oil with a concentration of 8%–10% is used, with a compression rate of 13% per pass and a drawing speed of 1000m / min. An online eddy current detector is installed at the wire drawing machine outlet, with a detection frequency of 50kHz, to remove defective wires with surface microcracks exceeding 2μm in depth and internal pore diameters exceeding 5μm.

[0020] S2. Nanocomposite Insulating Enamel Coating: A φ0.1mm copper wire undergoes four layers of insulating coating using a vertical enameling machine, with a total of 8 coats and 8 baking cycles. The first layer is a polyurethane primer, 0.8μm thick, cured at 280℃; the second layer is a polyesterimide intermediate varnish, 2.5μm thick, cured at 350℃; the third layer is a polyamide-imide topcoat, 1.5μm thick, cured at 350℃; and the fourth layer is a nano self-lubricating coating, 0.4μm thick, cured at 320℃. The enameled wire runs at a speed of 180m / min, and the drying tunnel is 15m long. An online pinhole detector is installed at the wire outlet, using a high-voltage DC method with a test voltage of 500V. The detection sensitivity is one pinhole per meter, and the machine automatically alarms and shuts down if the number of pinholes exceeds the limit. The final outer diameter of the enameled wire is 0.109±0.001mm, and the breakdown voltage is greater than 1500V.

[0021] S3. First-stage stranding and pre-twisting: The 400 strands of enameled wire are divided into 5 sub-bundles, each with 80 strands. Each sub-bundle is first pre-twisted in the same direction by a pre-twisting device at a pre-twisting angle of 5° / cm, with the pre-twisting speed synchronized with the stranding speed. Then, it enters the first-stage stranding machine, using a 630-type high-speed stranding machine at a stranding speed of 3000 rpm. The pitch is gradually increased from the center of the sub-bundle outwards: 12mm for the center layer, 12.6mm for the middle layer, and 13.2mm for the outer layer, with a 5% increase in pitch. The stranding direction uses an alternating SZ direction, changing direction 1.5 times per meter to ensure sufficient transposition of the single wires within the sub-bundle. Each single wire pay-off stand is equipped with an independent tension control unit, set to a tension of 8cN with a control accuracy of ±1%.

[0022] S4. Secondary Re-twisting and Transposition: Five pre-twisted sub-bundles are fed into a 1250-type re-twisting machine for secondary re-twisting. The re-twisting revolution speed is 800 rpm, and each sub-bundle simultaneously rotates in the opposite direction at 200 rpm. The rotation speed to revolution speed ratio is precisely controlled at 1:4, ensuring that each sub-bundle rotates 90° per revolution, achieving complete spatial transposition between sub-bundles. The re-twisting pitch is set to 60 mm, which is 4.8 times the average pitch of the primary re-twisting bundle. The re-twisting tension is set to 10 cN, which is 25% higher than the primary re-twisting tension, ensuring a tight re-twisting structure. During the re-twisting process, the tension and rotation speed of each sub-bundle are monitored in real time, and the synchronization error is controlled within ±0.5%.

[0023] S5. Heat Setting and Stress Relief: After stranding, the Litz wire passes through a 6-meter-long segmented heating and setting channel, divided into three temperature zones: Zone 1 at 120°C, Zone 2 at 150°C, and Zone 3 at 180°C, with a wire speed of 50 m / min and a total residence time of 7.2 seconds. It then enters a 2-meter-long forced air cooling zone at a speed of 15 m / s, rapidly cooling to room temperature to eliminate torsional and bending internal stresses generated during stranding. The natural straightness of the Litz wire is greater than 98%.

[0024] S6. Multi-layer composite wrapping tape: Utilizing a double-layer wrapping tape consisting of a 0.025mm thick polyimide film and a 0.05mm thick non-woven fabric, with a semi-overlapping wrapping and an overlap rate of 50%. The wrapping machine head speed is 600 rpm, the tape tension is 8N, and tension fluctuation is controlled within ±5%. The outer diameter of the Litz wire after wrapping is approximately 3.8mm. The wrapping layers possess excellent insulation and mechanical protection properties while maintaining superior flexibility.

[0025] S7. Constant Tension Take-up and Coiling: An active double-reel take-up machine is used, with the take-up tension set at 50N. Closed-loop control via a tension sensor ensures tension fluctuations are within ±3%. The wire guide is servo-driven, with adaptive wire pitch to changes in wire diameter, and cross-winding prevents wire compression. The coiled inner diameter is 250mm, each coil is 3000m long, and weighs approximately 25kg. Automatic meter counting is performed during take-up, with an accuracy of ±0.1%.

[0026] like Figure 2 As shown, the Litz line online detection system of the present invention operates throughout the above-described preparation process. Specific implementation details are as follows: Monofilament quality inspection module: installed at the enameling machine outlet, includes: Laser diameter gauge: measuring range 0.05mm-0.5mm, accuracy ±0.0005mm, sampling frequency 10kHz, real-time monitoring of single filament diameter fluctuations, automatic alarm when exceeding ±0.001mm tolerance; Pinhole detector: DC high voltage 500V, sensitivity 1 pinhole / meter, immediately marks and records the location of the pinhole upon detection; Eddy current flaw detector: with a detection frequency of 50kHz, it can detect surface cracks larger than 2μm and internal defects larger than 5μm.

[0027] Twisting status detection module: installed at the outlet of the rewinder, including: Two sets of orthogonal linear array cameras: 4096 pixel resolution, 18000 lines / second scanning speed, acquiring XY and YZ plane images respectively; Structured light 3D scanner: laser line width 0.05mm, reconstruction accuracy 0.02mm, to acquire the 3D contour of the Litz line surface; Image decoupling algorithm: Separates the axial velocity v of the Litz wire from its circumferential rotational angular velocity ω. Calculates the actual stranding pitch P=2πv / ω using the displacement Δs and time Δt of the same filament in adjacent frames, eliminating motion blur and viewpoint distortion. Pitch measurement accuracy is ±0.1mm, with an error of less than 1.5%. Stranding quality assessment: Calculate the uniformity of single filament arrangement, stranding angle deviation, and pitch fluctuation rate. A comprehensive score of 95 or higher is considered qualified.

[0028] Tension distribution detection module: One high-precision tension sensor is installed on each of the 400 monofilament pay-off racks, with a measuring range of 0-20 cN, an accuracy of ±0.1 cN, and a sampling frequency of 1 kHz. The central control unit collects all tension data in real time, constructs a 400-dimensional tension distribution matrix, generates a tension distribution heat map, identifies abnormal monofilaments with tension deviating from the set value by ±5%, automatically adjusts the speed of the corresponding servo motor, and performs closed-loop correction of tension. The tension distribution standard deviation less than 0.5 cN is qualified.

[0029] Electrical performance detection module: Installed before finished product take-up, including: High-frequency impedance tester: Adopting the transformer coupling principle, with three test frequency points of 10 kHz, 100 kHz and 1 MHz, the test speed is synchronized with the production line, the impedance test repeatability is ±0.5%, and the Q value greater than 150 at 100 kHz is qualified; Insulation resistance tester: At DC 1000V, the insulation resistance greater than 10^12 Ω is qualified; Inter-strand short circuit detector: Using the pulse voltage method, it can detect insulation damage between any two strands, with a sensitivity of 1 pF; Automatic calibration unit: Calibrate once per hour by connecting a standard impedance component to ensure long-term test stability.

[0030] Appearance defect detection module: 360° surrounding vision array, 8 high-speed cameras with 5 million pixels, each covering a 45° field of view, uniformly illuminated by a ring light source, with a frame rate of 30 fps. The AI defect detection algorithm based on deep learning can identify 12 types of defects such as outer wrapping tape damage, overlapping defects, exposed wires, bulges, and jumpers, with a minimum recognition size of 0.1 mm, a defect detection rate of 99.8%, and a false detection rate of less than 0.1%.

[0031] Central control and data processing unit: Industrial-grade edge computing server, 32-core CPU, 64 GB RAM, 2 TB solid-state drive. Running dedicated quality control software, the functions include: 1. Data collection and storage: All detection data is sampled once per second and stored permanently, enabling traceability of complete quality data for every meter of product; 2. Digital twin modeling: Establish a quality digital twin model for litz wire to intuitively display the real-time status of all parameters; 3. Comprehensive quality scoring: Based on the analytic hierarchy process, the monofilament quality weight is 20%, the stranding quality weight is 30%, the tension distribution weight is 20%, the electrical performance weight is 20%, and the appearance quality weight is 10%, to calculate the comprehensive quality score; 4. Closed-loop process adjustment: When the quality score is lower than 90 points, automatically analyze the cause and adjust the corresponding process parameters, such as adjusting the stranding speed when the lay length is abnormal, and adjusting the pay-off servo when the tension is abnormal; 5. Machine learning prediction: Based on 10 million meters of historical production data, a quality prediction model is trained to identify process drift trends 10-30 seconds in advance and adjust parameters preventively; 6. Reports and Traceability: Automatically generates quality reports and supports quality traceability by batch, roll, and meter level.

[0032] The Litz wire prepared in this embodiment, after third-party testing, has the following key performance indicators: DC resistance: ≤0.58Ω / km, batch consistency deviation ±0.3%; 100kHz AC impedance: ≤1.25Ω / km, 28% lower than traditional processes; 100kHz Q value: ≥165, an 18% improvement over traditional processes; Insulation resistance: ≥5×10^12Ω・km; Breakdown voltage: ≥5000V; First-pass yield: 99.6%.

[0033] Example 2: Preparation of 0.05mm × 1200 strand Litz wire for wireless charging This embodiment prepares an ultrafine multi-strand Litz wire with a single filament diameter of 0.05 mm, a total of 1200 strands, and suitable for an 85 kHz wireless charging system. The process parameters are adjusted as follows: S1, Ultra-fine drawing: Final single filament diameter 0.050±0.0005mm, 21 drawing passes, compression rate of 12% per pass, drawing speed 800m / min; S2. Enameling process: The total insulation thickness is reduced to 6μm, the proportion of the four-layer structure remains unchanged, and the enamel coating speed is 150m / min. S3, First-level strand: 1200 strands divided into 6 sub-strands, each sub-strand with 200 strands, pre-twist angle 7° / cm, first-level pitch gradient 8mm, 8.5mm, 9mm, increasing by 6%; S4, Second-stage double twisting: Rotation-to-revolution ratio 1:5, double twisting pitch 40mm, double twisting tension 20% higher than that of the first stage; S5. Heat setting: Maximum temperature 160℃, to avoid excessive softening of ultrafine monofilaments; S6. Packaging tape: Uses only a single layer of 0.02mm polyimide film for packaging to maintain the product's flexibility.

[0034] The detection system optimizes image resolution and tension sensor range to address the characteristics of ultra-fine multi-strand wires. The final product has a 32% lower loss at 85kHz compared to traditional products, meeting the requirements of high-power wireless charging.

[0035] The key performance of Litz wire prepared by this process was compared with that of conventional process products using constant pitch stranding, open-loop tension control, and manual offline sampling inspection. The results are shown in the table below:

[0036] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0037] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A process for preparing Litz wire, characterized in that: Includes the following steps: S1. Preparation of ultra-fine single-crystal copper wire: Ultra-fine single-crystal copper wire with a diameter of 0.03mm-0.15mm is prepared by continuous extrusion and multi-die drawing composite process of oxygen-free copper rod. Gradient temperature drawing oil is used for cooling during the drawing process, and the die temperature gradually changes from 45℃ at the inlet to 30℃ at the outlet. The compression rate of each pass is controlled at 12%-15%. S2, Nanocomposite insulating coating: Four-layer composite insulating coating is applied to the ultra-fine copper wire, namely polyurethane primer, polyesterimide intermediate varnish, polyamideimide topcoat, and self-lubricating nano coating. Each coating is cured in a segmented baking oven. S3, First-stage stranding and pre-twisting: Divide N strands of enameled monofilament into M sub-bundles. Each sub-bundle is first pre-twisted in the same direction with a pre-twisting angle of 3°-8° / cm. Then, first-stage stranding is performed. The stranding pitch increases from the center of the sub-bundle to the outer layer in a gradient of 5%-10%. The stranding direction adopts SZ alternating direction. S4. Secondary Twisting and Transposition: The M pre-twisted sub-bundles are subjected to secondary twisting. During the twisting process, each sub-bundle rotates in the opposite direction along its own axis. The ratio of its rotation speed to its revolution speed is 1:(M-1), thus achieving complete transposition between the sub-bundles. S5. Heat setting and stress relief: The stranded Litz wire passes through a segmented heating and setting channel, where the temperature is linearly raised from 120°C to 180°C, and then forced to cool to room temperature. S6. Multi-layer composite strapping: The strapping uses a double-layer overlapping of polyimide film and non-woven fabric, with an overlap rate of 45%-55%. S7. Constant tension take-up and winding: Active constant tension take-up is adopted, and the tension fluctuation during take-up is controlled within ±3%.

2. The Litz wire preparation process according to claim 1, characterized in that: In steps S3 and S4, all monofilaments pass through an independent tension closed-loop control unit. Each control unit includes a servo motor, a tension sensor, and a guide wheel assembly. The tension sensor detects the tension of the monofilament in real time with a feedback frequency of 1kHz. The servo motor adjusts the wire feeding speed in real time according to the tension deviation, with a tension control accuracy of ±1%.

3. The Litz wire preparation process according to claim 1, characterized in that: The pre-twist angle in step S3 is adjusted according to the diameter of the single filament. When the diameter of the single filament is 0.03mm, the pre-twist angle is 8° / cm, and when the diameter of the single filament is 0.15mm, the pre-twist angle is 3° / cm, to ensure that all single filaments are of the same length after twisting.

4. The Litz wire preparation process according to claim 1, characterized in that: In step S4, the twisting pitch is 3-5 times the average pitch of the primary twisting bundle, and the twisting tension is 10%-15% higher than the tension of the primary twisting bundle.

5. The Litz wire preparation process according to claim 1, characterized in that: In step S1, the drawing speed is 800-1200 m / min, and online eddy current detection is used to remove surface microcracks and internal pore defects; in step S2, the enameled wire speed is 150-200 m / min, and the online pinhole detector has a detection sensitivity of 1 pinhole per meter.

6. An online detection system for Litz wire, integrated into each key process node of the preparation process according to any one of claims 1-5, characterized in that, include: The monofilament quality inspection module is located at the exit of the enameling process and includes a laser diameter gauge, a pinhole detector, and an eddy current flaw detector to detect monofilament diameter tolerance, insulation layer pinholes, and conductor internal defects in real time. The stranding status detection module is located at the exit of the re-stranding process. It includes two sets of orthogonally arranged line array cameras and a structured light 3D scanner. It calculates the stranding pitch, stranding angle, and uniformity of single filament arrangement through continuous image sequence analysis. The tension distribution detection module, installed on each single filament pay-off frame, includes a high-precision tension sensor to monitor the tension value of all single filaments in real time and construct a tension distribution heat map; The electrical performance testing module is installed before the finished product is wound up. It includes a high-frequency impedance tester, an insulation resistance tester, and an inter-strand short circuit tester. It adopts the non-contact electromagnetic coupling principle to test the AC impedance and quality factor Q value in the 10kHz-1MHz frequency band online. The appearance defect detection module is set after the wrapping process and includes a 360° surround vision inspection array to detect defects such as outer wrapping tape damage, poor overlap, exposed threads, and bulges. The central control and data processing unit receives data from all detection modules, establishes a digital twin model of the Leeds line quality, calculates the comprehensive quality score in real time, and automatically alarms and provides feedback to adjust process parameters when the quality exceeds the tolerance range.

7. The online detection system for the Litz wire according to claim 6, characterized in that: The twisting state detection module uses a spiral motion image decoupling algorithm to separate the axial motion and circumferential rotation of the Litz wire. It calculates the actual twisting pitch by matching feature points in adjacent frames, eliminating the effects of motion blur and viewpoint distortion, and the pitch measurement error is less than 2%.

8. The online detection system for the Leeds line according to claim 6, characterized in that: The line scan camera has a resolution of 4096 pixels, a scanning speed of 18000 lines / second, and a pitch measurement accuracy of ±0.1mm; the tension sensor has a sampling frequency of 1kHz, and the data sampling frequency of all detection modules is not less than 10kHz.

9. The online detection system for the Litz wire according to claim 6, characterized in that: The electrical performance testing module includes a standard impedance calibration unit that automatically calibrates once per hour, with a high-frequency impedance test repeatability of ±0.5%; the appearance defect detection module consists of a 360° array of 8 high-speed cameras, with a defect identification accuracy of 0.1mm.

10. The online detection system for the Litz wire according to claim 6, characterized in that: The central control unit uses machine learning algorithms to build a quality prediction model based on historical data, identify process drift trends in advance, and achieve preventive quality control. It uses the analytic hierarchy process to calculate the comprehensive quality score, with single filament quality weighting 20%, stranding quality weighting 30%, tension distribution weighting 20%, electrical performance weighting 20%, and appearance quality weighting 10%.

Citation Information

Patent Citations

  • Square-pressed litz wire production process

    CN121122844A

  • Preparation method of pre-bonding self-bonding litz wire applied to high-frequency electronic product