Zinc oxide varistor and preparation method and application thereof

By employing a gradient doped layered structure in zinc oxide resistors, the performance contradiction caused by uniform distribution of doping additives is resolved, electric field optimization and energy dissipation balance are achieved, and electrical performance and service life are improved.

CN123143162APending Publication Date: 2026-11-20湖南防灾科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611270103.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The uniform distribution of doping additives in existing zinc oxide resistors leads to a contradiction between residual voltage and leakage current, microstructural inhomogeneity, and limited energy tolerance density, making it difficult to achieve simultaneous improvement in electrical performance and service life.

Method used

A gradient-doped layered structure is adopted, which forms a doped core layer, a doped transition layer and a doped surface layer by creating a gradient change in the concentration and type of additives along the thickness direction of the resistor sheet. The layers are continuously transitioned to optimize the electric field distribution and energy dissipation.

Benefits of technology

It achieves a balance between optimized electric field distribution and energy dissipation, improves electrical performance, including nonlinear coefficient, current carrying capacity and thermal stability, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143162A_ABST
    Figure CN123143162A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of overvoltage protection devices, in particular to a zinc oxide resistor disc and a preparation method and application thereof. The zinc oxide resistor disc comprises a doped core layer, a doped transition layer and a doped surface layer; the doped transition layer is located on at least one side surface of the doped core layer, and the doped surface layer is located on one side surface of the doped transition layer away from the doped core layer, wherein the doped surface layer is mainly added with ZrO2 and Bi2O3 to improve a potential gradient, the doped core layer is mainly added with Co2O3, Ni2O3 and Ga2O3 to improve a current passing capacity and thermal stability, the doped transition layer realizes linear gradient of doped components, and a fluxing agent is simultaneously added to optimize a crystal boundary structure and reduce porosity, so that the functional division of 'high potential gradient of the doped surface layer, large current passing capacity of the doped core layer and smooth connection of the doped transition layer' is realized, performance contradictions of uniform doping are avoided, electric field optimization distribution and energy dissipation balance are realized, and the electrical performance is comprehensively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of overvoltage protection device technology, and in particular to a zinc oxide resistor sheet, its preparation method, and its application. Background Technology

[0002] Zinc oxide (ZnO) resistors are widely used in overvoltage protection of power systems and electronic equipment due to their excellent nonlinear current-voltage characteristics. Their basic structure is based on ZnO as the main crystalline phase, with the addition of various metal oxides (such as Bi₂O₃, Sb₂O₃, Co₂O₃, MnO₂, Cr₂O₃, etc.) as modifying additives, forming a composite microstructure of grains, grain boundaries, and spinel phases.

[0003] In existing zinc oxide resistor chips, the doped additives are typically macroscopically uniformly distributed within the blank. While this method is simple, it suffers from the following inherent contradictions and limitations: 1. The contradiction between residual voltage and leakage current: To improve the nonlinear coefficient and reduce leakage current, it is usually necessary to strengthen the grain boundary barrier. However, this may lead to an increase in residual voltage, which is detrimental to the insulation coordination of the protected equipment. Conversely, reducing residual voltage may weaken grain boundary characteristics, resulting in increased leakage current and decreased aging performance.

[0004] 2. Insufficient uniformity of microstructure: During the sintering process, due to the different diffusion coefficients and volatility of each additive, local enrichment or depletion is easily caused, resulting in uneven microstructure electrical properties, which affects the current carrying capacity and shock resistance stability of the resistor sheet.

[0005] 3. Limited energy tolerance density: When a uniform structure is subjected to a large current impact, the energy dissipation distribution is uneven, which can easily lead to local overheating and thermal stress concentration, thereby reducing the square wave impact and energy tolerance of the resistor.

[0006] Currently, some technologies attempt to optimize resistor performance by adjusting the proportion of doping elements, but they still haven't overcome the limitations of uniform doping and cannot fundamentally solve the contradiction between potential gradient and current carrying capacity. Furthermore, they don't consider the differences in heat distribution during resistor operation, making it difficult to simultaneously improve electrical performance and lifespan. For example, patent CN112794714A discloses a high-potential-gradient, high-current-carrying zinc oxide resistor containing zirconium and bismuth, which achieves control over potential gradient and current carrying capacity by optimizing the raw material formulation. However, this technology still uses a uniform doping structure, failing to address issues such as localized hot spots and uneven aging. Other technologies optimize grain boundary structure by adding composites, but this doesn't create gradient doping, making it difficult to adapt to the performance requirements of different regions.

[0007] Therefore, it is desirable to provide a new zinc oxide resistor. Summary of the Invention

[0008] To address the aforementioned technical problems, this invention provides a zinc oxide resistor sheet, its preparation method, and its applications. The zinc oxide resistor sheet provided by this invention has a gradient-doped layered structure, creating a gradient change in the concentration and type of additives along the thickness direction of the resistor sheet. This achieves a balance between optimized electric field distribution and energy dissipation, thereby comprehensively improving electrical performance.

[0009] In a first aspect, the present invention provides a zinc oxide resistor sheet, the zinc oxide resistor sheet comprising a doped core layer, a doped transition layer and a doped surface layer; The doped transition layer is located on at least one side surface of the doped core layer, and the doped surface layer is located on the side surface of the doped transition layer away from the doped core layer; The doped surface layer includes a zinc oxide matrix and a flux and surface doping components distributed in the zinc oxide matrix. The surface doping components include Bi2O3, ZrO2, Sb2O3, SiO2 and Al(NO3)3. The doped transition layer includes a zinc oxide matrix and a flux and transition layer doping components distributed in the zinc oxide matrix. The transition layer doping components include Bi2O3, ZrO2, Sb2O3, Co2O3, MnO2, SiO2, and Al(NO3)3. The molar content of Bi2O3, ZrO2, Co2O3, MnO2, SiO2, and Al(NO3)3 in the doped transition layer decreases gradually from the doped surface layer to the doped core layer, while the molar content of Sb2O3 increases gradually from the doped surface layer to the doped core layer. The doped core layer includes a zinc oxide matrix and a flux and core layer doping components distributed in the zinc oxide matrix. The core layer doping components include Bi2O3, ZrO2, Sb2O3, Co2O3, MnO2, Ni2O3, B2O3 and Ga2O3. The molar content of Bi2O3 in the doped surface layer is greater than or equal to the maximum molar content of Bi2O3 in the doped transition layer, and the minimum molar content of Bi2O3 in the doped transition layer is greater than or equal to the molar content of Bi2O3 in the doped core layer. The molar content of ZrO2 in the doped surface layer is greater than or equal to the maximum molar content of ZrO2 in the doped transition layer, and the minimum molar content of ZrO2 in the doped transition layer is greater than or equal to the molar content of ZrO2 in the doped core layer. The molar content of SiO2 in the doped surface layer is greater than or equal to the maximum molar content of SiO2 in the doped transition layer. The molar content of Al(NO3)3 in the doped surface layer is greater than or equal to the maximum molar content of Al(NO3)3 in the doped transition layer; The minimum molar content of Co2O3 in the doped transition layer is greater than or equal to the molar content of Co2O3 in the doped core layer; The minimum molar content of MnO2 in the doped transition layer is greater than or equal to the molar content of MnO2 in the doped core layer; The molar content of Sb2O3 in the doped surface layer is less than or equal to the molar content of Sb2O3 in the doped core layer, and the molar content of Sb2O3 in the doped transition layer is greater than the minimum molar content of Sb2O3 in the doped surface layer and less than or equal to the maximum molar content of Sb2O3 in the doped core layer, so as to ensure the uniform transition of Sb2O3.

[0010] The zinc oxide resistive sheet provided by this invention has a gradient-doped layered structure, with continuous transitions between layers along the thickness direction and no obvious interfaces. This achieves functional zoning of "high potential gradient on the doped surface layer, large current-carrying capacity in the doped core layer, and smooth connection of the doped transition layers," avoiding the performance contradictions of uniform doping. It achieves a balance between optimized electric field distribution and energy dissipation, thereby comprehensively improving electrical performance. Specifically: The zinc oxide resistive chip provided by this invention has a gradient-doped layered structure, with targeted optimization of the doping formula for each layer. Specifically, the doped surface layer focuses on adding ZrO2 and Bi2O3 to enhance the potential gradient, while the doped core layer focuses on adding Co2O3, Ni2O3, and Ga2O3 to improve current carrying capacity and thermal stability. The doped transition layer achieves a linear gradient of doping components, and a flux is added to optimize the grain boundary structure and reduce porosity. Through the synergistic effect of the gradient structure and formula, the potential gradient and current carrying capacity are precisely adjustable, while simultaneously improving the nonlinear coefficient, reducing leakage current, improving heat distribution, and extending service life, thereby comprehensively improving electrical performance.

[0011] As a preferred embodiment of the present invention, the doped surface layer, in molar percentage, comprises: Zinc oxide matrix 94%-94.94%; Bi2O3 1.2%-1.5%; ZrO2 1.5%-2.0%; Sb₂O₃ 0.8%-1.2%; SiO2 1.0%-1.5%; Al(NO3) 30.06%-0.08%; Fluid content 0.5%.

[0012] The molar content of the zinc oxide matrix can be 94.1%, 94.2%, 94.4%, 94.6%, 94.8%, 94.9%, 94.94%, etc. When using ZnO as the matrix, it is necessary to ensure the stability of the main structure of the resistor sheet. The molar percentage must be controlled within the above range to ensure that the dopant functions effectively without compromising the basic electrical properties of ZnO.

[0013] The molar content of Bi2O3 can be 1.2%, 1.3%, 1.4%, 1.5%, etc.

[0014] The molar content of ZrO2 can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, etc.

[0015] The molar content of Sb2O3 can be 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, etc.

[0016] The molar content of SiO2 can be 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, etc.

[0017] The molar content of Al(NO3)3 can be 0.06%, 0.07%, 0.08%, etc.

[0018] This invention focuses on enhancing the potential gradient of the resistive sheet through doping. The synergistic effect of ZrO2 and Bi2O3 can significantly improve the voltage withstand capability of the resistive sheet per unit thickness. SiO2 can inhibit grain growth, increase the number of grain boundaries, and further enhance the potential gradient. At the same time, Al(NO3)3 can optimize the grain boundary barrier, improve the nonlinear coefficient, and ensure that the doped surface has good overvoltage protection capability. The synergistic effect of each component makes the potential gradient reach 450-600V / mm.

[0019] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of Bi2O3 decreases from 1.2% to 0.9% along the direction from the doped surface layer to the doped core layer.

[0020] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of ZrO2 decreases from 1.5% to 0.8% along the direction from the doped surface layer to the doped core layer.

[0021] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of Sb2O3 increases from 1.0% to 1.5% along the direction from the doped surface layer to the doped core layer.

[0022] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of Co2O3 decreases from 1.0% to 0.7% along the direction from the doped surface layer to the doped core layer.

[0023] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of MnO2 decreases from 0.7% to 0.6% along the direction from the doped surface layer to the doped core layer.

[0024] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of SiO2 decreases from 1.0% to 0.5% along the direction from the doped surface layer to the doped core layer.

[0025] As a preferred embodiment of the present invention, in the doped transition layer, the molar content of Al(NO3)3 decreases from 0.06% to 0.05% along the direction from the doped surface layer to the doped core layer.

[0026] In a preferred embodiment of the present invention, the molar content of the flux in the doped transition layer is 0.5%.

[0027] The core function of the doped transition layer in this invention is to alleviate the performance difference between the doped surface layer and the doped core layer, avoid stress concentration caused by sudden performance changes, achieve a smooth transition of potential gradient and current carrying capacity, reduce local electric field distortion under large current impact, reduce leakage current, and thus improve the overall stability of the resistor.

[0028] As a preferred embodiment of the present invention, the doped core layer comprises, in molar percentage, the following: Zinc oxide matrix 94%-95.4%; Bi2O3 0.8%-0.9%; ZrO2 0.1%-0.8%; Sb₂O₃ 1.2%-1.5%; Co2O3 0.5%-0.7%; MnO2 0.5%-0.6%; Ni2O3 0.4%-0.6%; B2O3 0.2%-0.4%; Ga2O3 0.4%-0.825%; Fluid content 0.5%.

[0029] The molar content of the zinc oxide matrix can be 94%, 94.2%, 94.5%, 94.8%, 95%, 95.2%, 95.4%, etc. When using ZnO as the matrix, it is necessary to ensure the stability of the main structure of the resistor sheet. The molar percentage must be controlled within the above range to ensure that the dopant can fully function without damaging the basic electrical properties of ZnO.

[0030] The molar content of Bi2O3 can be 0.8%, 0.82%, 0.84%, 0.86%, 0.88%, 0.9%, etc.

[0031] The molar content of ZrO2 can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, etc.

[0032] The molar content of Sb2O3 can be 1.2%, 1.3%, 1.4%, 1.5%, etc.

[0033] The molar content of Co2O3 can be 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, etc.

[0034] The molar content of MnO2 can be 0.5%, 0.52%, 0.54%, 0.56%, 0.58%, 0.6%, etc.

[0035] The molar content of Ni2O3 can be 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, etc.

[0036] The molar content of B2O3 can be 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, etc.

[0037] The molar content of Ga2O3 can be 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.825%, etc.

[0038] The core function of the doped core layer in this invention is to enhance the current-carrying capacity and thermal stability of the resistor. Co2O3 and MnO2 synergistically optimize the grain boundary conductivity, while Ni2O3 and Ga2O3 can improve the energy absorption capacity under high current impact and reduce heat accumulation. The low content of ZrO2 can avoid an excessively high potential gradient in the core layer, ensuring smooth conduction of high current. The synergistic effect of the components can achieve a current density of 50-65 A / cm² for a 2ms square wave. 2 It also has good aging resistance.

[0039] The effects of dopant selection and content gradient changes in the doped core layer, doped transition layer, and doped surface layer are as follows: (1) Zinc oxide matrix, as the base material of the resistor sheet, constitutes the main structure of the resistor sheet and is the basis for realizing electrical performance (potential gradient, current carrying capacity), providing basic conductivity and nonlinear characteristics.

[0040] (2) Add relevant doping components to enhance the potential gradient (focus on adding to the doped surface). Bi2O3: It works synergistically with ZrO2 to significantly improve the voltage withstand capability of resistive sheets per unit thickness and optimize the grain boundary barrier. It is the core dopant for enhancing the potential gradient. The doping content is highest in the surface layer, gradually changes in the doping transition layer, and lowest in the doping core layer, which is suitable for gradient performance requirements.

[0041] ZrO2: It inhibits excessive growth of ZnO grains, increases the number of grain boundaries, further enhances the potential gradient, and strengthens the mechanical strength of the resistor sheet. The doped surface layer has the highest content, and the doped core layer has the lowest content, which perfectly matches the gradient distribution of the potential gradient.

[0042] SiO2: It helps to inhibit grain growth, refine grain boundary structure, improve the stability of potential gradient, and reduce porosity. The content of doped surface layer is higher than that of doped transition layer, and no doped core layer is added, which meets the functional requirements of high potential gradient of doped surface layer.

[0043] (3) Dopants that improve current flow capacity and thermal stability (emphasis on adding to the doped core layer) Co2O3: Optimizes grain boundary conductivity, enhances energy absorption under high current impact, reduces heat accumulation, and strengthens thermal stability; the doped core layer content is 0.5-0.7%, the doped transition layer gradually changes from 0.7% to 1.0%, and no doping is added to the surface layer, which is suitable for the high current carrying capacity of the core layer.

[0044] MnO2: works synergistically with Co2O3 to further optimize grain boundary conductivity, reduce leakage current, and improve thermal stability; the doped core layer content is 0.5-0.6%, the doped transition layer gradually changes from 0.6% to 0.7%, and no doped surface layer is added.

[0045] Ni2O3: Improves the current carrying capacity and aging resistance of the resistor sheet, and enhances the structural stability under high current impact. It is added only to the doped core layer.

[0046] Ga2O3: Helps improve current flow capacity, optimizes heat conduction efficiency of doped core layer, reduces hot spot formation, and is added only to doped core layer.

[0047] B2O3: Refines the grain size of the doped core layer, reduces porosity, improves the density of the doped core layer structure, and indirectly enhances the flow capacity and thermal stability. It is added only to the doped core layer.

[0048] (4) Optimize grain boundary and nonlinear property related dopants (adapted to each layer) Sb2O3: Optimizes the ZnO grain boundary structure, improves the nonlinear coefficient of the resistor (α≥35), and enhances structural stability; the doped core layer has the highest content (1.2%-1.5%), the doped transition layer gradually changes from 1.5% to 1.0%, and the doped surface layer has the lowest content (0.8%-1.2%), which matches the gradient distribution of current carrying capacity.

[0049] Al(NO3)3: Optimizes grain boundary barrier, further improves nonlinear coefficient, and reduces leakage current (≤50μA); doped surface layer (0.06%-0.08%), doped transition layer gradually changes from 0.06% to 0.05%, doped core layer is not added, which meets the overvoltage protection requirements of the surface layer.

[0050] As a preferred embodiment of the present invention, the flux is a mixture of TiO2 and Cu(NO3)2 in a mass ratio of 1:1.

[0051] The flux provided by this invention can lower the sintering temperature (achieving low-temperature sintering of 1100-1125℃), promote uniform diffusion of various doped components, optimize grain boundary bonding, reduce porosity (≤1.5%), and at the same time avoid oxidation of raw materials during sintering, ensuring the continuity of the gradient structure (no obvious interface between layers).

[0052] As a preferred embodiment of the present invention, the thickness of the doped surface layer is 0.5-2 mm, for example, 0.5 mm, 1 mm, 1.5 mm, 2 mm, etc.

[0053] As a preferred embodiment of the present invention, the thickness of the doped transition layer is 1-3 mm, for example, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, etc.

[0054] As a preferred embodiment of the present invention, the thickness of the doped core layer is 2-5 mm, for example, 2 mm, 3 mm, 4 mm, 5 mm, etc.

[0055] In a second aspect, the present invention provides a method for preparing the zinc oxide resistor sheet described in the first aspect, the method comprising the following steps: (1) Add the raw materials for the preparation of the doped core layer and the doped surface layer to water and mix them to obtain the doped core layer slurry and the doped surface layer slurry; add the raw materials for the preparation of the doped transition layer to water and mix them to obtain at least three kinds of doped transition layer slurries containing different molar concentrations of transition layer doping components; centrifuge and granulate each slurry and dry them to obtain each group of powders. (2) The powders of each group are laid in the mold in the order of doped core layer, doped transition layer and doped surface layer. The molar content of Bi2O3, ZrO2, Co2O3, MnO2, SiO2 and Al(NO3)3 in the doped transition layer decreases in gradient from the doped surface layer to the doped core layer, and the molar content of Sb2O3 increases in gradient from the doped surface layer to the doped core layer. Vibration makes the interlayer transition natural, and pressing and densifying are used to obtain a green blank. Sintering is then performed to obtain the zinc oxide resistor sheet.

[0056] The preparation method provided by this invention is adapted to the gradient doped layered structure of zinc oxide resistor sheets. It adopts a layered material laying + double-sided pressing + sintering process to ensure tight interlayer bonding and uniform density. This results in zinc oxide resistor sheets with no obvious interfaces and an integral molded structure, which takes into account both molding precision and industrial mass production requirements.

[0057] As a preferred technical solution of the present invention, the mixing method in step (1) is sand milling, the sand milling rate is 1500 r / min, and the sand milling time is 2.5-3 h, for example 2.5 h, 2.6 h, 2.8 h, 3 h, etc.

[0058] As a preferred embodiment of the present invention, the rotation speed during centrifugal granulation is 1000 r / min, and the temperature during centrifugal granulation is 150-160℃, such as 150℃, 152℃, 154℃, 156℃, 158℃, 160℃, etc.

[0059] As a preferred embodiment of the present invention, the drying temperature is 110-115℃, such as 110℃, 111℃, 112℃, 113℃, 114℃, 115℃, etc.; the drying time is 5-6 h, such as 5 h, 5.2 h, 5.4 h, 5.6 h, 5.8 h, 6 h, etc.

[0060] As a preferred embodiment of the present invention, the particle size of the powder is 30-50 μm, such as 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.

[0061] As a preferred technical solution of the present invention, the vibration in step (2) is a vibration at 55Hz for 12-15 minutes, such as 12 minutes, 13 minutes, 14 minutes, 15 minutes, etc.

[0062] As a preferred embodiment of the present invention, the pressing pressure is 9 MPa, and the pressure holding time is 18-20 min.

[0063] As a preferred embodiment of the present invention, the sintering is carried out in an inert gas atmosphere. The sintering method is to raise the temperature to 420°C at 6°C / min, hold for 2.5 h to remove the binder, and then raise the temperature to 1110°C at 4°C / min and hold for 6 h.

[0064] As a preferred embodiment of the present invention, the sintering process is followed by post-processing, which involves polishing until the thickness error is ±0.1 mm.

[0065] Thirdly, the present invention provides the application of the zinc oxide resistive sheet described in the first aspect or the zinc oxide resistive sheet prepared by the preparation method described in the second aspect in lightning protection equipment or overvoltage protection equipment for power systems and electronic equipment.

[0066] The technical solution provided by the embodiments of the present invention has the following advantages compared with the prior art: The zinc oxide resistor sheet provided by this invention has a gradient doped layered structure, which creates a gradient change in the concentration and type of additives in the thickness direction of the resistor sheet, thereby achieving a balance between optimized electric field distribution and energy dissipation, and thus comprehensively improving electrical performance. Attached Figure Description

[0067] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0068] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0069] Figure 1 This is a schematic diagram of the structure of the zinc oxide resistor sheet described in Embodiment 1 of the present invention. Detailed Implementation

[0070] To better understand the above-mentioned objectives, features, and advantages of the present invention, the solutions of the present invention will be further described below. It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other.

[0071] Many specific details are set forth in the following description in order to provide a full understanding of the invention, but the invention may also be practiced in other ways different from those described herein; obviously, the embodiments in the specification are only some embodiments of the invention, and not all embodiments.

[0072] Example 1 This embodiment provides a zinc oxide resistor sheet and its preparation method. A schematic diagram of the zinc oxide resistor sheet structure is shown below. Figure 1 As shown, it includes a doped core layer (1 mm), a doped transition layer (2 mm), and a doped surface layer (3.5 mm). The doped transition layer is located on both sides of the doped core layer, and the doped surface layer is located on both sides of the doped transition layer away from the doped core layer. The doped surface layer, by molar percentage, comprises: ZnO 94.12%, Bi₂O₃ 1.5%, ZrO₂ 2.0%, Sb₂O₃ 0.8%, SiO₂ 1.0%, Al(NO₃)₃ 0.08%, and flux (a mixture of TiO₂ and Cu(NO₃)₂ in a 1:1 mass ratio) 0.5%. In the doped transition layer, the molar content of ZnO increases from 93.04% to 94.45% along the direction from the doped surface layer to the doped core layer; The molar content of Bi2O3 decreased from 1.2% to 0.9% along the direction from the doped surface layer to the doped core layer; the molar content of ZrO2 decreased from 1.5% to 0.8% along the direction from the doped surface layer to the doped core layer; the molar content of Sb2O3 increased from 1.0% to 1.5% along the direction from the doped surface layer to the doped core layer; the molar content of Co2O3 decreased from 1.0% to 0.7% along the direction from the doped surface layer to the doped core layer; the molar content of MnO2 decreased from 0.7% to 0.6% along the direction from the doped surface layer to the doped core layer; the molar content of SiO2 decreased from 1.0% to 0.5% along the direction from the doped surface layer to the doped core layer; the molar content of Al(NO3)3 decreased from 0.06% to 0.05% along the direction from the doped surface layer to the doped core layer; and the molar content of flux (a mixture of TiO2 and Cu(NO3)2 in a mass ratio of 1:1) was 0.5%. The doped core layer, by molar percentage, comprises: ZnO 94.7%, Bi₂O₃ 0.8%, ZrO₂ 0.8%, Sb₂O₃ 1.2%, Co₂O₃ 0.5%, MnO₂ 0.5%, Ni₂O₃ 0.4%, B₂O₃ 0.2%, Ga₂O₃ 0.4%, and flux (a mixture of TiO₂ and Cu(NO₃)₂ in a 1:1 mass ratio) 0.5%. The preparation method includes the following steps: (1) Raw material pretreatment: ZnO powder with a purity of 99.9% and various dopants and fluxes were selected and weighed according to the formula of this embodiment. Deionized water was added to each group (solid-liquid ratio 1:1.3), and the mixture was sand-milled at a speed of 1500 r / min for 2.5 h to obtain each layer of slurry. Each layer of slurry was centrifuged and granulated at 150℃ and a centrifugal pump speed of 1000 r / min to obtain powder balls of 30-50 μm. The granules were dried at 110℃ for 5 h for later use. Among them, 5 groups of doped transition layer powder balls were prepared, and the specific formula composition is shown in Table 1. Table 1

[0073] (2) Gradient molding: The doped core layer powder spheres, the doped transition layer powder spheres (group 1, group 2, group 3, group 4, group 5 in the direction from the doped surface layer to the doped core layer) and the doped surface layer powder spheres are sequentially laid in the mold and vibrated at 55 Hz for 12 min to ensure a natural transition between layers.

[0074] (3) Pressing and densification: Adjust the powder moisture content to 1.5%, apply a pressing pressure of 9 MPa, and hold for 18 min to obtain a green body with a density of 3.24 g / cm³. 3 .

[0075] (4) Sintering: Heat to 420℃ at 6℃ / min, hold for 2.5h to remove the binder; then heat to 1110℃ at 4℃ / min, hold for 6h to sinter, and introduce nitrogen gas for protection (pressure 0.12MPa); cool to room temperature at 2.5℃ / min.

[0076] (5) Post-processing: Grind and polish until the thickness error is ±0.1mm to obtain the zinc oxide resistor sheet.

[0077] Example 2 This embodiment provides a zinc oxide resistor sheet and its preparation method. The zinc oxide resistor sheet is the same as that in Embodiment 1, except that in this embodiment: The doped surface layer comprises: ZnO 93.875%, Bi2O3 1.2%, ZrO2 1.5%, Sb2O3 1.2%, SiO2 1.5%, Al(NO3)3 0.06%, and flux 0.5%. The doped core layer consists of: 94% ZnO, 0.9% Bi2O3, 0.1% ZrO2, 1.5% Sb2O3, 0.7% Co2O3, 0.6% MnO2, 0.6% Ni2O3, 0.4% B2O3, 0.7% Ga2O3, and 0.5% flux.

[0078] The preparation method is the same as in Example 1.

[0079] Example 3 This embodiment provides a zinc oxide resistor sheet and its preparation method. The zinc oxide resistor sheet is the same as that in Embodiment 1, except that in this embodiment: The doped surface layer comprises: ZnO 94.03%, Bi2O3 1.4%, ZrO2 1.7%, Sb2O3 1%, SiO2 1.3%, Al(NO3)3 0.07%, and flux 0.5%. The doped core layer consists of: ZnO 94.075%, Bi2O3 0.85%, ZrO2 0.5%, Sb2O3 1.3%, Co2O3 0.6%, MnO2 0.55%, Ni2O3 0.5%, B2O3 0.3%, Ga2O3 0.825%, and flux 0.5%.

[0080] The preparation method is the same as in Example 1.

[0081] Comparative Example 1 This comparative example provides a zinc oxide resistor sheet and its preparation method. The zinc oxide resistor sheet comprises: 93.745% ZnO, 1.05% Bi2O3, 1.15% ZrO2, 1.25% Sb2O3, 0.85% Co2O3, 0.65% MnO2, 0.75% Ni2O3, 0.055% Al(NO3)3, and 0.5% flux.

[0082] The preparation method includes: (1) Raw material pretreatment: Select ZnO powder with a purity of 99.9% and various dopants and fluxes, weigh them in groups according to the formula of this embodiment, add deionized water to each group (solid-liquid ratio 1:1.3), and grind at 1500r / min for 2.5 h to obtain slurry. Centrifuge the slurry at 150℃ and centrifugal pump speed of 1000r / min to obtain powder balls of 30-50 μm, and dry at 110℃ for 5 h for later use.

[0083] (2) Molding: The uniformly doped powder balls are laid in the mold and vibrated at 55 Hz for 12 min.

[0084] (3) Pressing and densification: Adjust the powder moisture content to 1.5%, apply a pressing pressure of 9 MPa, and hold for 18 min to obtain a green body with a density of 3.24 g / cm³. 3 .

[0085] (4) Sintering: Heat to 420℃ at 6℃ / min, hold for 2.5h to remove the binder; then heat to 1110℃ at 4℃ / min, hold for 6h to sinter, and introduce nitrogen gas for protection (pressure 0.12MPa); cool to room temperature at 2.5℃ / min.

[0086] (5) Post-processing: Grind and polish until the thickness error is ±0.1mm to obtain the zinc oxide resistor sheet.

[0087] Performance testing Homogeneous zinc oxide samples were prepared using the same formulation and sintering process as the zinc oxide resistive sheet doped surface provided in the examples and comparative examples. Silver electrodes (edge ​​thickness 8 μm) were prepared on both sides of the samples, and then they were tested and screened.

[0088] 1. Surface potential gradient (1) Test method A 1mA DC reference current was applied at 25℃ to test the varistor voltage U of the sample. 1mA Surface potential gradient E s =U 1mA / h, where h is the sample thickness. Five samples were used in each group, and the arithmetic mean was taken.

[0089] (2) Calculation formula Based on the synergistic enhancement effect of Bi2O3 and ZrO2, the grain refinement effect of SiO2, and the grain boundary optimization effect of Al(NO3)3, combined with the reference potential gradient of the ZnO matrix, the surface potential gradient is derived as follows:

[0090] : Potential gradient of doped surface (V / mm), the range of which is defined in this invention is 450-600V / mm, and the calculation result must fall within this range; Mole percentage (%) of Bi2O3 in the doped surface layer, ranging from 1.2% to 1.5%; Mole percentage (%) of doped ZrO2 on the surface, ranging from 1.5% to 2.0%; Mole percentage (%) of doped surface SiO2, ranging from 1.0% to 1.5%; Mole percentage (%) of Al(NO3)3 in the surface doped region, ranging from 0.06% to 0.08%; The synergy coefficient, determined experimentally, ranges from 120 to 130. : Optimization coefficient, determined experimentally, with a value of 800-850; The reference potential gradient of the ZnO matrix (V / mm) is 180-200 (the base potential gradient of the pure ZnO matrix, which is measured experimentally).

[0091] (3) Test results Table 2

[0092] As can be seen from Table 2, the surface potential gradient of the zinc oxide resistive sheet prepared in the embodiments of the present invention is significantly higher than that of the comparative example.

[0093] 2. Square wave current density in the doped core layer (1) Test method Homogeneous samples were prepared using the same formulation as the zinc oxide resistive sheet doped core layer provided in the examples and comparative examples, and the effective conductive area S of the electrodes was measured. A progressive impact test was conducted using a 2 ms square wave impulse current generator, with an impact interval of 60 s. The maximum withstand current I was determined based on the varistor voltage change ≤5% and the absence of cracking or breakdown after the impact. max Core layer square wave current density J c =I max / S.

[0094] (2) Calculation formula Based on the synergistic conductivity of Co2O3 and MnO2, the energy absorption of Ni2O3 and Ga2O3, and after deducting the inhibitory effect of ZrO2 on current flow, the core current flow density is derived by combining the reference current flow density of the ZnO matrix:

[0095] : 2 ms square wave current density of the doped core layer (A / cm) 2 The present invention limits the range to 50-65 A / cm², and the calculation results must fall within this range; Mole percentage (%) of Co2O3 in the doped core layer, ranging from 0.5% to 0.7%; Mole percentage (%) of MnO2 in the doped core layer, ranging from 0.5% to 0.6%; Mole percentage (%) of Ni2O3 in the doped core layer, ranging from 0.4% to 0.6%; Mole percentage (%) of Ga2O3 in the doped core layer, ranging from 0.4% to 0.825%; Mole percentage (%) of ZrO2 in the doped core layer, ranging from 0.1% to 0.8%; The cooperative conductivity coefficient, determined experimentally, ranges from 45 to 50. Energy absorption coefficient, determined experimentally, with a value of 35-40; Inhibition coefficient, determined experimentally, with a value of 10-15; The reference flux density (A / cm²) of the ZnO matrix is ​​25-30 (the basic flux capacity of the pure ZnO matrix, which is measured experimentally).

[0096] (3) Test results Table 3

[0097] As can be seen from Table 3, the core layer square wave current density of the zinc oxide resistor prepared in the embodiments of the present invention is significantly higher than that of the comparative example.

[0098] In summary, the zinc oxide resistive sheet provided by this invention has a gradient doped layered structure, which can achieve functional partitioning of "high potential gradient of the doped surface layer, large current carrying capacity of the doped core layer, and smooth connection of the doped transition layer", avoiding the performance contradiction of uniform doping, realizing the balance of optimized electric field distribution and energy dissipation, thereby comprehensively improving electrical performance.

[0099] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0100] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments described herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A zinc oxide resistor, characterized in that, The zinc oxide resistor sheet includes a doped core layer, a doped transition layer, and a doped surface layer; The doped transition layer is located on at least one side surface of the doped core layer, and the doped surface layer is located on the side surface of the doped transition layer away from the doped core layer; The doped surface layer includes a zinc oxide matrix and a flux and surface doping components distributed in the zinc oxide matrix. The surface doping components include Bi2O3, ZrO2, Sb2O3, SiO2 and Al(NO3)3. The doped transition layer includes a zinc oxide matrix and a flux and transition layer doping components distributed in the zinc oxide matrix. The transition layer doping components include Bi2O3, ZrO2, Sb2O3, Co2O3, MnO2, SiO2, and Al(NO3)3. The molar content of Bi2O3, ZrO2, Co2O3, MnO2, SiO2, and Al(NO3)3 in the doped transition layer decreases gradually from the doped surface layer to the doped core layer, while the molar content of Sb2O3 increases gradually from the doped surface layer to the doped core layer. The doped core layer includes a zinc oxide matrix and a flux and core layer doping components distributed in the zinc oxide matrix. The core layer doping components include Bi2O3, ZrO2, Sb2O3, Co2O3, MnO2, Ni2O3, B2O3 and Ga2O3. The molar content of Bi2O3 in the doped surface layer is greater than or equal to the maximum molar content of Bi2O3 in the doped transition layer, and the minimum molar content of Bi2O3 in the doped transition layer is greater than or equal to the molar content of Bi2O3 in the doped core layer. The molar content of ZrO2 in the doped surface layer is greater than or equal to the maximum molar content of ZrO2 in the doped transition layer, and the minimum molar content of ZrO2 in the doped transition layer is greater than or equal to the molar content of ZrO2 in the doped core layer. The molar content of SiO2 in the doped surface layer is greater than or equal to the maximum molar content of SiO2 in the doped transition layer. The molar content of Al(NO3)3 in the doped surface layer is greater than or equal to the maximum molar content of Al(NO3)3 in the doped transition layer; The minimum molar content of Co2O3 in the doped transition layer is greater than or equal to the molar content of Co2O3 in the doped core layer; The minimum molar content of MnO2 in the doped transition layer is greater than or equal to the molar content of MnO2 in the doped core layer; The molar content of Sb2O3 in the doped surface layer is less than or equal to the molar content of Sb2O3 in the doped core layer.

2. The zinc oxide resistor sheet according to claim 1, characterized in that, The doped surface layer, in molar percentage, comprises: Zinc oxide matrix 94%-94.94%; Bi2O3 1.2%-1.5%; ZrO2 1.5%-2.0%; Sb₂O₃ 0.8%-1.2%; SiO2 1.0%-1.5%; Al(NO3) 30.06%-0.08%; Fluid content 0.5%.

3. The zinc oxide resistor sheet according to claim 1 or 2, characterized in that, In the doped transition layer, the molar content of Bi2O3 decreases from 1.2% to 0.9% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of ZrO2 decreases from 1.5% to 0.8% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of Sb2O3 increases from 1.0% to 1.5% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of Co2O3 decreases from 1.0% to 0.7% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of MnO2 decreases from 0.7% to 0.6% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of SiO2 decreases from 1.0% to 0.5% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of Al(NO3)3 decreases from 0.06% to 0.05% along the direction from the doped surface layer to the doped core layer; And / or, in the doped transition layer, the molar content of the flux is 0.5%.

4. The zinc oxide resistor sheet according to any one of claims 1-3, characterized in that, The doped core layer comprises, in molar percentage, the following: Zinc oxide matrix 94%-95.4%; Bi2O3 0.8%-0.9%; ZrO2 0.1%-0.8%; Sb₂O₃ 1.2%-1.5%; Co2O3 0.5%-0.7%; MnO2 0.5%-0.6%; Ni2O3 0.4%-0.6%; B2O3 0.2%-0.4%; Ga2O3 0.4%-0.825%; Fluid content 0.5%.

5. The zinc oxide resistor sheet according to any one of claims 1-4, characterized in that, The flux is a mixture of TiO2 and Cu(NO3)2 in a mass ratio of 1:

1.

6. The zinc oxide resistor sheet according to any one of claims 1-5, characterized in that, The thickness of the doped surface layer is 0.5-2 mm; And / or, the thickness of the doped transition layer is 1-3 mm; And / or, the thickness of the doped core layer is 2-5 mm.

7. The method for preparing zinc oxide resistors according to any one of claims 1-6, characterized in that, The preparation method includes the following steps: (1) Add the raw materials for the preparation of the doped core layer and the doped surface layer to water and mix them to obtain the doped core layer slurry and the doped surface layer slurry; add the raw materials for the preparation of the doped transition layer to water and mix them to obtain at least three kinds of doped transition layer slurries containing different molar concentrations of transition layer doping components; centrifuge and granulate each slurry and dry them to obtain each group of powders. (2) The powders of each group are laid in the mold in the order of doped core layer, doped transition layer and doped surface layer. The molar content of Bi2O3, ZrO2, Co2O3, MnO2, SiO2 and Al(NO3)3 in the doped transition layer decreases in gradient from the doped surface layer to the doped core layer, and the molar content of Sb2O3 increases in gradient from the doped surface layer to the doped core layer. Vibration makes the interlayer transition natural, and pressing and densifying are used to obtain a green blank. Sintering is then performed to obtain the zinc oxide resistor sheet.

8. The preparation method according to claim 7, characterized in that, The mixing method described in step (1) is sand milling, with a milling rate of 1500 r / min and a milling time of 2.5-3 h; And / or, the centrifugal granulation speed is 1000 r / min, and the centrifugal granulation temperature is 150-160℃; And / or, the drying temperature is 110-115℃, and the drying time is 5-6 h; And / or, the particle size of the powder is 30-50 μm.

9. The preparation method according to claim 7 or 8, characterized in that, The vibration described in step (2) is a vibration at 55 Hz for 12-15 min; And / or, the crimping pressure is 9 MPa, and the pressure is held for 18-20 min; And / or, the sintering is carried out in an inert gas atmosphere, and the sintering method is to raise the temperature to 420°C at 6°C / min, hold for 2.5h to remove the binder; then raise the temperature to 1110°C at 4°C / min and hold for 6h.

10. The application of the zinc oxide resistor sheet according to any one of claims 1-6 or the zinc oxide resistor sheet prepared by the preparation method according to any one of claims 7-9 in lightning protection equipment or overvoltage protection equipment for power systems and electronic equipment.