A sodium-ion battery positive electrode material and a preparation method and application thereof
By spontaneously forming an entropy-stable amorphous coating on the surface of the cathode material of sodium-ion batteries, the problem of poor stability of layered oxides in air and moisture is solved, achieving excellent water resistance and air stability, making it suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202611447696.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-20
AI Technical Summary
Existing layered transition metal oxide sodium-ion battery cathode materials exhibit poor stability in air and moisture, leading to loss of active sodium, capacity decay, and battery safety risks. Existing strategies such as surface coating and element doping have limited effectiveness.
An entropy-stable amorphous coating is spontaneously formed on the material surface using an entropy engineering strategy, which acts as a kinetic barrier to increase the activation energy of harmful side reactions, thus preparing a core-shell structured sodium-ion battery cathode material.
It significantly improves the material's water resistance and air stability while maintaining its electrochemical performance and safety, making it suitable for large-scale industrial production.
Smart Images

Figure CN123143373A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery cathode material technology, specifically to a sodium-ion battery cathode material, its preparation method, and its application. Background Technology
[0002] Sodium-ion batteries (SIBs) are considered strong candidates for next-generation large-scale energy storage systems due to the abundance and low cost of sodium resources. Layered transition metal oxides are currently a research hotspot for cathode materials in sodium-ion batteries; however, these materials generally suffer from poor stability in air and moisture. Sodium ions readily react with H2O, O2, and CO2 in the air on the surface of the cathode material, forming surface passivation layers such as NaOH, Na2CO3, and NaHCO3, leading to loss of active sodium and rapid capacity decay. Simultaneously, the high impedance of the surface passivation layer increases interfacial impedance and voltage polarization, affecting the battery's rate performance. Furthermore, the decomposition of Na2CO3 and NaHCO3 in the passivation layer during cycling produces CO2 and CO gases, increasing the risk of battery explosion. Residual moisture can also cause the polyvinylidene fluoride (PVDF) binder to gel, losing its adhesive strength.
[0003] To improve the air and moisture stability of layered oxide cathode materials, existing technologies mainly employ two strategies: surface coating and elemental doping. Surface coating (such as metal oxides, metal phosphides, carbon materials, etc.) inhibits degradation by preventing direct contact between the cathode material and air / water. However, coating strategies typically involve complex fabrication processes, and lattice mismatch between the coating material and the substrate can lead to performance degradation. Elemental doping (such as Cu, Ti, Sn, F, etc.) suppresses sodium ion extraction from the cathode material and subsequent reactions with air components by reducing interlayer spacing and enhancing Na-O bond binding energy. However, the doping strategy has limited effect on improving stability.
[0004] Therefore, developing an intrinsic and efficient strategy that can simultaneously impart excellent water resistance and air stability to layered oxide cathode materials remains a pressing technical challenge in this field. Summary of the Invention
[0005] This invention addresses the shortcomings of existing technologies by providing a sodium-ion battery cathode material, its preparation method, and its application. Through an entropy engineering strategy, an entropy-stable amorphous coating is spontaneously formed on the material surface. This coating acts as a kinetic barrier, significantly increasing the activation energy of harmful side reactions, thereby achieving excellent water resistance and air stability.
[0006] To address the aforementioned technical problems, the first aspect of this invention provides a sodium-ion battery cathode material with the chemical formula Na. a Mg x Zn y Cu p Feq Mn r O2; where 0.7 ≤ a ≤ 0.9, 0.05 ≤ x ≤ 0.2, 0.05 ≤ y ≤ 0.2, 0.05 ≤ p ≤ 0.2, 0.05 ≤ q ≤ 0.2, 0.4 ≤ r ≤ 0.7, and x + y + p + q + r = 1; The sodium-ion battery cathode material has a core-shell structure, wherein the core is a P2-type layered crystal with a space group of P63 / mmc, and the outer shell is an amorphous coating.
[0007] Furthermore, the chemical formula of the sodium-ion battery cathode material is Na. 0.8 Mg 0.1 Zn 0.1 Cu 0.1 Fe 0.1 Mn 0.6 O2.
[0008] Furthermore, the amorphous coating is an entropy-stable amorphous oxide coating with a formation energy of 0.16 eV; The thickness of the amorphous coating is 5-15 nm.
[0009] Furthermore, in the outer shell, the content of Na and O gradually decreases from the surface inwards, while the content of Mg, Zn, Cu, Fe, and Mn gradually increases, and the valence state of Mn changes from that of Mn on the surface. 4+ Mn gradually transitions to near-surface Mn 3+ ; In the core, the elements Na, Mg, Zn, Cu, Fe, and Mn are evenly distributed.
[0010] A second aspect of the present invention provides a method for preparing the sodium-ion battery cathode material described in the first aspect, comprising the following steps: S1. Weigh out sodium, magnesium, zinc, copper, iron, and manganese sources according to the stoichiometric ratio, mix and ball-mill to obtain a primary mixed powder; wherein, the sodium source is in excess by 1.5-2.5 mol%; S2. The primary mixed powder is pressed into shape and calcined at high temperature in air atmosphere, and then naturally cooled to room temperature to obtain the sodium-ion battery cathode material.
[0011] Furthermore, the heating rate of the calcination treatment is 3-5℃ / min, the temperature is 800-900℃, and the time is 15-25h.
[0012] Furthermore, the sodium source is selected from at least one of Na2CO3, NaHCO3, NaOH, and Na2O; the magnesium source is selected from at least one of MgO and MgCO3; the zinc source is selected from at least one of ZnO and ZnCO3; the copper source is selected from at least one of CuO and CuCO3; the iron source is selected from at least one of Fe2O3 and Fe3O4; and the manganese source is selected from at least one of Mn2O3, MnO2, and MnCO3.
[0013] Furthermore, the ball milling process is carried out at a speed of 400-500 rpm for 6-10 hours. The pressure for compression molding is 5-15 kPa.
[0014] A third aspect of the present invention provides a positive electrode sheet for a sodium-ion battery, comprising the sodium-ion battery positive electrode material described in the first aspect.
[0015] A fourth aspect of the present invention provides a sodium-ion battery, comprising the positive electrode sheet described in the third aspect.
[0016] The beneficial effects of this invention are: This invention reduces the formation energy of amorphous products to 0.16 eV by using a high entropy composition ratio, making surface amorphization thermodynamically highly favorable. Combined with a natural cooling process, the difference in cooling rate between the surface and the bulk phase is utilized to kinetically freeze surface atoms in a disordered state, thereby spontaneously forming an entropy-stable amorphous coating.
[0017] The amorphous coating of this invention acts as a kinetic barrier, significantly improving the activation energy of the harmful H2O / O2 side reaction, and exhibits excellent water resistance and air stability. Example results show that the cathode material retains its structural integrity after immersion in water for 90 days, and no characteristic peaks of hydrated phase or Na2CO3 appear in the XRD pattern; while the comparative low-entropy material (Na... 0.8 Mg 0.2 Mn 0.8 After soaking in water for 7 days, O2 showed obvious hydration phase and Na2CO3, and after soaking for 30 days, the layered structure basically collapsed.
[0018] The cathode material of this invention exhibits an initial reversible capacity of 90 mAh / g (0.1 C) after immersion in water for 90 days, almost indistinguishable from the unimmersed sample (92 mAh / g); after 100 cycles at a current density of 0.2 C, the capacity retention rate reaches 99%, demonstrating excellent electrochemical performance. In contrast, the comparative material exhibits an initial reversible capacity of only 45 mAh / g after immersion in water for 90 days, and a sudden decrease in capacity occurs during cycling.
[0019] The Na content of the cathode material of this invention remains basically unchanged after treatment in air and water, while the Na content of the comparative low-entropy material drops from 0.792 to 0.505 after soaking in water for 30 days, resulting in a serious loss of active sodium.
[0020] The amorphous surface coating of the cathode material of this invention effectively suppresses side reactions and improves safety: it prevents the formation of byproducts such as Na2CO3 and NaHCO3, avoids the decomposition of these byproducts during charging and discharging to produce CO2 and CO gas, reduces the risk of battery explosion, and improves battery safety.
[0021] The preparation process of this invention is simple and can be prepared by conventional solid-state sintering method. It does not require complicated coating or surface treatment processes, is compatible with existing sodium-ion battery cathode material production processes, and is suitable for large-scale industrial production. Attached Figure Description
[0022] To more clearly illustrate the technical solution of the present invention, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is the XRD pattern of the cathode material obtained in Example 1 of the present invention; Figure 2 These are TEM images of the cathode material obtained in Example 1 of the present invention; Figure 3 This is an EDS elemental distribution diagram of the cathode material obtained in Example 1 of the present invention; Figure 4 This is an XPS Na / O elemental depth profile of the cathode material obtained in Example 1 of the present invention; Figure 5 This is an XPS elemental depth profile of the cathode material obtained in Example 1 of this invention, showing the Mg / Cu / Mn / Zn / Fe elements. Figure 6 These are the XRD patterns of the cathode materials prepared in Example 1 and Comparative Example 1 of the present invention after being immersed in water for different times; Figure 7 These are SEM images of the cathode materials prepared in Example 1 and Comparative Example 1 of this invention after immersion in water for different times; Figure 8 This is a comparison of the first charge-discharge curves of the assembled batteries with positive electrode materials prepared in Example 1 and Comparative Example 1 of the present invention before and after immersion in water; Figure 9 This is a comparison chart of the cycle performance of the battery assembled with the positive electrode material prepared in Example 1 and Comparative Example 1 of the present invention before and after immersion in water; Figure 10 This is a comparison diagram of the GITT polarization potentials of the assembled batteries prepared with positive electrode materials in Example 1 and Comparative Example 1 of the present invention before and after immersion in water. Detailed Implementation
[0024] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] This embodiment relates to a sodium-ion battery cathode material with the chemical formula Na. a Mg x Zn y Cu p Fe q Mn r O2; wherein, 0.7 ≤ a ≤ 0.9, 0.05 ≤ x ≤ 0.2, 0.05 ≤ y ≤ 0.2, 0.05 ≤ p ≤ 0.2, 0.05 ≤ q ≤ 0.2, 0.4 ≤ r ≤ 0.7, and x + y + p + q + r = 1; the sodium-ion battery cathode material has a core-shell structure, wherein the core is a P2-type layered crystal with space group P63 / mmc, and the outer shell is an amorphous coating. Preferably, the chemical formula of the sodium-ion battery cathode material is Na. 0.8 Mg 0.1 Zn 0.1 Cu 0.1 Fe 0.1 Mn 0.6 O2; the amorphous coating is an entropy-stable amorphous oxide coating with a formation energy of 0.16 eV; the thickness of the amorphous coating is 5-15 nm.
[0026] In some embodiments, in the outer shell, the content of Na and O gradually decreases from the surface inwards, while the content of Mg, Zn, Cu, Fe, and Mn gradually increases, and the valence state of Mn changes from that of Mn on the surface. 4+ Mn gradually transitions to near-surface Mn 3+ In the core, the elements Na, Mg, Zn, Cu, Fe, and Mn are evenly distributed.
[0027] Another embodiment relates to a method for preparing the sodium-ion battery cathode material described in the above embodiments, comprising the following steps: S1. Weigh out sodium, magnesium, zinc, copper, iron, and manganese sources according to the stoichiometric ratio, mix and ball-mill to obtain a primary mixed powder; wherein, the sodium source is in excess by 1.5-2.5 mol%; S2. The primary mixed powder is pressed into shape and calcined at high temperature in air atmosphere, and then naturally cooled to room temperature to obtain the sodium-ion battery cathode material.
[0028] In some embodiments, the calcination treatment has a heating rate of 3-5℃ / min, a temperature of 800-900℃, and a time of 15-25h; the ball milling treatment has a rotation speed of 400-500rpm and a time of 6-10h; and the pressing pressure is 5-15kPa. In some embodiments, the sodium source is selected from at least one of Na2CO3, NaHCO3, NaOH, and Na2O; the magnesium source is selected from at least one of MgO and MgCO3; the zinc source is selected from at least one of ZnO and ZnCO3; the copper source is selected from at least one of CuO and CuCO3; the iron source is selected from at least one of Fe2O3 and Fe3O4; and the manganese source is selected from at least one of Mn2O3, MnO2, and MnCO3.
[0029] Another embodiment relates to a sodium-ion battery positive electrode sheet, comprising the sodium-ion battery positive electrode material described in the above embodiments.
[0030] Another embodiment relates to a sodium-ion battery, including the positive electrode sheet described in the above embodiments.
[0031] Example 1 This embodiment relates to a sodium-ion battery cathode material (HEO:Na) 0.8 Mg 0.1 Zn 0.1 Cu 0.1 Fe 0.1 Mn 0.6 The preparation method of O2 includes the following steps: (1) Weigh out Na2CO3 (Aladdin, 99.99%), MgO (Aladdin, 99.99%), ZnO (Aladdin, 99.99%), CuO (Aladdin, 99.99%), Fe2O3 (Aladdin, 99.99%) and Mn2O3 (Aladdin, 99.95%) according to the stoichiometric ratio of the positive electrode material chemical formula, wherein Na2CO3 is in excess by 2 mol% to compensate for the loss of sodium volatilization during high-temperature sintering.
[0032] (2) The above raw materials were placed in a high-energy ball mill and ball-milled at 450 rpm for 8 hours. The ball-milled mixed powder was pressed into shape under a pressure of 10 kPa, and then the blank was placed in a muffle furnace and heated to 850 ℃ at a heating rate of 4 ℃ / min in air atmosphere, held at the temperature for 20 hours, and then naturally cooled to room temperature to obtain HEO cathode material.
[0033] The XRD results of the obtained HEO cathode material are as follows: Figure 1 As shown, its crystal structure is a P2-type layered structure with space group P63 / mmc and lattice parameters a=b=2.900351 Å and c=11.211350 Å. TEM image ( Figure 2 The EDS elemental distribution map shows that the material surface has an amorphous coating with a thickness of approximately 10 nm. Figure 3 The results show that Na, Mg, Zn, Cu, Fe, and Mn are uniformly distributed within the particles. XPS depth profiling ( Figures 4-5 The data shows that in the amorphous coating, the Na and O content gradually decreases from the surface inwards, while the transition metal content gradually increases. The valence state of Mn changes from the surface Mn... 4+ Mn gradually transitions to near-surface Mn 3+ .
[0034] Comparative Example 1 This comparative example relates to a sodium-ion battery cathode material (NMMO: Na). 0.8 Mg 0.2 Mn 0.8 The preparation method of O2 involved weighing Na2CO3 (Aladdin, 99.99%), MgO (Aladdin, 99.99%), and Mn2O3 (Aladdin, 99.95%) according to their stoichiometric ratios, with Na2CO3 in excess at 2 mol% to compensate for sodium volatilization loss during high-temperature sintering. The NMMO cathode material was prepared using the same solid-state sintering process as in Example 1.
[0035] XRD results of the obtained NMMO cathode material showed that it also has a P2-type layered structure with space group P63 / mmc, but additionally, a Mg / Mn honeycomb ordered superlattice peak appeared at 20.5°. TEM images showed that there was no amorphous coating on the NMMO surface.
[0036] Comparative Example 2 The comparative example is the previously reported high-entropy layered oxide cathode material NaNi. 0.1 Mn 0.15 Co 0.2 Cu 0.1 Fe 0.1 Li 0.1 Ti 0.15 Sn 0.1 O2 and Na 0.95 Li 0.06 Ni 0.25 Cu 0.05 Fe 0.15 Mn 0.49 O2.
[0037] Application Example 1 The HEO positive electrode material obtained in Example 1 was mixed with acetylene black and PVDF binder at a mass ratio of 8:1:1. An appropriate amount of N-methylpyrrolidone (NMP) was added and ground to form a slurry. This slurry was coated onto aluminum foil, vacuum dried, and then cut into positive electrode sheets with a diameter of 12 mm. Using metallic sodium as the negative electrode, glass fiber as the separator, and a 1 M NaPF6 EC / DMC (volume ratio 1:1, containing 5% FEC) solution as the electrolyte, CR2032 coin cells were assembled in an argon-filled glove box.
[0038] Constant current charge-discharge tests were conducted within the voltage range of 2.0–4.3 V (vs. Na+ / Na). At a current density of 0.1 C, the first-cycle discharge specific capacity of HEO was 92 mAh / g; after 100 cycles at a current density of 0.2 C, the capacity retention rate was 99%.
[0039] Application Example 2 The HEO cathode material prepared in Example 1 was assembled into a full cell with a hard carbon (HC) anode. Preparation of the hard carbon anode: Hard carbon and sodium alginate (SA) binder were mixed at a mass ratio of 90:10, magnetically stirred to form a homogenate, and then coated onto aluminum foil. The mixture was vacuum dried overnight at 80°C. The electrolyte was a 1.0 M NaClO4 PC solution (containing 5 vol% FEC), and the separator was glass fiber. The anode / cathode (N / P) capacity ratio was 1.01.
[0040] Tested in the voltage range of 1.5 to 4.3 V, the full cell has a high initial reversible capacity at 0.1 C and a capacity retention rate of over 90% after 80 cycles at 1 C.
[0041] Test Example 1 1 g of the positive electrode material obtained in Example 1 and Comparative Example 1 was placed in a 30 mL centrifuge tube, filled with deionized water, stirred for 30 min, and then allowed to stand for 7 days, 30 days, and 90 days, respectively. After standing, the samples were removed and dried overnight in an oven at 100 °C. XRD test results showed ( Figure 6 HEO, after being soaked in water for 30 days, still showed no characteristic peaks of hydrated phase or Na2CO3, and the layered structure remained intact; NMMO, after being soaked in water for 7 days, showed characteristic peaks of hydrated phase (12.7°, 25.5°, 38.1°, 44.5°) and Na2CO3 (53.7°) in its XRD pattern; after 30 days of soaking, the (002) main peak almost disappeared, and the layered structure collapsed. SEM image ( Figure 7The results showed that HEO particles showed no cracks or byproducts on their surface after soaking in water for 30 days; NMMO particles showed obvious cracks. ICP-OES test results showed that the proportions of each element in HEO remained basically unchanged after soaking in water for 30 days (Na: 0.795, Mg: 0.088, Zn: 0.097, Cu: 0.094, Fe: 0.101, Mn: 0.62); while the Na content in NMMO decreased from 0.792 to 0.505 after soaking in water for 30 days.
[0042] The cathode material, after being soaked for 90 days, was used to prepare a battery according to the method in Application Example 1. The electrochemical test results of the cathode material before soaking (original sample) and after soaking for 90 days showed that... Figures 8-9 After being soaked in water for 90 days, HEO exhibited a reversible capacity of 90 mAh / g in the first week at 0.1 C, and a capacity retention rate of 99% after 100 cycles at 0.2 C, which was significantly better than the material reported in Comparative Example 2 (whose stability in humid air was only a few days (≤7 days)). In contrast, the cathode material NMMO in Comparative Example 1 had a reversible capacity of only 45 mAh / g in the first week at 0.1 C after being soaked in water for 90 days, and a sudden decrease in capacity occurred during cycling at 0.2 C.
[0043] Figure 10 This is a comparison of the GITT polarization potentials of the cathode materials prepared in Example 1 and Comparative Example 1 of this invention before and after immersion in water to assemble the battery. After immersion in water for 90 days (NMMO W-90), the polarization potential of Comparative Example 1 (NMMO) increased significantly compared to the original NMMO, indicating that a hydrated phase and byproducts such as Na2CO3 formed on the surface of NMMO during the water immersion process. These byproducts severely hindered the formation of Na2CO3 on the surface of NMMO. + The diffusion of water leads to a significant increase in interfacial impedance. However, after immersion in water for 90 days (HEO W-90), the polarization potential of the material in Example 1 of this invention only increased slightly compared to the original HEO, with very little difference. This further indicates that the amorphous coating on the HEO surface effectively inhibits the side reactions between water molecules and the matrix, maintaining good Na+ diffusion. + Transmission channel. Furthermore, the polarization potential of the original HEO is significantly lower than that of the original NMMO, indicating that the high-entropy structure itself helps to reduce electrochemical polarization, fully demonstrating the significant improvement in interface stability achieved by the amorphous coating of this invention.
[0044] In summary, this invention reduces the formation energy of amorphous products to 0.16 eV through a high-entropy composition ratio, making surface amorphization thermodynamically highly favorable. Combined with a natural cooling process, utilizing the difference in cooling rates between the surface and bulk phases, surface atoms are kinetically frozen into a disordered state, thus spontaneously forming an entropy-stable amorphous coating. This amorphous coating, acting as a kinetic barrier, significantly increases the activation energy of harmful H2O / O2 side reactions and exhibits excellent water resistance and air stability. The results of the examples show that the cathode material retains its structural integrity after immersion in water for 90 days, and no characteristic peaks of hydrated phase or Na2CO3 appear in the XRD pattern; while the comparative low-entropy material (Na... 0.8 Mg 0.2 Mn 0.8 After immersion in water for 7 days, the O2 material exhibited a clear hydrated phase and Na2CO3, and after 30 days, the layered structure essentially collapsed. After immersion in water for 90 days, the cathode material achieved an initial reversible capacity of 90 mAh / g (0.1 C), almost indistinguishable from the unimmersed sample (92 mAh / g). After 100 cycles at a current density of 0.2 C, the capacity retention rate reached 99%, demonstrating excellent electrochemical performance. In contrast, the comparative material, after immersion in water for 90 days, only achieved an initial reversible capacity of 45 mAh / g, and experienced a sudden capacity decrease during cycling. The Na content of the cathode material remained essentially unchanged after treatment in air and water, while the Na content of the comparative low-entropy material decreased from 0.792 to 0.505 after immersion in water for 30 days, indicating significant loss of active sodium. The amorphous surface coating of the cathode material effectively suppressed side reactions and improved safety: it prevented the formation of byproducts such as Na2CO3 and NaHCO3, avoiding the decomposition of these byproducts during charging and discharging to produce CO2 and CO gas, thus reducing the risk of battery explosion and improving battery safety.
[0045] The present invention features a simple preparation process, employing conventional solid-state sintering without complex coating or surface treatment processes. It is compatible with existing sodium-ion battery cathode material production processes and suitable for large-scale industrial production. This material exhibits excellent water resistance and air stability, significantly reducing the environmental control requirements for sodium-ion battery cathode materials during storage, transportation, and battery assembly, thus helping to lower production costs, improve production efficiency, and increase product yield. Simultaneously, the material's excellent cycle stability helps extend the lifespan of sodium-ion batteries, showing broad application prospects in large-scale energy storage, low-speed electric vehicles, and electric bicycles. The technical solution of this invention can also be extended to lithium-ion and potassium-ion battery systems.
[0046] The present invention has been described in detail above with reference to specific embodiments and exemplary examples; however, these descriptions should not be construed as limiting the present invention. Those skilled in the art will understand that various equivalent substitutions, modifications, or improvements can be made to the technical solutions and embodiments of the present invention without departing from the spirit and scope of the invention, and all such modifications and improvements fall within the scope of the present invention. The scope of protection of the present invention is defined by the appended claims.
Claims
1. A sodium-ion battery cathode material, characterized in that, Its chemical formula is Na a Mg x Zn y Cu p Fe q Mn r O2; where 0.7 ≤ a ≤ 0.9, 0.05 ≤ x ≤ 0.2, 0.05 ≤ y ≤ 0.2, 0.05 ≤ p ≤ 0.2, 0.05 ≤ q ≤ 0.2, 0.4 ≤ r ≤ 0.7, and x + y + p + q + r = 1; The sodium-ion battery cathode material has a core-shell structure, wherein the core is a P2-type layered crystal with a space group of P63 / mmc, and the outer shell is an amorphous coating.
2. The sodium-ion battery cathode material as described in claim 1, characterized in that, The chemical formula of the sodium-ion battery cathode material is Na. 0.8 Mg 0.1 Zn 0.1 Cu 0.1 Fe 0.1 Mn 0.6 O2.
3. The sodium-ion battery cathode material as described in claim 2, characterized in that, The amorphous coating is an entropy-stable amorphous oxide coating with a formation energy of 0.16 eV; The thickness of the amorphous coating is 5-15 nm.
4. The sodium-ion battery cathode material as described in claim 2, characterized in that, In the outer shell, the content of Na and O gradually decreases from the surface inwards, while the content of Mg, Zn, Cu, Fe, and Mn gradually increases, and the valence state of Mn changes from that of Mn on the surface. 4+ Mn gradually transitions to near-surface Mn 3+ ; In the core, the elements Na, Mg, Zn, Cu, Fe, and Mn are evenly distributed.
5. A method for preparing the sodium-ion battery cathode material according to any one of claims 1-4, characterized in that, Includes the following steps: S1. Weigh out sodium, magnesium, zinc, copper, iron, and manganese sources according to the stoichiometric ratio, mix and ball-mill to obtain a primary mixed powder; wherein, sodium source is in excess by 1.5-2.5 mol%; S2. The primary mixed powder is pressed into shape and calcined at high temperature in air atmosphere, and then naturally cooled to room temperature to obtain the sodium-ion battery cathode material.
6. The method for preparing the sodium-ion battery cathode material as described in claim 5, characterized in that, The calcination process involves a heating rate of 3-5℃ / min, a temperature of 800-900℃, and a time of 15-25h.
7. The method for preparing the sodium-ion battery cathode material as described in claim 5, characterized in that, The sodium source is selected from at least one of Na2CO3, NaHCO3, NaOH, and Na2O; the magnesium source is selected from at least one of MgO and MgCO3; the zinc source is selected from at least one of ZnO and ZnCO3; the copper source is selected from at least one of CuO and CuCO3; the iron source is selected from at least one of Fe2O3 and Fe3O4; and the manganese source is selected from at least one of Mn2O3, MnO2, and MnCO3.
8. The method for preparing the sodium-ion battery cathode material as described in claim 5, characterized in that, The ball milling process is carried out at a speed of 400-500 rpm for 6-10 hours. The pressure for compression molding is 5-15 kPa.
9. A positive electrode sheet for a sodium-ion battery, characterized in that, Includes the sodium-ion battery cathode material according to any one of claims 1-4.
10. A sodium-ion battery, characterized in that, Includes the positive electrode sheet as described in claim 9.