Cable morphology PANI@CNT nanocomposite material, preparation method thereof and application thereof in semi-solid zinc ion battery

By preparing cable-morphological PANI@CNT nanocomposites, the strong π-π interaction between carbon nanotubes and polyaniline was utilized to solve the problems of insufficient conductivity and structural stability of PANI/CNT composites in zinc-ion battery cathodes in the prior art, thus achieving high specific capacity and good cycle stability.

CN123143377APending Publication Date: 2026-11-20YANGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611497641.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing PANI/CNT composite materials in zinc-ion battery cathodes suffer from low conductivity, poor structural stability, and slow reaction kinetics, failing to fully leverage the synergistic effect between carbon nanotubes and polyaniline, particularly in terms of controlling the nanostructure morphology of PANI and enhancing interfacial interactions.

Method used

Through specific preparation methods, including pre-dispersion, high-speed dispersion and nano-milling of multi-walled carbon nanotubes, combined with in-situ polymerization of aniline monomers, a cable-morphological PANI@CNT nanocomposite material is formed. The strong π-π interaction between carbon nanotubes and polyaniline forms a core-shell structure, increases the electrochemical active sites, and improves the thermal and structural stability of the material.

Benefits of technology

It significantly improves the thermal and structural stability of the material, enhances electron and ion transport performance, increases specific capacity, solves the polarization and degradation problems of PANI electrodes, and improves cycle stability and electrochemical activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143377A_ABST
    Figure CN123143377A_ABST
Patent Text Reader

Abstract

The application relates to a cable-shaped PANI@CNT nanocomposite material, a preparation method thereof and application of the cable-shaped PANI@CNT nanocomposite material in a semi-solid zinc ion battery. The cable-shaped PANI@CNT nanocomposite material is prepared by in-situ oxidative polymerization of aniline in a uniformly dispersed multi-walled carbon nanotube suspension, has a cable-shaped core-shell structure, the core layer is a carbon nanotube, the shell layer is formed by closely arranging and assembling polyaniline nanoparticles with a size of 30-50 nm, and strong pi-pi interaction is formed between the interfaces of the core layer and the shell layer; compared with pure polyaniline, the thermal decomposition temperature is increased to 514.0 DEG C; as a positive electrode material of the semi-solid zinc ion battery, the specific capacity reaches 205.9 mAh / g under 0.1C, the capacity retention rate is 79.2% after 500 cycles, the specific capacity is maintained at 112 mAh / g under 2A / g, the rate reaches 72% (0.1C-1C), the problems of polyaniline electrode polarization and degradation are effectively solved, and the cycle stability and rate performance of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanocomposite materials and energy storage battery technology, specifically relating to a cable-morphology PANI@CNT nanocomposite material, its preparation method, and its application in semi-solid zinc-ion batteries. Background Technology

[0002] Rechargeable aqueous zinc-ion batteries (AZIBs) possess advantages such as high energy density, high power density, good safety and efficiency, non-toxicity, low cost, and simple preparation methods. The electrolytes of AZIBs are neutral or weakly acidic, causing no pollution during production and use. Therefore, zinc-ion batteries are an environmentally friendly, sustainable battery system with promising applications in power battery devices. Currently, the low capacity or unsatisfactory cycle performance of cathode materials limits the further application and development of rechargeable zinc-ion batteries. Researchers expect cathode materials to provide higher capacity during charge-discharge cycles while maintaining initial structural stability. Therefore, extensive research is dedicated to the design and development of high-quality cathode materials to further improve the performance of zinc-ion batteries.

[0003] Currently, research on zinc-ion battery cathodes mainly focuses on the modification of traditional manganese-based and vanadium-based compounds. On the other hand, novel zinc-ion storage materials are also being explored, such as Prussian blue analogs and conductive polymer materials. Although manganese-based and vanadium-based cathode materials possess high specific capacity and suitable zinc-ion intercalation potentials, their low conductivity, poor structural stability, and slow reaction kinetics limit their industrialization and large-scale application.

[0004] Conductive polymers, due to their structural diversity and controllable molecular weight, are also used as cathode materials for zinc-ion batteries. For example, polyaniline (PANI) is considered a novel cathode material for advanced rechargeable zinc-ion batteries due to its simple and inexpensive synthesis, high conductivity, excellent doping performance, high redox reversibility, and environmental friendliness. As early as 1986, Kitani et al. studied and reported on electrochemically synthesized PANI as an electroactive material in aqueous zinc rechargeable batteries. The prepared zinc-PANI battery exhibited a 108 mAh·g-1 mAh / g-1. -1 The reversible specific capacity was maintained, and the coulombic efficiency remained at 100% after 2000 cycles. In 2003, Karami et al. prepared PANI through chemical synthesis, pressing PANI powder, graphite, and acetylene black into a positive electrode material, with pressed zinc powder as the anode. The assembled battery had a specific capacity of 125.43 mA·h·g. -1 The coulombic efficiency is no less than 95% within 100 cycles. In 2007, Ghanbari et al. prepared a PANI / graphite composite thin film material as a positive electrode using an electrochemical method, and the assembled zinc-ion battery achieved a coulombic efficiency of 0.6 mA·cm⁻¹.-2 The maximum reversible capacity is 142 mAh·g -1 After 200 cycles, the coulomb efficiency remains above 97%.

[0005] Current research on rechargeable zinc / PANI batteries reveals drawbacks compared to traditional lithium-ion batteries, including lower specific capacity and shorter cycle life. These drawbacks are attributed to zinc dendrite growth, zinc electrode passivation, and the polarization and degradation of the PANI electrode. Therefore, to successfully implement the PANI cathode in zinc-ion batteries, it is necessary to address the existing polarization and degradation issues of the PANI electrode.

[0006] Chinese patent CN115548295A discloses a method for preparing a polyaniline composite material for the cathode of a Zn-ion battery. By adding carbon nanotubes and zinc ions to the cathode material of a zinc-ion battery, a Zn-doped polyaniline composite material is formed, solving the problems of electrochemical degradation and volume expansion of polyaniline, improving the mechanical strength and conductivity of the material, extending the cycle life of the battery, and reducing manufacturing costs. However, in this technical solution, the carbon nanotubes and polyaniline are physically mixed or polycondensed together, without addressing the precise control of the carbon nanotube pre-dispersion process and dosage to regulate the nanostructure morphology of polyaniline, nor does it address the strengthening of π-π interactions between the core and shell layers.

[0007] Chinese patent CN1302486C discloses a conductive polymer-carbon nanotube nanocable and its preparation method. The conductive polymer-carbon nanotube nanocable is prepared by using surfactants and ultrasonic dispersion technology in an acidic aqueous solution, solving the problem of carbon nanotube dispersion in insoluble polymers, improving electrical conductivity and mechanical properties, and making it suitable for various high-performance applications. The shell can be a polyaniline-based conductive polymer, and the core can be a single-walled / double-walled / multi-walled carbon nanotube. Conductive polymer monomers are polymerized in situ after the carbon nanotubes are dispersed by surfactants. However, considering that the document discloses the concept of "nanocable" and the core-shell structure, but does not limit the shell to be composed of tightly packed 30-50 nm PANI nanoparticles, and does not involve zinc-ion battery applications, the existing technology appears somewhat insufficient.

[0008] Although there are reports on PANI / CNT composite materials in the prior art, there is no technical solution that clearly defines the cable-shaped core-shell structure and the shell layer is composed of tightly arranged PANI particles of 30-50nm. This specific morphology is achieved through the synergistic effect of CNT pre-dispersion treatment, composite dispersant, high-speed dispersion and nano-sand milling, CNT dosage control, aniline monomer of 0.8-1.2%, and in-situ polymerization process.

[0009] Although the π-π interaction between PANI and CNTs has been mentioned in the literature, the existence of this interfacial interaction and its regulation of PANI's electronic structure and crystallization behavior have not been systematically characterized and confirmed using multiple methods such as FT-IR, UV-Vis, and XRD. Existing technologies have reported the use of carbon nanotubes and polyaniline composites in zinc-ion battery cathodes, but the resulting composites are mostly simple physical mixtures or non-directional composites, failing to fully utilize the synergistic effect between carbon nanotubes and polyaniline, particularly in regulating the nanostructure morphology of PANI, enhancing interfacial interactions, and improving structural stability. Summary of the Invention

[0010] Technical problem to be solved: This invention aims to provide a cable-morphology PANI@CNT nanocomposite material, its preparation method and application. By forming a strong π-π interaction between carbon nanotubes and polyaniline, the nanostructure morphology of PANI can be effectively controlled, increasing the electrochemical active sites and improving the specific capacity. At the same time, it significantly improves the thermal stability and structural stability of the material, effectively solving the polarization and degradation problems of PANI electrodes, thereby improving the electron and ion transport performance, electrochemical activity and cycle stability of the cathode material.

[0011] Purpose of the invention: This invention aims to provide a PANI@CNT nanocomposite material with cable morphology. By utilizing the strong π-π interaction formed at the phase interface, it can not only effectively regulate the nanostructure morphology of PANI, increase the active sites of PANI, and improve the specific capacity, but also effectively solve the polarization and degradation problems of PANI electrode, thereby improving the electron and ion transport performance, electrochemical activity and cycle stability of the cathode material.

[0012] Technical solution: A method for preparing PANI@CNT nanocomposite material with cable morphology, comprising the following steps: Step (1): Multi-walled carbon nanotubes were dispersed in water using a composite dispersant. The dispersion was carried out at 1500 r / min for 2 h at room temperature, followed by nano-milling at 1000 r / min for 3 h to obtain a monodisperse carbon nanotube aqueous suspension with a mass fraction of 4%. Step (2): Mix the carbon nanotube aqueous suspension obtained in step (1) with aniline monomer, add acidic solution, and ultrasonically disperse at 400W to allow the carbon nanotubes to fully adsorb the aniline monomer; Step (3): Under ice bath conditions, add oxidant solution dropwise to the mixture obtained in step (2) and react at 0~5℃ for 10~14h; Step (4): After the reaction is complete, filter and wash, use alkaline solution to carry out the doping reaction, wash until neutral, dry, and obtain EB-PANI@CNT nanocomposite powder, that is, cable morphology PANI@CNT nanocomposite material.

[0013] Furthermore, in step (1), the composite dispersant is a mixture of ethynyl alcohol and dispersant NSF 15 in a mass ratio of 1:1. It is firmly bound to the CNT surface through π-π interaction, thereby stabilizing the dispersion stability of CNT in the aqueous medium through steric repulsion.

[0014] Furthermore, in step (2), the mass of the carbon nanotubes is 0.8-1.2% of the mass of the aniline monomer, and the acidic solution in step (2) is a hydrochloric acid solution with a concentration of 0.5-2M and an ultrasonic dispersion time of 1h.

[0015] Furthermore, the oxidant mentioned in step (3) is ammonium persulfate, and the molar ratio of ammonium persulfate to aniline is 1~1.2:1.

[0016] Furthermore, in step (4), the alkaline solution is a 0.05~0.2M NaOH solution, the drying temperature is 50~70℃, the drying time is 4~8h, the filtration is carried out by suction filtration using a Buchner funnel with a filter diameter of 0.22μm, the washing steps are as follows: first wash with anhydrous ethanol 3 times, 20mL each time, then wash with distilled water 3 times, 50mL each time, and the dopant removal reaction time is 6h.

[0017] A cable-shaped PANI@CNT nanocomposite material prepared by any of the above preparation methods, wherein the PANI@CNT nanocomposite material has a cable-shaped core-shell structure, the core layer is a multi-walled carbon nanotube, and the shell layer is composed of tightly packed polyaniline nanoparticles of 30~50nm, wherein a π-π interaction is formed between the core layer and the shell layer, and the diameter of the multi-walled carbon nanotube is 6~12nm; the diameter of the PANI@CNT nanocomposite material is 100~200nm.

[0018] Furthermore, the PANI@CNT nanocomposite material has a thermal decomposition onset temperature of 468.5℃ and a maximum decomposition rate temperature of 514.0℃; after 500 cycles at a current density of 1A / g, the capacity retention rate is 79.2%.

[0019] This application also discloses the application of the cable morphology PANI@CNT nanocomposite material prepared by any of the above preparation methods in a semi-solid zinc-ion battery, wherein the semi-solid zinc-ion battery comprises a positive electrode, a zinc negative electrode and a semi-solid electrolyte membrane.

[0020] Furthermore, the positive electrode uses carbon paper as the current collector. The positive electrode material is prepared by coating a mixture of cable-morphological PANI@CNT nanocomposite material, zinc salt, conductive agent, binder, thickener, and water onto carbon paper and then drying it. The mass fraction of the cable-morphological PANI@CNT nanocomposite material is 70-90 wt%, the mass fraction of the conductive agent is 0.5-10 wt%, the mass fraction of the binder is 5-15 wt%, and the mass fraction of the thickener is 1-5 wt%. The molar amount of zinc salt is 25-50% of PANI.

[0021] Furthermore, the carbon paper has a thickness of 50 μm and an areal loading of 1-2 mg / cm². 2 The conductive agent is one or more of carbon nanotubes, graphene, and Ketjen black; the zinc salt is zinc sulfate or zinc chloride; the binder is styrene-butadiene latex; the thickener is sodium carboxymethyl cellulose; the semi-solid electrolyte membrane is a polyacrylamide-based semi-solid electrolyte membrane with a thickness of 0.8~0.9 mm; the specific capacity of the semi-solid zinc-ion battery is 205.9 mAh / g at a current density of 0.1 C, and 112 mAh / g at a current density of 2 A / g, with a rate of 72% (0.1C~1C).

[0022] Explanation of the principle: This invention involves the in-situ oxidative polymerization of aniline in a uniformly dispersed multi-walled carbon nanotube suspension, allowing aniline monomers to preferentially adsorb onto the carbon nanotube surface, resulting in the in-situ polymerization and growth of polyaniline on the carbon nanotube surface. The inherent delocalized π-electron system of carbon nanotubes forms a strong π-π conjugation interaction with the quinone rings on the polyaniline backbone. This interaction drives the polyaniline molecular chain to preferentially bind to the carbon nanotube surface in a quinone conformation, forming a tight core-shell encapsulation structure. The π-π conjugated anchoring network constructs dense physical cross-linking points between the polyaniline molecular chain and the carbon nanotube surface, effectively constraining the thermal motion of the polymer chain and significantly increasing the thermal decomposition temperature of the material. Simultaneously, the carbon nanotubes, as a highly conductive framework, provide efficient and rapid electron transport channels. The 30-50 nm polyaniline nanoparticles in the shell significantly increase the specific surface area and porosity, exposing more electrochemically active sites, which is beneficial for the insertion / extraction of zinc ions. The key process parameter control principle of this invention is as follows: The composite dispersant (acetylene alcohol and polystyrene grafted maleic anhydride in a 1:1 mass ratio) binds to the CNT surface through π-π interactions, stabilizing the dispersion of CNTs in the aqueous medium through steric repulsion; the synergistic effect of high-speed dispersion (1500 r / min, 2 h) and nano-grinding (1000 r / min, 3 h) achieves monodispersion of CNTs, which is a prerequisite for forming a uniform cable morphology. The CNT dosage is controlled within the range of 0.8~1.2% of the aniline monomer mass to ensure that the CNT surface is fully coated with PANI without excess. Exceeding this range (such as 0.5% or 1.5%) will not form a cable morphology and will weaken the interfacial π-π interactions.

[0023] Beneficial effects: 1. The PANI@CNT nanocomposite material prepared by this invention has a unique cable-shaped core-shell structure. The core layer is carbon nanotubes, and the shell layer is composed of tightly packed PANI nanoparticles of 30~50nm. This structure is achieved through strong π-π interactions between the carbon nanotubes and PANI interface, fundamentally changing the intrinsic thermal decomposition mechanism of PANI, improving heat resistance and structural stability, mitigating volume cycling changes during PANI cycling, and improving the cycle stability of the battery. After 500 cycles (1C), the capacity retention rate is 79.2%, and the thermal decomposition temperature is significantly increased from 196.8~356.7℃ of PANI to 514.0℃, an increase of about 300℃; 2. When the composite material of this invention is used as a positive electrode material for semi-solid zinc-ion batteries, the conductive framework of carbon nanotubes effectively reduces the electrode polarity. The EB-PANI@CNT nanocomposite material significantly improves the reversibility of the electrode reaction, and the quinone / benzene structure ratio is significantly increased, which can significantly increase the specific capacity of the battery. Under 0.1C conditions, the specific capacity increases from 100.5 mAh / g of pure PANI to 205.9 mAh / g, an increase of about 105%. 3. The composite material of this invention effectively solves the polarization and degradation problems of PANI electrodes, accelerates the transport of electrons and ions, and has excellent rate performance. The rate characteristic from 0.1A / g to 1A / g is 72%, and the specific capacity is still maintained at 112 mAh / g under a high current density of 2A / g, which can effectively solve the polarization and degradation problems of PANI electrodes. 4. The cable morphology of the EB-PANI@CNT nanocomposite material has a significant improvement in conductivity compared to EB-PANI. The preparation method of this invention is simple and mild, which is conducive to large-scale production. Attached Figure Description

[0024] Figure 1 These are microscopic morphology images of the CNTs used in Example 1 of the present invention and the prepared EB-PANI@CNT nanocomposite material; wherein (a1) is a TEM image of CNTs, (a2) is a TEM image of EB-PANI@CNTs, (b1) is a cross-sectional SEM image of EB-PANI@CNTs, and (b2) is a high-magnification SEM image of EB-PANI@CNTs. Figure 2 Comparison of Fourier transform infrared (FT-IR) and ultraviolet-visible (UV-Vis) spectra of EB-PANI and EB-PANI@CNT composite materials; where (a1) is the FT-IR spectrum and (a2) is the UV-Vis spectrum. Figure 3 Thermogravimetric analysis (TGA) and differential thermal analysis (DTA) curves of EB-PANI and EB-PANI@CNT composite materials are shown; where (a1) is the thermogravimetric analysis curve and (a2) is the differential thermal analysis curve. Figure 4 X-ray diffraction (XRD) patterns of EB-PANI and EB-PANI@CNT composite materials; Figure 5 Electrochemical impedance spectroscopy (EIS) and cyclic voltammetry (CV) curves of EB-PANI and EB-PANI@CNT coin cells are shown; where (a1) is the EIS spectrum and (a2) is the CV curve. Figure 6 The graphs show the cycle performance and rate performance of the EB-PANI@CNT button cell; where (a1) shows the results of 500 cycles at a current density of 1A / g, and (a2) shows the rate performance at different rates. Figure 7 The diagrams show the equivalent circuit diagrams of the cathode materials EB-PANI and EB-PANI@CNT of this application, with the upper diagram showing the equivalent circuit diagram of EB-PANI and the lower diagram showing the equivalent circuit diagram of EB-PANI@CNT. Figure 8 The morphology is shown when the CNT content is 0.5%; Figure 9 The morphology is shown when the CNT content is 1.5%; Figure 10 This is a dispersion diagram of CNTs without the use of composite dispersants and nano-sand milling process; Figure 11 The morphology of the composite material without the use of composite dispersants and nano-sand milling process; Figure 12 This is a SEM image of the electrode material after 500 cycles. Detailed Implementation

[0025] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. The following embodiments are only for illustrating the present invention and are intended to limit the scope of the invention. Unless otherwise specified, the experimental techniques and methods involved in the embodiments are all common techniques and are carried out under conventional conditions. The CNT aqueous suspension used in the following embodiments is obtained by dispersing multi-walled carbon nanotubes in water with a composite dispersant, dispersing at high speed at 1500 r / min for 2 h at room temperature, and then treating it by nano-milling at 1000 r / min for 3 h to obtain a monodisperse carbon nanotube aqueous suspension with a mass fraction of 4%, i.e., CNT aqueous suspension. The composite dispersant is composed of ethynyl alcohol and dispersant NSF 15 mixed in a mass ratio of 1:1. It is firmly bound to the CNT surface through π-π interaction, thereby stabilizing the dispersion stability of CNTs in the aqueous medium through steric repulsion. The dispersant NSF 15 is purchased from Changshu Naisu.

[0026] Example 1: A method for preparing a PANI@CNT nanocomposite material with cable morphology, comprising the following steps: (1) Weigh 2.325g of 4% CNT aqueous suspension (CNT content 0.093g) into a 100mL beaker, mix it with 0.93g of aniline, and add 50mL of 1M HCl solution; sonicate for 1h to allow CNTs to fully adsorb aniline monomers; add the resulting mixture into a three-necked flask equipped with a stirrer and a dropping funnel; (2) Place the above device in an ice bath; (3) In a 100mL beaker, add 10mL of 1M HCl solution and 40mL of deionized water, then add 2.4g of ammonium persulfate (APS) and dissolve to obtain an APS solution; (4) The above APS solution was added dropwise to a three-necked flask over 0.5 h and reacted at 0~5℃ for 12 h. (5) After the reaction is complete, filter the sample and wash it three times with ethanol and three times with distilled water. (6) The above filter cake was subjected to a doping reaction using 0.1M NaOH solution, filtered, washed with distilled water until the pH of the filtrate was 7, and vacuum dried at 60℃ for 6h to obtain EB-PANI@CNT nanocomposite powder.

[0027] As a control, EB-PANI was synthesized using the same process as EB-PANI@CNT, but without introducing CNT suspension into the synthesis system.

[0028] The performance test results of EB-PANI and EB-PANI@CNT nanocomposites are as follows: Figure 1 The microstructure of the CNTs used in Example 1 and the prepared EB-PANI@CNT nanocomposite material is shown. The diameter of the CNTs is approximately 6-12 nm.Figure 1 As shown in (a1), the diameter of the EB-PANI@CNT composite material is 100~200nm, as... Figure 1 As shown in (a2); by Figure 1 The cross-sectional morphology of (b1) clearly reveals its hollow tubular structure, with an inner core of multi-walled carbon nanotubes and an outer shell of PANI grown in situ on the CNT surface. High-magnification SEM images are shown below. Figure 1 Figure (b2) shows that the shell is composed of tightly packed PANI nanoparticles of 30-50 nm, forming a core-shell encapsulation morphology resembling a "cable".

[0029] Figure 2 The comparison results of Fourier transform infrared (FT-IR) and ultraviolet-visible (UV-Vis) spectra of EB-PANI and PANI@CNT composite materials are presented. Figure 2 As shown in Figure (a1), EB-PANI values ​​at 1587.3, 1495.6, 1305.0, 1160.0, and 826 cm⁻¹ -1 The characteristic absorption peaks at these locations can be attributed to the C=C stretching vibrations of the quinone ring, the C=C stretching vibrations of the benzene ring, the C–N stretching vibrations of aromatic amines, and the C–N stretching vibrations related to charge delocalization. + Stretching vibrations and out-of-plane bending vibrations of the para-substituted benzene ring C–H. Compared to EB-PANI, the FT-IR spectrum of the PANI@CNT composite not only retains all the above characteristic peaks, but also shows a significant enhancement in the relative absorption peak intensity of the quinone C=C stretching vibration, while at 1380.5 cm⁻¹... -1 A new absorption peak appeared. These spectral changes clearly demonstrate that a strong electronic interaction occurred between CNTs and PANI (especially its quinone structure). The inherent delocalized π-electron system of carbon nanotubes can form a strong π-π conjugation with the quinone ring on the PANI backbone, which drives the PANI molecular chain to preferentially bind to the CNT surface in the quinone conformation. Figure 2(a2) Comparison of the UV-Vis absorption spectra of EB-PANI and CNT@PANI composites shows that EB-PANI exhibits two characteristic absorption peaks at 328.7 nm and 627.1 nm, attributed to the π→π* electronic transition of the benzene ring and the exciton transition of the quinone ring, respectively. In contrast, the spectrum of the PANI@CNT composite exhibits significant peak splitting in both the low and high energy regions, splitting into two doublets at 319.0 / 340.9 nm and 581.1 / 690.3 nm, respectively. Specifically, the absorption peak at 319.0 nm shows a significant blue shift compared to the 328.7 nm peak of EB-PANI. This phenomenon is generally explained by the confined polymerization of PANI on the CNT surface, which shortens its effective conjugation length, thereby increasing the π→π* transition energy. On the other hand, the single peak at 627.1 nm splits into two peaks at 581.1 nm and 690.3 nm, with the new peak at 690.3 nm showing a significant redshift relative to the quinone exciton peak of EB-PANI. This redshift can be attributed to photoinduced charge transfer between CNTs and PANI: CNTs, acting as electron acceptors, attract some electrons from the quinone ring of PANI through their delocalized π-electron system, causing a partial transformation of the benzene ring structure into a quinone structure (consistent with FT-IR results), equivalent to p-type doping of PANI. This doping effect introduces intermediate energy levels such as polarons into the PANI band gap, thereby lowering the electronic transition energy, leading to a redshift of the absorption peak and the emergence of a new absorption feature at 581.1 nm. Combining these spectral changes, it is clear that there is a strong electronic coupling between CNTs and PANI, rather than a simple physical blending.

[0030] Figure 3 Thermogravimetric analysis (TGA) and differential thermal analysis (DTA) results of EB-PANI and PANI@CNT composites were compared. Figure 3As shown in (a1), the mass loss of EB-PANI before 100℃ is attributed to the removal of physically adsorbed water; subsequently, significant thermal decomposition begins at 192.2℃, exhibiting continuous mass decay until 800℃. Its DTA curve shows four endothermic peaks at 50, 196.8, 269.9, and 356.7℃, corresponding to dehydration, oligomer removal, and multi-step thermal oxidative degradation processes. In stark contrast, the thermal decomposition initiation temperature of the PANI@CNT composite material is significantly delayed to 468.5℃, and the maximum decomposition rate temperature increases to 514.0℃, indicating that the introduction of CNTs has a significant thermal stabilization effect on the PANI matrix. This significant improvement in thermal stability can be attributed to the π–π conjugated anchoring network formed at the "cable" core-shell interface of the composite material, especially the strong electronic coupling between the delocalized π-electron system of CNTs and the quinone structure of PANI. These interfacial interactions create dense physical crosslinking points between the PANI molecular chains and the CNT surface, effectively constraining the thermal motion of the polymer chains. This necessitates overcoming these interfacial energy barriers during thermal decomposition, significantly increasing the decomposition activation energy. The low decomposition temperature of pure PANI (approximately 200℃) and the multiple endothermic peaks in its DTA curve reflect its inherent thermal instability, particularly its susceptibility to oligomer depolymerization and chain breakage. In the PANI@CNT system, the electron acceptor properties of CNTs cause PANI to maintain a higher oxidation state (increased proportion of quinone structures). This electronic structure regulation effectively suppresses thermally induced chain degradation, raising the significant main chain breakage temperature by approximately 300℃. Notably, in the DTA curve of PANI@CNT, multiple thermal effect peaks of pure PANI completely disappear, with only a sharp main decomposition peak appearing at 514.0℃. This indicates that its thermal decomposition pathway has shifted from a multi-step, complex process to a simplified, centralized decomposition mode. This result strongly demonstrates that the introduction of CNTs fundamentally alters the intrinsic thermal decomposition mechanism of PANI, rather than a simple physical additive effect.

[0031] Figure 4The X-ray diffraction (XRD) patterns of the EB-PANI and PANI@CNT composites are shown. For EB-PANI, the diffraction peaks at 2θ = 8.94°, 15.1°, 20.2°, and 25° are attributed to the (001), (010), (100), and (110) crystal planes, respectively, consistent with PDF card No. 03-065-5714, confirming the semi-crystalline nature of PANI. In contrast, the XRD pattern of PANI@CNT exhibits significantly different diffraction characteristics: the characteristic peaks attributed to PANI crystal planes almost completely disappear, while two strong and broad diffraction peaks appear at 19.1° and 23.2°, and a new weak diffraction peak is observed at 41.8°. The two strong peaks at 19.1° and 23.2° cannot be attributed to any known crystal plane of PANI, and are more likely to originate from the ordered superstructure induced by the π–π stacking interaction between CNT and PANI. Notably, pure CNTs exhibit only a broad diffraction peak at ~25.6°, while in the composite material, this peak not only shifts significantly but also splits into two new peaks. This indicates that the π–π conjugation interaction between CNTs and PANI drives the ordered arrangement of molecular chains, forming a novel ordered structure distinct from the semi-crystalline state of pure PANI. Furthermore, the new weak peak at 41.8° also does not correspond to the diffraction of the PANI crystal plane; its position is close to the characteristic diffraction of the (100) crystal plane of CNTs (~42°), suggesting that this peak may originate from the ordered stacking characteristics between the CNT tube walls. This peak was observed only in the composite sample, implying that ordered molecular assembly behavior may exist at the CNT-PANI interface.

[0032] Example 2, Preparation of EB-PANI@CNT cathode material: (1) Weigh 160 mg of the EB-PANI@CNT composite material prepared in Example 1, 20 mg of Ketjen black, 20 mg of styrene-butadiene latex, 6 mg of CMC, and 60 mg of ZnCl2, add an appropriate amount of distilled water, and stir magnetically for 6 h to prepare electrode nanoslurry; (2) The above nano-slurry was uniformly coated onto carbon paper using a doctor blade coater; (3) Place the coated electrode in a drying oven at 60-80℃ and dry for 6 h.

[0033] Preparation of semi-solid electrolyte membrane: The polyacrylamide-based semi-solid electrolyte membrane prepared according to the patent of this research group (acceptance number: 2026103228012) is transparent in appearance and the thickness is controlled between 0.8 and 0.9 mm.

[0034] The components were assembled into a CR2032 coin cell casing in the order of zinc anode / semi-solid electrolyte membrane / positive electrode to obtain a semi-solid zinc-ion battery. Coin cells were prepared using EB-PANI and the EB-PANI@CNT nanocomposite material from Example 1 as the positive electrode active material, respectively. The electrochemical performance test results are as follows: Figure 5 (a1) Comparison of the electrochemical impedance spectroscopy (EIS) spectra of EB-PANI and the EB-PANI@CNT coin cells in Example 1 before cycling. Both impedance spectra consist of a semicircle in the high-frequency region and a slanted line in the low-frequency region. The semicircle in the high-frequency region corresponds to the charge transfer process at the electrode / semi-solid electrolyte interface, while the slanted line in the low-frequency region reflects the Zn... 2+ The diffusion behavior of the EB-PANI cell. The equivalent circuit fitting results (Table 1) show the ohmic resistance (Rs), charge transfer resistance (Rct), and Zn content of the EB-PANI cell. 2+ The diffusion coefficients (D) are 88.2 Ω, 293.1 Ω, and 6.5 × 10⁻⁶, respectively. -12 cm 2 / s. The corresponding values ​​for the PANI@CNT battery were significantly optimized to 9.9 Ω, 203.9 Ω, and 3.1 × 10⁻⁶ Ω. -11 cm 2 The / s indicates that the introduction of CNTs simultaneously reduced ohmic polarization and interfacial reaction resistance, and increased ion diffusion rate. These differences can be explained from three aspects. First, regarding Rs, it mainly reflects the bulk resistance within the semi-solid electrolyte and electrode material. Pure EB-PANI is intrinsically non-conductive, and electron transport within its aggregates is severely hindered, resulting in a high bulk resistance. CNTs, as a highly conductive framework, form a cable-like core-shell coating structure with PANI, providing an efficient and rapid electron transport channel, thus significantly reducing the electron conduction resistance within the electrode material and causing a significant decrease in Rs. Second, the reduction in Rct stems from the synergistic effect of multiple factors: on the one hand, the introduction of CNTs modulates the shell PANI into spherical particles of 30–50 nm, effectively inhibiting excessive PANI aggregation, increasing the specific surface area and porosity of the composite material, exposing more electrochemical active sites, which is beneficial for Zn. 2+ Contact with the electrode surface; on the other hand, the excellent conductivity and potential synergistic catalytic effect of CNTs themselves reduce the Zn content. 2+ The reaction energy barrier across the electrode / semi-solid electrolyte interface facilitates the interfacial charge transfer process. Finally, the porous network structure constructed by CNTs is beneficial for Zn. 2+ The rapid migration of ions significantly reduces the Warburg diffusion impedance in the low-frequency region, resulting in an increase of nearly an order of magnitude in the fitted diffusion coefficient D, further demonstrating the improving effect of CNTs on ion transport dynamics.

[0035] Table 1. Equivalent circuit diagram fitting results for the two electrode materials. .

[0036] Figure 5 Figure (a2) compares the cyclic voltammetry (CV) curves of EB-PANI and the EB-PANI@CNT button cell from Example 1 after activation at a 5V / s scan. The oxidation and reduction peaks of the EB-PANI cell are located near 1.5V and 0.9V, respectively; while the corresponding peaks of the PANI@CNT cell appear at 1.4V and 0.95V, respectively, with the oxidation peak shifting negatively and the reduction peak shifting positively, and the peak potential difference significantly narrowing. This indicates that the introduction of CNTs constructs an efficient electron transport pathway and increases the electrochemical active area, effectively reducing electrode polarization and significantly improving the reversibility of the electrode reaction. In addition, the integral area of ​​the CV curve of EB-PANI@CNT is much larger than that of EB-PANI, indicating that it has a higher specific capacity. This improvement stems primarily from three aspects: First, the CNT conductive framework enables more electroactive components in PANI to effectively participate in electrochemical reactions, preventing their "deactivation" within the insulating aggregates; second, CNT modulates the shell PANI into spherical particles of 30–50 nm, significantly increasing the specific surface area and porosity, thus exposing more Zn. 2+ Thirdly, as shown in the EIS results, the porous network constructed by CNTs enables Zn... 2+ The diffusion coefficient was increased by nearly an order of magnitude, ensuring the full progress of the bulk reaction.

[0037] Figure 6 Figure (a1) shows the test results of the EB-PANI@CNT battery after 500 cycles at a current density of 1 A / g (1C). Its initial specific capacity is 167.9 mAh / g, and the capacity retention rate after 500 cycles is 79.2% (132.9 mAh / g). Figure 6 Figure (a2) illustrates the rate performance of the button battery of the present invention in the range of 0.1C to 2C. At a current density of 0.1 A / g, the initial specific capacity of the battery is 205.9 mAh / g; when the current density is increased to 2 A / g, it can still maintain a specific capacity of 112 mAh / g, with a rate of 72% (0.1C to 1C).

[0038] Comparative Example 1 differs from Example 1 in that the amount of CNT used is 0.5% of the mass of the aniline monomer, while the other conditions are the same as in Example 1.

[0039] Comparative Example 2 differs from Example 1 in that the amount of CNT used is 1.5% of the mass of aniline monomer, while the other conditions are the same as in Example 1.

[0040] like Figure 8 andFigure 9 As shown, Figure 8 The morphology is shown when the CNT content is 0.5%. Figure 9 The morphology is shown when the CNT content is 1.5%. If it exceeds the range of 0.8-1.2%, the cable morphology cannot be formed, which weakens the π-π interaction at the interface. Comparative Example 3 differs from Example 1 in that: no composite dispersant is used in step (1), and no nano-grinding is performed; only conventional ultrasonic dispersion is used.

[0041] like Figure 10 As shown, the CNT dispersion state without the composite dispersant / nano-milling process is that the CNTs exhibit an aggregated morphology, such as... Figure 11 As shown, the morphology of the composite material without the composite dispersant / nano-sand milling process is that the composite material has an agglomerated morphology and does not have the microstructure of cable morphology. like Figure 12 As shown in the SEM image after 500 cycles, the morphology did not change significantly, indicating that CNTs play a mechanical stabilizing role in the insertion and extraction of ions.

[0042] In summary, this application has achieved a PANI@CNT nanocomposite material with a specific cable morphology (core CNT + shell 30-50nm PANI particles) through a specific CNT pre-dispersion process and precise raw material ratio. This material exhibits significantly improved thermal stability, specific capacity and cycle stability driven by π-π interface interaction, and has been successfully applied to the cathode of semi-solid zinc-ion batteries.

[0043] The embodiments described above are only some, not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. The scope of protection of the present invention is determined by the scope claimed in the claims. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A method for preparing a PANI@CNT nanocomposite material with cable morphology, characterized in that, Includes the following steps: Step (1): Multi-walled carbon nanotubes were dispersed in water using a composite dispersant. The dispersion was carried out at 1500 r / min for 2 h at room temperature, followed by nano-milling at 1000 r / min for 3 h to obtain a monodisperse carbon nanotube aqueous suspension with a mass fraction of 4%. Step (2): Mix the carbon nanotube aqueous suspension obtained in step (1) with aniline monomer, add acidic solution, and ultrasonically disperse at 400W to allow the carbon nanotubes to fully adsorb the aniline monomer; Step (3): Under ice bath conditions, add oxidant solution dropwise to the mixture obtained in step (2) and react at 0~5℃ for 10~14h; Step (4): After the reaction is complete, filter and wash, use alkaline solution to carry out the doping reaction, wash until neutral, dry, and obtain EB-PANI@CNT nanocomposite powder, that is, cable morphology PANI@CNT nanocomposite material.

2. The method for preparing the PANI@CNT nanocomposite material with cable morphology according to claim 1, characterized in that, In step (1), the composite dispersant is a mixture of ethynyl alcohol and dispersant NSF 15 in a mass ratio of 1:

1. It is firmly bound to the CNT surface through π-π interaction, thereby stabilizing the dispersion stability of CNT in the aqueous medium through steric repulsion.

3. The method for preparing the PANI@CNT nanocomposite material with cable morphology according to claim 1, characterized in that, The mass of the carbon nanotubes in step (2) is 0.8-1.2% of the mass of the aniline monomer, and the acidic solution in step (2) is a hydrochloric acid solution with a concentration of 0.5-2M and an ultrasonic dispersion time of 1h.

4. The method for preparing the PANI@CNT nanocomposite material with cable morphology according to claim 1, characterized in that, The oxidant mentioned in step (3) is ammonium persulfate, and the molar ratio of ammonium persulfate to aniline is 1~1.2:

1.

5. The method for preparing the PANI@CNT nanocomposite material with cable morphology according to claim 1, characterized in that, The alkaline solution in step (4) is a 0.05~0.2M NaOH solution. The drying temperature is 50~70℃ and the drying time is 4~8h. The filtration is carried out by suction filtration using a Buchner funnel with a filter diameter of 0.22μm. The washing steps are as follows: first, wash with anhydrous ethanol 3 times, 20mL each time, and then wash with distilled water 3 times, 50mL each time. The doping removal reaction time is 6h.

6. A PANI@CNT nanocomposite material with cable morphology prepared by the preparation method according to any one of claims 1-5, characterized in that, The PANI@CNT nanocomposite material has a cable-shaped core-shell structure, with a core layer of multi-walled carbon nanotubes and a shell layer composed of tightly packed polyaniline nanoparticles of 30-50 nm. A π-π interaction is formed between the core layer and the shell layer interface. The diameter of the multi-walled carbon nanotubes is 6-12 nm. The diameter of the PANI@CNT nanocomposite material is 100-200 nm.

7. The PANI@CNT nanocomposite material with cable morphology according to claim 6, characterized in that, The PANI@CNT nanocomposite material has a thermal decomposition initiation temperature of 468.5℃ and a maximum decomposition rate temperature of 514.0℃; after 500 cycles at a current density of 1A / g, the capacity retention rate is 79.2%.

8. The application of the PANI@CNT nanocomposite material with cable morphology prepared by the preparation method according to any one of claims 1-5 in a semi-solid zinc-ion battery, characterized in that, The semi-solid zinc-ion battery comprises a positive electrode, a zinc negative electrode, and a semi-solid electrolyte membrane.

9. The application according to claim 8, characterized in that, The positive electrode uses carbon paper as the current collector. The positive electrode material is prepared by coating a mixture of cable-morphological PANI@CNT nanocomposite material, zinc salt, conductive agent, binder, thickener and water onto carbon paper and then drying it. The mass fraction of cable-morphological PANI@CNT nanocomposite material is 70~90wt%, the mass fraction of conductive agent is 0.5~10wt%, the mass fraction of binder is 5~15wt%, the mass fraction of thickener is 1~5wt%, and the molar amount of zinc salt is 25~50% of PANI.

10. The application according to claim 9, characterized in that, The carbon paper has a thickness of 50 μm and an area loading of 1-2 mg / cm². 2 The conductive agent is one or more of carbon nanotubes, graphene, and Ketjen black; the zinc salt is zinc sulfate or zinc chloride; the binder is styrene-butadiene latex; the thickener is sodium carboxymethyl cellulose; the semi-solid electrolyte membrane is a polyacrylamide-based semi-solid electrolyte membrane with a thickness of 0.8~0.9 mm; the specific capacity of the semi-solid zinc-ion battery is 205.9 mAh / g at a current density of 0.1 C, and 112 mAh / g at a current density of 2 A / g, with a rate of 72% (0.1C~1C).

Citation Information

Patent Citations

  • Preparation method of polyaniline composite material for positive electrode of Zn ion battery

    CN115548295A

  • Conducting polymer carbon nanotube nano cable and preparation method thereof

    CN1302486C