A lithium manganese iron phosphate material, a preparation method and application thereof

CN123143379APending Publication Date: 2026-11-20SHANGHAI XUANYI NEW ENERGY DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611579773.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

其中,金属氧化物包覆层能够物理阻隔电解液的侵蚀,但存在导电性差、包覆层易开裂等问题;导电聚合物包覆层具有较好的柔韧性和导电性,但其对Mn2+的阻隔能力有限

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application belongs to the field of lithium ion batteries, and particularly relates to a lithium manganese iron phosphate material and a preparation method and application thereof. x Fe 1‑x PO4, wherein 0.1<=x<=0.9, the chemical anchoring layer is formed by in-situ carbonization of a metal organic framework and comprises a carbon skeleton and metal oxides dispersed in the carbon skeleton, and the multifunctional composite layer is formed by cross-linking of a conductive polymer and a carbon material. The lithium manganese iron phosphate material of the application realizes efficient capture and physical shielding of dissolved manganese ions through the synergistic effect of the chemical anchoring layer and the multifunctional composite layer, and significantly improves the high-temperature cycle stability of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion batteries, specifically relating to a lithium manganese iron phosphate material, its preparation method, and its application. Background Technology

[0002] Lithium manganese iron phosphate (LiMn) x Fe 1-x PO4 (LMFP) has become a research hotspot for next-generation lithium-ion battery cathode materials due to its high voltage platform, high safety, and low cost. However, this material faces a serious manganese leaching problem during high-temperature cycling. The root cause of manganese leaching lies in the Mn content on the material surface. 3+ Jahn-Teller distortion is prone to occur and disproportionation reaction (2Mn) is induced. 3 + →Mn 2+ + Mn 4+ ), generating Mn 2+ Dissolves in the electrolyte and migrates to the negative electrode, damaging the SEI film and causing a sharp decline in battery performance.

[0003] To address the manganese leaching problem, current technologies primarily employ surface coating strategies. Common coating materials include carbon materials, metal oxides (such as Al₂O₃, TiO₂, and ZrO₂), and conductive polymers (such as PEDOT:PSS and polyaniline). While metal oxide coatings can physically block electrolyte erosion, they suffer from poor conductivity and susceptibility to cracking. Conductive polymer coatings offer good flexibility and conductivity, but their effectiveness against Mn is limited. 2+ Its barrier properties are limited.

[0004] Therefore, there is an urgent need to develop a composite interface layer that combines chemical anchoring capability, high conductivity, and structural stability, which is of great significance for solving the manganese leaching problem of lithium manganese iron phosphate. Summary of the Invention

[0005] To address the aforementioned problems in the prior art, this invention proposes a lithium manganese iron phosphate material, its preparation method, and its applications.

[0006] Specifically, this invention provides a lithium manganese iron phosphate material, which includes a core and a chemical anchoring layer and a multifunctional composite layer sequentially coated on the surface of the core. The core is LiMn. x Fe 1-x PO4, wherein 0.1≤x≤0.9, the chemical anchoring layer is formed by in-situ carbonization of a metal-organic framework, comprising a carbon skeleton and metal oxides dispersed in the carbon skeleton, and the multifunctional composite layer is formed by crosslinking of a conductive polymer and carbon materials.

[0007] In one or more embodiments, the kernel LiMnx Fe 1-x In PO4, x satisfies 0.6 ≤ x ≤ 0.7.

[0008] In one or more embodiments, the metal-organic framework is selected from one or more of aluminum-based MOFs, iron-based MOFs, copper-based MOFs, zinc-based MOFs, cerium-based MOFs, zirconium-based MOFs, and titanium-based MOFs.

[0009] In one or more embodiments, the metal oxide is selected from one or more of Al2O3, Fe2O3, CuO, ZnO, CeO2, ZrO2 and TiO2, preferably one or more of Al2O3, ZnO and CeO2.

[0010] In one or more embodiments, the conductive polymer is selected from one or more of poly(3,4-ethylenedioxythiophene):polystyrene sulfonate, sulfonated polyaniline, and sulfonated polypyrrole.

[0011] In one or more embodiments, the carbon material is selected from one or more of carboxylated carbon nanotubes, graphene oxide, and aminated carbon nanotubes.

[0012] In one or more embodiments, the aluminum-based MOF is selected from one or more of MIL-53(Al), MIL-100(Al), Al-BDC, and CAU-10-H.

[0013] In one or more embodiments, the iron-based MOF is selected from one or both of MIL-53(Fe) and MnFe-MOF.

[0014] In one or more embodiments, the copper-based MOF is selected from one or both of Cu3(HITP)2 and Cu-BTC.

[0015] In one or more embodiments, the zinc-based MOF is selected from one or more of ZIF-8, MOF-5, and MOF-177.

[0016] In one or more embodiments, the cerium-based MOF is selected from one or more of Ce-BDC, Ce-BTC, and Ce-UiO-66.

[0017] In one or more embodiments, the zirconium-based MOF is selected from one or more of UiO-66, UiO-67 and MOF-808.

[0018] In one or more embodiments, the titanium-based MOF is selected from one or both of MIL-125(Ti) and NH2-MIL-125(Ti).

[0019] In one or more embodiments, the thickness of the chemical anchoring layer is 5-50 nm, preferably 10-30 nm.

[0020] In one or more embodiments, the pore size of the chemical anchoring layer is 2-50 nm, preferably 5-20 nm.

[0021] In one or more embodiments, the particle size of the metal oxide is 5-50 nm, preferably 10-30 nm.

[0022] In one or more embodiments, the thickness of the multifunctional composite layer is 3-30 nm, preferably 5-15 nm.

[0023] In one or more embodiments, the D50 particle size of the lithium manganese iron phosphate material is 0.5-3 μm, preferably 1-2 μm.

[0024] The present invention also provides a method for preparing the lithium manganese iron phosphate material according to any embodiment of the present invention, the method comprising: (1) Add lithium source, iron source, manganese source, phosphorus source and chelating agent to water, mix evenly to obtain wet gel; (2) The wet gel is dried and pre-calcined to obtain lithium manganese iron phosphate precursor powder; (3) The lithium manganese iron phosphate precursor powder is dispersed in a solution containing a metal source, an organic ligand and an organic solvent, and then subjected to solvothermal reaction, drying and heat treatment to obtain material A; (4) The material A is mixed with a coating liquid containing conductive polymer and carbon material and dried to obtain lithium manganese iron phosphate material.

[0025] In one or more embodiments, the heat treatment includes: heating to 350-650°C and holding at that temperature for 3-8 hours.

[0026] In some preferred embodiments, the heat treatment is a gradient heat treatment, which includes: first heating to 350-450℃ and holding for 1-3 hours, then heating to 500-650℃ and holding for 2-5 hours.

[0027] In one or more embodiments, the molar ratio of lithium in the lithium source, manganese in the manganese source and iron in the iron source satisfies: (n(Mn)+n(Fe)):n(Li) =1, and 0.1≤n(Mn):n(Li)≤0.9.

[0028] In one or more embodiments, the molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and phosphorus in the phosphorus source satisfies: n(P):(n(Li)+n(Mn)+n(Fe))=1:2.

[0029] In one or more embodiments, the molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source and the chelating agent satisfies: n(chelating agent):(n(Li)+n(Mn)+n(Fe))=(1.2-1.5):1.

[0030] In one or more embodiments, the lithium source is selected from one or more of lithium carbonate, lithium acetate, and lithium nitrate.

[0031] In one or more embodiments, the manganese source is selected from one or more of manganese sulfate, manganese carbonate, manganese nitrate, manganese oxalate, manganese acetate, and manganese chloride.

[0032] In one or more embodiments, the iron source is selected from one or more of ferrous sulfate, ferrous chloride, ferrous bromide, ferrous oxalate, ferrous acetate, and ferrous nitrate.

[0033] In one or more embodiments, the phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and potassium dihydrogen phosphate.

[0034] In one or more embodiments, the chelating agent is selected from one or more of citric acid, ascorbic acid, and ethylenediaminetetraacetic acid.

[0035] In one or more embodiments, the metal source is selected from one or more of aluminum, iron, copper, zinc, cerium, zirconium, and titanium; the aluminum source is selected from one or more of aluminum isopropoxide, aluminum nitrate, and aluminum chloride; the iron source is selected from one or more of ferric chloride, ferrous oxalate, and ferric phosphate; the copper source is selected from one or more of copper chloride, copper nitrate, copper acetate, and copper sulfate; the zinc source is selected from one or more of zinc nitrate, zinc nitrate hexahydrate, zinc acetate dihydrate, and zinc chloride; the cerium source is selected from one or more of cerium nitrate, cerium chloride, and cerium sulfate; the zirconium source is selected from one or more of zirconium tetrachloride, zirconium oxychloride, and zirconium oxynitrate; and the titanium source is selected from one or more of tetrabutyl titanate, tetraisopropyl titanate, and tetraethyl titanate.

[0036] In one or more embodiments, the organic ligand is selected from one or more of terephthalic acid, trimesic acid, 2-aminoterephthalic acid, and 2-methylimidazole.

[0037] In one or more embodiments, the organic solvent is selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone, methanol, and anhydrous ethanol.

[0038] In one or more embodiments, the mass ratio of the lithium manganese iron phosphate precursor powder to the metal source is 1:(0.05-0.5), preferably 1:(0.1-0.3).

[0039] In one or more embodiments, the mass ratio of the lithium manganese iron phosphate precursor powder to the organic ligand is 1:(0.03-0.3), preferably 1:(0.05-0.2).

[0040] In one or more embodiments, the mass ratio of material A to the conductive polymer is 1:(0.005-0.05), preferably 1:(0.01-0.03).

[0041] In one or more embodiments, the mass ratio of material A to the carbon material is 1:(0.001-0.02), preferably 1:(0.003-0.01).

[0042] In one or more embodiments, the mass fraction of the conductive polymer in the coating solution is 0.5%-5%.

[0043] In one or more embodiments, the mass fraction of carbon material in the coating liquid is 0.05%-1%.

[0044] In one or more embodiments, the solvent in the coating solution is selected from one or more of deionized water, anhydrous ethanol, and a mixture of deionized water and ethanol.

[0045] In one or more embodiments, in step (1), the pH of the solution is 3.0-5.0.

[0046] In one or more embodiments, in step (1), the mixture is stirred in a water bath at a temperature of 60-90°C for 4-6 hours and at a speed of 200-500 rpm.

[0047] In one or more embodiments, in step (2), vacuum drying is used, the drying temperature is 100-150℃, and the drying time is 10-15h.

[0048] In one or more embodiments, in step (2), the gas is pre-fired in an inert atmosphere at a temperature of 600-800°C for 4-10 hours. The inert atmosphere is nitrogen or argon.

[0049] In one or more embodiments, in step (3), ultrasonic dispersion is used, with an ultrasonic power of 300-500W and an ultrasonic time of 30-60min.

[0050] In one or more embodiments, in step (3), the solvothermal reaction temperature is 80-150°C and the reaction time is 12-36h.

[0051] In one or more embodiments, in step (3), vacuum drying is used, the drying temperature is 50-80℃, and the drying time is 10-15h.

[0052] In one or more embodiments, in step (3), heat treatment is performed under an inert atmosphere, which is nitrogen or argon.

[0053] In one or more embodiments, in step (3), the heating rate of the heat treatment is 1-5 °C / min.

[0054] In one or more embodiments, in step (4), stirring is used for mixing for a time of 1-6 hours, preferably 2-4 hours, and the mixing rate is 200-1000 rpm, preferably 400-600 rpm.

[0055] In one or more embodiments, in step (4), the drying is vacuum drying or spray drying. The temperature of vacuum drying is 60-120°C, preferably 80-100°C, and the time of vacuum drying is 4-12h, preferably 8-12h. The inlet temperature of spray drying is 150-250°C, preferably 180-220°C, the outlet temperature is 80-110°C, preferably 90-100°C, and the time of spray drying is 5-30s.

[0056] The present invention also provides a lithium manganese iron phosphate material prepared by the method described in any embodiment of the present invention.

[0057] The present invention also provides a positive electrode sheet comprising the lithium manganese iron phosphate material described in any embodiment of the present invention.

[0058] The present invention also provides a lithium-ion battery comprising the above-described positive electrode.

[0059] The present invention also provides an electrical device comprising the above-described lithium-ion battery.

[0060] This invention overcomes the problems of limited functionality and insufficient long-term stability of the surface coating layer in existing lithium manganese iron phosphate materials by providing a lithium manganese iron phosphate cathode material with a dual chemical anchoring interface. Through the synergistic effect of the "inner chemical anchoring layer" and the "outer multifunctional conductive network," this material achieves efficient capture and physical shielding of dissolved manganese ions, significantly improving the material's high-temperature cycling stability. Detailed Implementation

[0061] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used herein are explained and defined in general terms below. Unless otherwise specified, all technical and scientific terms used herein have the common meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0062] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0063] In this document, the terms “contains,” “includes,” “containing,” and similar terms encompass the meanings of “basically composed of” and “composed of.” For example, when this document discloses “A contains B and C,” “A is basically composed of B and C” and “A is composed of B and C” should be considered as having been disclosed in this document.

[0064] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0065] Unless otherwise specified, percentages refer to mass percentages and proportions refer to mass ratios in this article.

[0066] In this article, the sum of the percentages of all components in the composition is 100%.

[0067] In this document, when describing embodiments or examples, it should be understood that it is not intended to limit the invention to those embodiments or examples. Rather, all alternatives, modifications, and equivalents of the methods and materials described herein are covered within the scope of this invention.

[0068] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0069] The functionalized carbon materials in this invention refer to carbon materials.

[0070] This invention provides a lithium manganese iron phosphate material, comprising a core and a chemical anchoring layer and a multifunctional composite layer sequentially coated on the surface of the core, wherein the core is LiMn. x Fe 1-xPO4, where 0.1≤x≤0.9, the chemical anchoring layer is formed by in-situ carbonization of a metal-organic framework, containing a carbon skeleton and metal oxides dispersed in the carbon skeleton, and the multifunctional composite layer is formed by cross-linking of conductive polymers and carbon materials.

[0071] In this invention, the kernel LiMn x Fe 1-x In PO4, x satisfies 0.1≤x≤0.9, preferably 0.6≤x≤0.7, for example, x is 0.6, 0.65, or 0.7.

[0072] In this invention, the metal-organic framework can be selected from one or more of aluminum-based MOFs, iron-based MOFs, copper-based MOFs, zinc-based MOFs, cerium-based MOFs, zirconium-based MOFs, and titanium-based MOFs.

[0073] In this invention, the metal oxide may be selected from one or more of Al2O3, Fe2O3, CuO, ZnO, CeO2, ZrO2 and TiO2.

[0074] In some preferred embodiments, the metal oxide may be selected from one or more of Al2O3, ZnO and CeO2.

[0075] In this invention, the chemical anchoring layer can be formed by in-situ carbonization transformation of at least one of aluminum-based MOF, iron-based MOF, copper-based MOF, zinc-based MOF, cerium-based MOF, zirconium-based MOF or titanium-based MOF, and includes uniformly dispersed metal oxide nanoparticles and a porous carbon framework derived from organic ligands.

[0076] Among them, aluminum-based MOFs can be selected from one or more of MIL-53(Al), MIL-100(Al), Al-BDC, and CAU-10-H. Iron-based MOFs can be selected from one or two of MIL-53(Fe) and MnFe-MOF. Copper-based MOFs can be selected from one or two of Cu3(HITP)2 and Cu-BTC. Zinc-based MOFs can be selected from one or more of ZIF-8, MOF-5, and MOF-177. Cerium-based MOFs can be selected from one or more of Ce-BDC, Ce-BTC, and Ce-UiO-66. Zirconium-based MOFs can be selected from one or more of UiO-66, UiO-67, and MOF-808. Titanium-based MOFs can be selected from one or two of MIL-125(Ti) and NH2-MIL-125(Ti).

[0077] Different metal oxides can react with dissolved Mn through various mechanisms 2+ Chemical reactions occur; for example, the surfaces of Al₂O₃, ZrO₂, and TiO₂ are rich in Lewis acid sites and oxygen vacancies, enabling them to react with Mn. 2+Chemisorption occurs, forming stable Mn-OM bonds; CeO2 possesses unique redox properties and abundant oxygen vacancies, enabling efficient chemisorption of Mn. 2+ It also generates thermodynamically stable manganate salts (such as MnCeO3); Fe2O3 can form a synergistic effect with Fe in lithium iron manganese materials, improving the stability of the interface structure; CuO and ZnO can provide active interfaces and fix Mn through ion exchange mechanisms. 2+ Cu-based MOF derivatives also have the ability to enrich Mn 4+ It has the unique function of inhibiting disproportionation reactions.

[0078] Furthermore, the mesoporous carbon framework formed by MOF derivation not only provides lithium-ion transport channels but also increases the interaction between metal oxides and Mn. 2+ The increased contact area improves anchoring efficiency. The MOF layer is grown in situ on the LMFP surface, and the metal oxide formed after heat treatment is chemically bonded to the core, resulting in a strong interfacial bond that is not easily detached.

[0079] In this invention, the conductive polymer may be selected from one or more of poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS), sulfonated polyaniline (SPANi), and sulfonated polypyrrole (SPPy).

[0080] In this invention, the carbon material can be selected from one or more of carboxylated carbon nanotubes (CNT-COOH), graphene oxide (GO), and aminated carbon nanotubes (CNT-NH2).

[0081] In this invention, the multifunctional composite layer is cross-linked from a conductive polymer with cation exchange function and a functionalized carbon material. It not only provides physical shielding and enhanced conductivity, but also endows the material with a second layer of chemical anchoring capability. The principle is as follows: Ion exchange harvesting: The sulfonic acid groups (-SO3H) in conductive polymers (such as PEDOT:PSS) are negatively charged and can actively adsorb and exchange positively charged Mn. 2+ This creates an "ion sieve" effect, preventing trace amounts of Mn from "escaping" from the inner layer. 2+ Secondary harvesting; Three-dimensional conductive network: Functionalized carbon materials (such as CNT-COOH) can form a three-dimensional framework in the coating layer, which can work together with conductive polymers to build a highly conductive network and reduce interfacial impedance; Dynamic hydrogen bond self-healing: The sulfonic acid groups in the conductive polymer form reversible hydrogen bonds with the carboxyl / amino groups in the carbon material, giving the coating a certain self-healing ability. When microcracks occur, they can heal themselves and maintain the integrity of the interface.

[0082] In this invention, the thickness of the chemical anchoring layer can be 5-50 nm, preferably 10-30 nm, such as 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, 22 nm, 24 nm, 26 nm, 28 nm, and 30 nm. If the chemical anchoring layer is too thin, there will be insufficient anchoring points; if it is too thick, it will hinder lithium-ion diffusion and increase interfacial impedance. Controlling the thickness of the chemical anchoring layer within the above-mentioned range helps to improve the high-temperature stability of lithium manganese iron phosphate materials and reduce the dissolution rate of manganese ions.

[0083] In this invention, the pore size of the chemical anchoring layer can be 2-50 nm, preferably 5-20 nm, such as 5 nm, 8 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, and 20 nm. The mesoporous carbon framework (porous carbon framework) formed by heat treatment of organic ligands has a porous structure that is beneficial for electrolyte wetting and lithium-ion transport, and also increases the interaction between metal oxides and Mn. 2+ The contact area. By controlling the pore size of the chemical anchoring layer within the above range, sufficient specific surface area can be ensured for anchoring Mn. 2+ This also avoids the structural strength reduction caused by excessively large pores. MOF-derived materials typically have high porosity, and their pore size can be adjusted by selecting different MOF precursors and controlling heat treatment conditions.

[0084] In this invention, the particle size of the metal oxide can be 5-50 nm, preferably 10-30 nm, such as 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, 22 nm, 24 nm, 26 nm, 28 nm, and 30 nm. The metal oxide nanoparticles are derived from the metal nodes of MOFs, and their particle size directly affects their specific surface area and the number of anchoring sites. Within the aforementioned particle size range, the metal oxide can possess a high specific surface area and provide abundant surface active sites (such as oxygen vacancies) and Mn. 2+ Chemisorption occurs.

[0085] In this invention, the thickness of the multifunctional composite layer can be 3-30nm, preferably 5-15nm, such as 5nm, 8nm, 10nm, 12nm, 14nm, and 15nm.

[0086] If the thickness of the multifunctional composite layer is too thin, it cannot effectively isolate the electrolyte, making it difficult to suppress side reactions on the material surface (such as electrolyte decomposition and HF erosion); at the same time, an excessively thin multifunctional composite layer will affect the Mn content. 2+ Insufficient physical barriers and ion exchange capture capabilities will result in an incomplete three-dimensional conductive network and discontinuous electron conduction paths.

[0087] If the multifunctional composite layer is too thick, it will increase the resistance to lithium-ion transport, leading to increased interfacial impedance and affecting rate performance. Furthermore, an excessively thick oxide / polymer layer may also disrupt the electronic connection between the active material and the conductive agent, reducing the overall volumetric energy density of the material. In addition, when the outer polymer layer is too thick, the active sites of the inner chemical anchoring layer are excessively shielded, affecting Mn... 2+ It is difficult to contact the inner metal oxide layer.

[0088] In this invention, the D50 particle size of the lithium manganese iron phosphate material can be 0.5-3μm, preferably 1-2μm, such as 1μm, 1.5μm, or 2μm.

[0089] In the lithium manganese iron phosphate material of the present invention, the two-layer structure of the chemical anchoring layer and the multifunctional composite layer forms a dual protection system of "inner layer chemical anchoring as the main function and outer layer dynamic capture as the auxiliary function": the inner porous metal oxide layer is responsible for efficiently chemically fixing most of the dissolved manganese ions; the outer conductive polymer layer provides a conductive path on the one hand, and acts as a "second line of defense" to capture a very small amount of escaped Mn on the other hand. 2+ At the same time, it physically prevents further corrosion from the electrolyte. This dual chemical anchoring strategy fundamentally solves the problem of manganese ion migration to the negative electrode from a mechanistic perspective.

[0090] The present invention also provides a method for preparing the lithium manganese iron phosphate material of the present invention, the method comprising: (1) Add lithium source, iron source, manganese source, phosphorus source and chelating agent to water, mix evenly to obtain wet gel; (2) The wet gel is dried and pre-calcined to obtain lithium manganese iron phosphate precursor powder; (3) The lithium manganese iron phosphate precursor powder is dispersed in a solution containing a metal source, an organic ligand and an organic solvent, and then subjected to solvothermal reaction, drying and heat treatment to obtain material A; (4) The material A is mixed with a coating liquid containing conductive polymer and carbon material and dried to obtain lithium manganese iron phosphate material.

[0091] In this invention, the molar ratio of lithium in the lithium source, manganese in the manganese source, and iron in the iron source can satisfy: (n(Mn)+n(Fe)):n(Li) =1, and 0.1≤n(Mn):n(Li)≤0.9.

[0092] In this invention, the molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and phosphorus in the phosphorus source can satisfy: n(P):(n(Li)+n(Mn)+n(Fe))=1:2.

[0093] In this invention, the molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and chelating agent can satisfy: n(chelating agent):(n(Li)+n(Mn)+n(Fe))=(1.2-1.5):1, for example 1.2:1, 1.3:1, 1.4:1, 1.5:1.

[0094] In this invention, the lithium source can be selected from one or more of lithium carbonate, lithium acetate, and lithium nitrate.

[0095] In this invention, the manganese source can be selected from one or more of manganese sulfate, manganese carbonate, manganese nitrate, manganese oxalate, manganese acetate, and manganese chloride.

[0096] In this invention, the iron source can be selected from one or more of ferrous sulfate, ferrous chloride, ferrous bromide, ferrous oxalate, ferrous acetate, and ferrous nitrate.

[0097] In this invention, the phosphorus source may be selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and potassium dihydrogen phosphate.

[0098] In this invention, the chelating agent may be selected from one or more of citric acid, ascorbic acid, and ethylenediaminetetraacetic acid.

[0099] In this invention, the metal source can be selected from one or more of aluminum, iron, copper, zinc, cerium, zirconium and titanium sources.

[0100] In this invention, the iron source can be selected from one or more of ferric chloride, ferrous oxalate (FeC2O4·2H2O) and ferric phosphate (FePO4).

[0101] In this invention, the copper source can be selected from one or more of copper chloride, copper nitrate (Cu(NO3)2·3H2O), copper acetate (Cu(CH3COO)2·H2O), and copper sulfate (CuSO4·5H2O).

[0102] In this invention, the zinc source can be selected from one or more of zinc nitrate, zinc nitrate hexahydrate (Zn(NO3)2·6H2O), zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and zinc chloride (ZnCl2).

[0103] In this invention, the zirconium source can be selected from one or more of zirconium tetrachloride (ZrCl4), zirconium oxychloride (ZrOCl2·8H2O), and zirconium oxynitrate (ZrO(NO3)2).

[0104] In this invention, the titanium source can be selected from one or more of tetrabutyl titanate, tetraisopropyl titanate, and tetraethyl titanate.

[0105] In this invention, the aluminum source can be selected from one or more of aluminum isopropoxide, aluminum nitrate (Al(NO3)3·9H2O) and aluminum chloride (AlCl3·6H2O).

[0106] In this invention, the cerium source can be selected from one or more of cerium nitrate (Ce(NO3)3·6H2O), cerium chloride (CeCl3·7H2O), and cerium sulfate (Ce2(SO4)3).

[0107] In this invention, the organic ligand may be selected from one or more of terephthalic acid, pyromellitic acid, 2-aminoterephthalic acid, and 2-methylimidazole.

[0108] In this invention, the organic solvent may be selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone, methanol, and anhydrous ethanol.

[0109] In this invention, the mass ratio of lithium manganese iron phosphate precursor powder to metal source can be 1:(0.05-0.5), preferably 1:(0.1-0.3), for example 1:0.1, 1:0.12, 1:0.14, 1:0.16, 1:0.18, 1:0.2, 1:0.24, 1:0.26, 1:0.28, 1:0.3.

[0110] By controlling the mass ratio of lithium manganese iron phosphate precursor powder to metal source within the above range, it can be ensured that a continuous and uniform chemical anchoring layer (MOF coating) can be formed on the surface of lithium manganese iron phosphate (LMFP) particles. If the amount of metal source is too low, the chemical anchoring layer cannot completely cover the particle surface, resulting in insufficient anchoring points and limited manganese dissolution inhibition effect. If the amount of metal source is too high, the chemical anchoring layer will be too thick, which will lead to: (1) an extended lithium-ion diffusion path and increased interfacial impedance; (2) excessive metal oxide content after heat treatment, which may affect the overall electrochemical performance of the material; and (3) increased cost.

[0111] In this invention, the mass ratio of lithium manganese iron phosphate precursor powder to organic ligand can be 1:(0.03-0.3), preferably 1:(0.05-0.2), for example 1:0.05, 1:0.1, 1:0.12, 1:0.14, 1:0.16, 1:0.18, 1:0.2.

[0112] The amount of organic ligands used needs to be considered in conjunction with the metal source. In the synthesis of chemical anchoring layers, the molar ratio of metal source ions to organic ligands is a key parameter that determines the crystal structure, crystallinity, and morphology of MOFs.

[0113] Controlling the mass ratio of lithium manganese iron phosphate precursor powder to organic ligands within the aforementioned range ensures sufficient coordination of the organic ligands with the metal ions to form a complete MOF framework structure. This avoids the formation of an excessively thick carbon layer after heat treatment due to excessive organic ligands, which increases interfacial impedance; it also prevents residual excessive organic ligands from affecting material purity.

[0114] In this invention, the mass ratio of material A to the conductive polymer can be 1:(0.005-0.05), preferably 1:(0.01-0.03), for example 1:0.01, 1:0.015, 1:0.02, 1:0.025, 1:0.03.

[0115] In this invention, the mass ratio of material A to carbon material can be 1:(0.001-0.02), preferably 1:(0.003-0.01), for example 1:0.003, 1:0.004, 1:0.006, 1:0.008, 1:0.01.

[0116] In this invention, the mass fraction of the conductive polymer in the coating liquid can be 0.5%-5%, for example 0.5%, 1%, 2%, 3%, 4%, 5%.

[0117] In this invention, the mass fraction of carbon material in the coating liquid can be 0.05%-1%, for example 0.05%, 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, or 1%.

[0118] In this invention, the solvent in the coating solution can be selected from one or more of deionized water, anhydrous ethanol, and a mixture of deionized water and ethanol.

[0119] In step (1), the pH of the solution can be 3.0-5.0, for example 3.0, 4.0, 5.0.

[0120] In step (1), the mixing method can be stirring in a water bath. The water bath temperature can be 60-90℃, for example, 60℃, 70℃, 80℃, or 90℃. The mixing time can be 4-6h, for example, 4h, 5h, or 6h. The mixing speed can be 200-500rpm, for example, 200rpm, 300rpm, 400rpm, or 500rpm.

[0121] In step (2), vacuum drying can be used. The drying temperature can be 100-150℃, such as 100℃, 120℃, 130℃, 140℃, 150℃, and the drying time can be 10-15h, such as 10h, 12h, 14h, 15h.

[0122] In step (2), pre-burning can be carried out in an inert atmosphere. The pre-burning temperature can be 600-800℃, for example, 600℃, 700℃, 800℃. The pre-burning time can be 4-10h, for example, 4h, 5h, 6h, 7h, 8h, 9h, 10h. The inert atmosphere can be nitrogen or argon.

[0123] In step (3), ultrasonic dispersion can be used. The ultrasonic power can be 300-500W, for example 300W, 400W, 500W, and the ultrasonic time can be 30-60min, for example 30min, 40min, 50min, 60min.

[0124] In step (3), the solvothermal reaction temperature can be 80-150℃, for example 80℃, 100℃, 120℃, 140℃, 150℃, and the reaction time can be 12-36h, for example 12h, 20h, 22h, 26h, 30h, 32h, 36h. Through solvothermal reaction, a MOF layer can be grown in situ on the surface of lithium manganese iron phosphate particles to form LiMn. x Fe 1-x PO4@MOF (LMFP@MOF) core-shell composite material.

[0125] In step (3), vacuum drying can be used. The drying temperature can be 50-80℃, for example 50℃, 60℃, 70℃, 80℃, and the drying time can be 10-15h, for example 10h, 12h, 14h, 15h.

[0126] In this invention, the heat treatment includes: heating to 350-650℃ and holding at that temperature for 3-8 hours. The heat treatment temperature can be 350-650℃, for example, 350℃, 400℃, 450℃, 500℃, 550℃, 600℃, or 650℃, and the heat treatment time can be 3-8 hours, for example, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, or 8 hours.

[0127] In some preferred embodiments, the heat treatment is a gradient heat treatment, which preferably includes: first heating to a first temperature of 350-450°C and holding for 1-3 hours, then heating to a second temperature of 500-650°C and holding for 2-5 hours.

[0128] In some preferred embodiments, the organic ligands are first held at 350-450℃ for 1-3 hours to partially carbonize them, forming a mesoporous carbon framework. Then, the temperature is raised to 500-650℃ and held for 2-5 hours to convert the metal nodes in the MOF layer into metal oxide nanoparticles, which are then uniformly embedded in the porous carbon layer in LiMn. x Fe 1-x A carbide MOF layer containing metal oxides, i.e. a chemical anchoring layer, is formed on the PO4 surface to obtain the final product.

[0129] In some preferred embodiments, the first temperature is 350-450°C, for example 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 420°C, 440°C, 450°C, and the holding time at the first temperature is 1-3 hours, for example 1 hour, 2 hours, 3 hours.

[0130] In some preferred embodiments, the first temperature is 380-420°C, for example 380°C, 400°C, 410°C, 420°C, and the holding time at the first temperature is 2-3 hours, for example 2 hours, 2.5 hours, 3 hours.

[0131] If the first temperature is too low (<350℃), on the one hand, the organic ligands will not be fully pyrolyzed, the carboxyl groups in the MOF framework will not be effectively removed, and the carbon framework will be difficult to form effectively; on the other hand, the metal nodes will not be able to form oxide nuclei in advance, resulting in the metal oxide particles obtained in the subsequent high-temperature stage being larger in size and unevenly distributed; at the same time, the mesoporous structure of the carbon framework will not be fully developed, and the specific surface area will be lower, resulting in a reduction of anchoring points.

[0132] If the initial temperature is too high (>450℃), the following problems may occur: the organic ligands will pyrolyze too quickly and the gas release rate will be too high, which may cause the pore structure to shrink drastically or even collapse; the metal nodes may be over-reduced at low temperatures, partially converting to a metallic state and losing their chemical anchoring activity; the graphitization degree of the carbon skeleton will be too high and the mesoporous structure will be reduced, which is not conducive to electrolyte wetting and interaction with Mn. 2+ Contact.

[0133] In some preferred embodiments, the second temperature is 500-650°C, for example 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 580°C, 600°C, 620°C, 640°C, or 650°C, and the holding time at the second temperature is 2-5 hours, for example 2 hours, 3 hours, 4 hours, or 5 hours.

[0134] In some more preferred embodiments, the second temperature is 550-620°C, for example 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, and the holding time at the second temperature is 3-4 hours, for example 3 hours, 3.5 hours, 4 hours.

[0135] If the second temperature is too low (<500℃), on the one hand, the MOF metal nodes cannot be completely converted into metal oxides, the MOF framework remains, and the chemical anchoring function is incomplete; on the other hand, the graphitization degree of the carbon framework is insufficient, the electronic conductivity is poor, and the rate performance of the material is affected; at the same time, the resulting material has low crystallinity and unstable crystal structure.

[0136] If the second temperature is too high (>650℃), high-temperature side effects will occur: metal oxide nanoparticles will undergo severe aggregation and growth, the specific surface area will decrease sharply, and a large number of surface active sites (oxygen vacancies) will be annihilated; the carbon skeleton will be excessively graphitized, the mesoporous structure will collapse, and the lithium-ion transport channels will be blocked; the metal oxide may also be reduced to a metallic state by carbothermal processes, losing its chemically adsorbed Mn. 2+ Furthermore, the lithium manganese iron phosphate core itself may undergo excessive crystal growth at excessively high temperatures, resulting in obvious particle agglomeration under electron microscopy.

[0137] In this invention, the heating rate of the heat treatment is preferably 1-5℃ / min, for example 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, or 5℃ / min.

[0138] In this invention, the heat treatment is preferably carried out under an inert atmosphere, which can be nitrogen or argon.

[0139] In step (4), stirring can be used for mixing. The mixing time can be 1-6 hours, preferably 2-4 hours, such as 2 hours, 3 hours, or 4 hours. The mixing rate can be 200-1000 rpm, preferably 400-600 rpm, such as 400 rpm, 500 rpm, or 600 rpm.

[0140] In step (4), the drying can be vacuum drying or spray drying. The temperature of vacuum drying can be 60-120℃, preferably 80-100℃, such as 80℃, 90℃, 100℃, and the time of vacuum drying can be 4-12h, preferably 8-12h, such as 8h, 9h, 10h, 11h, 12h.

[0141] The inlet temperature of the spray dryer can be 150-250℃, preferably 180-220℃, such as 180℃, 190℃, 200℃, 210℃, or 220℃, and the outlet temperature can be 80-110℃, preferably 90-100℃, such as 90℃, 92℃, 94℃, 96℃, 98℃, or 100℃. The spray drying time can be 5-30 seconds, such as 5 seconds, 10 seconds, 15 seconds, 20 seconds, 25 seconds, or 30 seconds.

[0142] In some implementations, the powder obtained in step (3) is dispersed in a coating liquid containing conductive polymer and functionalized carbon material. After stirring evenly, the conductive polymer and functionalized carbon material can be self-assembled and deposited on the particle surface through electrostatic adsorption and hydrogen bonding. Then, the powder is spray-dried or vacuum-dried to obtain lithium manganese iron phosphate cathode material with dual chemical anchoring interfaces.

[0143] The present invention also provides lithium manganese iron phosphate materials prepared by the method described herein.

[0144] The present invention also provides a positive electrode sheet comprising the aforementioned lithium manganese iron phosphate material. The positive electrode sheet is manufactured by coating an aluminum foil current collector with a positive electrode material comprising the lithium manganese iron phosphate material, a conductive agent, a binder, and a solvent, followed by drying and roll forming.

[0145] The solvent for the positive electrode slurry can be N-methylpyrrolidone (NMP). The conductive agent for the positive electrode can be one or more of conductive carbon black, conductive graphite, acetylene black, carbon nanotubes, carbon nanofibers, graphene, and VGCF. The binder for the positive electrode can be one or more of polyvinylidene fluoride (PVDF), PVDF-HFP, PTFE, and polyimide.

[0146] The percentage of each solid substance in the positive electrode slurry by mass can be conventional. For example, the mass percentage of lithium manganese iron phosphate material can be 92-99%, preferably 95-98%; the mass percentage of conductive agent can be 0.5-4%, preferably 0.5-2%; the mass percentage of binder can be 0.5-4%, preferably 0.5-2%; and the mass percentage of solvent in the slurry can be 30-50%, preferably 35-45%. More preferably, the weight percentage of solvent in the positive electrode slurry is 40%, and the mass percentage of solid substances is 60%. Specifically, in the total mass of solid substances, the mass percentage of positive electrode material can be 97%, the mass percentage of conductive agent can be 1.5%, and the mass percentage of binder can be 1.5%.

[0147] The present invention also provides a lithium-ion battery, which includes: a positive electrode, a separator, and a negative electrode. The positive electrode is the positive electrode of the present invention, the separator can be a separator commonly used in the art (such as a polypropylene microporous membrane), and the negative electrode can be a negative electrode commonly used in the art (such as lithium metal or graphite).

[0148] In this invention, the positive and negative electrode sheets and the separator are first assembled in the order of negative electrode sheet-separator-positive electrode sheet-separator to obtain a bare cell. Then, a lithium-ion battery with a capacity of 10Ah is obtained by sealing, ultrasonic welding, top sealing, vacuum baking, electrolyte injection, wetting, formation and aging, secondary sealing, and capacity testing. The electrolyte is a commonly used electrolyte in the art that is compatible with the above system.

[0149] The present invention also provides an electrical device comprising the above-described lithium-ion battery.

[0150] The beneficial effects of this invention include: (1) Dual chemical anchoring, highly efficient suppression of manganese leaching: The synergistic effect of the chemical adsorption of metal oxides in the inner chemical anchoring layer and the ion exchange of the outer conductive polymer reduces the amount of manganese deposited on the negative electrode by about 90% after cycling; (2) MOF materials are flexible in selection and have strong applicability: different MOF precursors can be used to derive a variety of metal oxides, which can be flexibly selected according to cost and process requirements, and all of them can achieve chemical anchoring function. (3) Excellent high-temperature cycling performance: At a high temperature of 55°C, the capacity retention rate of the material of the present invention can reach 85% or even more than 90% after 1000 cycles, which is far superior to the material with a single coating layer. (4) Good conductivity and rate performance: The outer three-dimensional conductive network effectively reduces electrode polarization and makes up for the lack of conductivity of the metal oxide layer; (5) The preparation process is controllable and suitable for large-scale production: the in-situ growth + self-assembly method is adopted, the process conditions are mild, the raw materials are widely available, and it is suitable for industrial production.

[0151] The present invention will be described below by way of specific embodiments. It should be understood that these embodiments are merely illustrative and are not intended to limit the scope of the invention. The methods, reagents, and materials used in the embodiments and comparative examples are conventional methods, reagents, and materials in the art, unless otherwise stated. The starting material compounds in the embodiments and comparative examples are all commercially available.

[0152] In Examples 1-3, the thickness of the chemical anchoring layer is in the range of 10-30 nm, the pore size of the chemical anchoring layer is in the range of 5-20 nm, the particle size of the metal oxide in the chemical anchoring layer is in the range of 10-30 nm, the thickness of the multifunctional composite layer is in the range of 5-15 nm, and the D50 particle size of the lithium manganese iron phosphate material is in the range of 1-2 μm.

[0153] Example 1

[0154] The preparation steps of the lithium manganese iron phosphate material in Example 1 are as follows: (1) Preparation of lithium manganese iron phosphate precursor by sol-gel method: Li₂CO₃, MnCO₃, FeC₂O₄·2H₂O, and NH₄H₂PO₄ were weighed as raw materials according to the molar ratio of n(Li):n(Mn):n(Fe):n(P) = 1:0.6:0.4:1. At the same time, an appropriate amount of citric acid was weighed as a chelating agent. The molar ratio of citric acid to metal ions satisfied n(citric acid):(n(Li)+n(Mn)+n(Fe)) = 1.5:1. Dissolve the above raw materials in deionized water, adjust the pH of the solution to 4.0 with ammonia, and stir in an 80°C water bath for 4 hours at a stirring speed of 350 rpm to form a wet gel. The wet gel was dried in a vacuum drying oven at 120°C for 12 hours to obtain a dry gel. The dried gel was then pre-calcined at 700°C for 6 hours under a nitrogen atmosphere to obtain lithium iron manganese phosphate powder, denoted as LiMn. 0.6Fe 0.4 PO4 (LMFP).

[0155] (2) Preparation of MIL-53(Al) MOF layer

[0156] Dissolve 0.6 g of AlCl3·6H2O and 0.4 g of terephthalic acid in 100 mL of DMF to form a mixed solution; Weigh 5g of the prepared LMFP powder and disperse it in 100mL of the above mixed solution. Disperse the mixture ultrasonically for 30 minutes at a power of 300W to obtain the mixed solution. The mixed solution was transferred to a 200 mL stainless steel high-pressure reactor lined with polytetrafluoroethylene for a solvothermal reaction at a temperature of 150 °C for 24 hours. After the reaction was completed, the product was naturally cooled to room temperature. After washing the product three times with DMF and methanol respectively, the filter residue was vacuum dried at 60°C for 12 hours to obtain LMFP@MIL-53(Al) core-shell composite material.

[0157] (3) Preparation of chemical anchoring layer

[0158] The dried LMFP@MIL-53(Al) composite material was placed in a tube furnace and heated to 400°C at a rate of 2°C / min under nitrogen protection, held for 2 hours, and then heated to 600°C at a rate of 3°C / min, held for 3 hours, for gradient heat treatment. It was then naturally cooled to room temperature to obtain lithium manganese iron phosphate material with an Al2O3 / C chemical anchoring layer, denoted as LMFP@Al2O3 / C.

[0159] (4) Preparation of multifunctional composite layer

[0160] Add 0.5g of PEDOT:PSS to 100mL of deionized water and stir magnetically for 30 minutes to obtain a well-mixed solution. Weigh 0.05g of carboxylated carbon nanotubes (CNT-COOH), add them to the above solution, and ultrasonically disperse for 1 hour to obtain a uniform and stable coating solution; 10g of the prepared LMFP@Al2O3 / C powder was weighed and added to the above coating solution. The mixture was magnetically stirred for 2 hours at a stirring speed of 500 rpm. Subsequently, spray drying was performed at an inlet temperature of 200℃ and an outlet temperature of 90℃ for 20s to obtain a lithium manganese iron phosphate material with a dual chemical anchoring interface, denoted as LMFP@Al2O3 / C@PEDOT:PSS / CNT.

[0161] The battery preparation process in Example 1 is as follows: (1) Preparation of positive electrode sheet: The prepared lithium manganese iron phosphate material, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride PVDF) are mixed in a mass ratio of 97:1.5:1.5. An appropriate amount of 1-methyl-2-pyrrolidone (NMP) solvent is added and stirred evenly to obtain a positive electrode slurry. The viscosity and solid content of the positive electrode slurry are adjusted to be suitable for coating. The positive electrode slurry is uniformly coated on an aluminum foil current collector, dried and then rolled to form a positive electrode sheet. The single-sided density of the positive electrode material layer on the positive electrode sheet is 200 g / m². 2 The compacted density is 2.4 g / cm³. 3 .

[0162] (2) Preparation of negative electrode sheet: Graphite (Gr), conductive agent (SP), CMC and SBR are mixed evenly in a ratio of 96.5:0.5:1.2:1.8 to obtain a negative electrode slurry. The viscosity and solid content of the negative electrode slurry are adjusted to be suitable for coating. The negative electrode slurry is evenly coated on a copper foil current collector, dried and then rolled to form a negative electrode sheet.

[0163] (3) Preparation of electrolyte: Prepare lithium-ion battery electrolyte in a glove box (in an argon protective atmosphere). Dissolve LiPF6 in a mixture of ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) (the volume ratio of EC, DMC and EMC is 1:1:1) to prepare a 1 mol / L LiPF6 solution.

[0164] (4) The positive and negative electrode plates and separators are first stacked and assembled in the order of negative electrode plate-separator-positive electrode plate-separator to obtain a bare cell. Then, a lithium-ion battery with a capacity of 10Ah is obtained by sealing, ultrasonic welding, top sealing, vacuum baking, electrolyte injection, wetting, formation and aging, second sealing and capacity testing.

[0165] Example 2

[0166] The preparation method of the lithium manganese iron phosphate material in Example 2 is basically the same as that in Example 1. The only difference is that in step (2), AlCl3·6H2O is replaced with an equal mass of Zn(NO3)2·6H2O, terephthalic acid is replaced with an equal mass of 2-methylimidazole, DMF is replaced with an equal volume of methanol, and the solvothermal reaction temperature is changed to 80℃ to obtain the LMFP@ZIF-8 core-shell composite material. In step (3), the dried LMFP@ZIF-8 composite material is placed in a tube furnace and heated to 350℃ at a heating rate of 2℃ / min under nitrogen protection. The temperature is held for 2 hours, and then heated to 550℃ at a heating rate of 3℃ / min. The temperature is held for 3 hours to obtain the lithium manganese iron phosphate material with a dual chemical anchoring interface, which is denoted as LMFP@ZnO / C@PEDOT:PSS / CNT material.

[0167] The preparation method of the battery in Example 2 is basically the same as that in Example 1, except that the lithium manganese iron phosphate material prepared in Example 1 is replaced with an equal mass of lithium manganese iron phosphate material prepared in Example 2.

[0168] Example 3

[0169] The preparation method of the lithium manganese iron phosphate material in Example 3 is basically the same as that in Example 1. The only difference is that in step (2), AlCl3·6H2O is replaced with an equal mass of Ce(NO3)3·6H2O, and terephthalic acid is replaced with an equal mass of trimesic acid to obtain LMFP@Ce-BTC core-shell composite material; in step (3), the dried LMFP@Ce-BTC composite material is placed in a tube furnace and heated to 400℃ at a heating rate of 2℃ / min under nitrogen protection, and held for 2 hours. Then, it is heated to 650℃ at a heating rate of 3℃ / min and held for 3 hours to finally obtain lithium manganese iron phosphate material with dual chemical anchoring interface, which is denoted as LMFP@CeO2 / C@PEDOT:PSS / CNT material.

[0170] The preparation method of the battery in Example 3 is basically the same as that in Example 1, except that the lithium manganese iron phosphate material prepared in Example 1 is replaced with an equal mass of lithium manganese iron phosphate material prepared in Example 3.

[0171] Example 4

[0172] The preparation method of the lithium manganese iron phosphate material in Example 4 is basically the same as that in Example 1. The only difference is that in step (3), the dried LMFP@MIL-53(Al) composite material is placed in a tube furnace and heated to 400°C at a heating rate of 2°C / min under nitrogen protection. The temperature is held for 5 hours to finally obtain the LMFP@Al2O3 / C@PEDOT:PSS / CNT material.

[0173] The preparation method of the battery in Example 4 is basically the same as that in Example 1, except that the lithium manganese iron phosphate material prepared in Example 1 is replaced with an equal mass of lithium manganese iron phosphate material prepared in Example 4.

[0174] Comparative Example 1

[0175] The preparation method of lithium manganese iron phosphate material in Comparative Example 1 is basically the same as that in Example 1, except that only step (1) is performed. The lithium manganese iron phosphate powder obtained in step (1) is used as the final material and is denoted as LiMn. 0.6 Fe 0.4 PO4 (LMFP).

[0176] The preparation method of the battery in Comparative Example 1 is basically the same as that in Example 1, except that the lithium manganese iron phosphate material prepared in Example 1 is replaced with an equal mass of lithium manganese iron phosphate material prepared in Comparative Example 1.

[0177] Comparative Example 2

[0178] The preparation method of the lithium manganese iron phosphate material in Comparative Example 2 is basically the same as that in Example 1. The only difference is that only steps (1), (2) and (3) are performed, and step (4) is skipped. The lithium manganese iron phosphate material with only a chemical anchoring layer obtained in step (3) is the final material, denoted as LMFP@Al2O3 / C.

[0179] The preparation method of the battery in Comparative Example 2 is basically the same as that in Example 1, except that the lithium manganese iron phosphate material prepared in Example 1 is replaced with an equal mass of lithium manganese iron phosphate material prepared in Comparative Example 2.

[0180] Comparative Example 3

[0181] The preparation method of the lithium manganese iron phosphate material in Comparative Example 3 is basically the same as that in Example 1, except that after step (1), steps (2) and (3) are skipped, and then step (4) is performed: the LiMn prepared in step (1) is... 0.6 Fe 0.4 PO4 (LMFP) powder is added to the coating solution in step (4) to finally obtain a lithium manganese iron phosphate material with only a multifunctional composite layer, denoted as LMFP@PEDOT:PSS / CNT.

[0182] The preparation method of the battery in Comparative Example 3 is basically the same as that in Example 1, except that the lithium manganese iron phosphate material prepared in Example 1 is replaced with an equal mass of lithium manganese iron phosphate material prepared in Comparative Example 3.

[0183] Test case

[0184] I. Electrochemical Performance Testing

[0185] High-temperature cycling test: At 55℃, after resting for 10 min, charge at 1C constant current to 4.2V, rest for 10 min, discharge at 1C constant current to 2.5V, cycle 1000 times, and calculate the capacity retention rate of the battery after 1000 cycles: Capacity retention rate of the battery after 1000 cycles = (Discharge capacity after the 1000th cycle / Discharge capacity of the first cycle) 100%.

[0186] II. Test of manganese deposition on the negative electrode after cycling

[0187] The deposition of manganese on the negative electrode after cycling was tested using the ICP standard curve method (GB / T 38823-2020) and the instrument used was an inductively coupled plasma atomic emission spectrometer (Perkin Elmer Optima ICP-OES AVio200).

[0188] III. Particle Size Testing

[0189] The particle size of the example and comparative sample was tested according to GB / T 19077-2016 "Particle size analysis - Laser diffraction method". The instrument used was a Malvern 3000 analyzer.

[0190] The performance tests of the samples prepared in Examples 1-4 and Comparative Examples 1-3 are shown in Table 1.

[0191] Table 1: Performance tests of samples prepared in Examples 1-4 and Comparative Examples 1-3

[0192] As can be seen from the experimental results of Examples 1-3 and Comparative Examples 1-3 in Table 1, the cycle retention rate of Examples 1-3 after 1000 cycles is higher than 90%, which is far better than the cycle retention rate of lithium manganese iron phosphate materials containing only chemical anchoring layers (such as Comparative Example 2) and only polymer conductive / carbon material composite layers (such as Comparative Example 3), demonstrating the synergistic effect of dual-layer chemical anchoring.

[0193] As can be seen from the experimental results of Examples 1-3 in Table 1, the metal oxides derived from Al-based MOF, Zn-based MOF and Ce-based MOF can all effectively inhibit manganese leaching, indicating that the technical solution of the present invention has good universality and flexibility in material selection.

[0194] As can be seen from the experimental results of Examples 1-3 and Comparative Examples 1-3 in Table 1, the amount of manganese deposited in the negative electrode of Examples 1-3 is only 8%-11% of that of Comparative Example 1, which is significantly better than that of Comparative Examples 2 and 3 with a single coating layer, indicating that dual chemical anchoring can more effectively fix manganese ions.

[0195] As can be seen from the experimental results of Examples 1-3 and Example 4 in Table 1, the retention rate of Examples 1-3 after 1000 cycles is higher than 90%, and the amount of manganese deposited in the negative electrode is much lower than that in Example 4. This indicates that the performance of the lithium manganese iron phosphate material prepared by gradient heat treatment is better than that prepared by isothermal heat treatment.

Claims

1. A lithium manganese iron phosphate material, characterized in that, The lithium manganese iron phosphate material comprises a core and a chemical anchoring layer and a multifunctional composite layer sequentially coated on the surface of the core, wherein the core is LiMn. x Fe 1-x PO4, wherein 0.1≤x≤0.9, the chemical anchoring layer is formed by in-situ carbonization of a metal-organic framework, comprising a carbon skeleton and metal oxides dispersed in the carbon skeleton, and the multifunctional composite layer is formed by crosslinking of a conductive polymer and carbon materials.

2. The lithium manganese iron phosphate material as described in claim 1, characterized in that, The lithium manganese iron phosphate material has one or more of the following characteristics: The kernel LiMn x Fe 1-x In PO4, x satisfies 0.6 ≤ x ≤ 0.7; The metal-organic framework is selected from one or more of aluminum-based MOFs, iron-based MOFs, copper-based MOFs, zinc-based MOFs, cerium-based MOFs, zirconium-based MOFs, and titanium-based MOFs; The metal oxide is selected from one or more of Al2O3, Fe2O3, CuO, ZnO, CeO2, ZrO2 and TiO2, preferably one or more of Al2O3, ZnO and CeO2; The conductive polymer is selected from one or more of poly(3,4-ethylenedioxythiophene):polystyrene sulfonate, sulfonated polyaniline, and sulfonated polypyrrole; The carbon material is selected from one or more of carboxylated carbon nanotubes, graphene oxide, and aminated carbon nanotubes.

3. The lithium manganese iron phosphate material as described in claim 2, characterized in that, The metal-organic framework has one or more of the following characteristics: The aluminum-based MOF is selected from one or more of MIL-53(Al), MIL-100(Al), Al-BDC, and CAU-10-H; The iron-based MOF is selected from one or both of MIL-53(Fe) and MnFe-MOF; The copper-based MOF is selected from one or both of Cu3(HITP)2 and Cu-BTC; The zinc-based MOF is selected from one or more of ZIF-8, MOF-5, and MOF-177; The cerium-based MOF is selected from one or more of Ce-BDC, Ce-BTC, and Ce-UiO-66; The zirconium-based MOF is selected from one or more of UiO-66, UiO-67 and MOF-808; The titanium-based MOF is selected from one or both of MIL-125(Ti) and NH2-MIL-125(Ti).

4. The lithium manganese iron phosphate material as described in claim 1, characterized in that, The lithium manganese iron phosphate material has one or more of the following characteristics: The thickness of the chemical anchoring layer is 5-50 nm, preferably 10-30 nm; The pore size of the chemical anchoring layer is 2-50 nm, preferably 5-20 nm; The particle size of the metal oxide is 5-50 nm, preferably 10-30 nm; The thickness of the multifunctional composite layer is 3-30 nm, preferably 5-15 nm; The D50 particle size of the lithium manganese iron phosphate material is 0.5-3 μm, preferably 1-2 μm.

5. A method for preparing lithium manganese iron phosphate material according to any one of claims 1-4, characterized in that, The method includes: (1) Add lithium source, iron source, manganese source, phosphorus source and chelating agent to water, mix evenly to obtain wet gel; (2) The wet gel is dried and pre-calcined to obtain lithium manganese iron phosphate precursor powder; (3) The lithium manganese iron phosphate precursor powder is dispersed in a solution containing a metal source, an organic ligand and an organic solvent, and then subjected to solvothermal reaction, drying and heat treatment to obtain material A; (4) The material A is mixed with a coating liquid containing conductive polymer and carbon material and dried to obtain lithium manganese iron phosphate material.

6. The method as described in claim 5, characterized in that, The heat treatment includes heating to 350-650℃ and holding for 3-8 hours.

7. The method as described in claim 6, characterized in that, The heat treatment is a gradient heat treatment, which includes: first heating to 350-450℃ and holding for 1-3 hours, then heating to 500-650℃ and holding for 2-5 hours.

8. The method as described in claim 5, characterized in that, The method has one or more of the following characteristics: The molar ratio of lithium in the lithium source, manganese in the manganese source, and iron in the iron source satisfies: (n(Mn)+n(Fe)):n(Li) =1, and 0.1≤n(Mn):n(Li)≤0.9; The molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and phosphorus in the phosphorus source satisfies: n(P):(n(Li)+n(Mn)+n(Fe))=1:2; The molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and the chelating agent satisfies: n(chelating agent):(n(Li)+n(Mn)+n(Fe))=(1.2-1.5):1; The lithium source is selected from one or more of lithium carbonate, lithium acetate, and lithium nitrate; The manganese source is selected from one or more of manganese sulfate, manganese carbonate, manganese nitrate, manganese oxalate, manganese acetate, and manganese chloride; The iron source is selected from one or more of ferrous sulfate, ferrous chloride, ferrous bromide, ferrous oxalate, ferrous acetate, and ferrous nitrate. The phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and potassium dihydrogen phosphate; The chelating agent is selected from one or more of citric acid, ascorbic acid, and ethylenediaminetetraacetic acid.

9. The method as described in claim 5, characterized in that, The method has one or more of the following characteristics: The metal source is selected from one or more of aluminum, iron, copper, zinc, cerium, zirconium, and titanium sources; the aluminum source is selected from one or more of aluminum isopropoxide, aluminum nitrate, and aluminum chloride; the iron source is selected from one or more of ferric chloride, ferrous oxalate, and ferric phosphate; the copper source is selected from one or more of copper chloride, copper nitrate, copper acetate, and copper sulfate; the zinc source is selected from one or more of zinc nitrate, zinc nitrate hexahydrate, zinc acetate dihydrate, and zinc chloride; the cerium source is selected from one or more of cerium nitrate, cerium chloride, and cerium sulfate; the zirconium source is selected from one or more of zirconium tetrachloride, zirconium oxychloride, and zirconium oxynitrate; and the titanium source is selected from one or more of tetrabutyl titanate, tetraisopropyl titanate, and tetraethyl titanate. The organic ligand is selected from one or more of terephthalic acid, trimesic acid, 2-aminoterephthalic acid and 2-methylimidazole; The organic solvent is selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone, methanol, and anhydrous ethanol; The mass ratio of the lithium manganese iron phosphate precursor powder to the metal source is 1:(0.05-0.5), preferably 1:(0.1-0.3); The mass ratio of the lithium manganese iron phosphate precursor powder to the organic ligand is 1:(0.03-0.3), preferably 1:(0.05-0.2).

10. The method as described in claim 5, characterized in that, The method has one or more of the following characteristics: The mass ratio of material A to the conductive polymer is 1:(0.005-0.05), preferably 1:(0.01-0.03); The mass ratio of material A to carbon material is 1:(0.001-0.02), preferably 1:(0.003-0.01); The mass fraction of the conductive polymer in the coating solution is 0.5%-5%; The mass fraction of carbon material in the coating solution is 0.05%-1%; The solvent of the coating solution is selected from one or more of deionized water, anhydrous ethanol, and a mixture of deionized water and ethanol.

11. The method as described in claim 5, characterized in that, The method has one or more of the following characteristics: In step (1), the pH of the solution is 3.0-5.0; In step (1), the mixture is stirred in a water bath at a temperature of 60-90°C for 4-6 hours and at a speed of 200-500 rpm. In step (2), vacuum drying is used, the drying temperature is 100-150℃, and the drying time is 10-15h; In step (2), the gas is pre-fired in an inert atmosphere at a temperature of 600-800°C for 4-10 hours. The inert atmosphere is nitrogen or argon. In step (3), ultrasonic dispersion is used, with an ultrasonic power of 300-500W and an ultrasonic time of 30-60min; In step (3), the solvothermal reaction temperature is 80-150℃ and the reaction time is 12-36h; In step (3), vacuum drying is used, the drying temperature is 50-80℃, and the drying time is 10-15h; In step (3), heat treatment is performed under an inert atmosphere, wherein the inert atmosphere is nitrogen or argon. In step (3), the heating rate of the heat treatment is 1-5℃ / min; In step (4), stirring is used for mixing. The mixing time is 1-6 hours, preferably 2-4 hours, and the mixing rate is 200-1000 rpm, preferably 400-600 rpm. In step (4), the drying is vacuum drying or spray drying. The temperature of vacuum drying is 60-120℃, preferably 80-100℃, and the time of vacuum drying is 4-12h, preferably 8-12h. The inlet temperature of spray drying is 150-250℃, preferably 180-220℃, the outlet temperature is 80-110℃, preferably 90-100℃, and the time of spray drying is 5-30s.

12. Lithium manganese iron phosphate material prepared by any one of claims 5-11.

13. A positive electrode plate, characterized in that, The positive electrode comprises lithium manganese iron phosphate material as described in any one of claims 1-4 and 12.

14. A lithium-ion battery, characterized in that, The lithium-ion battery includes the positive electrode as described in claim 13.

15. An electrical appliance, characterized in that, The electrical device includes the lithium-ion battery as described in claim 14.