Low-expansion silicon-carbon negative electrode material and preparation method and application thereof

By using curtain-type coating equipment and multi-target magnetron sputtering technology to form hollow silicon/carbon composite layers and protective layers in lithium-ion battery anode materials, the problem of volume expansion of silicon materials is solved, the stability and capacity of the battery are improved, and an efficient and environmentally friendly production process is achieved.

CN123143383APending Publication Date: 2026-11-20NINGBO YUNTU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611638037.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing lithium-ion battery anode materials, the volume expansion problem of silicon materials has not been effectively solved, leading to electrode structure cracking and poor cycle stability. Furthermore, existing magnetron sputtering processes are difficult to achieve uniform deposition of multilayer composite structures.

Method used

A curtain-type coating device is used to form a hollow, low-expansion silicon-carbon anode material by sequentially depositing a silicon/carbon framework composite layer and a protective layer on the surface of the substrate material. This is combined with a multi-target magnetron sputtering process to achieve continuous deposition of a multi-layer composite structure.

Benefits of technology

It effectively limits the volume expansion of silicon, improves the structural stability and capacity characteristics of the battery, simplifies the production process, reduces energy consumption and labor costs, improves the uniformity of the deposited layer and the stability of batch processing, and meets the requirements of green and low-carbon production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143383A_ABST
    Figure CN123143383A_ABST
Patent Text Reader

Abstract

The application relates to the fields of electrochemical energy storage technology and magnetron sputtering technology, and discloses a low-expansion silicon-carbon negative electrode material and a preparation method and application thereof. The method comprises the following steps of substrate pretreatment, parameter setting, silicon / carbon skeleton composite layer deposition, protective layer deposition, substrate material removal and post-treatment, the removable substrate material is placed in a curtain powder coating device, a silicon / carbon skeleton composite layer and a protective layer are sequentially sputtered and deposited under vacuum conditions, and finally, the low-expansion silicon-carbon negative electrode material is obtained. The application innovatively designs a three-layer structure of a hollow center, a silicon / carbon skeleton composite layer and a protective layer, the carbon network in the skeleton composite layer formed by the co-sputtering of silicon and carbon is closely combined with silicon, the aggregation and expansion of silicon particles are limited, the protective layer optimizes ion transmission and interface stability, the first coulomb efficiency of the battery is better, and the application scenarios are more extensive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of electrochemical energy storage technology and magnetron sputtering technology, specifically to the preparation technology of silicon-carbon anode materials for lithium-ion batteries, and particularly to a low-expansion silicon-carbon anode material, its preparation method and application. Background Technology

[0002] With the rapid development of new energy vehicles, smart grids, distributed energy storage, and 3C electronic products, the market has placed higher demands on the energy density, cycle life, and safety of lithium-ion batteries. Currently, commercially available lithium-ion battery anodes mainly use graphite-based materials, but their theoretical specific capacity is only 372 mAh / g, which is insufficient to meet high-capacity requirements. Silicon, with its ultra-high theoretical specific capacity of 4200 mAh / g, has become one of the most promising alternatives to graphite.

[0003] Silicon materials exhibit a massive volume expansion exceeding 300% during charge and discharge, which can easily lead to electrode structure cracking and active material shedding. It also causes repeated formation and destruction of the SEI film, severely impacting battery cycle stability. Currently, researchers often employ hollow structure designs to address the silicon volume expansion problem; however, existing methods for preparing hollow silicon-carbon anodes still have shortcomings.

[0004] Coating technologies are mostly single-material coatings or stepwise coatings, making it difficult to form structurally stable composite layers. The bonding force between silicon and carbon is weak, and separation easily occurs during cycling, failing to effectively limit the volume expansion of silicon. Although some methods can prepare hollow structures, the substrate material removal process is complex, or the coating layer does not bond firmly to the substrate material, resulting in poor batch stability and hindering industrial mass production. In addition, existing magnetron sputtering processes in the field of powder coating are mostly used for single-target coating, lacking multi-layer composite structure designs for hollow silicon-carbon anodes. Furthermore, the powder flow equipment used suffers from insufficient coating uniformity and the inability to continuously coat multiple targets, limiting its application in the preparation of high-performance anode materials. Summary of the Invention

[0005] To address at least one of the aforementioned problems, this invention provides a low-expansion silicon-carbon anode material, its preparation method, and its application. The method uses a removable substrate material as a template, and combines a curtain-type coating device to sequentially deposit a silicon / carbon framework composite layer and a protective layer on the surface of the substrate material. Finally, the substrate is removed to form a hollow structure, ultimately obtaining a three-layer structure of "hollow center - silicon / carbon framework composite layer - protective layer" for a low-expansion hollow silicon-carbon anode material.

[0006] In a first aspect, the present invention provides a method for preparing a low-expansion silicon-carbon anode, comprising the following steps:

[0007] S1. Substrate pretreatment: Select a removable substrate material, dry the substrate material, then open the shell and cavity of the curtain-type covering equipment, and feed the dried substrate material into the storage bin at the bottom of the cavity. Use the through hole at the bottom of the storage bin to allow the substrate material to enter the circulating conveying mechanism.

[0008] S2. Parameter settings: Install the silicon / carbon skeleton composite layer target and the protective layer target in the sputtering assembly along the circumferential direction of the cavity center, and then preset the first sputtering process parameters of the silicon / carbon skeleton composite layer and the second sputtering process parameters of the protective layer in the controller.

[0009] S3, Silicon / Carbon Framework Composite Layer Deposition: Close the shell and the cavity, start the vacuum mechanism by the controller to complete the vacuuming and introduce argon gas, so that the inside of the shell is in a vacuum-sealed state; start the circulating material conveying mechanism to transport the substrate material to the cavity, and sputter and deposit a silicon / carbon framework composite layer on the surface of the substrate material according to the first sputtering process parameters to obtain the first substrate composite material;

[0010] S4. Protective layer deposition: Start the circulating material conveying mechanism to continue circulating the first substrate composite material into the cavity, and deposit a protective layer on the first substrate composite material according to the second sputtering process parameters to obtain the second substrate composite material.

[0011] S5. Substrate material removal: After deposition, cool to room temperature, turn off the power, break the vacuum and remove the second substrate composite material. Place the second substrate composite material in an acidic solution and stir and wash until the filtrate is neutral, or place the second substrate composite material in a furnace for thermal decomposition to remove the substrate material in the second substrate composite material, thereby obtaining a substrate-free composite material.

[0012] S6. Post-processing: The substrate-free composite material is dried to obtain a low-expansion silicon-carbon anode material.

[0013] Optionally, the deposition method of the silicon / carbon skeleton composite layer in step S3 is as follows: after starting the circulating feeding mechanism, the substrate material is fed to the redistributor above the cavity. Under its own gravity, the substrate material slides down the surface of the redistributor to the bottom of the cavity, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and according to the first sputtering process parameters, a substrate material for a first-time deposition of silicon / carbon skeleton composite layer is deposited on the surface of the substrate material. The steps after starting the circulating feeding mechanism in this step are repeated until the silicon / carbon skeleton composite layer of the target thickness is deposited, and sputtering is stopped to obtain the first substrate composite material.

[0014] Optionally, the method for depositing the protective layer in step S4 is as follows: After starting the circulating feeding mechanism, the first substrate composite material is fed to the redistributor above the cavity. Under its own gravity, the first substrate composite material slides down the surface of the redistributor to the bottom of the cavity, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and the protective layer is deposited on the surface of the first substrate composite material according to the second sputtering process parameters. The steps after starting the circulating feeding mechanism in this step are repeated until the protective layer of the target thickness is deposited, and sputtering is stopped to obtain the second substrate composite material.

[0015] Optionally, the protective layer is at least one of a carbon layer, a LiF ion transport layer, and an Al2O3 hard layer; the target material selected for the protective layer is at least one of a carbon target, a LiF target, and an Al2O3 target; when the protective layer is a carbon layer, the target material is a carbon target, and the sputtering conditions are an argon flow rate of 100~300 sccm, a target power of 5~10 kW, a deposition time of 20~60 min, and a layer thickness of 20~100 nm; when the protective layer is a LiF ion transport layer, the target material is a LiF target, and the sputtering conditions are an argon flow rate of 100~200 sccm, a target power of 2~5 kW, a deposition time of 15~40 min, and a layer thickness of 10~30 nm; when the protective layer is an Al2O3 hard layer, the target material is an Al2O3 target, and the sputtering conditions are an argon flow rate of 100~200 sccm, a target power of 4~8 kW, a deposition time of 20~50 min, and a layer thickness of 10~20 nm.

[0016] Optionally, the thickness of the silicon / carbon framework composite layer in step S3 is 50~500nm; the mass ratio of silicon to carbon is 3:1~7:1.

[0017] Optionally, the substrate material in step S1 is at least one of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, copper chloride, calcium sulfate, glucose, and polymethyl methacrylate microspheres; the particle size of the substrate material is 10~30μm; and the shape of the substrate material is one of spherical, near-spherical, and irregular shapes.

[0018] Optionally, the pH of the acidic solution in step S5 is 2~5, and the stirring time is 2~6h; the drying temperature of the post-treatment in step S6 is 80~120℃, and the drying time is 4~8h.

[0019] The low-expansion silicon-carbon anode preparation method provided by this invention has at least the following beneficial effects:

[0020] 1. This invention innovatively designs a three-layer structure of "hollow center, silicon / carbon skeleton composite layer, and protective layer". In the skeleton composite layer formed by simultaneous co-sputtering of silicon and carbon, the carbon network is tightly bonded to silicon, which effectively restricts the aggregation and expansion of silicon particles. The protective layer optimizes ion transport and interface stability, further improving structural stability. The hollow structure provides sufficient buffer space for silicon expansion. The silicon / carbon skeleton composite layer also supports the high capacity characteristics of the battery, making the battery's first coulombic efficiency better.

[0021] 2. This invention allows for the simultaneous or continuous sputtering deposition of different materials within a cavity, enabling integrated production of multi-layer composite deposition coating of substrate particles. This invention eliminates the need for frequent cavity openings to change targets or transfer powder between different devices, significantly shortening the production cycle, improving equipment utilization and production efficiency, and effectively reducing energy consumption and labor costs in multi-material deposition processes.

[0022] 3. The present invention uses a curtain-type coating device to form a multi-layer curtain of substrate material during the falling process. The material is in an orderly, dispersed and dynamically circulating state, which effectively avoids local accumulation and flow dead zones. In addition, each particle can be uniformly and fully exposed to the sputtering atomic bombardment range, which significantly improves the thickness consistency and structural uniformity of the deposition layer. It solves the problem of uneven deposition caused by disordered movement of substrate material and ensures the stability and repeatability of deposition quality between particles during batch processing.

[0023] 4. This invention adopts a completely dry magnetron sputtering process, which generates and emits no wastewater or waste gas throughout the process. It completely avoids the environmental governance pressure and pollutant treatment costs brought about by traditional wet deposition coating processes, meets the development requirements of green, low-carbon and clean production in modern manufacturing, and has significant environmental benefits and industrial sustainability.

[0024] Secondly, the present invention provides a low-expansion silicon-carbon anode material, which is prepared by the above-mentioned method for preparing low-expansion silicon-carbon anode materials.

[0025] Thirdly, the present invention also provides an application of the method for preparing low-expansion silicon-carbon anode materials, wherein the application employs the above-mentioned method for preparing low-expansion silicon-carbon anode materials, and the application is used to prepare lithium-ion batteries, wherein the lithium-ion batteries are used in new energy vehicles, energy storage systems or 3C electronic products.

[0026] Optionally, the negative electrode preparation process of the lithium-ion battery includes the following steps: uniformly dispersing silicon-carbon negative electrode material, conductive additives, and binders in a certain proportion, and then coating the uniformly dispersed slurry onto a metal substrate and drying it to obtain a negative electrode sheet; the mass ratio of the silicon-carbon negative electrode material, the conductive additives, and the binders is 80-90:5-10:5-10; the binder is at least one of sodium carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, sodium alginate, and polyvinylidene fluoride.

[0027] Compared with the prior art, the low-expansion silicon-carbon anode material preparation method of the present invention has the same advantages as the above-mentioned silicon-carbon anode material preparation method, and will not be repeated here. Attached Figure Description

[0028] Figure 1 A flowchart of a method for preparing a low-expansion silicon-carbon anode material is provided in this application;

[0029] Figure 2 This is a schematic diagram of the overall curtain-type covering equipment used in this application;

[0030] Figure 3 This is a partial structural diagram of the curtain-type covering device used in this application;

[0031] Figure 4 This is a top view of the cavity of the curtain-type covering device used in this application;

[0032] Reference numerals: 1. Shell; 2. Cavity; 23. Storage bin; 231. Through hole; 24. Redistributor; 241. First umbrella-shaped slide plate; 242. Second umbrella-shaped slide plate; 243. Third umbrella-shaped slide plate; 25. Support rod; 26. Sputtering assembly; 3. Circulating conveying mechanism; 31. First horizontal conveying assembly; 32. Vertical conveying assembly; 33. Second horizontal conveying assembly; 331. Powder buffer bin; 4. Vacuum mechanism. Detailed Implementation

[0033] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0034] See Figure 1 This application provides a method for preparing a low-expansion silicon-carbon anode, comprising the following steps:

[0035] S1. Substrate pretreatment: Select a removable substrate material, dry the substrate material, then open the shell 1 and cavity 2 of the curtain-type covering equipment, and feed the dried substrate material into the storage bin 23 at the bottom of the cavity 2. Use the through hole 231 at the bottom of the storage bin 23 to allow the substrate material to enter the circulating conveying mechanism 3.

[0036] S2. Parameter settings: Install the silicon / carbon skeleton composite layer target and the protective layer target in the sputtering assembly 26 along the circumferential direction of the center of the cavity 2, and then preset the first sputtering process parameters of the silicon / carbon skeleton composite layer and the second sputtering process parameters of the protective layer in the controller.

[0037] S3, Silicon / Carbon Framework Composite Layer Deposition: Close the shell 1 and cavity 2, start the vacuum mechanism 4 by the controller to complete the vacuuming and introduce argon gas, so that the inside of the shell 1 is in a vacuum-sealed state; start the circulating material conveying mechanism 3 to transport the substrate material to the cavity 2, and deposit the silicon / carbon framework composite layer on the surface of the substrate material according to the first sputtering process parameters to obtain the first substrate composite material.

[0038] S4. Protective layer deposition: Start the circulating material conveying mechanism 3 to continue circulating and conveying the first substrate composite material into the cavity 2. According to the second sputtering process parameters, a protective layer is sputtered and deposited on the first substrate composite material to obtain the second substrate composite material.

[0039] S5. Substrate material removal: After deposition, cool to room temperature, turn off the power, break the vacuum and remove the second substrate composite material. Place the second substrate composite material in an acidic solution and stir and wash until the filtrate is neutral, or place the second substrate composite material in a furnace for thermal decomposition to remove the substrate material in the second substrate composite material and obtain a substrate-free composite material.

[0040] S6. Post-treatment: The substrate-free composite material is dried to obtain a low-expansion silicon-carbon anode material.

[0041] Specifically, the deposition method of the silicon / carbon skeleton composite layer in step S3 is as follows: After starting the circulating material feeding mechanism 3, the substrate material is fed to the redistributor 24 in the cavity 2. Under its own gravity, the substrate material slides down the surface of the redistributor 24 to the bottom of the cavity 2, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and according to the first sputtering process parameters, the substrate material for the first deposition of silicon / carbon skeleton composite layer is obtained by depositing on the surface of the substrate material. The steps after starting the circulating material feeding mechanism in this step are repeated until the silicon / carbon skeleton composite layer of the target thickness is deposited, and sputtering is stopped to obtain the first substrate composite material.

[0042] Specifically, the method for depositing the protective layer in step S4 is as follows: After starting the circulating material conveying mechanism 3, the first substrate composite material is conveyed to the redistributor 24 in the cavity 2. Under its own gravity, the first substrate composite material slides down the surface of the redistributor 24 to the bottom of the cavity 2, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and according to the second sputtering process parameters, a protective layer is deposited on the surface of the first substrate composite material. The steps after starting the circulating material conveying mechanism in this step are repeated until a protective layer of the target thickness is deposited, and sputtering is stopped to obtain the second substrate composite material.

[0043] See Figure 2 , Figure 3 and Figure 4 The low-expansion silicon-carbon anode material prepared in this invention employs a curtain-type coating device. The substrate material is placed within the curtain-type coating device, and a magnetron sputtering process is used to deposit a substrate composite material with a silicon / carbon framework composite layer and a protective layer. This is followed by post-processing to obtain the silicon-carbon anode material. The curtain-type coating device includes a control system (not shown in the figures) and a sealed housing 1. The housing 1 houses a circulating conveying mechanism 3, a cavity 2, and a vacuum mechanism 4. The cavity 2 houses multiple sputtering components 26, a storage bin 23 at the bottom of the cavity 2, and a redistributor 24 at the top of the cavity 2. The circulating conveying mechanism 3 has a feed port and a discharge port. The feed port is connected to the storage bin 23, and the discharge port is connected to the top of the redistributor 24. Multiple sputtering components 26 are arranged circumferentially on the inner wall of the cavity 2. In this application, the sputtering components 26 are... The number of each type of target material, including silicon target, graphite target, and protective layer target, is not limited, but preferably an even number. The specific installation order within the cavity is not limited, but preferably the same type of target material is installed diagonally. The cavity 2 is also equipped with a support rod 25 for supporting the redistributor 24. The redistributor 24 includes multiple interconnected umbrella-shaped slide plates, which are concentrically distributed from the inside to the outside, and the diameter of the lower end face of the umbrella-shaped slide plates gradually increases from the inside to the outside. The vacuum mechanism 4 is installed outside the cavity 2. The vacuum mechanism 4, the circulating material conveying mechanism 3, and the sputtering assembly 26 are all electrically connected to the control system. Specifically, the circulating material conveying mechanism 3, the cavity 2, and the vacuum mechanism 4 are installed in the same housing 1, which saves equipment installation space. The housing 1 has a high degree of integration and can be directly connected to the magnetron sputtering power supply and vacuum system. Multiple umbrella-shaped drop plates and multiple sputtering components 26 work together to make the substrate material more evenly dispersed during the drop process, reducing substrate material agglomeration. The falling substrate material can shield the sputtering area. During the sputtering process, target atoms are uniformly deposited on the surface of the substrate material. This enables uniform and controllable thickness of the silicon / carbon skeleton composite layer and protective layer deposited on the surface of the substrate material particles, without the risk of incomplete deposition.

[0044] See Figure 3The circulating material conveying mechanism 3 in step S1 includes a first horizontal conveying component 31, a second horizontal conveying component 33, and a vertical conveying component 32. The lower port of the vertical conveying component 32 is connected to the first horizontal conveying component 31, and the upper outlet of the vertical conveying component 32 is connected to a powder buffer silo 331. The powder buffer silo 331 is connected to the second horizontal conveying component 33, and the other end of the second horizontal conveying component 33 is connected to a discharge port. The circulating material conveying mechanism 3 is at least one of a bucket elevator, an auger conveyor, and a vibrating conveyor. In this embodiment, both the first horizontal conveying component 31 and the second horizontal conveying component 33 are auger conveyors. The auger conveyor includes a first cylinder and an auger transmission shaft (existing technology, not shown in the figure) disposed within the first cylinder. The vertical conveying component 32 is a bucket elevator. The bucket elevator includes a second cylinder and a hopper transmission silo (existing technology, not shown in the figure) disposed within the second cylinder. The auger conveyor and bucket elevator are connected by bolts and both adopt a fully enclosed structure, which is simple, compact, and easy to integrate with the cavity 2, realizing sealed feeding of the substrate material. By adjusting the auger speed, the conveying efficiency of the substrate material can be precisely controlled, thereby achieving continuous, stable and uniform feeding of the substrate material, forming a stable powder flow shielding curtain in the sputtering area, which is more conducive to the subsequent coating of the substrate material. The bucket elevator adopts a unidirectional conveying method of bottom feeding and top discharge, which effectively prevents material backflow and cross-contamination, saves equipment floor space, and is easy to integrate with the sputtering cavity. The entire circulating conveying mechanism causes the material to undergo tumbling during transportation, which can effectively disperse powder agglomerates and is more conducive to the uniformity of deposition coating.

[0045] See Figure 4 In step S3, the redistributor 24 includes multiple interconnected and spaced-apart umbrella-shaped slide plates. The substrate material collides and contacts the multiple umbrella-shaped slide plates under its own gravity, then slides down the surface of the multiple umbrella-shaped slide plates to the edge and falls vertically to form a multi-layer curtain. The substrate material that has undergone a single deposition of the silicon / carbon skeleton composite layer falls into the storage bin 23 inside the cavity 2, and the feeding and deposition are repeated multiple times until the silicon / carbon skeleton composite layer of the target thickness is obtained. Sputtering is then stopped, and the first substrate composite material is obtained. The multiple umbrella-shaped slide plates are concentrically arranged and inclinedly stacked from the inside to the outside, and the diameter of the lower end face of the umbrella-shaped slide plates gradually increases from the inside to the outside. In this embodiment, there are 3 umbrella-shaped slide plates. The substrate material is dispersed radially as it slides down the first umbrella-shaped slide plate 241, the second umbrella-shaped slide plate 242, and the third umbrella-shaped slide plate 243 to form a three-layer curtain. During sputtering, the three-layer curtain can be sputtered and deposited simultaneously, making the deposition on the surface of a single substrate material more uniform and the material consistency better.

[0046] Specifically, the protective layer in step S2 is at least one of a carbon layer, a LiF ion transport layer, and an Al2O3 hard layer; the target material selected for the protective layer is at least one of a carbon target, a LiF target, and an Al2O3 target. When the protective layer is a carbon layer, the target material is a carbon target, and the sputtering conditions are an argon flow rate of 100-300 sccm, a target power of 5-10 kW, a deposition time of 20-60 min, and a layer thickness of 20-100 nm; when the protective layer is a LiF ion transport layer, the target material is a LiF target, and the sputtering conditions are an argon flow rate of 100-200 sccm, a target power of 2-5 kW, a deposition time of 15-40 min, and a layer thickness of 10-30 nm; when the protective layer is an Al2O3 hard layer, the target material is an Al2O3 target, and the sputtering conditions are an argon flow rate of 100-200 sccm, a target power of 4-8 kW, a deposition time of 20-50 min, and a layer thickness of 10-20 nm. By setting corresponding sputtering conditions and reactive gas parameters according to the differences in the conductivity and binding energy of the target materials, the technical problems of low target utilization and poor process stability when using fixed process parameters to deposit different target materials in the prior art are solved. High-quality compatible deposition of multiple target materials on the same equipment is achieved, and no process redevelopment is required after changing the target, which significantly reduces the process debugging cost and cycle.

[0047] Specifically, in step S3, the thickness of the silicon / carbon framework composite layer is 50~500nm; as an example, the deposition thickness of the silicon / carbon framework composite layer can be any value among 50nm, 70nm, 90nm, 100nm, 200nm, 300nm, 400nm, and 500nm, or any value between two of these. The silicon target power is 5~12kW; as an example, the silicon target power can be any value among 5kW, 6kW, 7kW, 8kW, 11kW, and 12kW, or any value between two of these. The graphite target power is 2~8kW; as an example, the graphite target power can be any value among 2kW, 3kW, 4kW, 5kW, 7kW, and 8kW, or any value between two of these. The silicon / carbon mass ratio is 3:1~7:1, for example, any ratio among 3:1, 4:1, 5:1, 6:1, and 7:1, or any ratio between two of these. In actual magnetron sputtering, the silicon / carbon mass ratio can be flexibly adjusted by regulating the sputtering power, enabling the surface of the substrate material to effectively build a carbon framework during sputtering deposition. This further enhances the material's resistance to expansion and achieves a precise balance between the specific capacity and cycle stability of the silicon-carbon anode material. Furthermore, by controlling the deposition time, the thickness of the silicon / carbon framework composite layer can be controlled, ultimately yielding the first substrate material with a silicon / carbon framework composite layer of the target thickness.

[0048] Specifically, in step S1, the substrate material is at least one selected from sodium chloride, potassium chloride, magnesium chloride, calcium chloride, copper chloride, calcium sulfate, glucose, and polymethyl methacrylate microspheres. The selected substrate material is easy to remove, and the removal method is gentle, unlikely to damage the external deposition layer, which is beneficial for forming a hollow structure. In the embodiments of this application, the substrate material is preferably sodium chloride, calcium sulfate, and magnesium chloride. In step S1, the drying temperature of the substrate material is 80~120℃, and the drying time is 2~4h. In the embodiments of this application, the drying temperature is preferably 100~110℃, and the drying time is preferably 3~3.5h.

[0049] Specifically, the substrate material has a particle size of 10~30μm. Using a substrate material with this particle size results in a hollow structure with uniform dimensions. Excessively large particle sizes can lead to the collapse of the hollow structure, while excessively small particle sizes can easily cause agglomeration, affecting the uniformity of subsequent deposition. The substrate material can be spherical, near-spherical, or irregular in shape. Preferably, the substrate material is spherical, as spherical materials are more conducive to the uniform deposition of a protective layer on the surface of the silicon / carbon framework composite layer in the hollow structure, thereby improving energy density.

[0050] Specifically, in step S5, the pH of the acidic solution is 2-5, and the stirring time is 2-6 hours. As an example, the pH of the acidic solution can be any value from 2, 3, 4, and 5, or any value between two of these; the stirring time can be any value from 2 hours, 3 hours, 4 hours, 5 hours, and 6 hours, or any value between two of these. In this embodiment, the pH of the acidic solution is preferably 3-4, and the stirring time is preferably 4-5 hours. In step S6, the drying temperature for the post-treatment is 80-120°C, and the drying time is 4-8 hours. As an example, the drying temperature can be any value from 80°C, 90°C, 100°C, 110°C, and 120°C, or any value between two of these; the drying time can be any value from 4 hours, 5 hours, 6 hours, 7 hours, and 8 hours, or any value between two of these. In this embodiment, the drying temperature is preferably 90-120°C, and the drying time is preferably 5-7 hours.

[0051] Specifically, in step S5, the substrate material removal can also be achieved by thermal decomposition. The substrate material with deposited silicon / carbon skeleton composite layer and protective layer is placed in a heating furnace, heated at 400~500℃ for 0.5~1h. After the substrate material is removed by thermal decomposition, the low-expansion silicon-carbon anode composite material can be obtained.

[0052] This invention provides a low-expansion silicon-carbon anode material, which is prepared by the above-described preparation method.

[0053] The present invention also provides an application of the low-expansion silicon-carbon anode preparation method. This application uses the above-mentioned low-expansion silicon-carbon anode material preparation method and is used to prepare lithium-ion batteries, which are used in new energy vehicles, energy storage systems or 3C electronic products.

[0054] Specifically, the preparation process of the negative electrode for a lithium-ion battery includes the following steps: uniformly dispersing silicon-carbon negative electrode material, conductive additives, and binders in a certain proportion; then coating the uniformly dispersed slurry onto a metal substrate and drying it to obtain a negative electrode sheet; the mass ratio of silicon-carbon negative electrode material, conductive additives, and binders is 80-90:5-10:5-10; the binder is at least one of sodium carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, sodium alginate, and polyvinylidene fluoride. In the embodiments of this application, acetylene black is selected as the conductive additive, and sodium carboxymethyl cellulose is selected as the binder.

[0055] Example 1

[0056] This embodiment includes the following steps:

[0057] S1. Substrate pretreatment: Select spherical sodium chloride with a particle size of 20μm as the substrate material, vacuum dry it at 100℃ for 3h, then open the shell 1 and cavity 2 of the curtain-type coating equipment, and feed the dried sodium chloride powder into the storage bin 23 at the bottom of the cavity 2. Use the through hole 231 at the bottom of the storage bin 23 to allow the sodium chloride powder to enter the circulating conveying mechanism 3.

[0058] S2. Parameter settings: According to the sodium chloride deposition requirements, the silicon target, graphite target, and carbon target in the sputtering assembly 26 are installed inside the cavity 2 along the circumferential position of the center of the cavity 2. Then, the process parameters are preset in the controller. First sputtering process parameters: silicon target power 5kW, graphite target power 4kW, argon flow rate 100sccm, deposition time 5h; Second sputtering process parameters: carbon target power 5kW, argon flow rate 150sccm, deposition time 30min.

[0059] S3, Silicon / Carbon Framework Composite Layer Deposition: Close housing 1 and cavity 2, activate vacuum mechanism 4 via controller, evacuate and introduce argon gas to working pressure 2.0 × 10⁻⁶. -3Pa, and the inside of the shell is in a vacuum-sealed state; after the circulation feeding mechanism 3 is started, the sodium chloride powder is fed to the top of the redistributor 24. Under its own gravity, the powder slides down the surface of the redistributor 24 to the bottom of the cavity 2, forming a vertical curtain during the sliding process; at the same time, the sputtering power supply is started, and according to the first sputtering process parameters, a sodium chloride powder with a silicon / carbon skeleton composite layer is deposited on the surface of the sodium chloride powder. The steps after starting the circulation feeding mechanism 3 in this step are repeated to complete multiple cycles of feeding and deposition until the thickness of the deposited silicon / carbon skeleton composite layer (silicon / carbon mass ratio of 5:1) is 50nm, then sputtering is stopped to obtain the first substrate composite material;

[0060] S4. Protective layer deposition: After starting the circulating material feeding mechanism 3, the first substrate composite material is fed to the redistributor 24 in the cavity 2. Under its own gravity, the first substrate composite material slides down the surface of the redistributor 24 to the bottom of the cavity 2, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and a protective layer is deposited on the surface of the first substrate composite material according to the second sputtering process parameters. The steps after starting the circulating material feeding mechanism in this step are repeated until the protective layer thickness is 30nm. Then the sputtering is stopped to obtain the second substrate composite material.

[0061] S5. Substrate material removal: After deposition, cool to room temperature, turn off the main power, break the vacuum and remove the second substrate composite material. Place the second substrate composite material in a hydrochloric acid solution with pH=3 and stir at room temperature for 4 hours. After filtration, wash with anhydrous ethanol until neutral.

[0062] S6. Post-treatment: The composite material without sodium chloride substrate was vacuum dried at 100℃ for 6 hours to obtain a low-expansion hollow silicon-carbon anode material.

[0063] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 2913 mAh / g and the initial efficiency was 92%.

[0064] Example 2

[0065] This embodiment includes the following steps:

[0066] S1. Substrate pretreatment: The same treatment method as step S1 in Example 1 is used, except that spherical calcium sulfate with a particle size of 25 μm is selected as the substrate material and vacuum dried at 110°C for 3.5 h.

[0067] S2. Parameter Settings: According to the deposition requirements of calcium sulfate, the silicon target, graphite target, and Al2O3 target in the sputtering assembly 26 are installed at intervals along the circumferential position of the center of the cavity 2 inside the cavity 2. Then, the process parameters are preset in the controller. First sputtering process parameters: silicon target power 7kW, graphite target power 3kW, argon flow rate 200sccm, deposition time 6h; Second sputtering process parameters: Al2O3 target power 6kW, argon flow rate 150sccm, deposition time 35min.

[0068] S3, Deposition of silicon / carbon framework composite layer: The same operation method as step S3 in Example 1 is used, except that the silicon / carbon mass ratio is 4:1 and the thickness of the silicon / carbon framework composite layer is 150nm.

[0069] S4. Deposition of protective layer: The same operation method as step S4 in Example 1 is adopted, except that the thickness of the Al2O3 hard protective layer is 10nm.

[0070] S5. Removal of substrate material: The same operation method as step S5 in Example 1 is used, except that the hydrochloric acid solution pH=4 and the stirring time is 5h.

[0071] S6. Post-processing: The same operation method as step S6 in Example 1 is adopted, except that the drying temperature is 90°C and the drying time is 7 hours.

[0072] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 2834 mAh / g and the initial efficiency was 93%.

[0073] Example 3

[0074] This embodiment includes the following steps:

[0075] S1. Substrate pretreatment: The same treatment method as step S1 in Example 1 is adopted, except that spherical magnesium chloride with a particle size of 15 μm is selected as the substrate material and vacuum dried at 100°C for 3 h.

[0076] S2. Parameter settings: According to the deposition requirements of magnesium chloride, the silicon target, graphite target, and LiF target in the sputtering assembly 26 are installed at intervals along the circumferential position of the center of the cavity 2 inside the cavity 2. Then, the first sputtering process parameters are preset in the controller: silicon target power 10kW, graphite target power 5kW, argon flow rate 200sccm, deposition time 6h; the second sputtering process parameters are: LiF target power 3kW, argon flow rate 150sccm, deposition time 20min.

[0077] S3, Deposition of silicon / carbon framework composite layer: The same operation method as step S3 in Example 1 is used, except that the silicon / carbon mass ratio is 7:1 and the thickness of the silicon / carbon framework composite layer is 300nm.

[0078] S4. Deposition of protective layer: The same operation method as step S4 in Example 1 is used, except that the thickness of the LiF ion transport layer is 10 nm.

[0079] S5. Removal of substrate material: The same operation method as step S5 in Example 1 is used, except that the hydrochloric acid solution pH=4 and the stirring time is 5h.

[0080] S6. Post-processing: The same operation method as step S6 in Example 1 is adopted, except that the drying temperature is 120℃ and the drying time is 5h.

[0081] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 3114 mAh / g and the initial efficiency was 89%.

[0082] Example 4

[0083] This embodiment includes the following steps:

[0084] S1. Substrate pretreatment: The same treatment method as step S1 in Example 1 was used, except that polymethyl methacrylate microspheres (PMMA microspheres) with a particle size of 30 μm were selected as the substrate material and vacuum dried at 110°C for 3 h.

[0085] S2. Parameter settings: According to the deposition requirements of PMMA microspheres, the silicon target, graphite target, and LiF target in the sputtering assembly 26 are installed at intervals along the circumferential position of the center of the cavity 2 inside the cavity 2, and then the process parameters are preset in the controller; First sputtering process parameters: silicon target power 6kW, graphite target power 6kW, argon flow rate 150sccm, deposition time 4h; Second sputtering process parameters: LiF target power 3kW, argon flow rate 150sccm, deposition time 30min;

[0086] S3, Deposition of silicon / carbon framework composite layer: The same operation method as step S3 in Example 1 is used, except that the silicon / carbon mass ratio is 6:1 and the thickness of the silicon / carbon framework composite layer is 200nm.

[0087] S4. Deposition of protective layer: The same operation method as step S4 in Example 1 is used, except that the thickness of the LiF ion transport layer is 30 nm.

[0088] S5. Substrate material removal: After deposition, cool to room temperature, turn off the main power, break the vacuum and remove the second substrate composite material. Place the second substrate composite material in a heating furnace for heating at 500℃ for 30 minutes to thermally decompose the PMMA microspheres and obtain the low-expansion silicon-carbon anode composite material with the substrate removed.

[0089] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 3042 mAh / g and the initial efficiency was 90%.

[0090] Comparative Example 1

[0091] This comparative example includes the following steps:

[0092] S1. Substrate pretreatment: The same treatment method as step S1 in Example 1 is adopted, except that spherical sodium chloride with a particle size of 8μm is selected as the substrate material and vacuum dried at 110°C for 3.5h.

[0093] S2. Parameter settings: Use the same sputtering process parameters as in Example 1;

[0094] S3, Deposition of silicon / carbon framework composite layer: The same operation method as step S3 in Example 1 is used;

[0095] S4. Deposition of protective layer: The same operation method as step S4 in Example 1 is used;

[0096] S5. Removal of substrate material: The same operation method as step S5 in Example 1 is used;

[0097] S6. Post-processing: The same operation method as step S6 in Example 1 is adopted.

[0098] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 2748 mAh / g and the initial efficiency was 87%.

[0099] Comparative Example 2

[0100] S1. Substrate pretreatment: The same treatment method as step S1 in Example 2 is adopted, except that spherical calcium sulfate with a particle size of 40 μm is selected as the substrate material and vacuum dried at 110°C for 3.5 h.

[0101] S2. Parameter settings: Use the same sputtering process parameters as in Example 2;

[0102] S3, Deposition of silicon / carbon framework composite layer: The same operation method as step S3 in Example 2 is used;

[0103] S4. Deposition of protective layer: The same operation method as step S4 in Example 2 is adopted;

[0104] S5. Removal of substrate material: The same operation method as step S5 in Example 2 is used;

[0105] S6. Post-processing: The same operation method as step S6 in Example 2 is adopted.

[0106] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 2651 mAh / g and the initial efficiency was 84%.

[0107] Comparative Example 3

[0108] This comparative example includes the following steps:

[0109] S1. Substrate pretreatment: The same treatment method as step S1 in Example 1 is adopted, except that calcium sulfate with a particle size of 25 μm is selected as the substrate material and vacuum dried at 100°C for 3 h.

[0110] S2. Parameter settings: According to the deposition requirements of calcium sulfate, the silicon target, graphite target, and Al2O3 target in the sputtering assembly 26 are installed at intervals along the circumferential position of the center of the cavity 2 inside the cavity 2. Then, the first sputtering process parameters are preset in the controller: silicon target power 6kW, graphite target power 6kW, argon flow rate 150sccm, deposition time 4h; the second sputtering process parameters are: Al2O3 target power 8kW, argon flow rate 150sccm, deposition time 50min.

[0111] S3, Deposition of silicon / carbon framework composite layer: The same operation method as step S3 in Example 1 is used, except that the silicon / carbon mass ratio is 8:1 and the thickness of the silicon / carbon framework composite layer is 300nm.

[0112] S4. Deposition of protective layer: The same operation method as step S4 in Example 1 is adopted, except that the thickness of the Al2O3 hard layer is 20nm.

[0113] S5. Substrate material removal: After deposition, cool to room temperature, turn off the main power, break the vacuum and remove the second substrate composite material. Place the second substrate composite material in a hydrochloric acid solution with pH=3 and stir at room temperature for 4 hours. After filtration, wash with anhydrous ethanol until neutral.

[0114] S6. Post-processing: The composite material from which the calcium sulfate substrate was removed in step S5 is vacuum dried at 100°C for 6 hours to obtain a low-expansion hollow silicon-carbon anode material.

[0115] The performance of the obtained low-expansion hollow silicon-carbon anode material was tested. The specific steps were as follows: silicon-carbon anode material, acetylene black and polyvinylidene fluoride binder were mixed in a mass ratio of 85:10:5, dispersed in deionized water to make a slurry, coated on a copper foil current collector, dried and cold-pressed to obtain anode sheet, and the anode sheet was assembled with lithium sheet into a button battery and tested; the initial capacity was 2755 mAh / g and the initial efficiency was 85%.

[0116] As can be seen from the test results of Examples 1-4 and Comparative Examples 1-3 as described above, this application uses a curtain-type coating device to sequentially deposit a silicon / carbon framework composite layer and a protective layer on the surface of a removable substrate, constructing a unique structure of "hollow center, silicon / carbon framework composite layer, and protective layer". The hollow structure provides sufficient buffer space for silicon expansion. The silicon / carbon framework composite layer is prepared by co-sputtering silicon and graphite targets, and the carbon network is formed in situ and tightly bonded to silicon, fundamentally suppressing the volume expansion and particle agglomeration of silicon, laying the foundation for the high capacity of the material. The protective layer optimizes ion transport and interface stability. The three work synergistically to achieve a combination of low expansion and high capacity.

[0117] While the disclosure is as stated above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of this disclosure, and all such changes and modifications will fall within the protection scope of this invention.

Claims

1. A method for preparing a low-expansion silicon-carbon anode material, characterized in that, Includes the following steps: S1. Substrate pretreatment: Select a removable substrate material, dry the substrate material, then open the shell and cavity of the curtain-type covering equipment, and feed the dried substrate material into the storage bin at the bottom of the cavity. Use the through hole at the bottom of the storage bin to allow the substrate material to enter the circulating conveying mechanism. S2. Parameter settings: Install the silicon / carbon skeleton composite layer target and the protective layer target in the sputtering assembly along the circumferential direction of the cavity center, and then preset the first sputtering process parameters of the silicon / carbon skeleton composite layer and the second sputtering process parameters of the protective layer in the controller. S3, Silicon / Carbon Framework Composite Layer Deposition: Close the shell and the cavity, start the vacuum mechanism by the controller to complete the vacuuming and introduce argon gas, so that the inside of the shell is in a vacuum-sealed state; The circulating material conveying mechanism is activated to transport the substrate material into the cavity, and a silicon / carbon skeleton composite layer is sputtered and deposited on the surface of the substrate material according to the first sputtering process parameters to obtain the first substrate composite material. S4. Protective layer deposition: Start the circulating material conveying mechanism to continue circulating the first substrate composite material into the cavity, and deposit a protective layer on the first substrate composite material according to the second sputtering process parameters to obtain the second substrate composite material. S5. Substrate material removal: After deposition, cool to room temperature, turn off the power, break the vacuum and remove the second substrate composite material. Place the second substrate composite material in an acidic solution and stir and wash until the filtrate is neutral, or place the second substrate composite material in a furnace for thermal decomposition to remove the substrate material in the second substrate composite material, thereby obtaining a substrate-free composite material. S6. Post-processing: The substrate-free composite material is dried to obtain a low-expansion silicon-carbon anode material.

2. The method for preparing low-expansion silicon-carbon anode material according to claim 1, characterized in that, The deposition method of the silicon / carbon framework composite layer in step S3 is as follows: After starting the circulating feeding mechanism, the substrate material is fed to the redistributor above the cavity. Under its own gravity, the substrate material slides down the surface of the redistributor to the bottom of the cavity, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and according to the first sputtering process parameters, a substrate material for a first-time deposition of silicon / carbon framework composite layer is obtained by depositing on the surface of the substrate material. The steps after starting the circulating feeding mechanism in this step are repeated until the silicon / carbon framework composite layer of the target thickness is deposited. Sputtering is then stopped to obtain the first substrate composite material.

3. The method for preparing low-expansion silicon-carbon anode material according to claim 1, characterized in that, The method for depositing the protective layer in step S4 is as follows: After starting the circulating material feeding mechanism, the first substrate composite material is fed to the redistributor in the cavity. Under its own gravity, the first substrate composite material slides down the surface of the redistributor to the bottom of the cavity, forming a vertical curtain during the sliding process. At the same time, the sputtering power supply is started, and the protective layer is deposited on the surface of the first substrate composite material according to the second sputtering process parameters. The steps after starting the circulating material feeding mechanism in this step are repeated until the protective layer of the target thickness is deposited, and sputtering is stopped to obtain the second substrate composite material.

4. The method for preparing low-expansion silicon-carbon anode material according to claim 1, characterized in that, The protective layer is at least one of a carbon layer, a LiF ion transport layer, and an Al2O3 hard layer; the target material selected for the protective layer is at least one of a carbon target, a LiF target, and an Al2O3 target; when the protective layer is a carbon layer, the target material is a carbon target, and the sputtering conditions are an argon flow rate of 100~300 sccm, a target power of 5~10 kW, a deposition time of 20~60 min, and a layer thickness of 20~100 nm; when the protective layer is a LiF ion transport layer, the target material is a LiF target, and the sputtering conditions are an argon flow rate of 100~200 sccm, a target power of 2~5 kW, a deposition time of 15~40 min, and a layer thickness of 10~30 nm; when the protective layer is an Al2O3 hard layer, the target material is an Al2O3 target, and the sputtering conditions are an argon flow rate of 100~200 sccm, a target power of 4~8 kW, a deposition time of 20~50 min, and a layer thickness of 10~20 nm.

5. The method for preparing low-expansion silicon-carbon anode material according to claim 1, characterized in that, The thickness of the silicon / carbon framework composite layer in step S3 is 50~500nm; the mass ratio of silicon to carbon is 3:1~7:

1.

6. The method for preparing low-expansion silicon-carbon anode material according to claim 1, characterized in that, The substrate material in step S1 is at least one of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, copper chloride, calcium sulfate, glucose, and polymethyl methacrylate microspheres; the particle size of the substrate material is 10~30μm; and the shape of the substrate material is one of spherical, near-spherical, and irregular shapes.

7. The method for preparing low-expansion silicon-carbon anode material according to claim 1, characterized in that, The pH of the acidic solution in step S5 is 2-5, and the stirring time is 2-6 hours; the drying temperature of the post-treatment in step S6 is 80-120°C, and the drying time is 4-8 hours.

8. A low-expansion silicon-carbon anode material, characterized in that, The low-expansion silicon-carbon anode material is prepared by any one of the low-expansion silicon-carbon anode material preparation methods according to claims 1-7.

9. An application of a method for preparing low-expansion silicon-carbon anode material, characterized in that, The application employs the preparation method of the low-expansion silicon-carbon anode material according to any one of claims 1-7, and the application is used to prepare lithium-ion batteries, which are used in new energy vehicles, energy storage systems, or 3C electronic products.

10. The application of the method for preparing low-expansion silicon-carbon anode material according to claim 9, characterized in that, The negative electrode preparation process of the lithium-ion battery includes the following steps: uniformly dispersing silicon-carbon negative electrode material, conductive additives, and binders in a certain proportion, and then coating the uniformly dispersed slurry onto a metal substrate and drying it to obtain a negative electrode sheet; the mass ratio of the silicon-carbon negative electrode material, the conductive additives, and the binders is 80-90:5-10:5-10; the binder is at least one of sodium carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, sodium alginate, and polyvinylidene fluoride.