Silicon-based material, preparation thereof, negative electrode sheet, battery, battery pack, and electric device

By optimizing the X-ray diffraction and Raman spectral characteristics of silicon-based materials and adjusting their crystallinity and disordered structure, the volume expansion problem of silicon-based materials during lithium intercalation was solved, thereby improving the first-efficiency and rate performance of the battery.

CN123143384APending Publication Date: 2026-11-20BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511566719.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-29
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

During lithium intercalation, silicon-based materials undergo drastic deformation, leading to volume expansion, which causes the negative electrode to detach from the current collector and interface failure, affecting the battery's initial efficiency and rate performance.

Method used

By adjusting the half-peak width at half-peak and the ratio of Raman spectral features of the characteristic diffraction peaks in the X-ray diffraction pattern of silicon-based materials, their crystallinity and disordered structure can be optimized, suitable ion diffusion channels can be formed, the lithium intercalation overpotential can be reduced, and the uniformity of lithium intercalation can be improved.

Benefits of technology

It improves the initial efficiency and rate performance of the battery, reduces deformation and interface failure in solid-state batteries, and enhances structural stability and ion conduction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143384A_ABST
    Figure CN123143384A_ABST
Patent Text Reader

Abstract

Embodiments of the present application provide a silicon-based material, a preparation method thereof, a negative electrode sheet, a battery, a battery pack and an electrical equipment. The silicon-based material has a first characteristic diffraction peak at a 2theta position of 28.5±2° in an X-ray diffraction spectrum, and a half-peak width FWHM of the first characteristic diffraction peak satisfies 2.5°≤FWHM≤10.5°. The silicon-based material comprises pure silicon, and the mass ratio of the pure silicon to the silicon-based material is greater than or equal to 98%. The silicon-based material can effectively improve the lithium intercalation uniformity of the silicon-based material, reduce the lithium intercalation overpotential of the silicon negative electrode, and improve the electrochemical performance of the battery, such as the initial efficiency, the rate performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of batteries, and more particularly to a silicon-based material and its preparation method, a negative electrode, a battery, a battery pack, and an electrical device. Background Technology

[0002] With the current trend of iterative upgrades in energy storage technology, portable electronic devices, new energy vehicles, and smart grid energy storage require secondary batteries with higher performance. Silicon-based materials have attracted widespread attention as negative electrode active materials due to their high theoretical capacity. However, repeated lithium intercalation in silicon-based materials can cause drastic deformation and volume expansion, leading to the detachment of silicon-based materials from the negative electrode current collector and interfacial failures between materials, especially the failure of the solid-solid interface physical contact, which forms ion transport barriers. These problems, in turn, affect the battery's electrochemical performance, such as its initial efficiency and rate capability. Summary of the Invention

[0003] This application provides a silicon-based material and its preparation method, a negative electrode, a battery, a battery pack, and electrical equipment, which can effectively improve the uniformity of lithium intercalation in silicon-based materials, reduce the overpotential of lithium intercalation in silicon negative electrodes, and improve the electrochemical performance of batteries, such as first-time efficiency and rate performance.

[0004] In a first aspect, embodiments of this application provide a silicon-based material, wherein the X-ray diffraction pattern of the silicon-based material has a first characteristic diffraction peak at a 2θ position of 28.5±2°, and the full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 2.5°≤FWHM≤10.5°; the silicon-based material comprises pure silicon, and the mass ratio of pure silicon to the silicon-based material is greater than or equal to 98%.

[0005] According to one embodiment of the present invention, 5.5°≤FWHM≤10.5°.

[0006] According to one embodiment of the present invention, the Raman spectroscopy results of the silicon-based material satisfy the following condition: 0.06 ≤ I1 / I2 ≤ 0.18, where I1 is the Raman shift of 250 cm⁻¹. -1 -350cm -1 The peak intensity in the range, I2 is the Raman shift of 450 cm. -1 -550cm -1 The peak intensity of the interval; preferably, 0.14≤I1 / I2≤0.18.

[0007] According to one embodiment of the present invention, the particle size D of the silicon-based material n 50 is 50 nm to 2 μm; preferably, the particle size D of the silicon-based material is... n 50 refers to 50nm to 1μm.

[0008] According to one embodiment of the present invention, the silicon-based material further includes a metal layer present on the surface of the pure silicon; and / or, the metal layer includes one or more of silver, indium, and tin.

[0009] According to one embodiment of the present invention, the lithium intercalation uniformity R of the silicon-based material in the lithium intercalation state at 80% SOC satisfies 80%≤R≤100%.

[0010] Secondly, embodiments of this application provide a method for preparing the above-mentioned silicon-based material, comprising the following steps: subjecting an organosilicon source to a pyrolysis reaction to obtain the silicon-based material.

[0011] According to one embodiment of the present invention, the process of pyrolyzing the organosilicon source includes: mixing an organosilicon with a fluidizing gas and then carrying out the pyrolysis reaction to obtain the silicon-based material; and / or, the flow rate of the fluidizing gas is 600 mL / min-1000 mL / min; and / or, the fluidizing gas includes nitrogen and / or argon; and / or the temperature of the pyrolysis reaction is 400℃~750℃; and / or, the method for preparing the silicon-based material further includes: after the pyrolysis reaction is completed, cooling the obtained pyrolysis reaction product at a rate of 10℃ / s-20℃ / s to generate the silicon-based material.

[0012] According to one embodiment of the present invention, the method further includes: after the pyrolysis reaction is completed, coating the obtained pyrolysis reaction product with a metal material to form a metal layer on the surface of the pyrolysis reaction product, thereby obtaining the silicon-based material.

[0013] Thirdly, embodiments of this application provide a negative electrode sheet, including a negative electrode current collector and a negative electrode active layer present on at least one side of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material, which includes the silicon-based material described above or a silicon-based material prepared according to the silicon-based material preparation method described above.

[0014] According to one embodiment of the present invention, the content of conductive material in the negative electrode active layer is 0.

[0015] Fourthly, embodiments of this application provide a battery including the aforementioned negative electrode sheet.

[0016] According to one embodiment of the present invention, the battery is a solid-state battery.

[0017] Fifthly, embodiments of this application provide a battery pack comprising at least two batteries as described above that are interconnected.

[0018] Sixthly, embodiments of this application provide an electrical device including the battery or battery pack described above.

[0019] This application provides a silicon-based material and its preparation method, a negative electrode, a battery, a battery pack, and an electrical device. In the X-ray diffraction pattern of the silicon-based material, there is a first characteristic diffraction peak at the 2θ position at 28.5±2°, and the full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 2.5°≤FWHM≤10.5°. The silicon-based material includes pure silicon, and the mass ratio of pure silicon to the silicon-based material is greater than or equal to 98%. The first characteristic diffraction peak of the X-ray diffraction pattern of this silicon-based material has a full width at half maximum (FWHM) of 2.5°≤FWHM≤10.5°, and the pure silicon content is greater than or equal to 98%. This gives the silicon-based material suitable crystallinity and disordered structure, which can effectively increase the number of ion diffusion channels and ion migration rate in the silicon-based material. It can optimize the ion-electron conductivity network of the negative electrode sheet using this silicon-based material as the negative electrode active material, improve the lithium intercalation uniformity of the silicon-based material, reduce the lithium intercalation overpotential (lithium intercalation polarization overpotential) of the silicon negative electrode, and thus improve the electrochemical performance of the battery, such as the first efficiency and rate performance. Attached Figure Description

[0020] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0021] Figure 1 X-ray diffraction (XRD) spectra of silicon-based materials of Example 1 and Comparative Example 1 provided in this application.

[0022] The accompanying drawings illustrate specific embodiments of this application, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the concept in any way, but rather to illustrate the concept of this application to those skilled in the art through reference to particular embodiments. Detailed Implementation

[0023] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims.

[0024] Silicon-based materials have attracted widespread attention due to their high theoretical capacity and can be used as anode active materials in anode sheets. However, due to factors such as the tendency of silicon-based materials to undergo anisotropic volume expansion and poor conductivity, silicon-based materials generally suffer from poor lithium intercalation uniformity and high lithium intercalation overpotential, which affect the electrochemical performance of batteries, such as initial efficiency and rate performance.

[0025] For example, repeated lithium intercalation of silicon-based materials can easily cause severe deformation and volume expansion, leading to problems such as the separation of silicon-based materials from the negative electrode current collector and the failure of physical contact between the materials, resulting in ion transport barriers. This results in poor lithium intercalation uniformity and high polarization overpotential in the negative electrode, affecting the battery's first charge-discharge efficiency (first efficiency) and rate performance, among other electrochemical properties.

[0026] Especially for solid-state batteries, the drastic deformation caused by repeated lithium intercalation during battery charging and discharging of silicon-based materials can lead to stress concentration in the solid electrolyte layer, making it prone to cracking. This, in turn, can cause interfacial failure between the negative electrode and the solid electrolyte layer, as well as a sharp drop in capacity. Simultaneously, the expansion and contraction of silicon-based material particles can easily cause the silicon-based materials in the negative electrode to detach from the negative electrode current collector. This makes it more susceptible to the formation of ion transport barriers due to the failure of physical contact between materials, deteriorating the uniformity of lithium intercalation in the silicon-based materials, increasing the lithium intercalation overpotential of the negative electrode, and affecting the initial efficiency and rate performance of the negative electrode.

[0027] According to the inventors' research, by adjusting the crystal structure of silicon-based materials, the overall ionic and electronic conductivity network of silicon-based materials can be optimized and the lithium intercalation uniformity of silicon-based materials can be improved, thereby reducing the lithium intercalation overpotential of silicon anodes. This can be a direction that takes into account both improving the first-efficiency and rate performance of batteries.

[0028] In view of this, the present invention proposes a silicon-based material, wherein the X-ray diffraction (XRD) spectrum of the silicon-based material has a first characteristic diffraction peak at the 2θ position at 28.5±2°, and the full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 2.5°≤FWHM≤10.5°; the silicon-based material includes pure silicon, and the mass ratio of pure silicon to the silicon-based material is greater than or equal to 98%.

[0029] This invention provides a silicon-based material with a pure silicon content of ≥98% and a specific microstructure. The material exhibits a first characteristic diffraction peak at the 2θ position (28.5±2°) in its X-ray diffraction (XRD) spectrum, with a full width at half maximum (FWHM) within the range of 2.5°≤FWHM≤10.5°. This silicon-based material possesses suitable crystallinity and a disordered structure, enabling isotropic ion diffusion channels. Using this silicon-based material as the negative electrode active material effectively increases the number and migration rate of ion diffusion channels for active ions such as lithium ions, improves the ion conductivity network, enhances the uniformity of lithium intercalation, and reduces the lithium intercalation overpotential of the silicon negative electrode. This, in turn, improves the battery's first charge / discharge efficiency (first efficiency) and rate performance. Furthermore, the ≥98% pure silicon content results in fewer inactive impurities and better electrochemical activity when applied to solid-state batteries.

[0030] The reason for this is that the full width at half maximum (FWHM) of the characteristic diffraction peak at 28.5 ± 2° in the X-ray diffraction (XRD) spectrum of silicon-based materials is within the range of 2.5° ≤ FWHM ≤ 10.5°, indicating that they possess suitable crystallinity and order. The larger the FWHM of the first characteristic diffraction peak of silicon-based materials, the more disordered structures exist within the silicon material. If FWHM < 2.5°, the internal order of the silicon-based material is too high, resulting in a single ion diffusion channel, which leads to low ion conduction efficiency, poor lithium intercalation uniformity, and high overpotential for lithium intercalation at the negative electrode. Therefore, FWHM ≥ 2.5° helps to construct relatively more ion diffusion channels and improve ion migration rate. When the FWHM of the first characteristic diffraction peak increases infinitely, the amorphization degree of the silicon-based material approaches 10. At 0%, the silicon-based material exhibits a highly disordered lattice structure. However, this structure results in poor stability and demanding storage conditions. Therefore, the full width at half maximum (FWHM) of the first characteristic diffraction peak of the aforementioned silicon-based material, which is 2.5°≤FWHM≤10.5°, helps maintain a suitable degree of amorphization, enabling the silicon-based material to maintain good structural stability and other properties. This also suppresses volume expansion, homogenizes the lithium intercalation process, improves the uniformity of lithium intercalation, and reduces the overpotential of lithium intercalation.

[0031] Therefore, the silicon-based material provided in this application embodiment has a first characteristic diffraction peak at the 2θ position of 28.5±2°, and the full width at half maximum (FWHM) of the first characteristic diffraction peak is between 2.5° and 10.5°. This can simultaneously improve the structural stability and ion conduction efficiency of the silicon-based material, reduce the lithium intercalation overpotential of the negative electrode, and improve the lithium intercalation uniformity of the silicon-based material. In particular, it can improve the first-cycle lithium intercalation uniformity of the silicon-based material, thereby improving the electrochemical performance of the battery, such as the initial efficiency and rate capability.

[0032] The silicon-based materials of this invention are particularly applicable to solid-state batteries, reducing the deformation of silicon-based materials during battery charging and discharging, avoiding stress concentration and cracking of the solid electrolyte layer, which in turn leads to interfacial failure and a sudden drop in capacity between the negative electrode and the solid electrolyte layer. Simultaneously, it avoids the problems of silicon-based materials in the negative electrode separating from the negative electrode current collector due to the expansion and contraction of silicon-based material particles, forming ion transport barriers due to solid-solid interface physical contact failure, and thus affecting the capacity utilization and kinetic performance of the negative electrode. Furthermore, it can reduce side reactions between silicon-based materials and solid electrolytes (such as sulfide solid electrolytes), lower the interfacial resistance between materials, and reduce capacity loss (for example, it can reduce the charging capacity in the 1.0V-3.0V voltage range of the battery, reducing the capacity loss rate), thereby simultaneously improving the electrochemical performance of solid-state batteries, including initial efficiency, rate performance, specific capacity, and cycle stability.

[0033] For example, the full width at half maximum (FWHM) of the first characteristic diffraction peak can be a range of 2.5°, 3°, 4°, 5°, 6°, 7°, 8°, 9°, 10°, 10.5° or any combination thereof.

[0034] In some preferred embodiments, the full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 5.5°≤FWHM≤10.5°. For example, it can be a range of 5.5°, 7°, 8°, 9°, 10.5° or any combination thereof. This is beneficial for further reducing the overpotential of lithium intercalation in the silicon anode, improving the uniformity of lithium element distribution after lithium intercalation in a single silicon particle (silicon-based material) and the initial coulombic efficiency of the silicon-based material, while also improving the electrochemical performance of the battery, such as initial efficiency and rate performance.

[0035] It is understandable that the first characteristic diffraction peak is a broadened arc-shaped diffraction peak, and its overall range includes intervals greater than 28.5±2°. The 2θ position of the first characteristic diffraction peak mentioned above refers to the peak position corresponding to the maximum peak intensity of the first diffraction characteristic peak of the silicon-based material (i.e., the 2θ angle corresponding to the maximum peak intensity of the first diffraction characteristic peak). The full width at half maximum (FWHM) is used to describe the peak shape characteristics of the signal. It is defined as the peak width at 50% of the peak height. The smaller the FWHM, the sharper the signal, reflecting a higher degree of internal order in the material. Conversely, the larger the FWHM, the broader the signal, reflecting a lower degree of internal order in the material.

[0036] In this embodiment of the invention, silicon-based materials can be XRD tested using conventional XRD testing methods to obtain the X-ray diffraction pattern of the silicon-based materials and the full width at half maximum (FWHM) of the first characteristic diffraction peak.

[0037] In some embodiments, the Raman spectral test results of silicon-based materials satisfy the following condition: 0.06 ≤ I1 / I2 ≤ 0.18, where I1 is the Raman shift of 250 cm⁻¹. -1 -350cm -1 The peak intensity in the range, I2 is the Raman shift of 450 cm. -1 -550cm -1 The peak intensity in the range is beneficial for further reducing the overpotential of lithium intercalation in silicon anodes, reducing the polarization overpotential during the first charge of the battery, improving the uniformity of lithium intercalation in silicon anodes, and also improving the structural stability of silicon-based materials.

[0038] The reason is that 250cm -1 -350cm -1 The signal peaks in the interval correspond to the defect structures in the shallow surface layer of silicon-based materials, while the 450cm peak... -1 -550cm -1The signal peak in the range is closely related to the shallow crystalline silicon structure of silicon-based materials, 450 cm⁻¹ -1 -550cm -1 The intensity variation of the signal peaks within a given range can reflect the degree of crystallinity in the shallow surface layer of silicon-based materials. Therefore, the I1 / I2 ratio reflects the crystallization state and lattice defects of silicon-based materials. An I1 / I2 ratio of not less than 0.06 indicates that the crystallinity of the silicon-based material is within the range of 250 cm⁻¹. -1 -350cm -1 The stronger the signal peak intensity in the interval, the better, at 450cm. -1 -550cm -1 The weaker the signal peak intensity in the interval, the more defective structures the silicon material has. At this time, the more disordered the internal structure of the silicon-based material, the more conducive it is to the formation of isotropic ion diffusion channels. An I1 / I2 ratio of no more than 0.18 is more conducive to the preparation of silicon-based materials. Therefore, 0.06≤I1 / I2≤0.18 can further reduce the diffusion activation energy of active ions such as lithium ions in silicon-based materials, thereby significantly reducing the polarization overpotential in the first charge of the battery negative electrode. At the same time, it can also improve the uniformity of lithium intercalation and structural stability of silicon materials, as well as improve the fabrication feasibility of silicon-based materials.

[0039] For example, I1 / I2 is a range of 0.06, 0.08, 0.11, 0.14, 0.16, 0.18 or any two of them.

[0040] In some preferred embodiments, 0.14≤I1 / I2≤0.18, further reducing the overpotential of lithium intercalation in the negative electrode and improving the uniformity and structural stability of lithium intercalation in the negative electrode.

[0041] In this embodiment of the invention, the silicon-based material can be subjected to Raman testing using conventional Raman spectroscopy testing methods to obtain the Raman spectrum of the silicon-based material and the aforementioned peak intensities I1 and I2, thereby obtaining I1 / I2.

[0042] In some embodiments, the particle size D of the silicon-based material n 50 can be from 50nm to 2μm, for example, it can be a range of 50nm, 80nm, 200nm, 500nm, 1μm, 1.5μm, 1.8μm, 2μm or any combination thereof. Thus, the particle size D of the silicon-based material... n A particle size of at least 50 nm ensures the crystallographic parameters of silicon-based materials and further avoids agglomeration during the fabrication of negative electrodes, thus facilitating the capacity utilization of silicon-based materials. Simultaneously, the particle size D of the silicon-based material... n A particle size of 50 μm or less than 2 μm is more conducive to improving the structural stability of silicon-based materials and reducing their volume expansion rate. Therefore, the particle size D of silicon-based materials... nThe range of 50 nm to 2 μm is more conducive to the capacity utilization of silicon-based materials and reduces the volume expansion rate of silicon-based materials.

[0043] In some preferred embodiments, the particle size D of the silicon-based material n The value of 50 can be 50nm to 1μm, which is beneficial for reducing the first-cycle polarization overpotential of the battery negative electrode and improving the uniformity and structural stability of lithium intercalation in silicon materials, while also reducing the volume expansion rate of silicon materials and the negative electrode polarization overpotential, and improving the uniformity and structural stability of lithium intercalation in silicon materials.

[0044] In this embodiment of the invention, the particle size D n 50 (also known as the number median particle size) means that in the particle size distribution, 50% of the particles have a particle size smaller than this value, while 50% of the particles have a particle size greater than or equal to this value.

[0045] Particle size D of silicon-based materials n 50 can be measured by the following method: Particle size distribution can be obtained by analyzing the scattered light generated when a laser passes through a particle suspension. Based on the relationship between the intensity of the scattered light and the particle size, the particle size distribution can be determined. The testing method refers to the standard GB / T19077-2024 "Particle Size Analysis: Laser Diffraction Method" for testing the particle size D of silicon-based materials. n 50. It should be noted that, due to the small particle size and high surface energy of nano-silicon, agglomeration is prone to occur, resulting in uneven dispersion in suspensions. In such cases, the particle size D of silicon-based materials can be tested according to the test standard GB / T 42208-2022 "Measurement of Nanoparticle Size in Multiphase Systems of Nanotechnology by Transmission Electron Microscopy Imaging". n 50. Specifically, after the silicon-based material is made into a negative electrode or battery, the battery can be disassembled to remove the negative electrode. The powder on the surface of the negative electrode can be scraped off with a scraper, dispersed in a solvent, and then subjected to particle size testing according to the steps described above to obtain the particle size D of the silicon-based material. n 50.

[0046] In some embodiments, the silicon-based material further includes a metal layer present on the surface of pure silicon, i.e., a metal layer is coated on the surface of pure silicon. This is beneficial to further improve the electronic conductivity of the silicon-based material and improve the rate performance of the battery, in addition to improving the uniformity and structural stability of lithium intercalation and reducing the first-cycle polarization overpotential of the battery negative electrode.

[0047] Specifically, the metal layer may include one or more of silver (Ag), indium (In), and tin (Sn).

[0048] In some embodiments, the metal layer may include one or more of Ag metal layer, In metal layer, and Sn metal layer.

[0049] In some embodiments, the thickness of the metal layer is 2nm-5nm, for example, it can be a range of 2nm, 3nm, 4nm, 5nm or any combination thereof. The thickness of the metal layer is not less than 2nm, which is beneficial to further improve the electronic conductivity of the silicon-based material. At the same time, the thickness of the metal layer is not more than 5nm, which is more beneficial to the capacity utilization of pure silicon in the silicon-based material, improves the lithium intercalation uniformity of the silicon-based material, and reduces the lithium intercalation polarization overpotential of the silicon anode. Therefore, a metal layer thickness of 2nm-5nm is more beneficial to reducing the lithium intercalation polarization overpotential of the silicon anode, improving the lithium intercalation uniformity of the silicon-based material, and facilitating the capacity utilization of the silicon-based material.

[0050] In this embodiment of the invention, the thickness of the metal layer can be obtained by the following method: Specifically, the thickness of the metal layer on the surface of silicon-based material particles can be tested by transmission electron microscopy (TEM). The average value of the metal layer thickness of 20 silicon-based material particles is taken after statistical testing.

[0051] In this embodiment of the invention, pure silicon can be coated using a conventional vapor deposition method to form a metal layer on its surface.

[0052] In this embodiment of the invention, the lithium intercalation uniformity R of the silicon-based material in the lithium intercalation state at 80% SOC satisfies 80%≤R≤100%. For example, it can be 80%, 85%, 90%, 92%, 97%, 100%, or any two of these ranges, which is beneficial to further improve the performance of the silicon-based material, such as the first-round lithium intercalation uniformity.

[0053] In this embodiment of the invention, silicon-based materials can be assembled into a full cell to measure its lithium intercalation uniformity R.

[0054] In practice, the test method for the lithium intercalation uniformity R of silicon-based materials during the first charge and discharge cycle can include:

[0055] S101. Assemble silicon-based materials into a negative electrode sheet (or silicon negative electrode, silicon-based electrode sheet).

[0056] S102. After assembling the negative electrode into a battery, apply current (i.e. charge the battery) to insert lithium into the silicon negative electrode. After reaching the above-mentioned SOC state (i.e., 80% state of charge), disassemble the battery and remove the negative electrode.

[0057] The specific calculation method for the SOC state is as follows:

[0058] State of Charge (SOC) = Lithium intercalation capacity / (m 硅 ×C 硅 );

[0059] Where, m 硅 C represents the mass of the silicon-based material on the negative electrode. 硅This represents the theoretical specific capacity of silicon-based materials.

[0060] For example, the lithium intercalation capacity can be obtained through the following specific test: Assemble a battery by combining a negative electrode, a positive electrode, and a sulfide electrolyte, setting the ratio of negative electrode capacity to positive electrode capacity (N / P ratio) to be 1:1, where C 硅 The value is 3579 mAh / g. Taking the lithium intercalation uniformity R at 80% SOC as an example, the lithium intercalation capacity = m 硅 ×C 硅 ×0.8, using this calculated value as the capacity cutoff condition for the charging process, and setting the current magnitude to 0.01C (based on the negative electrode surface capacity calculation). When the charging reaches this cutoff capacity, the negative electrode lithium intercalation state is 80% SOC state of charge.

[0061] Specifically, when measuring the lithium intercalation uniformity R of silicon-based materials, the lithium intercalation state of the negative electrode can be between 1% SOC and 100% SOC. Under different SOC states, the observed lithium intercalation uniformity R of silicon-based materials shows the same trend, with R all within the range of 1% ≤ R ≤ 100%. 25% SOC-80% SOC is preferred, as it has a better observation effect on lithium intercalation uniformity R.

[0062] S103. The states of lithium-intercalated silicon-based materials and non-lithium-intercalated silicon-based materials have significant differences in lithium element distribution, color contrast, electrochemical behavior, and mechanical behavior. Scanning electron microscopy (SEM) can be used to identify the color degree differences in different regions of the negative electrode caused by the distribution of lithium elements. Then, the area S1 of the region where lithium elements are distributed in a single silicon particle after lithium intercalation and the cross-sectional integral area S2 of a single silicon particle can be obtained. R can be calculated according to R=S1 / S2×100%.

[0063] Specifically, the negative electrode sheet can be cut along the thickness direction perpendicular to the negative electrode sheet using methods such as focused ion beam (FIB). The cut cross section formed during the cutting of the negative electrode sheet is the cross section to be measured. The cross section to be measured is scanned by SEM, and S1 / S2 is obtained by integration. That is, the negative electrode sheet is deeply etched and image identified using focused ion beam scanning electron microscopy (FIB-SEM), and the area S1 of the region where lithium element is distributed in a single silicon particle after lithium intercalation and the cross-sectional integrated area S2 of a single silicon particle are obtained by integration. R is then calculated according to R=S1 / S2×100%.

[0064] In step S102, the negative electrode (working electrode), solid electrolyte membrane, and positive electrode (counter electrode) are assembled into a battery. The solid electrolyte membrane is formed of Li6PS5Cl, and the negative electrode is prepared according to the negative electrode preparation process in Example 1 below, which will not be repeated here.

[0065] In addition, in a full cell, the positive electrode may include positive electrode active materials such as lithium phosphate, lithium transition metal oxide and its coating, and doped modified compounds.

[0066] In specific operation, the positive electrode in the full cell is an NCM811 positive electrode, which is prepared according to the positive electrode preparation process in Example 1 below, and will not be repeated here.

[0067] In this embodiment of the invention, a method for preparing a silicon-based material is also provided, comprising the following steps: subjecting an organosilicon source to a pyrolysis reaction to obtain a silicon-based material.

[0068] In some embodiments, the pyrolysis reaction time can be from 0.5 seconds to 30 seconds (s), for example, it can be a range of 0.5 seconds, 1 second, 5 seconds, 10 seconds, 15 seconds, 20 seconds, 25 seconds, 30 seconds or any two of these, which is beneficial to suppress the growth of silicon crystal nuclei and form the above-mentioned silicon-based material.

[0069] In some embodiments, the organosilicon source includes silane, which may include silane (SiH4), which is more conducive to obtaining silicon-based materials with low crystallinity.

[0070] In some embodiments, a fluidizing gas can be used as a carrier to allow the organosilane to undergo pyrolysis in a fluidized state.

[0071] In some embodiments, the process of pyrolyzing an organosilicon source may include: mixing an organosilicon with a fluidizing gas and then pyrolyzing the mixture to obtain a silicon-based material.

[0072] The flow rate of the fluidizing gas can be 600 mL / min to 1000 mL / min, for example, it can be 600 mL / min, 700 mL / min, 800 mL / min, 900 mL / min, 1000 mL / min or any combination thereof. The organosilicon and the fluidizing gas can undergo pyrolysis reaction in a fluidized bed reactor. The pressure in the fluidized bed reactor can be between atmospheric pressure (i.e., standard atmospheric pressure, 101325 Pa) and 0.5 bar. A flow rate of not less than 600 mL / min is beneficial to avoid excessive pyrolysis of the organosilicon source and to inhibit the growth of crystalline silicon. A flow rate of not more than 1000 mL / min is beneficial to the full pyrolysis reaction of the organosilicon source. Therefore, a flow rate of 600 mL / min to 1000 mL / min is more conducive to achieving stable fluidization of silicon particles, inhibiting the growth of silicon crystal nuclei, and thus more conducive to obtaining the above-mentioned silicon-based materials, and further optimizing the lithium intercalation uniformity and other properties of the silicon-based materials.

[0073] In some embodiments, the fluidizing gas may include nitrogen and / or argon, which is more conducive to generating silicon-based materials with high internal disorder.

[0074] In some embodiments, the volume ratio of the organosilicon source to the fluidizing gas can be 1:20 to 1:3, for example, it can be a range of 1:20, 1:15, 1:10, 1:5, 1:3 or any two of them, which is beneficial to further improve the preparation efficiency of silicon-based materials.

[0075] In some embodiments, the temperature of the pyrolysis reaction can be 400℃~750℃, for example, it can be a range of 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃ or any combination thereof. The temperature of the pyrolysis reaction is not less than 400℃, which can further promote the pyrolysis reaction of the organosilicon source. The temperature of the pyrolysis reaction is not greater than 750℃, which can avoid over-pyrolysis of the organosilicon source and is conducive to further suppressing the growth of silicon crystal nuclei. Therefore, completing the pyrolysis of the organosilicon source in this reaction zone is more conducive to improving the preparation efficiency of silicon-based materials and their lithium intercalation uniformity and other properties. At the same time, the pyrolysis process has low energy consumption, which is more conducive to industrial application.

[0076] In this embodiment of the invention, the method for preparing silicon-based materials may further include: after the pyrolysis reaction is completed, cooling the obtained pyrolysis reaction products at a cooling rate of 10℃ / s-20℃ / s to obtain the silicon-based material. For example, the cooling rate can be 10℃ / s, 13℃ / s, 15℃ / s, 18℃ / s, 20℃ / s, or any combination thereof. Specifically, the silicon source undergoes a pyrolysis reaction at the above-mentioned pyrolysis reaction temperature. After the pyrolysis reaction is completed, the temperature is reduced at a rate of 10℃ / s-20℃ / s, that is, the temperature is reduced by 10℃-20℃ per second, to obtain the silicon-based material. A cooling rate of not less than 10℃ / s is more conducive to cooling the pyrolysis reaction products and more conducive to locking the amorphous structure of the pyrolysis reaction products, thereby obtaining the silicon-based material. The reason for this is that rapidly cooling the pyrolysis reaction products at a rate of at least 10°C / s is more conducive to freezing atomic motion, shortening the time for silicon atoms to arrange themselves in an ordered manner, and kinetically blocking the formation and growth of the silicon crystal structure. This makes it easier to obtain the aforementioned silicon-based materials and further enhances the disorder of the silicon-based materials, improving properties such as the uniformity of lithium intercalation. A cooling rate of no more than 20°C / s avoids excessively rapid temperature drops that could lead to an increased volume expansion rate in the prepared silicon-based materials. Therefore, cooling the obtained pyrolysis reaction products at a rate of 10°C / s-20°C / s is more conducive to enhancing the disorder of the silicon-based materials and reducing their volume expansion rate.

[0077] In practice, the organosilicon source and fluidized gas are mixed and introduced into a fluidized bed reactor. The organosilicon source undergoes pyrolysis under the aforementioned pyrolysis reaction temperature and other conditions. The pyrolysis reaction rate can be controlled by adjusting the pyrolysis temperature of the fluidized bed reactor, and the pyrolysis reaction time can be controlled by controlling the flow rate of the organosilicon source, thereby controlling the degree of pyrolysis of the organosilicon and generating silicon-based materials. During the pyrolysis reaction, the generated silicon atoms (pyrolysis reaction products) can undergo amorphous deposition on the surface of pre-set attachment sites. To reduce impurity adsorption, separation devices such as two-stage cyclone separators and / or ceramic filters can be used to continuously remove unreacted organosilicon source and by-product powder from the pyrolysis reaction products. Simultaneously, conventional cooling methods such as water-cooled jackets are used to rapidly cool the pyrolysis reaction products at 10℃ / s-20℃ / s to lock in the amorphous structure, resulting in silicon-based materials.

[0078] In some embodiments, the method for preparing silicon-based materials further includes: after the pyrolysis reaction is completed, coating the obtained pyrolysis reaction product with a metal material to form a metal layer on the surface of the pyrolysis reaction product, thereby obtaining a silicon-based material with a metal coating layer.

[0079] When the silicon-based material also includes a metal layer coated on the surface of the silicon substrate, the pyrolysis reaction products are rapidly cooled at 10℃ / s-20℃ / s to obtain a silicon substrate. Subsequently, conventional coating methods such as chemical vapor deposition (CVD) can be used to coat the obtained silicon substrate to form a metal layer on its surface. The thickness and other characteristics of the formed metal layer (coating layer) can be controlled by conventional methods, without any particular limitation.

[0080] In this embodiment of the invention, a negative electrode sheet is also provided, comprising a negative electrode current collector and a negative electrode active layer present on at least one side of the negative electrode current collector. The negative electrode active layer comprises a negative electrode active material, which includes the aforementioned silicon-based material or a silicon-based material prepared according to the aforementioned method for preparing silicon-based materials. This negative electrode sheet has advantages corresponding to the aforementioned silicon-based materials, which will not be elaborated further.

[0081] Specifically, a negative electrode active layer can be provided on one side of the negative electrode current collector, or a negative electrode active layer can be provided on both the positive and negative sides of the negative electrode current collector.

[0082] The negative electrode current collector can be a conventional negative electrode current collector in the art. For example, the negative electrode current collector may include copper foil (or copper foil substrate), but is not limited to this.

[0083] In this embodiment of the invention, the negative electrode active layer may further include an adhesive, which can bond the negative electrode active material and other material particles in the negative electrode active layer of the negative electrode sheet, as well as the negative electrode active layer and the negative electrode current collector, to further improve the structural stability of the negative electrode sheet, while also improving the uniformity of lithium intercalation of silicon-based materials at the individual silicon particle unit level and the electrode sheet level, and reducing the overpotential of lithium intercalation of the negative electrode.

[0084] In some embodiments, the mass ratio of the binder to the negative electrode active layer can be 1% to 10%, for example, it can be 1%, 3%, 5%, 7%, 9%, 10%, or any combination thereof. This is beneficial for further improving the uniformity of lithium intercalation and structural stability of the negative electrode sheet, while also facilitating the preparation of the negative electrode sheet. Specifically, when preparing a negative electrode sheet by coating, the negative electrode active material and binder are usually mixed with a solvent to prepare a negative electrode slurry. The negative electrode slurry is then coated onto the negative electrode current collector to form the negative electrode active layer, thus obtaining the negative electrode sheet. When the amount of binder is within the above-mentioned range (i.e., the mass ratio of the binder to the total mass used to form the negative electrode active layer is within the range of 1% to 10%), it is beneficial for the uniform mixing of the negative electrode slurry and for giving the negative electrode slurry good viscosity and fluidity. While leveraging the adhesive effect of the binder, it also facilitates the coating process of the negative electrode slurry, improving the preparation efficiency of the negative electrode sheet.

[0085] In some embodiments, the electronic conductivity σ of the adhesive is ≥ 1 × 10⁻⁶ -4 S / m can promote the construction of the overall ion and electron conductive network of the negative electrode, improve the conductivity of the negative electrode, and optimize the transport efficiency of active ions such as lithium ions.

[0086] In some embodiments, the binder may contain metal elements (i.e., the binder in the negative electrode may include a metal-modified binder). That is, the binder (or functional binder) may include a binder matrix and metal elements present in the binder matrix. Metal element modification facilitates the formation of a functional binder with electronic conductivity, thereby improving the electronic conductivity of the binder. Simultaneously, by combining silicon-based materials with metal-modified binders, the intrinsic properties of the material can be reconstructed at the atomic scale, providing a fundamental material optimization scheme for high-energy-density batteries (especially high-energy-density solid-state batteries).

[0087] Specifically, by introducing a metal element-modified binder into the negative electrode active layer containing the above-mentioned silicon-based material, it is beneficial to further improve the following effects: (1) improve the specific capacity and first efficiency of the negative electrode and the battery, and reduce the overpotential of lithium intercalation of the negative electrode; (2) reduce the expansion rate of lithium intercalation of the negative electrode, for example, the ratio of the fully charged volume to the zero-charged volume of the battery can be as low as 210% or less, and the thickness change of the negative electrode after 300 cycles of the battery is reduced; (3) improve the structural stability of the negative electrode, and further improve the cycle life and capacity retention of the battery; (4) reduce the interfacial impedance between materials and the capacity loss due to side reactions. For example, when the negative electrode is applied to a solid-state battery, the interfacial impedance between the negative electrode material and the solid electrolyte can be reduced, and the side reactions between materials and the resulting capacity loss can be reduced.

[0088] In some embodiments, the metal element includes one or more of silver, indium, and tin, which helps to further optimize the electron and ion transport network of the negative electrode and improve the uniformity of lithium intercalation and the performance of multiple charge and discharge.

[0089] In some embodiments, metal elements can be combined with the binder matrix in one or more forms, such as nanowires, nanosheets, and nanospheres (nanoparticles), to form a functional binder with electronic conductivity, which is beneficial for further improving both the bonding and conductivity properties of the binder.

[0090] In some embodiments, the mass ratio of the metal element to the binder matrix can be 1:19 to 1:1, for example, it can be a range of 1:19, 1:16, 1:13, 1:10, 1:7, 1:4, 1:2, 1:1 or any combination thereof. A mass ratio of the metal element to the binder matrix of not less than 1:19 is beneficial to further enhance the electronic conductivity of the binder. A mass ratio of the metal element to the binder matrix of not more than 1:1 is beneficial to improve the adhesive strength of the binder. Therefore, when the mass ratio of the metal element to the binder matrix is ​​1:19 to 1:1, it is beneficial to further improve both the adhesive performance and the conductivity of the binder.

[0091] Specifically, the aforementioned adhesive or adhesive matrix may include a polymeric adhesive, which may be a conventional polymeric adhesive in the art. For example, the polymeric adhesive may include polyacrylic acid (PAA) and / or carboxymethyl cellulose salt, and the carboxymethyl cellulose salt may include sodium carboxymethyl cellulose (CMC-Na).

[0092] For example, the above-mentioned adhesive may include one or more of the following: a PAA modified with silver (Ag) nanowires, a PAA modified with silver (Ag) nanoparticles, a PAA modified with tin (Sn) nanowires, and a PAA modified with indium (In) nanoparticles. The PAA modified with silver nanowires includes a PAA (adhesive matrix) and silver elements present in the PAA, wherein the silver elements are composited with the PAA in the form of nanowires. The PAA modified with silver nanoparticles has silver elements composited with the PAA in the form of nanoparticles. The PAA modified with tin nanowires has tin elements composited with the PAA in the form of nanowires. The PAA modified with indium nanoparticles has indium elements composited with the PAA in the form of nanowires.

[0093] In this embodiment of the invention, metal element modified binders can be obtained by conventional methods, such as commercially available ones, or by self-made using conventional methods in the art. For example, a desired amount of metal nanowires can be introduced into the binder matrix by conventional methods to obtain metal nanowire modified binders (such as the aforementioned silver nanowire modified PAA, etc.), and there are no particular limitations on this.

[0094] In this embodiment of the invention, no conductive agent may be added to the negative electrode active layer (i.e., the content of conductive material in the negative electrode active layer can be essentially zero). Specifically, the silicon-based material in this embodiment of the invention has abundant ion diffusion channels and a good electronic conductivity network. It can maintain a high ion transport efficiency and electron transport efficiency of the negative electrode without the use of a conductive agent. Especially when using the above-mentioned binder containing metal elements (i.e., a binder modified with metal elements), it is more conducive to building a good ion and electron conductivity network in the negative electrode active layer, improving the conductivity of the negative electrode, optimizing the ion transport path, improving the ion transport rate and lithium intercalation uniformity of the negative electrode, and reducing problems such as lithium intercalation overpotential and volume expansion of the negative electrode.

[0095] In some embodiments, the negative electrode active layer may be composed of a negative electrode active material and a binder (i.e., the negative electrode active layer does not contain conductive agents or other materials).

[0096] In this embodiment of the invention, the negative electrode sheet can be prepared by conventional methods such as coating. Specifically, the components used to form the negative electrode active layer, such as the negative electrode active material and binder, can be dispersed in a negative electrode solvent and mixed evenly by stirring to prepare a negative electrode slurry. This slurry is then coated onto the surface of the negative electrode current collector, and after drying, rolling (cold pressing), slitting, and cutting, the negative electrode sheet is obtained. The negative electrode solvent may include, for example, water. The coating, drying, rolling, slitting, and cutting processes are conventional operations for preparing negative electrode sheets using the coating method and are not particularly limited thereto.

[0097] An embodiment of the present invention further provides a battery, comprising the negative electrode sheet described above. This battery has the advantages corresponding to the above silicon-based material or the above negative electrode sheet, which will not be repeated here.

[0098] In the embodiments of the present invention, the above battery may be a solid-state battery, and the solid-state battery may specifically include an all-solid-state battery. In some embodiments, the above battery may include a positive electrode sheet, a negative electrode sheet, and a solid electrolyte film located between the positive electrode sheet and the negative electrode sheet. The solid electrolyte film includes a solid electrolyte (also referred to as a solid electrolyte base material), and the solid electrolyte may include a lithium ion-conducting solid electrolyte (lithium ion conductor system).

[0099] In some embodiments, the solid electrolyte may include one or more of a sulfide solid electrolyte (also referred to as a sulfide ion conductor or a sulfide-type solid electrolyte), an oxide solid electrolyte (oxide solid ionic conductor), and a nitride solid electrolyte (nitride solid ionic conductor).

[0100] For example, the solid electrolyte may include a LISICON-type solid electrolyte (γ-Li3PO4), a NASICON-type solid electrolyte (Li 1+x Q x M 2-x (PO4)3, Q=Al / Cr / Ba, 0≤x<1), a garnet-type solid electrolyte (Li 7-x La3Zr 2-x M x O 12 , M=Nb / Ta, 0≤x<1), a LIPON-type amorphous solid electrolyte (Li x PO y N z , x / y / z∈(0,1]), a perovskite-type solid electrolyte (Li 3x Q 2 / 3-x MO3, Q=La / Sr, 0.04<x<0.17), an anti-perovskite-type solid electrolyte (Li3OCl), and a sulfide solid electrolyte. The sulfide solid electrolyte may include one or more of thiophosphates (Li3PS4 / Li6PS5Cl), halo-sulfur compounds (Li3InCl6), and multi-component complexes ((100-x)Li2S x M y Q, M=B2S3 / Al2S3, Q=oxide / halide, 20≤x≤30, 0≤y≤50).

[0101] In the embodiments of the present invention, a positive electrode sheet conventional in the art may be used, and no particular limitation is imposed thereon. For example, the positive electrode sheet may include a positive electrode current collector, and a positive electrode active layer present on at least one surface of the positive electrode current collector. Specifically, the positive electrode active layer may be provided on one surface of the positive electrode current collector, or the positive electrode active layer may be respectively provided on both the front and back surfaces of the positive electrode current collector.

[0102] Herein, the positive electrode current collector may be a positive electrode current collector conventional in the art, for example, the positive electrode current collector may include an aluminum foil, but is not limited thereto.

[0103] Herein, the positive electrode active layer may include a positive electrode active material, which may be a positive electrode active material conventional in the art. For example, the positive electrode active material may include a lithium-containing active material capable of deintercalating and intercalating lithium ions, that is, a positive electrode active material for lithium-ion batteries.

[0104] For example, the above positive electrode active material may include one or more of a layered transition metal oxide system positive electrode material, an olivine-type phosphate system positive electrode material, and a spinel-type lithium manganese oxide (LiMn2O4).

[0105] Herein, the layered transition metal oxide system positive electrode material may include one or more of LiMO2 type positive electrode materials (M=one or more of Co, Ni, Mn) and oxide positive electrode materials having a multi-metal solid solution structure, for example, lithium nickel cobalt manganese oxide (LiNi x Co y Mn z O2, where 0<x,y,z<1 and x+y+z=1), and stoichiometric variants thereof may include NCM333 (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), NCM622 (LiNi 0.6 Co 0.2 Mn 0.2 O2), high-nickel type NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2), NC (LiNi 0.85 Co 0.15 Al 0.05 O2), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and derivatives thereof treated by doping, coating and the like, and the like, one or more of which may be included.

[0106] In addition, the olivine-type phosphate system may include compounds having a LiMPO4 structure (M=Fe, Mn or a mixture thereof), and the compounds having a LiMPO4 structure may include lithium iron phosphate (LiFePO4, LFP) and iron-manganese mixed crystal phases thereof (such as LiFe 0.5Mn 0.5 One or more of the following: PO4, lithium manganese phosphate (LiMnPO4), and their nanocomposite modification products with the above materials.

[0107] For the aforementioned positive electrode active materials, a single positive electrode active material can be used alone, or multiple positive electrode active materials can be used in combination. For example, LFP and NCM622 can be used simultaneously as the positive electrode active materials of the positive electrode sheet (in this case, the positive electrode sheet is a mixed electrode of LFP and NCM622), or LFP, NCM622, and other positive electrode materials such as spinel-type lithium manganese oxide (LiMn2O4) can be used simultaneously as the positive electrode active materials of the positive electrode sheet. In addition, the aforementioned positive electrode active materials can be surface modified / coated (e.g., Al2O3 coating) or lattice doped (e.g., Mg). 2+ and / or Ti 4+ After being doped with elements such as metals or with particle size controlled (e.g., nano-processing), the electrochemical performance of the material can be further optimized. These surface modifications / coatings, dopings, and particle size controls can all be performed using conventional processes in the field, and there are no particular limitations on them.

[0108] In addition, the positive electrode active layer may also include a conductive agent and / or a binder, both of which can be conventional materials in the art. For example, the conductive agent may include one or more of carbon black, carbon nanotubes (CNT), acetylene black, graphene, Ketjen black, and carbon fiber, and the binder may include one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, etc.

[0109] In addition, the positive electrode active layer may also include a solid electrolyte, which may include a sulfide solid electrolyte and / or a halide solid electrolyte. For example, the sulfide solid electrolyte may include Li 6-a PS 5-a X 1+a One or more of LGPS, LPS, and Li2S-P2S5 glass-ceramic solid electrolytes, Li 6-a PS 5-a X 1+a In this context, X represents a halogen, 0 ≤ a ≤ 0.8, and halide solid electrolytes may include Li. b MX c O d and / or Li b MX c O dIn this formula, X represents a halogen, M represents a transition metal element, 1≤b≤3, 1≤c≤6, 0≤d≤1, but is not limited to these. The types of solid electrolytes in the positive electrode active layer can be found in the aforementioned introduction to the types of solid electrolytes in solid electrolyte membranes, and will not be elaborated upon further here. The solid electrolyte in the positive electrode active layer can be the same as or different from the solid electrolyte in the solid electrolyte membrane.

[0110] For example, the above-mentioned sulfide solid electrolyte may include Li6PS5Cl, Li 10 GeP2S 12 Li 5.5 PS5Cl 1.5 One or more of the following, halide solid electrolytes may include chloride solid electrolytes, and chloride solid electrolytes may include Li 1.75 ZrCl 4.75 O 0.5 .

[0111] In this embodiment of the invention, the positive electrode sheet can be prepared by conventional methods in the art, such as by coating. Specifically, the positive electrode active material, conductive agent, binder, and other components used to form the positive electrode active material layer can be dispersed in a positive electrode solvent, such as N-methylpyrrolidone (NMP), to prepare a positive electrode slurry. This slurry is then coated onto the surface of the positive electrode current collector, and after drying, rolling, and other processes, the positive electrode sheet is obtained. The coating, drying, and rolling processes involved are conventional operations for preparing positive electrode sheets using the coating method, and are not particularly limited thereto.

[0112] In this embodiment of the invention, the battery can be manufactured by conventional methods in the art, and there are no particular limitations thereto.

[0113] This invention also provides a battery pack comprising at least two interconnected batteries as described above. This battery pack has advantages corresponding to the silicon-based materials described above, which will not be elaborated further.

[0114] Generally, a battery pack includes multiple batteries as individual cells, which are connected to form the battery pack. These batteries can be electrically connected using methods conventional in the art, such as series connection, parallel connection, or a combination of these connection methods, without any particular limitation.

[0115] This invention also provides an electrical device, including the battery or battery pack described above. This electrical device has advantages corresponding to the silicon-based material described above, which will not be elaborated further.

[0116] The electrical equipment used in the embodiments of the present invention can be conventional electrical equipment in the art, such as power equipment (e.g., electric vehicles, electric cars), electronic equipment (e.g., mobile phones, tablets, laptops, digital cameras, etc.), wearable devices (e.g., watches, bracelets, VR glasses, etc.), energy storage power stations, etc., and there are no particular limitations on this.

[0117] The present invention will be further described below through specific embodiments.

[0118] Example 1

[0119] (1) Preparation of silicon-based materials

[0120] Using high-purity nitrogen as the fluidizing gas, silane (SiH4) and N2 were mixed at a volume ratio of 1:10 and then introduced into a fluidized bed reactor. The pyrolysis reaction was carried out in the reaction zone at 550℃. During the pyrolysis reaction, the pressure inside the reactor was controlled from atmospheric pressure to 0.3 bar, the gas flow rate was maintained at 800 mL / min, and the pyrolysis reaction time was 20 seconds. During the reaction, silicon atoms generated were deposited amorphously on the surface of pre-set attachment sites. Unreacted silane and by-product powder were continuously removed by a two-stage cyclone separator and a ceramic filter. At the same time, the pyrolysis reaction products were rapidly cooled at 15℃ / s by a water-cooled jacket to generate silicon-based materials (pure silicon, silicon content 99.9%).

[0121] Among them, the particle size D of the prepared silicon-based material n 50 = 1.0 μm. In its X-ray diffraction pattern, it has a first characteristic diffraction peak at the 2θ position at 28.5 ± 2°, with a full width at half maximum (FWHM) of 6 ± 0.5°. In its Raman spectroscopy results, I1 / I2 = 0.14, where I1 is the Raman shift of 250 cm⁻¹. -1 -350cm -1 The peak intensity in the range, I2 is the Raman shift of 450 cm. -1 -550cm -1 Peak intensity within the range.

[0122] (2) Preparation of negative electrode

[0123] Silicon-based materials, PAA, and CMC-Na were mixed in a pure water solvent at a mass ratio of 94:5:1. The mixture was stirred thoroughly with a stirrer to ensure uniform mixing of all components, thus obtaining the negative electrode slurry.

[0124] The negative electrode slurry is coated on both sides of the copper foil substrate, and then the negative electrode sheet is obtained through processes such as drying, cold pressing, slitting and cutting.

[0125] Examples 2-8:

[0126] The difference from Example 1 lies in the FWHM, the mass ratio of pure silicon to silicon-based material, I1 / I2, and the particle size D of the silicon-based material. n 50, R, the flow rate of the fluidizing gas, the temperature of the pyrolysis reaction, and the cooling rate of the pyrolysis reaction products are different, but the remaining steps and conditions are the same as in Example 1, as detailed in Table 1.

[0127] Example 9:

[0128] The difference from Example 1 is that the pure silicon prepared in Example 1 was mixed with 2 wt% nano-silver powder in an argon glove box, and loaded into a ball milling jar at a ball-to-material ratio of 20:1 (zirconia grinding balls with diameters of 3 / 5 / 10 mm). The mixture was ball-milled in stages at 300 rpm for 8 h (with cooling paused every 2 h) to prepare a silicon-based material modified with an Ag metal layer. The remaining steps and conditions were the same as in Example 1, as detailed in Table 1.

[0129] Comparative Example 1

[0130] The difference from Example 1 is that the micron-sized silicon prepared by the crushing method is used as the negative electrode active material. Specifically, silicon particles (particle size < 5 mm) and zirconia grinding balls are loaded into a planetary ball mill jar at a ball-to-material ratio of 10:1, and ball-milled at 300 rpm for 6 hours under argon protection. After pausing to cool down every 2 hours, the mixture is filtered through a sieve to obtain the aforementioned micron-sized silicon. The remaining steps and conditions are the same as in Example 1, as detailed in Table 1.

[0131] Comparative Example 2

[0132] The difference from Example 1 is that, in the preparation process of silicon-based materials, the pyrolysis reaction temperature was adjusted to 850°C and the gas flow rate was maintained at 500 mL / min. The remaining steps and conditions were the same as in Example 1, as detailed in Table 1.

[0133] Test case

[0134] The particle size D of the silicon-based materials in each embodiment and comparative example was tested using the following process. n 50. The uniformity R of lithium intercalation in silicon-based materials under 80% SOC lithium intercalation state, the full width at half maximum (FWHM) of the first characteristic diffraction peak in the XRD of silicon-based materials, the I1 / I2 ratio in the Raman spectroscopy test results of silicon-based materials, and the rate performance and first coulombic efficiency of the battery are shown in Tables 1 and 2.

[0135] 1. Particle size D of silicon-based materials n 50 Test: Particle Size D of Silicon-Based Materials n The measurement method for 50 is the same as described above and will not be repeated here.

[0136] 2. Test method for lithium intercalation uniformity R of silicon-based materials in an 80% SOC lithium intercalation state:

[0137] S101. Assemble silicon-based materials into a negative electrode sheet (or silicon negative electrode, silicon-based electrode sheet).

[0138] S102. After assembling the negative electrode, solid electrolyte membrane, and positive electrode (counter electrode) into a full cell, charge the battery to insert lithium into the negative electrode. After reaching 80% SOC, disassemble the battery and remove the negative electrode.

[0139] The solid electrolyte membrane is formed from Li6PS5Cl.

[0140] The positive electrode is prepared according to the following process: a lithium-nickel-cobalt-manganese ternary LiNi alloy is formed. 0.8 Co 0.1 Mn 0.1 O2 (D) n 50 = 6 μm, Young's modulus is 120 GPa, and specific surface area is 0.4 m². 2 The positive electrode slurry is obtained by thoroughly mixing (e.g., stirring for 240 min) the positive electrode material with thiophosphate (Li6PS5Cl), conductive carbon black, and binder PVDF in a weight ratio of 60:40:1:1 in NMP. This slurry is then coated onto both sides of an aluminum foil substrate. The substrate is then dried, compacted, slit, and cut to obtain the positive electrode sheet. The compaction process includes three stages: pre-compression, main compression, and holding pressure. The pre-compression pressure is 3 MPa; the main compression (high pressure) pressure is 100 MPa; and the holding pressure is maintained at the high pressure for 20 seconds.

[0141] S103. The negative electrode sheet is deeply etched and image recognized by FIB-SEM. The area S1 of the region where lithium element is distributed in a single silicon particle after lithium intercalation and the cross-sectional area S2 of a single silicon particle are obtained by integration. The lithium intercalation uniformity R is calculated according to R=S1 / S2×100%.

[0142] 3. XRD Testing of Silicon-Based Materials (Fifth of Half Peak (FWHM) Measurement of the First Characteristic Diffraction Peak): The XRD testing method for silicon-based materials is implemented according to GB / T 30904-2014 X-ray Diffraction Method for Crystal Structure Analysis of Inorganic Chemical Products. The definition and identification of the half-peak width (FWHM) can be obtained by referring to the method in GB / T 40219-2021. The FWHM of the first characteristic diffraction peak can then be measured. Figure 1 As shown.

[0143] 4. Raman Spectroscopy Test Method for Silicon-based Materials: The Raman spectroscopy test method for silicon-based materials shall be implemented in accordance with the method in GB / T40219-2021. After measuring the Raman spectrum of the silicon-based material, the Raman shift shall be recorded as 250 cm⁻¹. -1 -350cm -1 The peak intensity within the range is I1, and the recorded Raman shift is 450 cm⁻¹.-1 -550cm -1 The peak intensity within the range is I2, and thus I1 / I2 of silicon-based materials can be obtained.

[0144] 5. Test methods for battery rate performance:

[0145] (5-1) Preparation of positive electrode sheet

[0146] The preparation process of the positive electrode is the same as that of the positive electrode in the above-mentioned test of lithium intercalation uniformity R of silicon-based materials in 80% SOC lithium intercalation state.

[0147] (5-2) Ratio Performance Test

[0148] A coin cell is assembled from a negative electrode, a solid electrolyte membrane, and a positive electrode; the solid electrolyte membrane is formed from Li6PS5Cl.

[0149] The prepared button cell was charged at 25±2℃ with a constant current of 0.1C to the upper limit voltage of 4.2V, and then discharged at different rates of 0.1C and 0.5C with a constant current to 2.5V. The discharge capacity at 0.1C and 0.5C was recorded. The rate performance of the battery (i.e., the discharge capacity ratio of 0.5C / 0.1C) = discharge capacity at 0.5C / discharge capacity at 0.1C.

[0150] 6. First Coulomb efficiency test of the battery:

[0151] The button cell was prepared according to the above method;

[0152] The prepared coin cell was charged at 25±2℃ with a constant current of 0.1C to the upper limit voltage of 4.2V. After standing for 5 minutes, it was discharged at the same rate with a constant current to the cutoff voltage of 2.5V. The ratio of discharge capacity to charge capacity was recorded, which is the first coulombic efficiency (i.e., first coulombic efficiency = discharge capacity / charge capacity).

[0153] Table 1 Preparation of silicon-based materials

[0154]

[0155] Table 2 Performance Tests

[0156]

[0157] Compared to Comparative Examples 1-2, the X-ray diffraction patterns of the silicon-based materials in Examples 1-9 show a first characteristic diffraction peak at the 2θ position at 28.5±2°. The full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 2.5°≤FWHM≤10.5°. Furthermore, the silicon-based materials include pure silicon, with pure silicon accounting for more than or equal to 98% of the mass of the silicon-based materials. This can effectively improve the uniformity of lithium intercalation in the silicon-based materials, reduce the overpotential of lithium intercalation in the silicon anode, and improve the electrochemical performance of the battery, such as its initial efficiency and rate performance.

[0158] like Figure 1 As shown, the horizontal axis represents 2θ, with the unit being degrees (°), and the vertical axis represents intensity, where (au) is the unit of relative intensity. This can be seen from... Figure 1 As can be seen, the silicon-based material of Example 1 has a first characteristic diffraction peak at the 2θ position of 28.5±2°. The full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 2.5°≤FWHM≤10.5°, indicating that the silicon-based material has more disordered structures inside, which is more conducive to the formation of isotropic ion diffusion channels. In contrast, the characteristic diffraction peak of Comparative Example 1 at the 2θ position of 28.5±2° is sharp and narrow, indicating that the micron-sized silicon has a high degree of order and a single ion diffusion channel.

[0159] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A silicon-based material, characterized in that, In the X-ray diffraction pattern of the silicon-based material, there is a first characteristic diffraction peak at the 2θ position at 28.5±2°, and the full width at half maximum (FWHM) of the first characteristic diffraction peak satisfies: 2.5°≤FWHM≤10.5°. The silicon-based material includes pure silicon, and the pure silicon accounts for more than or equal to 98% of the mass of the silicon-based material.

2. The silicon-based material according to claim 1, characterized in that, 5.5°≤FWHM≤10.5°.

3. The silicon-based material according to claim 1 or 2, characterized in that, The Raman spectroscopy results of the silicon-based material satisfy the following condition: 0.06 ≤ I1 / I2 ≤ 0.18, where I1 is the Raman shift of 250 cm⁻¹. -1 -350cm -1 The peak intensity in the range, I2 is the Raman shift of 450 cm. -1 -550cm -1 Peak intensity within the range; Preferably, 0.14≤I1 / I2≤0.

18.

4. The silicon-based material according to any one of claims 1-3, characterized in that, The particle size D of the silicon-based material n 50 refers to the range of 50 nm to 2 μm; Preferably, the particle size D of the silicon-based material is... n 50 refers to 50nm to 1μm.

5. The silicon-based material according to any one of claims 1-4, characterized in that, The silicon-based material also includes a metal layer present on the surface of the pure silicon; And / or, the metal layer includes one or more of silver, indium, and tin.

6. The silicon-based material according to any one of claims 1-5, characterized in that, The uniformity R of lithium intercalation in the silicon-based material at 80% SOC satisfies 80% ≤ R ≤ 100%.

7. A method for preparing a silicon-based material according to any one of claims 1-6, characterized in that, Includes the following steps: The organosilicon source is subjected to a pyrolysis reaction to obtain the silicon-based material.

8. The method for preparing silicon-based materials according to claim 7, characterized in that, The process of pyrolyzing the organosilicon source includes: mixing the organosilicon with a fluidizing gas and then carrying out the pyrolysis reaction to obtain the silicon-based material. And / or, the flow rate of the fluidizing gas is 600 mL / min-1000 mL / min; And / or, the fluidizing gas includes nitrogen and / or argon; And / or the temperature of the pyrolysis reaction is 400℃~750℃; And / or, the method for preparing the silicon-based material further includes: after the pyrolysis reaction is completed, cooling the obtained pyrolysis reaction product at a rate of 10℃ / s-20℃ / s to generate the silicon-based material.

9. The method for preparing silicon-based materials according to claim 7 or 8, characterized in that, Also includes: After the pyrolysis reaction is completed, the obtained pyrolysis reaction product is coated with a metal material to form a metal layer on the surface of the pyrolysis reaction product, thereby obtaining the silicon-based material.

10. A negative electrode sheet, characterized in that, It includes a negative electrode current collector and a negative electrode active layer present on at least one side of the negative electrode current collector, the negative electrode active layer including a negative electrode active material, the negative electrode active material including the silicon-based material according to any one of claims 1-6 or the silicon-based material prepared according to the preparation method of the silicon-based material according to any one of claims 7-9.

11. The negative electrode sheet according to claim 10, characterized in that, The content of conductive material in the negative electrode active layer is 0.

12. A battery, characterized in that, Includes the negative electrode sheet as described in claim 10 or 11.

13. The battery according to claim 12, characterized in that, The battery is a solid-state battery.

14. A battery pack, characterized in that, It includes at least two interconnected batteries as described in claim 12 or 13.

15. An electrical appliance, characterized in that, Includes the battery as described in claim 12 or 13 or the battery pack as described in claim 14.