Method for manufacturing positive electrode slurry and positive electrode plate
By mixing lithium composite oxide particles of different sizes and structures in the positive electrode plate and ensuring the conductive path through a specific mixing process, the problem of reduced capacity retention in secondary batteries was solved, and the stability and safety of the batteries were improved.
Patent Information
- Application Number
- CN202610671433.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-19
- Filing Date
- 2026-05-15
- Publication Date
- 2026-11-20
AI Technical Summary
The capacity retention rate of the positive plate of a secondary battery decreases during use, especially due to the instability of the conductive path caused by the expansion and contraction of the positive electrode active material layer.
Lithium composite oxide particles with different particle sizes and structures are used as positive electrode active materials. A specific ratio and sequence of mixing process is used to ensure the contact area and conductive path between the conductive material and the active material. This includes mixing secondary particles formed by agglomerating more than 50 primary particles with single particles or secondary particles formed by agglomerating 2-10 primary particles, using a specific ratio of conductive material and binder, and adjusting the timing and amount of conductive material addition.
It improves the capacity retention rate of the secondary battery, reduces cracks in the active material caused by charging and discharging, suppresses heat generation during short circuits, and maintains the stability and performance of the battery.
Smart Images

Figure CN123143385A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a method for manufacturing a positive electrode slurry and a positive electrode plate. Background Technology
[0002] The positive electrode plate of the secondary battery has a layer of positive electrode active material containing positive electrode active material. As a positive electrode active material, condensed particles formed by the aggregation of single particles and multiple primary particles are known to be used (e.g., Japanese Patent Application Publication No. 2022-143761). Summary of the Invention
[0003] In cases where the positive electrode plate has a layer of positive electrode active material formed by mixing single particles and condensed particles, the capacity retention rate sometimes decreases when used in a secondary battery.
[0004] The purpose of this disclosure is to provide a method for manufacturing a positive electrode slurry and a positive electrode plate that can improve the capacity retention of a secondary battery.
[0005] [1] A method for manufacturing a positive electrode slurry, which is a method for manufacturing a positive electrode slurry for a non-aqueous electrolyte secondary battery.
[0006] The aforementioned positive electrode slurry comprises a first positive electrode active material as lithium composite oxide particles and a second positive electrode active material as lithium composite oxide particles.
[0007] The aforementioned first positive electrode active material is a secondary particle formed by the aggregation of more than 50 primary particles.
[0008] The aforementioned second positive electrode active material is a single particle or a secondary particle formed by the aggregation of 2 to 10 primary particles.
[0009] The above manufacturing method includes:
[0010] Step (a) involves mixing the first positive electrode active material, the first binder, and the first dispersion medium to obtain the first compound.
[0011] Step (b) of mixing the first compound and the first conductive material to obtain the second compound, and
[0012] Step (c) of mixing the second positive electrode active material, the second binder, and the second dispersion medium to obtain the third compound, and
[0013] The following [i] or [ii]:
[0014] [i] Step (d) of mixing the second compound, the third compound and the second conductive material.
[0015] [ii] The step (e) of mixing the third compound and the second conductive material to obtain the fourth compound and the step (f) of mixing the second compound and the fourth compound;
[0016] In the above manufacturing method, the first conductive material and the second conductive material are mixed in a weight ratio of 45:55 to 65:35.
[0017] [2] According to the manufacturing method of the positive electrode slurry described in [1], in the manufacturing method, the first positive electrode active material and the second positive electrode active material are mixed in a ratio of first positive electrode active material: second positive electrode active material = 70:30 to 30:70 (weight ratio).
[0018] [3] The method for manufacturing the positive electrode slurry according to [1] or [2], wherein the average particle size (D50) of the first positive electrode active material is greater than the average particle size (D50) of the second positive electrode active material.
[0019] [4] A method for manufacturing a positive electrode slurry according to any one of [1] to [3], wherein the first positive electrode active material and the second positive electrode active material are each independently a lithium composite oxide represented by the following formula (I).
[0020] Li 1.00+a1 Ni x1 Me 1.00-x1 O2 (I)
[0021] In formula (I),
[0022] a1 and x1 satisfy the relationships -0.30≤a1≤0.30 and 0.30≤x1≤1.00 respectively.
[0023] Me represents one or more elements selected from Co, Mn, Al, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Nb, Ti, Si, V, Cr, and Ge.
[0024] [5] A positive electrode plate having a positive current collector and a positive active material layer,
[0025] The aforementioned positive electrode active material layer includes a first positive electrode active material, a second positive electrode active material, a conductive material, and a binder.
[0026] Both the first and second positive electrode active materials mentioned above are lithium composite oxide particles.
[0027] The aforementioned first positive electrode active material is a secondary particle formed by the aggregation of more than 50 primary particles.
[0028] The aforementioned second positive electrode active material is a single particle or a secondary particle formed by the aggregation of 2 to 10 primary particles.
[0029] In the cross-section of the aforementioned positive electrode active material layer, the contact ratio (CCR1) between the first positive electrode active material and the conductive material and the contact ratio (CCR2) between the second positive electrode active material and the conductive material satisfy the following relationship (1).
[0030] 0.43≤CCR2 / CCR1≤0.70 (1)。
[0031] [6] According to the positive electrode plate described in [5], the contact ratio (CCR1) is 0.49 to 0.65.
[0032] [7] The positive electrode plate according to [5] or [6], wherein the contact ratio (CCR2) is 0.28 to 0.35.
[0033] [8] The positive electrode plate according to any one of [5] to [7], wherein the positive electrode active material layer comprises the first positive electrode active material and the second positive electrode active material in a weight ratio of first positive electrode active material: second positive electrode active material = 70:30 to 30:70.
[0034] [9] The positive electrode plate according to any one of [5] to [8], wherein the average particle size (D50) of the first positive electrode active material is greater than the average particle size (D50) of the second positive electrode active material.
[0035]
[10] The positive electrode plate according to any one of [5] to [9], wherein the positive electrode active material layer comprises the first positive electrode active material, the second positive electrode active material, the conductive material and the binder in a weight ratio of (first positive electrode active material + second positive electrode active material): conductive material: binder = 99.9 to 95.0: 0.05 to 2.00: 0.05 to 3.00.
[0036]
[11] The positive electrode plate according to any one of [5] to
[10] , wherein the first positive electrode active material and the second positive electrode active material are each independently a lithium composite oxide represented by the following formula (I).
[0037] Li 1.00+a1 Ni x1 Me 1.00-x1 O2 (I)
[0038] In formula (I),
[0039] a1 and x1 satisfy the relationships -0.30≤a1≤0.30 and 0.30≤x1≤1.00 respectively.
[0040] Me represents one or more elements selected from Co, Mn, Al, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Nb, Ti, Si, V, Cr, and Ge.
[0041] The above and other objects, features, aspects and advantages of the present invention will become apparent from the following detailed description relating to the invention, which will be understood in conjunction with the accompanying drawings. Attached Figure Description
[0042] Figure 1 This is a flowchart illustrating the manufacturing process of the positive electrode slurry in the embodiment.
[0043] Figure 2 This is a flowchart illustrating the manufacturing process of the positive electrode slurry according to another embodiment. Detailed Implementation
[0044] In this specification, unless otherwise specified, the numerical ranges "m~n" include both upper and lower limits. That is, "m~n" represents a numerical range "above m and below n". Any value selected from this range can be used as a new upper or lower limit. For example, a new numerical range can be set by arbitrarily combining values within the range with values recorded in other parts of this specification, tables, or figures.
[0045] (Manufacturing method of positive electrode slurry)
[0046] Figure 1 and Figure 2 This is a flowchart illustrating the manufacturing process of the positive electrode slurry according to the embodiment. The positive electrode slurry manufactured by the manufacturing method of this embodiment (hereinafter also referred to as "this slurry") can be used to form the positive electrode active material layer of the positive electrode plate in a non-aqueous electrolyte secondary battery (hereinafter also referred to as "secondary battery") such as a lithium-ion battery. The positive electrode plate may also be the positive electrode plate described later.
[0047] This slurry contains a first positive electrode active material (hereinafter also referred to as "the first active material") and a second positive electrode active material (hereinafter also referred to as "the second active material"). In addition to the first active material and the second active material, this slurry may also contain a first binder, a second binder, a first conductive material, a second conductive material, a first dispersion medium, and a second dispersion medium.
[0048] The solids concentration of this slurry is, for example, 40–85% by weight, 45–83% by weight, or 50–80% by weight. Solids refer to the components in this slurry other than the dispersion medium.
[0049] Both the first and second active materials are lithium composite oxide particles. The lithium composite oxide can be an oxide containing lithium and other metal elements, for example, it can have the composition described later. The first active material is a secondary particle formed by the aggregation of 50 or more primary particles. The second active material is a single particle or a secondary particle formed by the aggregation of 2 to 10 primary particles.
[0050] like Figure 1 and Figure 2 The method for manufacturing this slurry is shown below:
[0051] Step (a) (hereinafter also referred to as "step (a)"), involves mixing the first active substance, the first binder, and the first dispersion medium to obtain the first compound.
[0052] Step (b) (hereinafter also referred to as "step (b)"), involves mixing the first compound and the first conductive material to obtain the second compound.
[0053] Step (c) (hereinafter also referred to as "step (c)"), which involves mixing the second active material, the second binder, and the second dispersion medium to obtain the third compound, and
[0054] The following [i] or [ii].
[0055] [i] The step (d) of mixing the second compound, the third compound, and the second conductive material (hereinafter also referred to as "step (d)") Figure 1 ),
[0056] [ii] Step (e) of mixing the third compound and the second conductive material to obtain the fourth compound (hereinafter also referred to as "step (e)") and step (f) of mixing the second compound and the fourth compound (hereinafter also referred to as "step (f)") Figure 2 ).
[0057] The above manufacturing method involves mixing the first conductive material and the second conductive material in a weight ratio of 45:55 to 65:35. This ratio is the weight of the first conductive material used in the mixing process of step (b) to the weight of the second conductive material used in the mixing process of step (d) or step (e).
[0058] Processes (b), (d), (e), and (f) can be independently added to the dispersion medium and mixed with the above-mentioned components.
[0059] The positive electrode active material in the positive electrode plate expands and contracts due to the charging and discharging of the secondary battery. Since the first active material consists of secondary particles formed by the aggregation of multiple primary particles, the expansion and contraction of the first active material easily causes cracks at the particle boundaries of the secondary particles. In the manufacturing method of this slurry, such as... Figure 1 and Figure 2 As shown, in step (b), the first compound containing the first active material and the first binder is mixed with the first conductive material. Therefore, the mixing in step (b) increases the contact area between the first active material and the first conductive material. Thus, it is believed that even if the first active material cracks due to the charging and discharging of the secondary battery, the conductive path can be ensured by the first conductive material, thereby suppressing the electrical isolation of the first active material in the positive electrode active material layer.
[0060] In the manufacturing method of this slurry, such as Figure 1 and Figure 2 As shown, in step (d) or step (e), a third compound containing a second active material and a second binder is compounded with a second conductive material, and the amount of the second conductive material added in these steps is adjusted to be within the range described above relative to the amount of the first conductive material added in step (b). Therefore, it is believed that by compounding in step (d) or step (e), both the contact area between the second active material and the second conductive material and the conductive path around the second active material can be ensured.
[0061] Thus, even with repeated charging and discharging of the secondary battery, the conductive path in the positive electrode active material layer formed using this slurry can be ensured, thereby improving the capacity retention rate of the secondary battery with the positive electrode plate obtained using this slurry.
[0062] To ensure the conductive path of the positive electrode active material layer, it is considered to significantly increase the combined content of the first and second conductive materials in the positive electrode active material layer. In this case, the overall electronic conductivity of the positive electrode plate may sometimes be excessively increased, leading to increased heat generation during a short circuit in the secondary battery. In the manufacturing method of this slurry, even without increasing the combined content of the first and second conductive materials, the conductive path of the positive electrode active material layer can be ensured by adjusting the timing and amount of addition of the first and second conductive materials. By using this slurry to obtain a positive electrode plate without significantly increasing the combined content of the first and second conductive materials, excessive increase in the overall electronic conductivity of the positive electrode plate can be suppressed, thus also suppressing the heat generation during a short circuit in the secondary battery.
[0063] In the first active substance, the number of primary particles in the secondary particles is more than 50, it can be more than 100, or it can be more than 1000, but it is usually 5 × 10⁻⁶. 6 For numbers less than 1, it can also be 5×10. 5 The number of primary particles in the secondary particles is less than 2. When the second active substance is a secondary particle, the number of primary particles in the secondary particles is 2 to 10, 2 to 8, 2 to 5, or 3 to 5.
[0064] In this specification, the number of primary particles contained in secondary particles can be confirmed, for example, by using a scanning electron microscope (hereinafter also referred to as "SEM") to obtain an SEM image. Specifically, it can be confirmed by following these steps: First, assuming the secondary particle is a perfect sphere and the average particle size (D50) (described later) is the diameter of the secondary particle, the volume of the secondary particle is calculated. Next, the surface of the secondary particle is observed using an SEM at 5000x magnification to obtain a surface SEM image. The outline of each primary particle is determined by image analysis of the surface SEM image, and the number of primary particles present in the surface SEM image is determined. The average area of the primary particle is calculated by dividing the area occupied by the primary particles in the surface SEM image by the number of primary particles in the surface SEM image. Next, the cross-section of the secondary particle is observed using an SEM at 5000x magnification to obtain a cross-sectional SEM image. The outline of each primary particle is determined by image analysis of the cross-sectional SEM image, the radial length of the primary particles in the secondary particle is measured, and the average height of the primary particle is calculated. The product of the average area and the average height obtained for the primary particle is calculated as the average volume of the primary particle. Divide the calculated volume of the secondary particles by the average volume of the primary particles (volume of the secondary particles / average volume of the primary particles) to calculate the aggregation number of the primary particles within the secondary particles. The above image analysis can be performed, for example, using the image analysis software "ImageJ" (ver. 1.54g).
[0065] The average particle size (D50) of the first active material is preferably larger than that of the second active material. The D50 of the first active material is, for example, 5–20 μm, and can be 10–19 μm, preferably 15–18 μm. The D50 of the second active material is, for example, 0.5–10.0 μm, and can be 1.0–7.0 μm, preferably 3.5–4.5 μm. In this specification, the average particle size (D50) refers to the particle size in the volumetric particle size distribution where the frequency cumulatively reaches 50% from the smaller particle size side. The volumetric particle size distribution can be determined using a laser diffraction particle size distribution measuring device.
[0066] In the method for manufacturing this slurry, the mixing ratio of the first active substance to the second active substance (first active substance: second active substance (weight ratio)) is preferably 70:30 to 30:70, can be 60:40 to 40:60, or can be 55:45 to 45:55. This weight ratio is the ratio of the weight of the first active substance used in the mixing in step (a) to the weight of the second active substance used in the mixing in step (c).
[0067] The total content of the first and second active substances in this slurry, relative to the solid components in this slurry, can be 95.0–99.9% by weight, 96.0–99.5% by weight, 97.0–99.2% by weight, 97.5–99.0% by weight, or 98.0–98.5% by weight.
[0068] The first and second active materials can each independently contain one or more lithium composite oxides selected from LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. Here, for example, in the composition formula "Li(NiCoMn)O2", the sum of the composition ratios in parentheses is 1 (Ni + Co + Mn = 1). As long as the sum of the composition ratios is 1, the composition ratio of each element (Ni, Co, Mn) is arbitrary.
[0069] The first active material and the second active material can each be independently a lithium composite oxide, for example, represented by the following formula (I).
[0070] Li 1.00+a1 Ni x1 Me 1.00-x1 O2 (I)
[0071] In formula (I),
[0072] a1 and x1 satisfy the relationships -0.30≤a1≤0.30 and 0.30≤x1≤1.00 respectively.
[0073] Me represents one or more elements selected from Co (cobalt), Mn (manganese), Al (aluminum), Zr (zirconium), B (boron), Mg (magnesium), Fe (iron), Cu (copper), Zn (zinc), Sn (tin), Na (sodium), K (potassium), Ba (barium), Sr (strontium), Ca (calcium), W (tungsten), Mo (molybdenum), Nb (niobium), Ti (titanium), Si (silicon), V (vanadium), Cr (chromium), and Ge (germanium).
[0074] a1 can be -0.30 to 0.30, -0.20 to 0.20, or -0.10 to 0.10. x1 can be 0.30 to 1.00, 0.40 to 0.95, 0.45 to 0.90, or 0.50 to 0.85. Me preferably contains Co and Mn.
[0075] The lithium composite oxide particles constituting the first active material and the second active material can each be independently represented by, for example, the lithium composite oxide represented by the following formula (II).
[0076] Li 1.00+a2 Nix2 Co y2 Mn 1.00-x2-y2 O2 (II)
[0077] In formula (II),
[0078] a², x², and y² satisfy the relationships -0.30 ≤ a² ≤ 0.30, 0.40 ≤ x² ≤ 0.95, and 0.00 ≤ y² ≤ 0.60, respectively, and x² + y² ≤ 1.00.
[0079] a² can be -0.30 to 0.30, -0.20 to 0.20, or -0.10 to 0.10. x² can be 0.45 to 0.90 or 0.50 to 0.85. y² can be greater than 0.00 and less than 0.45, and can be 0.05 to 0.40, 0.10 to 0.35, or 0.15 to 0.30.
[0080] The composition of the first and second active substances in this slurry may be the same or different from each other. The composition of the first and second active substances can be determined by ICP (inductively coupled plasma) emission spectroscopy (ICP-AES).
[0081] The first conductive material and the second conductive material can each independently be one or more selected from carbon black (CB) such as acetylene black (AB), graphite, and fibrous carbon. Examples of fibrous carbon include carbon nanotubes (CNTs). CNTs can be single-layer carbon nanotubes (SWCNTs) or multilayer carbon nanotubes such as double-layer carbon nanotubes (DWCNTs). When mixing the first conductive material and the second conductive material with other components, either the first conductive material or the second conductive material can be used directly, or a dispersion in which the first conductive material or the second conductive material is dispersed can be used. Examples of dispersion media include those described in the section on the first and second dispersion media described later. The preferred dispersion media is N-methyl-2-pyrrolidone (NMP). The first conductive material and the second conductive material contained in this slurry can be the same conductive material or different conductive materials.
[0082] In the manufacturing method of this slurry, the mixing ratio of the first conductive material to the second conductive material (first conductive material: second conductive material (weight ratio)) is 45:55 to 65:35, or it can be 47:53 to 63:37, or it can be 50:50 to 60:40. By using a mixing ratio within the above range, the contact area between the first active material and the first conductive material, and the contact area between the second active material and the second conductive material, can be ensured, as well as the conductive path around the periphery of each of the first and second active materials. Therefore, in a secondary battery having a positive electrode plate obtained using this slurry, the capacity retention rate can be improved.
[0083] The total content of the first conductive material and the second conductive material used in the manufacturing method of this slurry, relative to the solid content in the slurry, can be 0.05 to 2.00% by weight, 0.10 to 1.50% by weight, 0.20 to 1.05% by weight, 0.30 to 1.00% by weight, or 0.50 to 0.95% by weight. If the above total content increases, the electronic conductivity of the positive electrode plate as a whole will be excessively increased, resulting in increased heat generation during short circuit of the secondary battery. Therefore, the upper limit of the above total content is preferably 1.00% by weight or less.
[0084] The total weight of the first conductive material and the second conductive material relative to the total weight of the conductive material contained in the slurry is preferably 95 to 100% by weight, but can be 97 to 100% by weight, 99 to 100% by weight, or 100% by weight.
[0085] The first binder and the second binder may each be independently selected from one or more fluoropolymers such as polyvinylidene fluoride (PVdF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVdF-HFP), and polytetrafluoroethylene (PTFE); cellulose resins such as carboxymethyl cellulose (CMC), methyl cellulose, and hydroxypropyl cellulose; styrene-butadiene rubber (SBR); and acrylic resins such as polyacrylic acid (PAA). The first binder and the second binder are preferably fluoropolymers, and more preferably PVdF. The first binder and the second binder contained in this slurry may be the same binder or different binders.
[0086] In the manufacturing method of this slurry, the mixing ratio of the first binder to the second binder (first binder: second binder (by weight)) is 30:70 to 80:20, or it can be 35:65 to 75:25, 40:60 to 70:30, 45:55 to 65:35, or 50:50 to 60:40. By using a mixing ratio within the above range, it is easy to ensure the contact area between the first active material and the first conductive material, as well as the contact area between the second active material and the second conductive material. Preferably, the range of the mixing ratio of the first binder and the second binder is the same as the range of the mixing ratio of the first conductive material and the second conductive material.
[0087] Relative to the solid components in this slurry, the total content of the first binder and the second binder used in the manufacturing method of this slurry can be 0.05 to 3.00% by weight, 0.10 to 2.50% by weight, 0.20 to 2.00% by weight, 0.30 to 1.50% by weight, or 0.50 to 1.00% by weight. The total content of the first binder and the second binder can be within the range of ±10% by weight of the total content of the first conductive material and the second conductive material.
[0088] The first and second dispersion media, as well as the dispersion media that may be added in steps (b) and (d) to (f) (hereinafter also referred to as the "third dispersion media"), are also referred to as solvents. The first, second, and third dispersion media may each be independently selected from one or more of N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethylformamide (DMF), methyl ethyl ketone (MEK), and dimethyl sulfoxide (DMSO). The first, second, and third dispersion media are preferably NMP. The first, second, and third dispersion media contained in this slurry may be the same or different dispersion media.
[0089] In step (a), the first active substance, the first binder, and the first dispersion medium are mixed ( Figure 1 and Figure 2 In step (a), for example, the first compound can be obtained by adding a first dispersion medium to the mixture obtained by mixing the first active material and the first binder and then kneading. In step (a), the first binder is preferably added in a manner that is 30 to 80% by weight relative to the total weight of the first binder and the second binder contained in the positive electrode active material layer formed using this slurry. The amount of the first binder added in step (a) is preferably within the range of ±10 [% by weight] of the amount of the first conductive material added in step (b).
[0090] Process (b) can be performed after process (a). Figure 1and Figure 2 In step (b), a second compound is obtained by adding a first conductive material to the first compound obtained in step (a) and then mixing. In step (b), it is preferable to add a dispersion medium together with the first conductive material to the first compound and then mix. In step (b), the first conductive material is added in a manner that is 45 to 65% by weight relative to the total weight of the first and second conductive materials contained in the positive electrode active material layer formed using this slurry. The amount of the first conductive material added can be 47 to 63% by weight or 50 to 60% by weight. By using the amount of the first binder and the first conductive material added as described in steps (a) and (b), the first active material and the first conductive material can be properly bonded in step (b).
[0091] Step (c) involves mixing the second active material, the second binder, and the second dispersion medium. Figure 1 and Figure 2 In step (c), for example, a third compound can be obtained by adding a second dispersion medium to the mixture obtained by mixing the second active material and the second binder and then kneading. Step (c) can be carried out independently of steps (a) and (b), for example, it can be carried out in parallel with steps (a) and / or steps (b), or it can be carried out before or after steps (a) and / or steps (b). In step (c), the second binder is preferably added in a manner that is 20 to 70% by weight relative to the total weight of the first binder and the second binder contained in the above-mentioned positive electrode active material layer. The amount of the second binder added in step (c) is preferably within the range of ±10 [% by weight] of the amount of the second conductive material added in step (d) or step (e).
[0092] Process (d) can be performed after processes (b) and (c). Figure 1 In step (d), the second compound obtained in step (b), the third compound obtained in step (c), and the second conductive material are mixed. In step (d), it is preferable to add a dispersion medium to the second compound, the third compound, and the second conductive material for mixing. In step (d), the second conductive material is added in an amount of 35 to 55% by weight relative to the total weight of the first and second conductive materials contained in the aforementioned positive electrode active material layer. The amount of the second conductive material added can be 37 to 53% by weight, or 40 to 50% by weight. By using the amount of the second binder and the second conductive material added as described in steps (c) and (d), the second active material and the second conductive material are easily and appropriately bonded in step (d).
[0093] Process (e) can be performed after process (c). Figure 2In step (e), a fourth compound is obtained by adding the second conductive material to the third compound obtained in step (c) and then mixing. In step (e), it is preferable to add a dispersion medium together with the second conductive material to the third compound and then mix. The range of the amount of the second conductive material added in step (e) can be cited from the range described in step (d). By using the amounts of the second binder and the second conductive material described in steps (c) and (e), the second active material and the second conductive material can be properly bonded in step (e).
[0094] Process (f) can be performed after processes (b) and (e). Figure 2 In step (f), the second compound obtained in step (b) and the fourth compound obtained in step (e) are mixed together.
[0095] The mixing in steps (a) to (f) can be carried out using a mixing device. There are no restrictions on the use of known devices such as a rotary blade mixer, a planetary mixer, a packed mixer (FILMIX), a media mill, or a twin-shaft mixer. The mixing in steps (a) to (f) can be carried out simply to moderately mix the components, and the mixing load and mixing time can be adjusted according to the size and type of the mixing device.
[0096] The compound obtained in step (d) or step (f) can be used as this slurry. The method for manufacturing this slurry may further include a step of adding a dispersion medium or the like to the compound obtained in step (d) or step (f) for further mixing. The compound obtained through this step can also be used as this slurry.
[0097] (Positive electrode plate)
[0098] The positive electrode plate of this embodiment (hereinafter also referred to as "this positive electrode plate") can be used in a secondary battery. This positive electrode plate has a positive current collector and a positive active material layer (hereinafter also referred to as "active material layer"). The active material layer can be formed on one or both sides of the positive current collector.
[0099] The active material layer of this positive electrode plate includes a first active material (first positive electrode active material), a second active material (second positive electrode active material), a conductive material, and a binder. Both the first and second active materials are lithium composite oxide particles. The first active material is a secondary particle formed by the aggregation of more than 50 primary particles. The second active material is a secondary particle formed by the aggregation of a single particle or 2 to 10 primary particles.
[0100] In the cross section of the active material layer of this positive electrode plate, the contact ratio of the first active material to the conductive material (CCR1) and the contact ratio of the second active material to the conductive material (CCR2) satisfy the following relationship (1).
[0101] 0.43≤CCR2 / CCR1≤0.70 (1)
[0102] As described above, the positive electrode active material contained in the positive electrode plate expands and contracts due to the charging and discharging of the secondary battery. Since the first active material is a secondary particle formed by the aggregation of multiple primary particles, it is prone to cracking due to the expansion and contraction of the first active material. In the active material layer of this positive electrode plate, the proportion of conductive material in contact with the first active material and the proportion of conductive material in contact with the second active material are adjusted as shown in Equation (1). Therefore, conductive paths around the first active material and around the second active material can be ensured. Thus, it is believed that even if the first active material cracks due to the charging and discharging of the secondary battery, the conductive material can ensure the conductive path, and since the conductive material can also ensure the conductive path around the second active material, the capacity retention rate of the secondary battery having this positive electrode plate can be improved.
[0103] As described above, in this positive electrode plate, the conductive path of the active material layer is ensured by adjusting the distribution of the conductive material in the active material layer. If the content of the conductive material in the active material layer is significantly increased, the overall electronic conductivity of the positive electrode plate will be excessively increased, leading to an increase in heat generation during a short circuit in the secondary battery. By obtaining this positive electrode plate without significantly increasing the content of the conductive material, the excessive increase in the overall electronic conductivity of the positive electrode plate can be suppressed, thus also suppressing the heat generation during a short circuit in the secondary battery.
[0104] The ratio of the contact ratio (CCR1) to the contact ratio (CCR2) in the cross section of the active material layer (CCR2 / CCR1) can be 0.43–0.70, 0.43–0.69, 0.44–0.68, 0.45–0.65, 0.46–0.60, 0.47–0.58, or 0.48–0.55.
[0105] The contact ratio (CCR1) is preferably 0.50–0.65, but can be 0.52–0.64 or 0.53–0.63. The contact ratio (CCR2) is preferably 0.28–0.34, but can be 0.29–0.33 or 0.29–0.32.
[0106] The contact ratios (CCR1) and (CCR2) can be determined according to the following steps. First, a SEM image of the cross-section of the positive electrode active material obtained by scanning electron microscopy (SEM) is compared with the resistance distribution obtained by scanning extended resistance microscopy (SSRM) of the aforementioned cross-section to identify the regions of the first active material, the second active material, the conductive material, and the pores in the SEM image. The contact ratio of the first active material to the conductive material and the contact ratio of the second active material to the conductive material within the SEM image of each identified region are calculated. More specifically, the contact ratios (CCR1) and (CCR2) can be determined according to the steps described in the embodiments described later.
[0107] The contact ratios (CCR1) and (CCR2) can be adjusted according to the mixing order and mixing ratio of the first active material, the second active material, and the conductive material when obtaining the positive electrode slurry used to form the active material layer. For example, by forming the active material layer using the positive electrode slurry manufactured according to the steps described in the above-described method for manufacturing the positive electrode slurry, the contact ratios (CCR1) and (CCR2) can be adjusted to the above range, and can be adjusted in a manner that satisfies the relationship of the above formula (1).
[0108] The first and second active materials may have the particle morphology, average particle size, and composition described in the method for manufacturing the positive electrode slurry. The conductive material may be any conductive material described for the first and second conductive materials. The binder may be any binder described for the first and second binders.
[0109] The ratio of the first active substance to the second active substance in the active substance layer (first active substance: second active substance (weight ratio)) is preferably 70:30 to 30:70, can be 60:40 to 40:60, or can be 55:45 to 45:55.
[0110] The total content of the first active substance and the second active substance relative to the total weight of the active substance layer can be 95.0–99.9% by weight, 96.0–99.5% by weight, 97.0–99.2% by weight, 97.5–99.0% by weight, or 98.0–98.5% by weight.
[0111] The content ratio of the first active material and the second active material, the conductive material and the binder in the active material layer ((first positive electrode active material + second positive electrode active material): conductive material: binder (weight ratio)) is preferably 99.9~95.0:0.05~2.00:0.05~3.00, more preferably 99.9~98.0:0.05~1.00:0.05~1.00.
[0112] The content of conductive material relative to the total weight of the active material layer can be 0.05–2.00% by weight, 0.10–1.50% by weight, 0.20–1.05% by weight, 0.30–1.00% by weight, or 0.50–0.95% by weight.
[0113] The binder content relative to the total weight of the active material layer can be 0.05–3.00% by weight, 0.10–2.50% by weight, 0.20–2.00% by weight, 0.30–1.50% by weight, or 0.50–1.00% by weight.
[0114] The positive current collector can be a conductive sheet, such as a metal foil made of aluminum materials such as aluminum and aluminum alloys.
[0115] The active material layer can be formed by coating a positive electrode slurry containing a first active material, a second active material, a conductive material, a binder, and a dispersion medium onto a positive electrode current collector, followed by drying and compression. The thickness of the active material layer can be, for example, 10–200 μm or 20–180 μm. The positive electrode slurry coated onto the positive electrode current collector only needs to have a thickness within the above range and be compressed such that the porosity of the active material layer is, for example, 15–40% or 20–35%. The porosity of the active material layer can be determined, for example, by mercury intrusion porosimetry or by calculation based on the density of the active material layer and the true density of the solid components determined using a gas displacement method; the porosity in this specification can be determined using the latter method. As the dispersion medium, the dispersion media described for the first, second, and third dispersion media can be used. The positive electrode slurry can be the aforementioned slurry.
[0116] The active material layer can be formed directly on the positive current collector, or it can be formed on the positive current collector through other positive active material layers. Other positive active material layers can be formed on the surface of the active material layer opposite to the positive current collector.
[0117] (Non-aqueous electrolyte secondary battery)
[0118] The secondary battery has the aforementioned positive electrode plate. The secondary battery may include an electrode body containing the positive electrode plate and a non-aqueous electrolyte, and may have a battery casing that contains the electrode body and the non-aqueous electrolyte. The battery casing may include an outer body with an opening and a sealing plate that closes the opening. The outer body and sealing plate are preferably made of metal, and may be formed using aluminum, aluminum alloys, iron, or iron alloys. A resin sheet serving as an electrode support may be disposed between the electrode body and the outer body. Alternatively, the battery casing may be formed of a laminated film. The laminated film, for example, has a laminated structure consisting of a metal layer and a resin layer. By overlapping and fusing the edges of the laminated film, a pouch-shaped battery casing can be formed.
[0119] The electrode body may include the aforementioned positive electrode plate, negative electrode plate, and separator. In the electrode body, the positive active material layer of the positive electrode plate and the negative active material layer of the negative electrode plate are positioned opposite each other, separated by the separator. The electrode body may be a stacked type formed by layering the positive electrode plate, negative electrode plate, and separator, or a wound type obtained by winding a strip-shaped stack formed by layering strip-shaped positive electrode plates, strip-shaped negative electrode plates, and strip-shaped separators. The wound type electrode body may have a flat shape formed by pressing the stacked body after winding.
[0120] A negative electrode plate typically has a negative current collector and a negative active material layer formed on one or both sides of the negative current collector. The negative current collector is a metal foil made of copper materials such as copper and copper alloys. The negative active material layer contains the negative active material and may further contain conductive materials and binders. The negative active material layer is formed by coating a negative slurry, obtained by adding a dispersion medium (solvent) such as water to the materials forming the negative active material layer (such as the negative active material, binder, and conductive material), onto the negative current collector and then drying and compressing it.
[0121] The negative electrode active material can be one or more selected from carbon-based active materials such as graphite, and metal-based active materials such as Si, SiOx (x = 0.5 to 1.5), Si and C composites, and Sn. The binder can be one or more selected from the above-mentioned cellulose-based resins, PAA, and SBR. The conductive material can be the conductive material described for the first and second conductive materials.
[0122] The insulating component has a substrate, which may have a functional layer on at least one side of the substrate. The substrate may be a membrane or a porous sheet such as a nonwoven fabric, made of polyolefins such as polyethylene and polypropylene, polyester, cellulose, or polyamide resins. The substrate may be a single-layer structure or a multi-layer structure; in the case of a multi-layer structure, the materials of each layer may be the same or different. Examples of functional layers include an adhesive layer formed by an adhesive and a heat-resistant layer containing inorganic fillers and adhesives.
[0123] The non-aqueous electrolyte preferably contains an electrolyte in a non-aqueous solvent such as an organic solvent. The electrolyte can be one or more selected from LiPF6, LiBF4, and LiClO4. LiPF6 is preferred. The concentration of the electrolyte in the non-aqueous electrolyte is preferably 0.7–1.3 mol / L.
[0124] As a non-aqueous solvent, organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones can be used. For example, one or more of the following can be used as a non-aqueous solvent: ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethylene monofluorocarbonate (MFEC), ethylene difluorocarbonate (DFEC), methyl monofluorodifluoromethyl carbonate (F-DMC), and dimethyl trifluorocarbonate (TFDMC).
[0125] Non-aqueous electrolytes may contain gas generators such as biphenyl (BP) and cyclohexylbenzene (CHB); film-forming agents such as oxalate coordination compounds containing boron and / or phosphorus atoms and vinylene carbonate (VC); dispersants; thickeners and other additives.
[0126] Example
[0127] The present disclosure will be described in more detail below with examples and comparative examples.
[0128] [Preparation of materials]
[0129] (First active material (first positive electrode active material))
[0130] Prepare secondary particles, namely lithium composite oxide particles, formed by the aggregation of more than 50 primary particles, as the first active material. The lithium composite oxide particles are within the composition range shown in the above formula (II).
[0131] (Second active material (Second positive electrode active material))
[0132] Prepare lithium composite oxide particles, which are secondary particles formed by the aggregation of single particles or 2 to 10 primary particles, as the second active material. The lithium composite oxide particles are within the composition range shown in the above formula (II).
[0133] (First conductive material and second conductive material)
[0134] Carbon nanotubes (CNTs) are prepared, and a first conductive material dispersion and a second conductive material dispersion in N-methyl-2-pyrrolidone (NMP) are prepared as the first conductive material and the second conductive material, respectively.
[0135] (First adhesive and second adhesive)
[0136] Prepare polyvinylidene fluoride (PVdF) as the first and second adhesives.
[0137] (First dispersion medium and second dispersion medium)
[0138] N-methyl-2-pyrrolidone (NMP) was prepared as the first and second dispersion media.
[0139] [Comparative Example 1 and Reference Example 1]
[0140] (Preparation of positive electrode slurry)
[0141] The first active material, the second active material, PVdF, and NMP were mixed to obtain a compound (c1). A CNT dispersion, which disperses CNTs in NMP, was added to the compound (c1) and the mixture was further mixed to obtain a positive electrode slurry. During the manufacture of the positive electrode slurry, the materials were mixed in the mixing ratios shown in Table 1. The conductive material content in Table 1 indicates the content of conductive material contained in the conductive material dispersion.
[0142] (Making the positive electrode plate)
[0143] The positive electrode slurry obtained above is coated onto the positive electrode current collector, which serves as an Al foil, and then dried and compressed to form a positive electrode active material layer. The material is then cut into a specified size to obtain a positive electrode plate.
[0144] [Comparative Examples 2 and 3, Examples 1 and 2]
[0145] (Preparation of positive electrode slurry)
[0146] A first compound is obtained by mixing the first active material, the first binder, and the first dispersion medium (step (a)). A second compound is obtained by mixing the first compound and the first conductive material dispersion (step (b)). A third compound is obtained by mixing the second active material, the second binder, and the second dispersion medium (step (c)). A positive electrode slurry is obtained by mixing the second compound, the third compound, and the second conductive material dispersion (step (d)). In manufacturing the positive electrode slurry, the materials are mixed in the manner shown in Table 1. The content of conductive material in Table 1 represents the total content of the first conductive material contained in the first conductive material dispersion and the second conductive material contained in the second conductive material dispersion.
[0147] (Making the positive electrode plate)
[0148] Using the positive electrode slurry obtained above, the positive electrode plate was obtained in accordance with the steps described in Comparative Example 1, except that.
[0149] [Comparative Examples 4 and 5, Examples 3 and 4]
[0150] (Preparation of positive electrode slurry)
[0151] A first compound is obtained by mixing the first active material, the first binder, and the first dispersion medium (step (a)). A second compound is obtained by mixing the first compound and the first conductive material dispersion (step (b)). A third compound is obtained by mixing the second active material, the second binder, and the second dispersion medium (step (c)). A fourth compound is obtained by mixing the third compound and the second conductive material dispersion (step (e)). The second and fourth compounds are then mixed (step (f)) to obtain a positive electrode slurry. In manufacturing the positive electrode slurry, the materials are mixed in the mixing ratios shown in Table 2. The conductive material content in Table 2 represents the total content of the first conductive material contained in the first conductive material dispersion and the second conductive material contained in the second conductive material dispersion.
[0152] (Making the positive electrode plate)
[0153] Using the positive electrode slurry obtained above, the positive electrode plate was obtained in accordance with the steps described in Comparative Example 1, except that.
[0154] [Determination of contact ratio (CCR1) and contact ratio (CCR2)]
[0155] The obtained positive electrode plate (cut to an appropriate size as needed) is embedded in resin. A cross-section of the resin-embedded positive electrode plate is formed using section polishing (CP). SEM images of the cross-section are obtained using scanning electron microscopy (SEM), and the extended resistance of the cross-section is measured using scanning extended resistance microscopy (SSRM). The SEM images are compared with the resistance distribution obtained from the extended resistance measurement to identify the regions of the first active material, second active material, conductive material, and pores in the SEM images. For each region of the first active material in the identified SEM images, the ratio of the total length of the contact portion between the first active material and the conductive material to the outer perimeter length of the first active material (total length of contact portion / total length of outer perimeter) is calculated, and the average value is taken as the contact ratio (CCR1). Similarly, for each region of the second active material in the identified SEM images, the ratio of the total length of the contact portion between the second active material and the conductive material to the outer perimeter length of the second active material (total length of contact portion / total length of outer perimeter) is calculated, and the average value is taken as the contact ratio (CCR2). The results are shown in Tables 1 and 2.
[0156] [Calculation of capacity retention of the test battery cell (non-aqueous electrolyte secondary battery)]
[0157] (Making the negative electrode)
[0158] Graphite as the negative electrode active material, carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) as binders, and water as the dispersion medium are prepared. A negative electrode slurry is obtained by mixing 98 parts by weight of graphite, 1 part by weight of CMC, 1 part by weight of SBR, and a specified amount of water. The negative electrode slurry is coated onto a Cu foil negative electrode current collector, dried, and compressed to form a negative electrode active material layer. The layer is then cut to a specified size to obtain a negative electrode plate.
[0159] (Fabrication of the experimental battery cell)
[0160] A tab terminal is attached to the positive electrode plate obtained above, and a tab terminal is attached to the negative electrode plate obtained above. A porous polyolefin sheet is prepared as a separator. The separator is sandwiched between the positive electrode active material layer and the negative electrode active material layer, and the positive electrode plate with the tab terminal attached and the negative electrode plate with the tab terminal attached are stacked to obtain the electrode body. The electrode body is inserted into a laminated film bag with aluminum and resin layers, electrolyte is injected, and the bag is sealed to obtain the test battery cell.
[0161] (Calculation of capacity retention rate)
[0162] The initial charge and discharge of the test battery cell was conducted at a temperature of 25°C. Then, the test battery cell was charged at a constant current of 0.1C until the positive electrode potential reached 4.2V (vs. Li). + Next, the test battery cell is charged at a constant voltage until the current reaches 0.05C. This completes the charging process. After a 10-minute pause, the test battery cell is discharged at a constant current of 1.0C until the positive electrode potential reaches 3.0V (vs. Li). + Until / Li), the discharge capacity at this point is measured and taken as the initial discharge capacity.
[0163] Next, at a temperature of 25°C, the test battery cells were charged to 4.2V using a constant current of 0.5C, and then discharged to 3.0V using a constant current of 0.5C. This charge-discharge cycle was considered one cycle, and the cycle was repeated 200 times. The discharge capacity was then measured following the above steps and taken as the discharge capacity after the cycle test. The capacity retention rate was calculated using the following formula. The results are shown in Tables 1 and 2.
[0164] Capacity retention rate [%] = (Discharge capacity after cycle test / Initial discharge capacity) × 100
[0165] [Determination of Acupuncture Heat]
[0166] The test battery cell obtained above was fully charged. The fully charged test battery cell was connected in parallel with a constant voltage power supply with a maximum current of 200A, and a nail was driven into the test battery cell to simulate the current flowing through a large battery cell. The cumulative heat generation [J] from the moment of detection to the moment when the voltage drop due to the short circuit caused by the nail penetration was displayed for 2 seconds was calculated, and the heat generation when the heat generation of the test battery cell of Comparative Example 1 was set to 100 was also calculated. The results are shown in Tables 1 and 2.
[0167] [Table 1]
[0168]
[0169] [Table 2]
[0170]
[0171] While embodiments of the invention have been described, it should be understood that the embodiments disclosed herein are illustrative in all respects and not restrictive. The scope of the invention is indicated by the scope of the claims and is intended to include all modifications within the meaning and scope equivalent to the scope of the claims.
Claims
1. A method for manufacturing a positive electrode slurry, which is a method for manufacturing a positive electrode slurry for non-aqueous electrolyte secondary batteries. The positive electrode slurry comprises a first positive electrode active material as lithium composite oxide particles and a second positive electrode active material as lithium composite oxide particles. The first positive electrode active material is a secondary particle formed by the aggregation of more than 50 primary particles. The second positive electrode active material is a single particle or a secondary particle formed by the aggregation of 2 to 10 primary particles. The manufacturing method includes: Step a, which involves mixing the first positive electrode active material, the first binder, and the first dispersion medium to obtain the first compound, Step b, which involves mixing the first compound and the first conductive material to obtain the second compound, and Step c, which involves mixing the second positive electrode active material, the second binder, and the second dispersion medium to obtain the third compound, and The following [i] or [ii]: [i] Step d, which involves mixing the second compound, the third compound, and the second conductive material. [ii] Step e, which involves mixing the third compound and the second conductive material to obtain the fourth compound, and step f, which involves mixing the second compound and the fourth compound; In the manufacturing method, the first conductive material and the second conductive material are mixed in a weight ratio of 45:55 to 65:
35.
2. The method for manufacturing the positive electrode slurry according to claim 1, wherein, In the manufacturing method, the first positive electrode active material and the second positive electrode active material are mixed in a weight ratio of first positive electrode active material: second positive electrode active material = 70:30 to 30:
70.
3. The method for manufacturing the positive electrode slurry according to claim 1 or 2, wherein, The average particle size D50 of the first positive electrode active material is greater than the average particle size D50 of the second positive electrode active material.
4. The method for manufacturing the positive electrode slurry according to claim 1 or 2, wherein, The first positive electrode active material and the second positive electrode active material are each independently a lithium composite oxide represented by the following formula (I). Li 1.00+a1 Ni x1 Along with 1.00-x1 O2 (I) In formula (I), a1 and x1 satisfy the relationships -0.30≤a1≤0.30 and 0.30≤x1≤1.00 respectively. Me represents one or more of the following: Co, Mn, Al, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Nb, Ti, Si, V, Cr, and Ge.
5. A positive electrode plate having a positive current collector and a positive active material layer, The positive electrode active material layer comprises a first positive electrode active material, a second positive electrode active material, a conductive material, and a binder. Both the first positive electrode active material and the second positive electrode active material are lithium composite oxide particles. The first positive electrode active material is a secondary particle formed by the aggregation of more than 50 primary particles. The second positive electrode active material is a single particle or a secondary particle formed by the aggregation of 2 to 10 primary particles. In the cross-section of the positive electrode active material layer, the contact ratio CCR1 between the first positive electrode active material and the conductive material and the contact ratio CCR2 between the second positive electrode active material and the conductive material satisfy the following relationship (1). 0.43≤CCR2 / CCR1≤0.70 (1)。 6. The positive electrode plate according to claim 5, wherein, The contact ratio CCR1 is 0.49 to 0.
65.
7. The positive electrode plate according to claim 5 or 6, wherein, The contact ratio CCR2 is 0.28 to 0.
35.
8. The positive electrode plate according to claim 5 or 6, wherein, The positive electrode active material layer contains the first positive electrode active material and the second positive electrode active material in a weight ratio of 70:30 to 30:
70.
9. The positive electrode plate according to claim 5 or 6, wherein, The average particle size D50 of the first positive electrode active material is greater than the average particle size D50 of the second positive electrode active material.
10. The positive electrode plate according to claim 5 or 6, wherein, The positive electrode active material layer comprises the first positive electrode active material, the second positive electrode active material, the conductive material, and the binder in a weight ratio of (first positive electrode active material + second positive electrode active material): conductive material: binder = 99.9~95.0: 0.05~2.00: 0.05~3.
00.
11. The positive electrode plate according to claim 5 or 6, wherein, The first positive electrode active material and the second positive electrode active material are each independently a lithium composite oxide represented by the following formula (I). Li 1.00+a1 Ni x1 Along with 1.00-x1 O2 (I) In formula (I), a1 and x1 satisfy the relationships -0.30≤a1≤0.30 and 0.30≤x1≤1.00 respectively. Me represents one or more of the following: Co, Mn, Al, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Nb, Ti, Si, V, Cr, and Ge.
Citation Information
Patent Citations
Positive electrode and nonaqueous electrolyte secondary battery
JP2022143761A