A lithium titanate phosphate-based electrode material, a preparation method thereof, and a battery

By forming a carbon coating layer in situ on the outer periphery of lithium titanium phosphate composite particles and constructing a multi-level porous structure, the problems of loose bonding and simple pore structure of lithium titanium phosphate materials are solved, improving the electronic conductivity and cycle stability of the electrode material, making it suitable for fast charging of lithium-ion batteries.

CN123143389APending Publication Date: 2026-11-20TAIZHOU SHANNENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611387451.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing spray-drying methods for preparing lithium titanium phosphate materials suffer from problems such as poor bonding between the carbon coating layer and active particles, a simple internal pore structure, and the tendency of traditional organic carbon sources to adhere to the walls and form large particle agglomerates, leading to uneven composition. These issues affect the rate performance and cycle stability of the electrode materials.

Method used

A carbon-containing complexing agent is used to generate coordination adsorption with Ti⁴⁺, forming a carbon coating layer in situ. A multi-level porous structure is constructed through coordination complexation reaction and mechanical grinding to ensure that the carbon coating layer is tightly bonded to the lithium titanium phosphate composite particles, inhibiting agglomeration and grain growth, and improving electronic conductivity and structural stability.

Benefits of technology

This method achieves low-resistance charge transfer contact between the carbon coating layer and lithium titanium phosphate composite particles, improving the electron transport performance and cycle stability of the electrode material, making it suitable for the fast charging field of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143389A_ABST
    Figure CN123143389A_ABST
Patent Text Reader

Abstract

The application discloses a lithium titanium phosphate-based electrode material and a preparation method and a battery thereof. The preparation method comprises the following steps: S100, dispersing a titanium source and a first complexing agent in a liquid medium to obtain a titanium complex compound solution; S200, adding a lithium source, a phosphorus source, a second complexing agent and a carbon-containing complexing agent into the titanium complex compound solution, and generating complex adsorption through the carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent and Ti 4+ to generate a first precursor mixed slurry; S300, grinding the first precursor mixed slurry to obtain a second precursor mixed slurry, and performing drying treatment on the second precursor mixed slurry to obtain a precursor powder; and S400, performing sintering treatment on the precursor powder, and generating lithium titanium phosphate composite particles through solid-phase reaction of titanium elements, lithium elements and phosphorus elements in the precursor powder during the sintering treatment, and simultaneously forming a carbon coating layer through in-situ carbonization of the carbon-containing complexing agent to obtain the lithium titanium phosphate-based electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrode material technology, and in particular to a lithium titanium phosphate-based electrode material, its preparation method, and a battery. Background Technology

[0002] Lithium-ion batteries, as a key carrier of new energy storage technology, are widely used in new energy vehicles, consumer electronics, and large-scale energy storage. With the market's increasing demands for lithium-ion battery performance, especially the increasingly stringent requirements for driving range and safety, lithium-ion battery technology continues to iterate and upgrade towards higher energy density and higher safety.

[0003] Lithium titanium phosphate (LiTi2(PO4)3) possesses a NASICON structure. The three-dimensional ion channels of LiTi2(PO4)3 endow it with high lithium-ion conductivity. Simultaneously, it exhibits a flat electrochemical reaction platform and good structural stability, making it a highly promising cathode material for lithium-ion batteries. However, LiTi2(PO4)3 itself has a relatively low electronic conductivity, approximately 10⁻⁶. - 8 The S / cm ratio severely limits its rate performance, making it difficult to meet the needs of applications such as fast charging of electric vehicles.

[0004] In existing technologies, spray drying is widely used to prepare powder materials with good flowability and uniform particle size distribution because it can achieve rapid drying of precursors and spherical granulation. However, lithium titanium phosphate materials prepared by conventional spray drying have the following problems: First, the bonding between the carbon coating layer and the active particles is not tight enough, and carbon layer peeling or uneven distribution is prone to occur during sintering; second, the internal pore structure of the material is simple, making it difficult to simultaneously achieve high tap density and good electrolyte wettability; third, traditional organic carbon sources are prone to wall adhesion during spray drying, reducing yield. In addition, if large particle agglomerates are present in the precursor slurry before spray drying, it will lead to uneven composition and morphological damage in the final product, seriously affecting the consistency and electrochemical performance of the final product. Summary of the Invention

[0005] One objective of this application is to provide a lithium titanium phosphate-based electrode material and its preparation method, as well as a battery, which facilitates the uniform dispersion of titanium ions, in-situ anchoring of carbon sources, and controllable construction of hierarchical porous structures, thereby improving the rate performance and cycle stability of the electrode material.

[0006] To achieve the above objectives, this application provides a lithium titanium phosphate-based electrode material, comprising: lithium titanium phosphate composite particles, wherein the chemical formula of the lithium titanium phosphate composite particles is LiTi2(PO4)3; and a carbon coating layer, wherein the carbon coating layer coats the outer periphery of the lithium titanium phosphate composite particles, the carbon coating layer being formed by in-situ carbonization of a carbon-containing complexing agent, wherein the molecular chain of the carbon-containing complexing agent contains at least one functional group selected from carbonyl, carboxyl, and hydroxyl groups, and the carbon-containing complexing agent is suitable for reacting with Ti. 4+ Coordination adsorption occurs.

[0007] In some embodiments, the lithium titanium phosphate-based electrode material satisfies at least one of the following conditions: (a) the mass fraction of carbon in the lithium titanium phosphate-based electrode material is 0.5wt%~3wt%; (b) the particle size of the lithium titanium phosphate composite particles is 100nm~500nm; (c) the specific surface area of ​​the lithium titanium phosphate-based electrode material is 8m². 2 / g~20m 2 / g, the particle size of the lithium titanium phosphate-based electrode material is 3μm~10μm; (d) the carbon-containing complexing agent is selected from at least one of polyvinylpyrrolidone, polyacrylic acid and polyvinyl alcohol.

[0008] In some embodiments, the lithium titanium phosphate composite particles have a macroporous structure, and the carbon coating layer has both a macroporous structure and a mesoporous structure. The pore size of the macroporous structure is greater than 50 nm, and the pore size of the mesoporous structure is 2 nm to 50 nm.

[0009] To achieve the above objectives, this application also provides a method for preparing a lithium titanium phosphate-based electrode material, comprising the steps of: S100, dispersing a titanium source and a first ligand in a liquid medium, wherein the first ligand and Ti 4+ A coordination complexation reaction is generated to prepare a titanium coordination complex solution; S200, a lithium source, a phosphorus source, a second ligand, and a carbon-containing complexing agent are added to the titanium coordination complex solution. The carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent react with the Ti in the titanium coordination complex solution. 4+ Coordination adsorption is generated to obtain a first precursor mixed slurry; S300, the first precursor mixed slurry is ground to obtain a second precursor mixed slurry, and the second precursor mixed slurry is dried to obtain precursor powder; S400, the precursor powder is sintered, and during the sintering process, the titanium, lithium and phosphorus elements in the precursor powder undergo a solid-phase reaction to generate lithium titanium phosphate composite particles, and at the same time, the carbon-containing complexing agent is carbonized in situ to form a carbon coating layer covering the outer periphery of the lithium titanium phosphate composite particles, thereby obtaining a lithium titanium phosphate based electrode material.

[0010] In some embodiments, the mass of the carbon-containing complexing agent is 5% to 15% of the theoretical mass of the lithium titanium phosphate composite particles, based on the theoretical mass of the obtained lithium titanium phosphate composite particles; the carbon-containing complexing agent is selected from at least one of polyvinylpyrrolidone, polyacrylic acid and polyvinyl alcohol.

[0011] In some embodiments, step S200 is as follows: after adding a lithium source, a phosphorus source, and a carbon-containing complexing agent to the titanium coordination complex solution, a second complexing agent is added until the pH of the slurry is adjusted to 3-5. The carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent react with the Ti in the titanium coordination complex solution. 4+ Coordination adsorption is generated to obtain a first precursor mixed slurry; the number of moles of titanium in the titanium source is n1, the number of moles of lithium in the lithium source is n2, and the number of moles of phosphorus in the phosphorus source is n3, and the ratio between n1, n2, and n3 is (1.5~2.5):(1~1.05):(2.5~3.5).

[0012] In some embodiments, step S400 is as follows: In a protective gas atmosphere, the precursor powder is subjected to a first sintering treatment to obtain a sintering intermediate; the sintering intermediate is subjected to a second sintering treatment to obtain a lithium titanium phosphate-based electrode material. The titanium, lithium, and phosphorus elements in the precursor powder undergo a solid-state reaction to generate lithium titanium phosphate composite particles. Simultaneously, the carbon-containing complexing agent is carbonized in situ to form a carbon coating layer around the lithium titanium phosphate composite particles. The temperature of the first sintering treatment is 300℃~400℃, the time of the first sintering treatment is 1h~3h, and the heating rate of the first sintering treatment is 2℃ / min~5℃ / min. The temperature of the second sintering treatment is 600℃~750℃, the time of the second sintering treatment is 4h~8h, and the heating rate of the second sintering treatment is 3℃ / min~6℃ / min.

[0013] In some embodiments, the first ligand is at least one of acetylacetone, citric acid, tartaric acid, and ethylenediaminetetraacetic acid, and the molar number of the first ligand is 0.5 to 2.0 times the molar number of the titanium source; the second ligand is at least one of ammonia, ethylenediamine, or triethanolamine, and the concentration of the second ligand is 0.1 mol / L to 5 mol / L; the liquid medium is a mixed solution of an alcohol and water, wherein the alcohol is anhydrous ethanol and / or isopropanol, and the volume ratio of the alcohol to water is (1 to 3):1.

[0014] To achieve the above objectives, this application also provides an electrode sheet, comprising the lithium titanium phosphate-based electrode material as described above, or the lithium titanium phosphate-based electrode material prepared by the aforementioned preparation method.

[0015] To achieve the above objectives, this application also provides a battery including at least one electrode as described above.

[0016] Compared with the prior art, the beneficial effects of this application are as follows: (1) This application selects materials that are compatible with Ti 4+ The carbon-containing complexing agent that generates coordination adsorption forms a carbon coating layer in situ on the outer periphery of the lithium titanium phosphate composite particles. Because the molecular chain of the carbon-containing complexing agent contains coordinating functional groups such as carbonyl, carboxyl, or hydroxyl groups, these groups can interact with Ti... 4+ This generates coordination interactions, thereby uniformly and firmly anchoring the carbon-containing complexing agent to Ti at the molecular scale. 4+ Surrounding the particles, a carbon-containing complexing agent forms an in-situ carbon coating layer after high-temperature carbonization. This carbon coating layer and the lithium titanium phosphate composite particles form a tight contact interface connected by chemical bonds. This tight interface not only improves the continuity and integrity of the carbon coating layer on the surface of the lithium titanium phosphate composite particles, preventing peeling and segregation during sintering or charge-discharge processes, but also enables low-resistance charge transfer contact between the carbon coating layer and the lithium titanium phosphate composite particles, thereby reducing the interfacial contact resistance between particles. Notably, the carbon coating layer formed by in-situ carbonization with the carbon-containing complexing agent is itself a conductive network. Its tight bonding with the substrate allows electrons to be efficiently transported from the carbon coating layer to the interior of each lithium titanium phosphate composite particle, thus compensating for the inherent low electronic conductivity of lithium titanium phosphate. Furthermore, due to the coordination and anchoring effect of the carbon-containing complexing agent, the in-situ carbon coating layer is uniformly dense, which helps suppress the agglomeration and grain growth of active particles during electrochemical cycling, further improving structural stability.

[0017] (2) This application uses a first coordinating agent to interact with Ti 4+ The resulting coordination complexation reaction inhibits local precipitation or agglomeration of the titanium source in the liquid medium due to excessively rapid hydrolysis, allowing titanium to be uniformly dispersed in the liquid medium in a stable complex form, which is beneficial to improving the uniformity and consistency of subsequent products. Furthermore, the carbonyl and / or carboxyl functional groups on the carbon-containing complexing agent molecular chain can coordinate with and complex Ti in the titanium complex solution. 4+Secondary coordination adsorption occurs, and this dual coordination design ensures that the spatial distribution of carbon and titanium elements highly overlaps. After drying, a precursor powder uniformly coated with carbon is formed. During sintering, in-situ carbonization generates a continuous carbon coating layer tightly bonded to the lithium titanium phosphate composite particles, reducing the occurrence of loose, peeling, or locally missing carbon coating layers. Simultaneously, mechanical grinding of the first precursor mixture slurry achieves particle size control, which helps eliminate large particle agglomerates in the first precursor mixture slurry, ensuring a uniform particle size distribution and good consistency in the precursor powder obtained after subsequent drying. Therefore, the solid-phase reaction can proceed simultaneously in each micro-region during sintering, which is beneficial for obtaining lithium titanium phosphate composite particles with good crystallinity and morphological uniformity. Attached Figure Description

[0018] Figure 1 This is a scanning electron microscope image of the lithium titanium phosphate-based electrode material prepared in Example 1 of this application. Detailed Implementation

[0019] The present application will be further described below with reference to specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0020] As used herein, the terms “prepared from” and “comprising” are synonymous. The terms “comprising,” “including,” “having,” “containing,” or any other variation thereof, as used herein, are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements and may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0021] When a quantity, concentration, or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range is disclosed as “1 to 5”, the described range should be interpreted as including ranges “1 to 4”, “1 to 3”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range includes its endpoints and all integers and fractions within that range.

[0022] Approximate terms used in the specification and claims to modify quantities indicate that the invention is not limited to that specific quantity, but also includes acceptable modifications close to that quantity that do not alter the relevant essential function. Correspondingly, the use of "about," "approximately," etc., to modify a numerical value means that the invention is not limited to that precise value. In some instances, approximate terms may correspond to the precision of the instrument used to measure the value. In this application's specification and claims, scope definitions can be combined and / or interchanged, unless otherwise stated, these scopes include all subscopes contained therein.

[0023] This application provides a lithium titanium phosphate-based electrode material, comprising: lithium titanium phosphate composite particles, the chemical formula of which is LiTi2(PO4)3; and a carbon coating layer, which coats the outer periphery of the lithium titanium phosphate composite particles. The carbon coating layer is formed by in-situ carbonization of a carbon-containing complexing agent. The molecular chain of the carbon-containing complexing agent contains at least one functional group selected from carbonyl, carboxyl, and hydroxyl groups, and the carbon-containing complexing agent is suitable for reacting with Ti. 4+ Coordination adsorption occurs.

[0024] This application selects materials compatible with Ti. 4+ The carbon-containing complexing agent that generates coordination adsorption forms a carbon coating layer in situ on the outer periphery of the lithium titanium phosphate composite particles. Because the molecular chain of the carbon-containing complexing agent contains coordinating functional groups such as carbonyl, carboxyl, or hydroxyl groups, these groups can interact with Ti... 4+ This generates coordination interactions, thereby uniformly and firmly anchoring the carbon-containing complexing agent to Ti at the molecular scale. 4+ Surrounding the particles, a carbon-containing complexing agent forms an in-situ carbon coating layer after high-temperature carbonization. This carbon coating layer and the lithium titanium phosphate composite particles form a tight contact interface connected by chemical bonds. This tight interface not only improves the continuity and integrity of the carbon coating layer on the surface of the lithium titanium phosphate composite particles, preventing peeling and segregation during sintering or charge-discharge processes, but also enables low-resistance charge transfer contact between the carbon coating layer and the lithium titanium phosphate composite particles, thereby reducing the interfacial contact resistance between particles. Notably, the carbon coating layer formed by in-situ carbonization with the carbon-containing complexing agent is itself a conductive network. Its tight bonding with the substrate allows electrons to be efficiently transported from the carbon coating layer to the interior of each lithium titanium phosphate composite particle, thus compensating for the inherent low electronic conductivity of lithium titanium phosphate. Furthermore, due to the coordination and anchoring effect of the carbon-containing complexing agent, the in-situ carbon coating layer is uniformly dense, which helps suppress the agglomeration and grain growth of active particles during electrochemical cycling, further improving structural stability.

[0025] In some embodiments, the mass fraction of carbon in the lithium titanium phosphate-based electrode material is 0.5wt% to 3wt%. By selecting an appropriate mass fraction of carbon, it is beneficial to obtain a lithium titanium phosphate-based electrode material with good electron transport performance, good stability in use, and long service life.

[0026] The mass fraction of carbon in lithium titanium phosphate-based electrode materials can be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, or 3wt%.

[0027] In some embodiments, the particle size of the lithium titanium phosphate composite particles is 100 nm to 500 nm, and the thickness of the carbon coating layer on one side is 2 nm to 10 nm. By selecting lithium titanium phosphate composite particles and carbon coating layers of suitable size, it is beneficial to obtain lithium titanium phosphate-based electrode materials with good electron transport performance, good stability in use, and long service life.

[0028] In some embodiments, the specific surface area of ​​the lithium titanium phosphate-based electrode material is 8 m². 2 / g~20m 2 / g, the particle size of lithium titanium phosphate-based electrode materials ranges from 3μm to 10μm. By controlling the specific surface area and particle size within a suitable range, it is beneficial to obtain lithium titanium phosphate-based electrode materials with good electron transport performance, good stability in use, and long service life.

[0029] In some embodiments, the carbon-containing complexing agent is selected from at least one of polyvinylpyrrolidone, polyacrylic acid, and polyvinyl alcohol. Preferably, the carbon-containing complexing agent is polyvinylpyrrolidone and / or polyacrylic acid, and more preferably, polyvinylpyrrolidone with the grade K30 is used. It should be understood that this application uses polymers such as polyvinylpyrrolidone and polyacrylic acid, which possess both coordination and carbonization capabilities, as carbon sources. The carbonyl and carboxyl functional groups on their molecular chains can interact with Ti. 4+ Coordination occurs, causing carbon source molecules to be tightly anchored around titanium atoms. After sintering, a continuous, uniform, and tightly bonded carbon conductive network is formed, which is beneficial to improving the electronic conductivity of the material.

[0030] This application also provides a method for preparing a lithium titanium phosphate-based electrode material, including the following steps: S100, dispersing a titanium source and a first ligand in a liquid medium, wherein the first ligand and Ti... 4+ A coordination complexation reaction is generated to prepare a titanium coordination complex solution; S200, a lithium source, a phosphorus source, a second ligand, and a carbon-containing complexing agent are added to the titanium coordination complex solution. The carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent react with the Ti in the titanium coordination complex solution. 4+Coordination adsorption is generated to obtain a first precursor mixed slurry; S300, the first precursor mixed slurry is ground to obtain a second precursor mixed slurry, and the second precursor mixed slurry is dried to obtain precursor powder; S400, the precursor powder is sintered. During the sintering process, the titanium, lithium and phosphorus elements in the precursor powder react in a solid phase to generate lithium titanium phosphate composite particles. At the same time, a carbon-containing complexing agent is carbonized in situ to form a carbon coating layer on the outer periphery of the lithium titanium phosphate composite particles, thus obtaining a lithium titanium phosphate-based electrode material.

[0031] This application utilizes a first coordinating agent and Ti 4+ The resulting coordination complexation reaction inhibits local precipitation or agglomeration of the titanium source in the liquid medium due to excessively rapid hydrolysis, allowing titanium to be uniformly dispersed in the liquid medium in a stable complex form, which is beneficial to improving the uniformity and consistency of subsequent products. Furthermore, the carbonyl and / or carboxyl functional groups on the carbon-containing complexing agent molecular chain can coordinate with and complex Ti in the titanium complex solution. 4+ Secondary coordination adsorption occurs, and this dual coordination design ensures that the spatial distribution of carbon and titanium elements highly overlaps. After drying, a precursor powder uniformly coated with carbon is formed. During sintering, in-situ carbonization generates a continuous carbon coating layer tightly bonded to the lithium titanium phosphate composite particles, reducing the occurrence of loose, peeling, or locally missing carbon coating layers. Simultaneously, mechanical grinding of the first precursor mixture slurry achieves particle size control, which helps eliminate large particle agglomerates in the first precursor mixture slurry, ensuring a uniform particle size distribution and good consistency in the precursor powder obtained after subsequent drying. Therefore, the solid-phase reaction can proceed simultaneously in each micro-region during sintering, which is beneficial for obtaining lithium titanium phosphate-based electrode materials with good crystallinity and morphological uniformity.

[0032] It should be understood that the preparation method provided in this application is simple to operate. By combining coordination-assisted grinding with a spray drying strategy, a tightly bound carbon conductive network and a hierarchical porous structure can be constructed in lithium titanium phosphate, thereby improving the rate performance and cycle stability of the electrode material. Therefore, the lithium titanium phosphate-based electrode material provided in this application has great application potential in the field of fast charging of lithium-ion batteries.

[0033] In some embodiments, the lithium titanium phosphate composite particles have a macroporous structure, and the carbon coating layer has both macroporous and mesoporous structures. The pore size of the macroporous structure is greater than 50 nm, and the pore size of the mesoporous structure is 2 nm to 50 nm. The specific surface area of ​​the lithium titanium phosphate composite particles is 5 m². 2 / g~15m 2 / g; In the carbon coating, the pore volume of macroporous structures accounts for 30%~50% of the total pore volume, and the pore volume of mesoporous structures accounts for 40%~60% of the total pore volume.

[0034] It can be understood that the first and second ligands, along with the carbon-containing complexing agent, generate gas escape during sintering, thereby forming a mesoporous-macroporous hierarchical pore structure in situ within the lithium titanium phosphate-based electrode material. By incorporating a macroporous structure within the lithium titanium phosphate composite particles, the electrolyte can fully wet and penetrate the core region of the particles during use, shortening the solid-phase diffusion distance of lithium ions from the electrolyte to the active interface inside the particles. Furthermore, the macroporous structure in the carbon coating layer can form a through-channel with the macropores inside the lithium titanium phosphate composite particles, allowing the external electrolyte to pass through the dense carbon coating layer and reach the surface of the lithium titanium phosphate composite particles. The mesoporous structure in the carbon coating layer provides nanoscale transport channels for the rapid insertion and extraction of lithium ions, thereby reducing the migration resistance of lithium ions within the carbon coating layer. Simultaneously, the mesoporous structure helps to increase the specific surface area, providing a sufficient solid-liquid reaction interface for charge transfer reactions. The three-dimensionally coated carbon coating layer provides electron transport pathways, thereby improving the specific capacity of the lithium titanium phosphate-based electrode material.

[0035] In some embodiments, based on the theoretical mass of the prepared lithium titanium phosphate composite particles, the mass of the carbon-containing complexing agent is 5% to 15% of the theoretical mass of the lithium titanium phosphate composite particles, more preferably 8% to 12%, and more preferably 10%; the carbon-containing complexing agent is selected from at least one of polyvinylpyrrolidone, polyacrylic acid, and polyvinyl alcohol. By selecting a suitable preparation method, it is beneficial to achieve uniform dispersion of titanium ions, in-situ anchoring of the carbon source, and controllable construction of a hierarchical porous structure, thereby improving the rate performance and cycle stability of the electrode material.

[0036] In some embodiments, step S200 is as follows: after adding a lithium source, a phosphorus source, and a carbon-containing complexing agent to the titanium coordination complex solution, a second complexing agent is added until the pH of the slurry is adjusted to 3-5, and the carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent react with the Ti in the titanium coordination complex solution. 4+ Coordination adsorption is generated to prepare a first precursor slurry. The molar number of titanium in the titanium source is n1, the molar number of lithium in the lithium source is n2, and the molar number of phosphorus in the phosphorus source is n3. The ratio of n1, n2, and n3 is (1.5~2.5):(1~1.05):(2.5~3.5). By selecting a suitable preparation method, it is beneficial to achieve uniform dispersion of titanium ions, in-situ anchoring of carbon sources, and controllable construction of hierarchical porous structures, thereby improving the rate performance and cycle stability of the electrode material.

[0037] The preferred ratio of n1, n2, and n3 is 2:(1.02~1.05):3, and more preferably, the preferred ratio of n1, n2, and n3 is 2:1.05:3.

[0038] In some embodiments, in step S300, the median particle size of the second precursor mixture slurry is 0.2 μm to 2.0 μm; more preferably, the median particle size of the second precursor mixture slurry is 0.3 μm to 1.0 μm; and even more preferably, the median particle size of the second precursor mixture slurry is 0.5 μm to 0.8 μm. It is worth mentioning that this application controls the median particle size of the second precursor mixture slurry within an optimized range by grinding it before drying, which helps to eliminate large particle agglomerates, further improving the sphericity and uniformity of the obtained product particles, thereby improving the consistency and electrochemical performance of the electrode material.

[0039] In some embodiments, the drying process in step S300 is spray drying. The inlet temperature of the spray drying process is 180°C to 260°C, more preferably 200°C to 240°C, and even more preferably 220°C. The outlet temperature of the spray drying process is 90°C to 120°C, more preferably 100°C to 110°C, and even more preferably 105°C. The atomizer speed in the spray drying process is 15000 rpm to 25000 rpm, more preferably 18000 rpm to 22000 rpm, and even more preferably 20000 rpm. The feed rate of the spray drying process is 20 mL / min to 50 mL / min, more preferably 25 mL / min to 35 mL / min, and even more preferably 30 mL / min.

[0040] In some embodiments, step S400 involves: in a protective gas atmosphere, a precursor powder undergoes a first sintering treatment to obtain a sintering intermediate; the sintering intermediate undergoes a second sintering treatment to obtain a lithium titanium phosphate-based electrode material. The titanium, lithium, and phosphorus elements in the precursor powder undergo a solid-state reaction to generate lithium titanium phosphate composite particles. Simultaneously, a carbon-containing complexing agent is used for in-situ carbonization, forming a carbon coating layer around the lithium titanium phosphate composite particles. The temperature of the first sintering treatment is 300℃~400℃, the time is 1h~3h, and the heating rate is 2℃ / min~5℃ / min. The temperature of the second sintering treatment is 600℃~750℃, the time is 4h~8h, and the heating rate is 3℃ / min~6℃ / min. By selecting a suitable preparation method, it is beneficial to achieve uniform dispersion of titanium ions, in-situ anchoring of the carbon source, and controllable construction of a hierarchical porous structure, thereby improving the rate performance and cycle stability of the electrode material.

[0041] The preferred temperature for the first sintering treatment is 330℃~370℃, more preferably 350℃. The preferred duration for the first sintering treatment is 1.5h~2.5h, more preferably 2h. The preferred heating rate for the first sintering treatment is 2℃ / min~4℃ / min, more preferably 3℃ / min. The preferred temperature for the second sintering treatment is 650℃~720℃, more preferably 700℃. The preferred duration for the second sintering treatment is 5h~7h, more preferably 6h. The preferred heating rate for the second sintering treatment is 4℃ / min~6℃ / min, more preferably 5℃ / min.

[0042] In some embodiments, the protective gas is selected from at least one of argon, nitrogen, and helium, with argon or nitrogen being preferred, and argon being even more preferred.

[0043] In some embodiments, the first ligand is at least one of acetylacetone, citric acid, tartaric acid, and ethylenediaminetetraacetic acid, and the molar amount of the first ligand is 0.5 to 2.0 times the molar amount of the titanium source; the second ligand is at least one of ammonia, ethylenediamine, or triethanolamine, and the concentration of the second ligand is 0.1 mol / L to 5 mol / L; the liquid medium is a mixed solution of an alcohol and water, wherein the alcohol is anhydrous ethanol and / or isopropanol, and the volume ratio of the alcohol to water is (1 to 3):1. By selecting a suitable preparation method, it is beneficial to achieve uniform dispersion of titanium ions, in-situ anchoring of the carbon source, and controllable construction of a hierarchical porous structure, thereby improving the rate performance and cycle stability of the electrode material.

[0044] The first ligand is preferably acetylacetone and / or citric acid, more preferably acetylacetone. The second ligand is preferably ammonia and / or ethylenediamine, more preferably ammonia. The molar number of the first ligand is preferably 0.8 to 1.5 times the molar number of the titanium source, more preferably 1 times. The concentration of the second ligand is preferably 0.5 mol / L to 3 mol / L, more preferably 1 mol / L to 2 mol / L. The volume ratio of the alcohol to water is preferably (2 to 3):1, more preferably 2:1.

[0045] This application also provides an electrode sheet, comprising the lithium titanium phosphate-based electrode material as described above, or the lithium titanium phosphate-based electrode material prepared by the aforementioned preparation method. By selecting suitable preparation conditions, it is beneficial to obtain an electrode sheet with good electron transport performance, good stability in use, and long service life.

[0046] This application also provides a battery including at least one electrode as described above. By using the electrode provided in this application, a battery with good electrochemical performance can be obtained.

[0047] Example 1 Example 1 provides a method for preparing lithium titanium phosphate-based electrode materials, electrode sheets, and batteries, including the following steps: (1) Dissolve 0.1 mol tetrabutyl titanate in 200 mL of mixed solvent, add 0.1 mol acetylacetone, stir in a 50 °C water bath for 45 min to form a complex solution. The mixed solvent is a mixture of ethanol and water, with a volume ratio of ethanol to water of 2:1.

[0048] (2) Add 0.0525 mol lithium hydroxide monohydrate and 0.15 mol ammonium dihydrogen phosphate to the complex solution, continue stirring for 30 min, then add 1.0 mol / L ammonia water to adjust the pH value to 4.0, add 4.0 g of polyvinylpyrrolidone of brand K30, stir until completely dissolved, and obtain the precursor mixture.

[0049] (3) The precursor mixture was ground in a grinder to obtain a mixed slurry, and the median particle size of the mixed slurry was controlled to be 0.8 μm. The mixed slurry was spray-dried to obtain precursor powder. The inlet temperature of the spray dryer was 220℃, the outlet temperature was 105℃, the atomizer speed was 20000 rpm, and the feed rate was 30 mL / min.

[0050] (4) In an argon atmosphere, the precursor powder was heated to 350°C at 3°C / min and held for 2 hours, and then heated to 700°C at 5°C / min and held for 6 hours for sintering treatment. The lithium titanium phosphate-based electrode material was obtained by natural cooling. Figure 1 This is a scanning electron microscope image of the lithium titanium phosphate-based electrode material prepared in Example 1 of this application.

[0051] (5) Lithium titanium phosphate-based electrode material, conductive carbon black, and PVDF binder were mixed in N-methylpyrrolidone at a mass ratio of 8:1:1 to prepare an electrode slurry. The electrode slurry was uniformly coated on aluminum foil, and the electrode sheet was compacted by rollers and then cut to obtain a positive electrode with a diameter of 12 mm. Using a lithium metal sheet as the counter electrode, a 1 mol / L LiPF6 electrolyte (the solvent components are ethylene carbonate (EC) and dimethyl carbonate (DMC), with a volume ratio of EC to DMC of 1:1) was used as the electrolyte, and Celgard 2400 was used as the separator. The CR2032 button cell was assembled in an argon-filled glove box.

[0052] Example 2 The difference between Example 2 and Example 1 is that the amount of lithium hydroxide monohydrate used is 0.05 mol, 0.1 mol acetylacetone is replaced with 0.15 mol citric acid, and 4.0 g polyvinylpyrrolidone is replaced with 3.2 g polyacrylic acid. In step (2), ammonia water with a concentration of 1.0 mol / L is added dropwise to adjust the pH value to 3.5. In step (3), the median particle size of the mixed slurry is 0.5 μm.

[0053] Example 3 The difference between Example 3 and Example 1 is that the amount of lithium hydroxide monohydrate used is 0.051 mol, the amount of acetylacetone used is 0.08 mol, and the amount of polyvinylpyrrolidone used is 4.8 g. In step (3), the median particle size of the mixed slurry is 0.3 μm.

[0054] Example 4 The difference between Example 4 and Example 1 is that in step (3), the median particle size of the mixed slurry is 1.5 μm.

[0055] Example 5 The difference between Example 5 and Example 1 is that in step (3), the median particle size of the mixed slurry is 2 μm.

[0056] Example 6 The difference between Example 6 and Example 1 is that the inlet temperature of the spray dryer is 260°C and the outlet temperature is 115°C. In step (3), the median particle size of the mixed slurry is 0.8 μm.

[0057] Example 7 The difference between Example 7 and Example 1 is that 4.0g of polyvinylpyrrolidone is replaced with 5.5g of polyvinyl alcohol.

[0058] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that acetylacetone was not added.

[0059] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that polyvinylpyrrolidone was replaced with an equal mass of glucose.

[0060] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that step (3) is as follows: the precursor mixture is ground in a grinder to obtain a mixed slurry, and the median particle size of the mixed slurry is controlled to be 0.8 μm. The mixed slurry is dried in an oven to obtain precursor powder. The temperature of the oven is 80°C and the drying time is 24 h.

[0061] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that step (3) involves spray drying the precursor mixture to obtain precursor powder. The inlet temperature of the spray dryer is 220°C, the outlet temperature is 105°C, the atomizer speed is 20000 rpm, and the feed rate is 30 mL / min. Obvious agglomerates are visible in the precursor mixture, with a median particle size of approximately 5.8 μm.

[0062] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that in step (3), the median particle size of the mixed slurry is 3 μm.

[0063] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that the amount of polyvinylpyrrolidone used is 8g.

[0064] Comparative Example 7 The difference between Comparative Example 7 and Example 1 is that the amount of polyvinylpyrrolidone used is 1g.

[0065] Performance testing The cycle performance and rate performance of the batteries prepared in Examples 1-6 and Comparative Examples 1-7 were tested. Charge-discharge tests were conducted using a LAND Mon V7 battery tester. Rate performance tests were performed at 25±2℃ with a voltage range of 2.5V~4.0V. The discharge specific capacity of each sample was tested at 0.1C, 1C, 10C, and 20C rates, and the capacity retention rate after 100 cycles at 20C was recorded. The test results are shown in Table 1.

[0066] Table 1: Performance Tests of Lithium-ion Batteries

[0067] Comparative examples 1-3 show that the optimal battery capacity and rate performance is achieved when the ratio of the molar amounts of titanium in the titanium source, lithium in the lithium source, and phosphorus in the phosphorus source is 2:1.05:3. Comparative examples 1 and 4-5 show that as the median particle size D50 of the mixed slurry increases from 0.8 μm to 2.0 μm, the battery's specific capacity and rate performance gradually decrease, indicating that controlling the median particle size of the mixed slurry within a smaller range is beneficial for improving the battery's electrochemical performance. When the median particle size D50 of the mixed slurry increases to 2.0 μm, the battery's 20C capacity retention decreases to 57.5%, but it is still better than the unground Comparative Example 4 (36.7%) and Comparative Example 5 (48.1%), proving that the grinding process is beneficial for improving the battery's electrochemical performance. Comparing Examples 1 and 6, it can be seen that when the inlet temperature of the spray dryer is too high (260°C), some precursors decompose too quickly, resulting in a slight decrease in the specific capacity of the battery. Comparing Examples 1 and 7, it can be seen that by selecting polymers such as polyvinylpyrrolidone and polyacrylic acid, which possess both coordination and carbonization capabilities, as carbon sources, the carbonyl and carboxyl functional groups on their molecular chains can interact with Ti. 4+ Coordination occurs, causing carbon source molecules to be tightly anchored around titanium atoms. After sintering, a continuous, uniform, and tightly bonded carbon conductive network is formed, which is beneficial to improving the electronic conductivity of the material.

[0068] As shown in Example 1 and Comparative Example 1, without the addition of acetylacetone, the rapid hydrolysis of the titanium source leads to uneven elemental distribution, resulting in reduced product purity and a significant decrease in rate performance. Analysis of Example 1 and Comparative Example 2 shows that common carbon sources (e.g., glucose) lack the coordination and anchoring ability with titanium ions, resulting in poor continuity of the carbon coating layer formed after sintering, thus reducing rate performance. Analysis of Example 1 and Comparative Example 3 shows that the product without spray drying and granulation has irregular particle morphology, wide particle size distribution, low tap density, and poor electrochemical performance. Comparing Example 1 and Comparative Example 4 shows that without grinding treatment, a large number of agglomerates exist in the precursor mixture, leading to poor sphericity and uneven composition of the spray-dried product, resulting in a significant decrease in rate performance. Comparing Example 1 and Comparative Example 5 shows that when the grinding particle size is too large, the particle refinement is insufficient, leading to a decrease in electrochemical performance. Comparing Example 1 and Comparative Examples 6-7 shows that selecting an appropriate amount of carbon-containing complexing agent is beneficial for obtaining batteries with good specific capacity and cycle stability.

[0069] The basic principles, main features, and advantages of this application have been described above. Those skilled in the art should understand that this application is not limited to the above embodiments. The embodiments and descriptions in the specification are merely the principles of this application. Various changes and modifications can be made to this application without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claims. The scope of protection claimed by this application is defined by the appended claims and their equivalents.

Claims

1. A lithium titanium phosphate-based electrode material, characterized in that, include: Lithium titanium phosphate composite particles, wherein the chemical formula of the lithium titanium phosphate composite particles is LiTi2(PO4)3; A carbon coating layer is formed on the outer periphery of the lithium titanium phosphate composite particles by in-situ carbonization of the carbon coating layer with a carbon-containing complexing agent. The carbon-containing complexing agent contains at least one functional group selected from carbonyl, carboxyl, and hydroxyl groups on its molecular chain, and the carbon-containing complexing agent is suitable for reacting with Ti. 4+ Coordination adsorption occurs.

2. The lithium titanium phosphate-based electrode material according to claim 1, characterized in that, At least one of the following conditions must be met: (a) The mass fraction of carbon in the lithium titanium phosphate-based electrode material is 0.5 wt% to 3 wt%; (b) The particle size of the lithium titanium phosphate composite particles is 100 nm to 500 nm; (c) The specific surface area of ​​the lithium titanium phosphate-based electrode material is 8 m². 2 / g~20m 2 / g, wherein the particle size of the lithium titanium phosphate-based electrode material is 3μm~10μm; (d) The carbon-containing complexing agent is selected from at least one of polyvinylpyrrolidone, polyacrylic acid and polyvinyl alcohol.

3. The lithium titanium phosphate-based electrode material according to claim 1, characterized in that, The lithium titanium phosphate composite particles have a macroporous structure, and the carbon coating layer has both macroporous and mesoporous structures. The pore size of the macroporous structure is greater than 50 nm, and the pore size of the mesoporous structure is 2 nm to 50 nm.

4. A method for preparing a lithium titanium phosphate-based electrode material, characterized in that, Including the following steps: S100. The titanium source and the first ligand are dispersed in a liquid medium, and the first ligand and Ti... 4+ A coordination complexation reaction is generated to prepare a titanium coordination complex solution; S200, A lithium source, a phosphorus source, a second ligand, and a carbon-containing complexing agent are added to the titanium coordination complex solution. The carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent react with the Ti in the titanium coordination complex solution. 4+ Coordination adsorption occurs, and a first precursor mixture slurry is obtained. S300: Grind the first precursor mixture slurry to obtain a second precursor mixture slurry, and dry the second precursor mixture slurry to obtain precursor powder. S400. The precursor powder is sintered. During the sintering process, the titanium, lithium and phosphorus elements in the precursor powder react in a solid phase to generate lithium titanium phosphate composite particles. At the same time, the carbon-containing complexing agent is carbonized in situ to form a carbon coating layer covering the outer periphery of the lithium titanium phosphate composite particles, thereby obtaining a lithium titanium phosphate-based electrode material.

5. The preparation method according to claim 4, characterized in that, Based on the theoretical mass of the lithium titanium phosphate composite particles obtained, the mass of the carbon-containing complexing agent is 5% to 15% of the theoretical mass of the lithium titanium phosphate composite particles; the carbon-containing complexing agent is selected from at least one of polyvinylpyrrolidone, polyacrylic acid and polyvinyl alcohol.

6. The preparation method according to claim 4, characterized in that, Step S200 is as follows: After adding a lithium source, a phosphorus source, and a carbon-containing complexing agent to the titanium coordination complex solution, a second complexing agent is added until the pH of the slurry is adjusted to 3-5. The carbonyl and / or carboxyl functional groups on the molecular chain of the carbon-containing complexing agent react with the Ti in the titanium coordination complex solution. 4+ Coordination adsorption occurs, and a first precursor mixture slurry is obtained. The number of moles of titanium in the titanium source is n1, the number of moles of lithium in the lithium source is n2, and the number of moles of phosphorus in the phosphorus source is n3. The ratio of n1, n2, and n3 is (1.5~2.5):(1~1.05):(2.5~3.5).

7. The preparation method according to claim 4, characterized in that, Step S400 is as follows: In a protective gas atmosphere, the precursor powder is subjected to a first sintering treatment to obtain a sintering intermediate, and the sintering intermediate is subjected to a second sintering treatment to obtain a lithium titanium phosphate-based electrode material. The titanium, lithium and phosphorus elements in the precursor powder are reacted in a solid phase to generate lithium titanium phosphate composite particles. At the same time, the carbon-containing complexing agent is carbonized in situ to form a carbon coating layer covering the outer periphery of the lithium titanium phosphate composite particles. The temperature of the first sintering treatment is 300℃~400℃, the time of the first sintering treatment is 1h~3h, and the heating rate of the first sintering treatment is 2℃ / min~5℃ / min. The temperature of the second sintering treatment is 600℃~750℃, the time of the second sintering treatment is 4h~8h, and the heating rate of the second sintering treatment is 3℃ / min~6℃ / min.

8. The preparation method according to any one of claims 4 to 7, characterized in that, The first ligand is at least one of acetylacetone, citric acid, tartaric acid, and ethylenediaminetetraacetic acid, and the molar number of the first ligand is 0.5 to 2.0 times the molar number of the titanium source; The second ligand is at least one of ammonia, ethylenediamine, or triethanolamine, and the concentration of the second ligand is 0.1 mol / L to 5 mol / L; The liquid medium is a mixed solution of alcohol and water, wherein the alcohol is anhydrous ethanol and / or isopropanol, and the volume ratio of alcohol to water is (1~3):

1.

9. An electrode sheet, characterized in that, It includes the lithium titanium phosphate-based electrode material as described in any one of claims 1 to 3, or the lithium titanium phosphate-based electrode material prepared by the preparation method described in any one of claims 4 to 8.

10. A battery, characterized in that, It includes at least one electrode as described in claim 9.