Composite zinc powder negative electrode paste and preparation method, composite zinc powder negative electrode and aqueous zinc metal battery

By introducing modified bismuth nanosheets and antimony nanosheets into the zinc powder anode, a stable three-dimensional conductive network was constructed, which solved the dendrite and corrosion problems of the zinc powder anode and improved the electrochemical stability and cycle life of the zinc powder anode.

CN123143391APending Publication Date: 2026-11-20FUDAN UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510645023.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-19
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Zinc powder anodes in aqueous zinc metal batteries suffer from dendrite formation, corrosion, and hydrogen evolution, resulting in short cycle life, which existing modification strategies struggle to address effectively.

Method used

A composite zinc powder negative electrode slurry is used, which includes zinc powder, modified bismuth nanosheets and/or modified antimony nanosheets and a binder. By adding modified nanosheets, a uniform electric field distribution and a stable three-dimensional conductive network are constructed, which inhibits zinc powder corrosion and dendrite growth.

Benefits of technology

It significantly improves the hydrogen evolution overpotential of zinc powder anode, suppresses corrosion and side reactions, achieves uniform deposition of zinc ions, prolongs the electrical performance and stability of electrode materials, and enhances battery cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143391A_ABST
    Figure CN123143391A_ABST
Patent Text Reader

Abstract

The application provides a composite zinc powder negative electrode slurry and a preparation method thereof, and a negative electrode and a battery using the composite zinc powder negative electrode slurry. In the technical scheme provided by the application, the composite zinc powder negative electrode slurry comprises zinc powder, modified bismuth nanosheets and / or modified antimony nanosheets, and a binder. By adding the modified bismuth nanosheets and / or modified antimony nanosheets, the problems of easy corrosion and generation of "dead zinc" of the zinc powder negative electrode during standing and cycling are solved. Not only is the hydrogen evolution overpotential of the zinc powder negative electrode significantly improved, and the corrosion and side reaction of the zinc powder are inhibited, but also the modified bismuth nanosheets and / or modified antimony nanosheets can construct a uniform electric field distribution as zinc-philic sites, induce uniform deposition of zinc ions, and improve the electrical performance and stability of the electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a negative electrode slurry and its preparation method, a negative electrode and a battery, specifically to a negative electrode slurry prepared using composite zinc powder and its preparation method, a composite zinc powder negative electrode and an aqueous zinc metal battery, belonging to the field of energy storage materials technology. Background Technology

[0002] Aqueous zinc metal batteries (AZMBs) benefit from abundant zinc reserves, good chemical stability, the environmental friendliness of aqueous electrolytes, and a high theoretical capacity (820 mAh g). -1 With its relatively low redox potential (compared to a standard hydrogen electrode of -0.76V), zinc powder has become one of the most promising alternative technologies for large-scale energy storage. In recent years, the design of AZMBs has become increasingly diversified. Among these, the zinc metal anode has always played a crucial role in the energy density and lifespan of AZMBs. Currently, the commonly used zinc foil anodes, which are tens or even hundreds of micrometers thick, are too thick, resulting in a low depth of discharge (DOD) when matched with the positive electrode's areal capacity. The excess zinc foil mass not only significantly reduces the energy density of the system itself but also greatly diminishes the practical applicability of many modification strategies. However, the thinnest zinc foil currently available commercially is 10 micrometers. Producing such thin zinc foil presents technical challenges and also increases production costs. Unlike zinc foil anodes, zinc powder anodes have recently become an attractive form of application for AZMBs. On the one hand, zinc powder is comparable in cost to zinc foil and is readily available, offering advantages such as large-scale processing, flexible adjustment, and versatility. More importantly, the amount of zinc powder used can be flexibly adjusted according to the positive electrode areal loading, which is crucial for controlling the N / P ratio and achieving high energy density in AZMBs. On the other hand, zinc powder can be made into a slurry and directly applied to existing mature electrode fabrication processes, such as wet coating. Furthermore, the three-dimensional structure of zinc powder anodes results in a more uniform electric field distribution compared to zinc foil anodes. Therefore, zinc powder anodes possess advantages that zinc foil anodes cannot match.

[0003] In recent years, zinc powder-based anodes have become the most promising anode choice for AZMBs (Alternative Acid-Based Metallic Electrolytes). However, due to the larger specific surface area and chemical activity of zinc powder, it not only faces more severe dendrite problems, but also, with limited zinc powder usage, zinc powder will undergo more severe corrosion and hydrogen evolution in aqueous electrolytes in a short time. Surface passivation further causes large-area failure of the limited contact between zinc powder particles, resulting in more "dead zinc," which makes batteries assembled using zinc powder anodes exhibit very unsatisfactory cycle life. To solve these problems, Chinese patent CN202310706415.X proposes to use zinc powder with different particle diameters combined with binders and conductive agents to construct gradient flexible zinc powder anode materials to improve the cycle reversibility of zinc powder anodes. Chinese patent CN202411543375.2 uses zinc powder as raw material and optimizes the morphology and crystal structure of zinc powder by controlling the ball milling and annealing processes, inducing the formation of (002) crystal plane orientation zinc powder anode materials to effectively suppress the formation of zinc dendrites. Chinese patents CN202410911708.6 and CN202211565949.7 employ various conductive components to coat zinc powder, effectively suppressing side reactions such as zinc dendrite formation and hydrogen evolution, improving zinc utilization, and enhancing the electrochemical stability of zinc metal. Chinese patent CN202211641851.5 constructs a conductive shell on the surface of zinc powder through a substitution reaction, simultaneously inducing uniform zinc ion deposition and improving structural corrosion on the zinc powder negative electrode surface.

[0004] To date, although research on zinc powder anodes has become increasingly in-depth, new and scalable technical solutions still need further development. Summary of the Invention

[0005] To address the problems existing in current zinc powder anode materials, the present invention aims to provide a composite zinc powder anode slurry and its preparation method, as well as an anode and battery using this composite zinc powder anode slurry. In the technical solution provided by the present invention, the composite zinc powder anode slurry includes zinc powder, modified bismuth nanosheets and / or modified antimony nanosheets, and a binder. The addition of modified bismuth nanosheets and / or modified antimony nanosheets solves the problems of easy corrosion and "dead zinc" formation during the static and cycling processes of current zinc powder anodes. This not only significantly improves the hydrogen evolution overpotential of the zinc powder anode and inhibits zinc powder corrosion and side reactions, but also, as zinc-loving sites, can construct a uniform electric field distribution, induce uniform zinc ion deposition, and improve the electrical performance and stability of the electrode material.

[0006] According to the first technical solution provided by the present invention, a composite zinc powder negative electrode slurry is provided.

[0007] A composite zinc powder negative electrode slurry, the composite zinc powder comprising:

[0008] The zinc powder comprises 80-99 parts by weight, preferably 82-98 parts by weight, and more preferably 85-95 parts by weight;

[0009] 1-20 parts by weight of modified bismuth nanosheets and / or modified antimony nanosheets, preferably 3-15 parts by weight, more preferably 5-10 parts by weight;

[0010] The adhesive is used in amounts of 0.5-10 parts by weight, preferably 0.8-8 parts by weight, and more preferably 1-5 parts by weight.

[0011] Preferably, the composite zinc powder comprises: 85-95 parts by weight of zinc powder, 4-7 parts by weight of modified bismuth nanosheets, 1-4 parts by weight of modified antimony nanosheets, and 1-5 parts by weight of binder.

[0012] In this invention, modified bismuth nanosheets are prepared by the following method: polyvinylpyrrolidone is dissolved in an organic solvent, bismuth powder is added, and the mixture is ground and separated to obtain bismuth nanosheets.

[0013] In this invention, the modified antimony nanosheets are prepared by the following method: dissolving polyvinylpyrrolidone in an organic solvent, adding antimony powder, grinding, and separating to obtain modified antimony nanosheets.

[0014] Preferably, the organic solvent is selected from isopropanol, ethanol, methanol, N,N-dimethylformamide, ethylene glycol, or N-methylpyrrolidone.

[0015] Preferably, the mass concentration of polyvinylpyrrolidone dissolved in the organic solvent is 10-30%.

[0016] Preferably, the grinding is ball milling.

[0017] Preferably, the separation is sedimentation, filtration, or centrifugation.

[0018] In this invention, the zinc powder has a particle size of 400-30000 mesh and a purity of greater than 99%.

[0019] Preferably, the adhesive is selected from at least one of PVA, HEC, PAAS, HPMC, PEO, CMC, SBR, PVDF, PTFE, and NMP.

[0020] According to a second embodiment of the present invention, a method for preparing the composite zinc powder negative electrode slurry described in the first embodiment is provided.

[0021] A method for preparing composite zinc powder negative electrode slurry, the method comprising the following steps:

[0022] S1. Preparation of modified bismuth nanosheets: Polyvinylpyrrolidone was added to an organic solvent and stirred to dissolve, obtaining a polymer-assisted exfoliation solution; bismuth powder and polymer-assisted exfoliation solution were mixed, ball-milled, separated, and dried to obtain modified bismuth nanosheets;

[0023] S2. Preparation of modified antimony nanosheets: Polyvinylpyrrolidone was added to an organic solvent and stirred to dissolve, obtaining a polymer-assisted exfoliation solution; antimony powder and polymer-assisted exfoliation solution were mixed, ball-milled, separated, and dried to obtain modified antimony nanosheets;

[0024] S3. Preparation of composite zinc powder anode slurry: Zinc powder, modified bismuth nanosheets, modified antimony nanosheets, and binder are mixed, solvent is added, and the mixture is stirred to obtain composite zinc powder anode slurry.

[0025] Preferably, the organic solvents used in steps S1 and S2 are selected from isopropanol, ethanol, methanol, N,N-dimethylformamide, ethylene glycol, or N-methylpyrrolidone.

[0026] Preferably, the adhesive used in step S3 is selected from at least one of PVA, HEC, PAAS, HPMC, PEO, CMC, SBR, PVDF, and PTFE.

[0027] Preferably, the solvent is selected from at least one of N-methylpyrrolidone, water, acetone, propylene carbonate, dimethylformamide, cyclohexanone, or methyl ethyl ketone.

[0028] Preferably, step S1 is as follows: weigh polyvinylpyrrolidone and add it to an organic solvent, stirring and dissolving until completely dissolved and transparent to obtain a polymer-assisted exfoliation solution; then, add bismuth powder, milling beads and polymer-assisted exfoliation solution to a ball mill jar and ball mill; centrifuge to remove insufficiently exfoliated bismuth powder and excess polyvinylpyrrolidone; ultrasonically disperse, wash and dry to obtain modified bismuth nanosheets.

[0029] Preferably, step S2 is as follows: weigh polyvinylpyrrolidone and add it to an organic solvent, stirring and dissolving until completely dissolved and transparent to obtain a polymer-assisted exfoliation solution; then, add antimony powder, milling beads and polymer-assisted exfoliation solution to a ball mill jar and ball mill; centrifuge to remove insufficiently exfoliated antimony powder and excess polyvinylpyrrolidone; ultrasonically disperse, wash and dry to obtain modified antimony nanosheets.

[0030] According to a third embodiment of the present invention, a composite zinc powder negative electrode is provided.

[0031] A composite zinc powder anode is obtained by coating a composite zinc powder anode slurry as described in the first embodiment or a composite zinc powder anode slurry prepared according to the method described in the second embodiment onto a current collector and drying it.

[0032] Preferably, the current collector is selected from one of zinc matrix, titanium foil, copper foil, and graphene current collector.

[0033] According to a fourth embodiment of the present invention, an aqueous zinc metal battery is provided.

[0034] An aqueous zinc metal battery includes a composite zinc powder negative electrode, a positive electrode, a separator, and an electrolyte as described in the third embodiment.

[0035] Preferably, the positive electrode is selected from manganese-based compounds (preferably MnO2, Mn2O3, Mn3O4) and vanadium-based compounds (preferably V2O5, VO2, V2O3, V6O4). 13 One of the following: halogen cathode (preferably Br2 or I2).

[0036] Preferably, the diaphragm is selected from either a glass fiber diaphragm or a cellulose diaphragm.

[0037] Preferably, the electrolyte is selected from one of ZnSO4, ZnCI2, Zn(CF3SO3)2, and Zn(ClO4)2 electrolytes.

[0038] In this invention, zinc powder refers to metallic zinc particles with a purity higher than 99%, and the particle size range can be controlled within 400-30000 mesh. As the main body of the negative electrode active material, its weight proportion determines the capacity contribution and structural compactness of the electrode. Modified bismuth nanosheets are two-dimensional nanomaterials prepared by polymer-assisted exfoliation, and the adsorption of polyvinylpyrrolidone on the surface enhances dispersibility. Its high specific surface area provides abundant nucleation sites, inducing uniform deposition of zinc ions. Modified antimony nanosheets have similar functions, and both can be used alone or in combination to adjust the hydrogen evolution overpotential of the electrode. The binder is selected from water-soluble polymers such as polyacrylic acid and carboxymethyl cellulose, which fix the zinc powder particles through hydrogen bonds and van der Waals forces to maintain the integrity of the electrode structure.

[0039] In this invention, zinc powder serves as the main active component, constructing a three-dimensional conductive framework. Its weight percentage is controlled at 80-99 parts to avoid excessive zinc leading to aggravated side reactions. Modified bismuth or antimony nanosheets are used as functional additives, utilizing their metallic properties to reduce local current density, inhibit dendrite growth, and simultaneously increase the hydrogen evolution overpotential, thus suppressing zinc powder corrosion side reactions. The layered structure of the nanosheets is interspersed within the zinc powder gaps, forming continuous electron transport channels and numerous nucleation sites. A binder forms a flexible coating layer on the surface of the zinc particles, preventing the active material from detaching while allowing electrolyte penetration. Through the synergistic effect of these three components, a stable ion / electron dual pathway is formed inside the electrode, while simultaneously reducing interfacial reaction kinetics.

[0040] Through the above technical solutions, this application effectively suppresses the uncontrolled growth of zinc dendrites, reduces the hydrogen evolution reaction rate, and slows down the zinc powder corrosion process. A stable three-dimensional conductive network is formed inside the electrode, reducing the direct contact area between the active material and the electrolyte and extending the cycle life. The composite structure enhances the mechanical bonding force between zinc powder particles, avoiding the structural pulverization problem during charge and discharge.

[0041] In a further preferred embodiment of the present invention, the composite zinc powder negative electrode slurry comprises 85-95 parts by weight of zinc powder, 4-7 parts by weight of modified bismuth nanosheets, 1-4 parts by weight of modified antimony nanosheets, and 1-5 parts by weight of binder.

[0042] In this invention, the zinc powder content in the composite zinc powder negative electrode slurry is controlled at 85-95 parts by weight to ensure sufficient zinc storage capacity, while avoiding excessive zinc powder leading to an excessively large specific surface area and exacerbating side reactions. Modified bismuth nanosheets refer to two-dimensional bismuth materials prepared by polyvinylpyrrolidone-assisted ball milling and exfoliation. Specifically, bismuth powder can be obtained by mixing bismuth powder with a polymer solution through ball milling and then centrifuging. Its content is limited to 4-7 parts by weight to provide uniform zinc deposition sites and inhibit dendrite growth. Modified antimony nanosheets refer to two-dimensional antimony materials prepared by a similar method. Specifically, antimony powder can be obtained by ball milling and exfoliation in an organic solvent. Its content is controlled at 1-4 parts by weight to utilize the high hydrogen evolution overpotential of antimony to reduce gaseous side reactions. The binder refers to a polymeric material used to maintain the integrity of the electrode structure. Specifically, at least one of PVA, HEC, or PAAS can be used, and its content is limited to 1-5 parts by weight to balance the mechanical strength and ion transport efficiency of the electrode.

[0043] In a preferred embodiment of the present invention, when the zinc powder content is controlled at 85-95 parts by weight, the contact area between the active material and the conductive network is optimized, effectively reducing the interfacial impedance. Modified bismuth nanosheets provide a uniform electric field distribution through their two-dimensional nanostructure; an addition of 4-7 parts by weight can form an effective dendrite suppression layer without affecting zinc ion transport. Modified antimony nanosheets are introduced at a low proportion of 1-4 parts by weight, forming a synergistic effect with the bismuth nanosheets. The former focuses on increasing the hydrogen evolution overpotential, while the latter focuses on regulating the zinc deposition path. When the binder content is controlled at 1-5 parts by weight, it can maintain the conductive pathway between zinc powders through the cross-linking effect of polymer chains, while avoiding excessive binder hindering electrolyte wetting. This solution, through the composite addition of bismuth and antimony nanosheets, constructs a multifunctional interfacial protective layer while maintaining the stability of the zinc powder conductive network.

[0044] Through the above technical solution, this application establishes a synergistic mechanism in the zinc powder anode. Modified bismuth nanosheets inhibit the vertical growth of zinc dendrites, while modified antimony nanosheets raise the energy barrier for the hydrogen evolution reaction. Together, they reduce the chemical activity of the zinc powder surface. Precise control of the binder content ensures the integrity of the electrode structure during cycling, thereby effectively mitigating contact failure between zinc powder particles and extending the battery's cycle life.

[0045] In this invention, dissolving polyvinylpyrrolidone in an organic solvent refers to dispersing the polymer in a liquid medium to form a uniform environment conducive to exfoliation. This can be achieved by stirring and dissolving. Polyvinylpyrrolidone coats the surface of metal particles through adsorption, reducing the tendency for aggregation during the grinding process. Grinding refers to exfoliating bulk metal particles into nanosheet structures using mechanical shear force, specifically achieved through ball milling. The collision between the milling beads and the metal particles, as well as the adhesive force between the polymer solution and the metal particles, work together to promote interlayer slippage and exfoliation. Separation refers to separating the exfoliated product from unreacted substances to purify the target nanosheets. This can be achieved through centrifugation, removing unexfoliated metal particles and excess polymer through density differences.

[0046] Specifically, with the assistance of polyvinylpyrrolidone, an organic solvent forms a stable dispersion system. During ball milling, the metal particles are subjected to continuous shear force, and the layered structure is exfoliated into nanosheets. Polymer molecular chains are adsorbed onto the nanosheet surface by van der Waals forces, creating a steric hindrance effect that prevents the nanosheets from re-stacking. Centrifugation yields polymer-coated modified nanosheets, whose two-dimensional structure can be embedded in the gaps between zinc powder particles to form a three-dimensional conductive network, homogenizing the electric field distribution. The polar groups on the nanosheet surface can adsorb zinc ions, forming directional deposition sites and inhibiting disordered dendrite growth. The introduction of bismuth or antimony alters the nucleation barrier for zinc deposition, inducing preferential deposition of zinc along specific crystal planes and reducing the probability of passivation layer formation.

[0047] Compared to existing technologies, traditional metal powder modification often employs physical mixing or chemical plating processes, which cannot control interfacial properties at the nanoscale. Existing methods produce metal additives with insufficient specific surface area, making it impossible to effectively construct conductive networks.

[0048] In this invention, the modified nanosheets prepared in this application possess high dispersibility and uniform coating characteristics, enabling the establishment of stable ion / electron transport channels between zinc powder particles. The functional groups on the nanosheet surface enhance the hydrogen evolution reaction barrier, suppressing side reactions. The alloying effect of bismuth or antimony modulates the zinc deposition kinetics, delaying the electrode passivation process. This technical solution effectively reduces the local current density of the zinc powder anode, improves the uniformity of zinc deposition, and enhances the cycle stability of the battery.

[0049] In this invention, when preparing modified bismuth nanosheets or modified antimony nanosheets, the organic solvent is selected from any one of isopropanol, ethanol, methanol, N,N-dimethylformamide, ethylene glycol, or N-methylpyrrolidone. The organic solvent refers to the liquid medium used to dissolve polyvinylpyrrolidone (PVP), specifically a solvent with moderate polarity and good polymer solubility. Such solvents can promote the full extension of PPVP molecular chains, forming a stable polymer solution, thereby effectively adsorbing onto the surface of the metal powder during ball milling and assisting in the exfoliation of the layered structure. Controlling the mass concentration of PPVP refers to adjusting the ratio of polymer to solvent, which can be achieved by adjusting the feed rate. Setting the concentration range to 10-30% ensures appropriate solution viscosity while preventing excessive polymer from causing nanosheet agglomeration. Ball milling refers to a process that uses grinding media to apply mechanical shear force to the raw material, specifically using a planetary ball mill or a drum ball mill. The controllable shear force generated helps in the uniform exfoliation of the metal layered structure. Separation methods refer to the operations of separating stripped products from unreacted substances. Specifically, centrifuges, filter membranes, or gravity sedimentation devices can be used. For example, centrifugation can quickly remove unstripped metal particles, while filtration or sedimentation can effectively remove free polymer residues.

[0050] In this invention, when preparing modified bismuth nanosheets or antimony nanosheets, polyvinylpyrrolidone is dissolved in a selected organic solvent to form a homogeneous solution. The solvent must simultaneously satisfy the requirements of polymer solubility and adaptability to the subsequent grinding process.

[0051] In this invention, the particle size range of zinc powder refers to a particle size distribution spanning from micrometers to submicrometers, which can be achieved through mechanical grinding or vapor deposition processes. The selection of the particle size range balances electrode porosity and active site density. Zinc powder purity greater than 99% means that the proportion of metallic zinc exceeds 99% (e.g., 99.1%, 99.5%, 99.9%, 99.99%, etc.), which can be achieved through electrolytic refining or zone melting processes. High-purity zinc powder can reduce impurity-induced localized electrochemical corrosion. The choice of binder refers to polymeric materials with different polar groups, which can be achieved through solution blending or in-situ polymerization processes. Different binders can adapt to the slurry processing requirements of aqueous or organic solvent systems. The design of the zinc powder particle size range allows fine particles to fill the gaps between coarse particles, forming a three-dimensional continuous conductive network and reducing interfacial contact resistance; high-purity zinc powder avoids hydrogen evolution reaction caused by heterogeneous metal impurities, reducing the self-corrosion rate; the binder coats the surface of zinc particles through molecular chain entanglement and functional group adsorption, inhibiting the formation of passivation layer caused by direct contact of electrolyte with zinc powder, while enhancing the mechanical bonding force between particles and preventing the electrode structure from collapsing during cycling.

[0052] Compared to existing technologies, traditional zinc powder modification methods often employ single metal powder additives or simple mechanical mixing, making it difficult to simultaneously achieve conductive network construction and side reaction suppression. For example, some techniques only improve zinc powder dispersibility through conductive agent coating, but fail to address the corrosion acceleration problem caused by high specific surface area. Other techniques use direct mixing of bismuth-based alloy powders, but fail to achieve the directional alignment of nanosheet structures. This method prepares bismuth and antimony nanosheets stepwise, combining their synergistic effects. Bismuth nanosheets optimize zinc deposition behavior, while antimony nanosheets inhibit hydrogen evolution reaction. Simultaneously, the combination of ball milling and polymer dispersion system ensures efficient exfoliation and stable dispersion of the nanosheets.

[0053] Through the above technical solutions, this application effectively reduces the local current density of the zinc powder anode, suppresses the vertical growth of dendrites, and reduces the formation of a passivation layer on the electrode surface. The three-dimensional conductive network constructed by the modified nanosheets maintains stable electrical contact between zinc powder particles, preventing the shedding of active material during cycling. The polymer residue layer on the nanosheet surface improves the stability of the electrode / electrolyte interface and slows down the chemical corrosion rate of the zinc powder. By controlling the composite ratio of bismuth and antimony nanosheets, the hydrogen evolution reaction barrier is significantly improved while ensuring the uniformity of zinc deposition, ultimately achieving a substantial improvement in the cycling stability of the zinc powder anode.

[0054] In this invention, grinding beads refer to hard media used for mechanical grinding, specifically zirconia or steel balls, which achieve layered exfoliation of metal powder through shear force generated by collision. Centrifugal separation refers to a separation method utilizing the density difference of different substances, specifically using equipment with a rotation speed range of 3000-10000 rpm, to effectively remove unexfoliated metal particles and free polymers. Ultrasonic dispersion washing refers to utilizing the cavitation effect of high-frequency sound waves, specifically using ultrasonic equipment with a frequency of 20-40 kHz, to remove polymer residues adsorbed on the surface of nanosheets.

[0055] In this invention, "scraping" refers to the process of uniformly coating the slurry onto the surface of the current collector, which can be achieved using a scraper or a coating machine. By controlling the coating thickness, a tight bond is achieved between the zinc powder active layer and the current collector, reducing interfacial contact resistance. After the composite zinc powder negative electrode slurry is uniformly coated onto the current collector surface, the binder forms a cross-linked network during the drying process, fixing the distribution of zinc powder and modified nanosheets, thus creating continuous electron conduction paths between the zinc powder particles. Modified bismuth or antimony nanosheets are embedded in the gaps between the zinc powder particles, suppressing side reactions by increasing the hydrogen evolution overpotential and simultaneously regulating zinc ion deposition behavior.

[0056] In this invention, the current collector refers to the conductive substrate that carries the active material. Specifically, it can be made of zinc substrate, titanium foil, copper foil or graphene material. It promotes charge transport and suppresses interfacial side reactions through high conductivity and chemical stability.

[0057] In this invention, during the preparation of modified bismuth nanosheets, the mass ratio of bismuth powder to polyvinylpyrrolidone is 1-10:1, preferably 1.5-5:1. During the preparation of modified antimony nanosheets, the mass ratio of antimony powder to polyvinylpyrrolidone is 1-10:1, preferably 1.5-5:1.

[0058] In this invention, PVA is polyvinyl alcohol, HEC is hydroxyethyl cellulose, PAAS is sodium polyacrylate, HPMC is hydroxypropyl methylcellulose, PEO is polyethylene oxide, CMC is carboxymethyl cellulose, SBR is styrene-butadiene rubber, PVDF is polyvinylidene fluoride, PTFE is polytetrafluoroethylene, and NMP is N-methyl-2-pyrrolidone. All of the above substances are used as binders in this application and are mature commercially available products in the prior art.

[0059] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0060] 1. The composite zinc powder anode slurry provided by the present invention effectively suppresses dendrite growth, hydrogen evolution and corrosion caused by the high specific surface area of ​​zinc powder anode by adding bismuth nanosheets and / or antimony nanosheets, improves the reversibility of zinc deposition and dissolution, and extends the cycle life of the battery.

[0061] 2. The technical solution of this invention solves the problem of short cycle life of zinc powder anodes caused by interface corrosion, hydrogen evolution and contact failure. It achieves stable bonding between zinc powder active material and current collector, forming a uniform ion / electron conduction network, inhibiting zinc dendrite growth, reducing dead zinc production, and thus improving the cycle stability of aqueous zinc metal batteries.

[0062] 3. The technical solution of the present invention has a simple process and strong operability in the preparation process, which can realize the large-scale and low-cost preparation of composite zinc powder anodes, and is suitable for industrial production. Attached Figure Description

[0063] Figure 1 This is a morphology diagram of the composite zinc powder negative electrode slurry prepared in Example 3 of the present invention;

[0064] Figure 2 The conductivity test graphs are for the composite zinc powder anodes prepared in Examples 1, 2, and 3 of this invention and the zinc powder anodes prepared in Comparative Example 2 (the horizontal axis represents the mass percentage of bismuth and / or antimony added in the composite zinc powder anode slurry used to prepare the composite zinc powder anode).

[0065] Figure 3 The graph shows the coulombic efficiency performance of the composite zinc powder anode asymmetric battery prepared in Application Example 3 and Comparative Example 1 of this invention.

[0066] Figure 4 The graphs show the performance testing results of the composite zinc powder negative electrode symmetric batteries prepared in Application Example 3 and Comparative Example 1 of this invention. Detailed Implementation

[0067] The technical solution of the present invention will be illustrated below with examples. The scope of protection sought by the present invention includes, but is not limited to, the following embodiments.

[0068] The sources of raw materials used in the embodiments of this invention are as follows:

[0069] Bismuth powder was purchased from Suzhou Luofei Nanotechnology Co., Ltd. Antimony powder was purchased from Suzhou Luofei Nanotechnology Co., Ltd. Polyvinylpyrrolidone (PVP, K-30) was purchased from Sinopharm Chemical Reagent Co., Ltd. Zinc powder (600 mesh, purity ≥99.99%) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. PVDF 900 (purity ≥99.5%) binder was purchased from Guangdong Zhuguang New Energy Technology Co., Ltd. GF / D glass fiber diaphragm was purchased from Whatman Ltd., UK (CAT No. 1823-090).

[0070] Preparation Example 1

[0071] Preparation of modified bismuth nanosheets:

[0072] (1) Weigh 100g of polyvinylpyrrolidone (PVP) and add it to 500mL of isopropanol. Stir and dissolve until completely dissolved and transparent.

[0073] (2) Weigh 200g of bismuth powder, 1000g of zirconia ball milling beads with a particle size distribution of 0.6-0.8mm and the pre-dissolved PVP solution and add them to a 2000mL zirconia ball milling jar. Use a planetary ball mill to continuously ball mill for 24 hours and then open the jar to take a sample.

[0074] (3) Centrifuge the ball-milled solution at 1000 r / min for 5 min to remove the bismuth powder that has not been fully stripped;

[0075] (4) Centrifuge three times at a speed of 10,000 r / min to remove excess PVP from the solution;

[0076] (5) After the centrifugation process is completed, the bismuth nanosheets after secondary purification are added to deionized water for ultrasonic dispersion, and then the aqueous dispersion of bismuth nanosheets is freeze-dried under vacuum to obtain modified bismuth nanosheet powder.

[0077] Preparation Example 2

[0078] Preparation of modified antimony nanosheets:

[0079] (1) Weigh 100g of polyvinylpyrrolidone (PVP) and add it to 500mL of isopropanol. Stir and dissolve until completely dissolved and transparent.

[0080] (2) Weigh 200g of antimony powder, 1000g of zirconia grinding beads with a particle size distribution of 0.6-0.8mm and pre-dissolved PVP solution and add them to a 100mL zirconia grinding jar. Use a planetary ball mill to continuously grind for 24 hours and then open the jar to take a sample.

[0081] (3) Centrifuge the ball-milled solution at 1000 r / min for 5 min to remove the antimony powder that has not been fully stripped;

[0082] (4) Centrifuge three times at a speed of 10,000 r / min to remove excess PVP from the solution;

[0083] (5) After the centrifugation process is completed, the antimony nanosheets after secondary purification are added to deionized water for ultrasonic dispersion, and then the aqueous dispersion of antimony nanosheets is freeze-dried under vacuum to obtain modified antimony nanosheet powder.

[0084] Example 1

[0085] Zinc powder, the modified bismuth nanosheets obtained in Example 1, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:8:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain composite zinc powder anode I. The mass loading of elemental zinc powder in the composite zinc powder anode was 13.5 mg / cm³. -2 .

[0086] Example 2

[0087] Zinc powder, the modified antimony nanosheets obtained in Preparation Example 2, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:8:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain composite zinc powder anode II. The mass loading of elemental zinc powder in the composite zinc powder anode was 13.1 mg / cm³. -2 .

[0088] Example 3

[0089] Zinc powder, modified bismuth nanosheets obtained in Preparation Example 1, modified antimony nanosheets obtained in Preparation Example 2, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:6:2:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain composite zinc powder anode III. The mass loading of elemental zinc powder in the composite zinc powder anode was 13.4 mg / cm³. -2 .

[0090] Example 4

[0091] Zinc powder, modified bismuth nanosheets obtained in Preparation Example 1, modified antimony nanosheets obtained in Preparation Example 2, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:3:5:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain composite zinc powder anode IV. The mass loading of elemental zinc powder in the composite zinc powder anode was 13.1 mg / cm³. -2 .

[0092] Example 5

[0093] Zinc powder, modified bismuth nanosheets obtained in Example 1, modified antimony nanosheets obtained in Example 2, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:4:4:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain the composite zinc powder anode V. The mass loading of elemental zinc powder in the composite zinc powder anode was 13.2 mg / cm³. -2 .

[0094] Example 6

[0095] Zinc powder, modified bismuth nanosheets obtained in Preparation Example 1, modified antimony nanosheets obtained in Preparation Example 2, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:7:1:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain composite zinc powder anode VI. The mass loading of elemental zinc powder in the composite zinc powder anode was 13.4 mg / cm³. -2 .

[0096] Example 7

[0097] Zinc powder, modified bismuth nanosheets obtained in Preparation Example 1, modified antimony nanosheets obtained in Preparation Example 2, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 85:8:5:2, followed by vigorous stirring for 12 hours to ensure thorough mixing; a composite zinc powder anode slurry was obtained. The mixed slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain composite zinc powder anode VII. The mass loading of elemental zinc powder in the composite zinc powder anode was 12.9 mg / cm³. -2 .

[0098] Comparative Example 1

[0099] Zinc powder and PVDF binder were mixed at a mass ratio of 98:2 in N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent, followed by vigorous stirring for 12 hours to ensure thorough mixing, thus obtaining a zinc powder anode slurry. The slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain the zinc powder anode DI. The mass loading of elemental zinc powder in the zinc powder anode was 14.2 mg / cm³. -2 .

[0100] Comparative Example 2

[0101] Zinc powder, bismuth powder, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:8:2, followed by vigorous stirring for 12 hours to ensure thorough mixing, thus obtaining a composite zinc powder anode slurry. The slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain the composite zinc powder anode D-II. The mass loading of elemental zinc powder in the composite zinc powder anode was 12.9 mg / cm³. -2 .

[0102] Comparative Example 3

[0103] Zinc powder, antimony powder, and PVDF binder were mixed in an N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent at a mass ratio of 90:8:2, followed by vigorous stirring for 12 hours to ensure thorough mixing, thus obtaining a composite zinc powder anode slurry. The slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain the composite zinc powder anode D-III. The mass loading of elemental zinc powder in the composite zinc powder anode was 12.8 mg / cm³. -2 .

[0104] Comparative Example 4

[0105] Zinc powder, bismuth powder, antimony powder, and PVDF binder were mixed in a mass ratio of 90:6:2:2 in N-methylpyrrolidone (NMP, analytical grade, Aladdin reagent) solvent, followed by vigorous stirring for 12 hours to ensure thorough mixing, thus obtaining a composite zinc powder anode slurry. The slurry was then coated onto titanium foil using a doctor blade and dried overnight under vacuum at 80°C to obtain the composite zinc powder anode D-IV. The mass loading of elemental zinc powder in the composite zinc powder anode was 12.9 mg / cm³. -2 .

[0106] Performance Test 1

[0107] The composite zinc powder anode III prepared in Example 3 was immersed in a 2M ZnSO4 aqueous electrolyte for 24 hours, then removed; the corrosion of the electrode was examined, and the scanning electron microscope image of the electrode is shown below. Figure 1 As shown, there is a uniform distribution of zinc, bismuth, and antimony, and no obvious corrosion products are generated, indicating that the composite zinc powder anode prepared by the technical solution of this invention has excellent corrosion resistance.

[0108] Performance Test 2

[0109] The conductivity of the composite zinc powder anode I prepared in Example 1, the composite zinc powder anode II prepared in Example 2, the composite zinc powder anode III prepared in Example 3, and the composite zinc powder anode D-II prepared in Comparative Example 2 were tested according to GB / T 351-2019. Furthermore, according to their respective technical solutions, the amounts of bismuth nanosheets, antimony nanosheets, and bismuth powder added to the composite zinc powder anode slurry were adjusted to prepare composite zinc powder anodes with different addition amounts, and the conductivity results of each were tested as follows: Figure 2 As shown in the figure, characterization revealed that the addition of bismuth nanosheets, antimony nanosheets, and bismuth powder all affected the conductivity of the prepared composite zinc powder anode. Among the composite zinc powder anodes, the composite zinc powder anode prepared by simultaneously adding bismuth nanosheets and antimony nanosheets exhibited the best conductivity, followed by the composite zinc powder anode prepared by adding antimony nanosheets, and then the composite zinc powder anode prepared by adding bismuth nanosheets. The composite zinc powder anode prepared by adding bismuth powder had the worst conductivity. Furthermore, the test results also showed that the amount of bismuth nanosheets, antimony nanosheets, or bismuth powder added also affected the conductivity of the composite zinc powder anode; as the amount of bismuth nanosheets, antimony nanosheets, or bismuth powder added increased, the conductivity of the composite zinc powder anode decreased.

[0110] Performance Test 3

[0111] Using the composite zinc powder anode III and copper foil prepared above as the two electrodes of the battery, and employing 2M ZnSO4 aqueous electrolyte and selected GF / D glass fiber as the separator, a zinc / copper half-cell was assembled and its cycle performance was tested. Using the composite zinc powder anode DI and copper foil prepared above as the two electrodes of the battery, and employing 2M ZnSO4 aqueous electrolyte and selected GF / D glass fiber as the separator, a zinc / copper half-cell was assembled and its cycle performance was tested. Its cycle performance is as follows: Figure 3 As shown, at 1mAh cm -2 and 1mA cm -2 Under the test parameters and with a depth of discharge (DOD) of 10%, the battery prepared using composite zinc powder anode III as the anode still maintained stable performance after 120 hours of cycling, while the battery prepared using composite zinc powder anode DI as the anode experienced more severe corrosion and "dead zinc" at low current, causing voltage polarization in the discharge curve after 45 hours of cycling.

[0112] Performance Test 4

[0113] A symmetrical battery was assembled using the composite zinc powder anode III prepared above as both electrodes. A 2M ZnSO4 aqueous electrolyte and GF / D glass fiber were selected as the separator. Cyclic performance tests were then conducted on the assembled zinc symmetrical battery. Similarly, a symmetrical battery was assembled using the composite zinc powder anode DI prepared above as both electrodes. A 2M ZnSO4 aqueous electrolyte and GF / D glass fiber were selected as the separator. The cycle performance was as follows: Figure 4 As shown, at 0.5mAh cm -2 and 2.5mA cm -2 Under the test parameters, the battery prepared using composite zinc powder anode III as the anode can still operate stably after 70 hours of cycling, while the battery prepared using composite zinc powder anode DI as the anode fails due to electrode corrosion and passivation, and the assembled symmetrical battery fails after less than 7 hours of operation due to voltage curve polarization.

[0114] Performance Test 5

[0115] The composite zinc powder anodes I to VII prepared in Examples 1-7 and the zinc powder anodes (or composite zinc powder anodes) DI to D-IV prepared in Comparative Examples 1-4 were used as anodes, manganese dioxide as cathode, 2M ZnSO4 aqueous electrolyte, and GF / D glass fiber as separator to assemble zinc / manganese dioxide full cells. After standing for 12 hours, the capacity retention was tested under test mode for 300 cycles. The results are shown in the table below.

[0116]

[0117] Through testing and analysis, the composite zinc powder anode slurry obtained by the technical solution of this invention, with the addition of bismuth nanosheets and / or antimony nanosheets to the slurry, can effectively inhibit the corrosion and side reactions of zinc powder. Moreover, as zinc-loving sites, it can construct a uniform electric field distribution and improve the capacity stability of the battery.

Claims

1. A composite zinc powder negative electrode slurry, characterized in that: The composite zinc powder includes: The zinc powder comprises 80-99 parts by weight, preferably 82-98 parts by weight, and more preferably 85-95 parts by weight; 1-20 parts by weight of modified bismuth nanosheets and / or modified antimony nanosheets, preferably 3-15 parts by weight, more preferably 5-10 parts by weight; The adhesive is used in amounts of 0.5-10 parts by weight, preferably 0.8-8 parts by weight, and more preferably 1-5 parts by weight.

2. The composite zinc powder negative electrode slurry according to claim 1, characterized in that: The composite zinc powder comprises: 85-95 parts by weight of zinc powder, 4-7 parts by weight of modified bismuth nanosheets, 1-4 parts by weight of modified antimony nanosheets, and 1-5 parts by weight of binder.

3. The composite zinc powder negative electrode slurry according to claim 1 or 2, characterized in that: Modified bismuth nanosheets were prepared by the following method: dissolving polyvinylpyrrolidone in an organic solvent, adding bismuth powder, grinding, and separating to obtain bismuth nanosheets; and / or The modified antimony nanosheets were prepared by the following method: polyvinylpyrrolidone was dissolved in an organic solvent, antimony powder was added, and the mixture was ground and separated to obtain antimony nanosheets.

4. The composite zinc powder negative electrode slurry according to claim 3, characterized in that: The organic solvent is selected from isopropanol, ethanol, methanol, N,N-dimethylformamide, ethylene glycol, or N-methylpyrrolidone; preferably, the mass concentration of polyvinylpyrrolidone dissolved in the organic solvent is 10-30%; and / or The grinding is ball milling; and / or The separation is achieved through sedimentation, filtration, or centrifugation.

5. The composite zinc powder negative electrode slurry according to any one of claims 1-4, characterized in that: The zinc powder has a particle size of 400-30000 mesh; the purity of the zinc powder is greater than 99%; and / or The adhesive is selected from at least one of PVA, HEC, PAAS, HPMC, PEO, CMC, SBR, PVDF, PTFE, and NMP.

6. A method for preparing the composite zinc powder negative electrode slurry according to any one of claims 1-5, the method comprising the following steps: S1. Preparation of modified bismuth nanosheets: Polyvinylpyrrolidone was added to an organic solvent and stirred to dissolve, obtaining a polymer-assisted exfoliation solution; bismuth powder and polymer-assisted exfoliation solution were mixed, ball-milled, separated, and dried to obtain modified bismuth nanosheets; S2. Preparation of modified antimony nanosheets: Polyvinylpyrrolidone was added to an organic solvent and stirred to dissolve, obtaining a polymer-assisted exfoliation solution; antimony powder and polymer-assisted exfoliation solution were mixed, ball-milled, separated, and dried to obtain modified antimony nanosheets; S3. Preparation of composite zinc powder anode slurry: Zinc powder, modified bismuth nanosheets, modified antimony nanosheets, and binder are mixed, solvent is added, and the mixture is stirred to obtain composite zinc powder anode slurry.

7. The method according to claim 6, characterized in that: The organic solvents mentioned in steps S1 and S2 are selected from any one of isopropanol, ethanol, methanol, N,N-dimethylformamide, ethylene glycol, or N-methylpyrrolidone; and / or The adhesive mentioned in step S3 is selected from at least one of PVA, HEC, PAAS, HPMC, PEO, CMC, SBR, PVDF, and PTFE; the solvent is selected from at least one of N-methylpyrrolidone, water, acetone, propylene carbonate, dimethylformamide, cyclohexanone, or methyl ethyl ketone.

8. The method according to claim 6 or 7, characterized in that: Step S1 specifically involves: weighing polyvinylpyrrolidone and adding it to an organic solvent, stirring and dissolving until completely dissolved and transparent, obtaining a polymer-assisted exfoliation solution; then, adding bismuth powder, milling beads, and the polymer-assisted exfoliation solution to a ball mill jar, and ball milling; centrifuging to remove insufficiently exfoliated bismuth powder and excess polyvinylpyrrolidone; ultrasonically dispersing, washing, and drying to obtain modified bismuth nanosheets; and / or Step S2 is as follows: Weigh polyvinylpyrrolidone and add it to an organic solvent, stirring and dissolving until completely dissolved and transparent to obtain a polymer-assisted exfoliation solution; then, add antimony powder, milling beads and polymer-assisted exfoliation solution to a ball mill jar and ball mill; centrifuge to remove insufficiently exfoliated antimony powder and excess polyvinylpyrrolidone; ultrasonically disperse, wash and dry to obtain modified antimony nanosheets.

9. A composite zinc powder negative electrode, characterized in that: The composite zinc powder anode slurry of any one of claims 1-5 or the composite zinc powder anode slurry prepared by any one of claims 6-8 is scraped onto the current collector and dried to obtain the composite zinc powder anode. Preferably, the current collector is selected from one of zinc matrix, titanium foil, copper foil, and graphene current collector.

10. An aqueous zinc metal battery, characterized in that, The aqueous zinc metal battery includes the composite zinc powder negative electrode, positive electrode, separator, and electrolyte as described in claim 9; Preferably, the positive electrode is selected from manganese-based compounds (preferably MnO2, Mn2O2, Mn3O4) and vanadium-based compounds (preferably V2O5, VO2, V2O3, V6O4). 13 One of the following: halogen cathode (preferably Br2, I2); and / or The diaphragm is selected from one of glass fiber diaphragms and cellulose diaphragms; and / or The electrolyte is selected from one of ZnSO4, ZnCI2, Zn(CF3SO3)2, and Zn(ClO4)2 electrolytes.

Citation Information

Patent Citations

  • Nitrogen-doped carbon-coated zinc powder negative electrode applied to zinc ion battery as well as preparation and application of nitrogen-doped carbon-coated zinc powder negative electrode

    CN115810708A

  • Zinc-based composite powder material as well as preparation method and application thereof

    CN116454221A

  • Gradient flexible zinc powder negative electrode material, preparation method and battery

    CN116759565A

  • Zinc powder negative electrode material, preparation method thereof and zinc ion battery

    CN118472159A

  • (002) crystal face oriented zinc powder negative electrode material as well as preparation method and application thereof

    CN119407158A