A polymer coating for lithium metal anode based on in-situ polymerization and its preparation method and application
By using a polymer coating formed by in-situ polymerization on the surface of lithium metal batteries, a continuous network is constructed using chemical bonds and ionic crosslinking agents, which solves the problem of lithium dendrite growth and achieves high cycle stability and safety of lithium anodes.
Patent Information
- Application Number
- CN202611314841.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, the random growth of lithium dendrites leads to reduced cycle life and safety risks in lithium metal batteries. Existing polymer coatings cannot simultaneously achieve a balance between tight chemical bonding, flexible volume adaptation, and uniform ion conduction.
A coating is formed on the surface of a lithium metal anode by in-situ polymerization of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine. A continuous ion transport network is constructed through O-Li and N-Li chemical bonds and ionic crosslinking agents to enhance interfacial bonding and uniform ion diffusion.
Chemical bonding between the lithium anode coating and the lithium substrate was achieved, which suppressed dendrite growth, improved cycle stability and safety, and achieved a capacity retention of 62%. No short circuits occurred during cycling, and the coating maintained its integrity during long-term cycling.
Smart Images

Figure SMS_4 
Figure SMS_5 
Figure SMS_6
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, and in particular to a metal lithium anode polymer coating based on in-situ polymerization, its preparation method, and its application. Background Technology
[0002] Lithium metal possesses extremely high theoretical specific capacity and the lowest standard electrode potential, making it an ideal core anode material for next-generation high-energy-density batteries (such as lithium metal batteries and lithium-sulfur batteries). However, the random growth of lithium dendrites during charging can puncture the separator, causing short circuits, and exacerbate side reactions with the electrolyte, leading to a sharp drop in cycle life, which seriously hinders its commercialization.
[0003] To address the lithium dendrite problem, in-situ polymerization to construct artificial interface layers has become an important approach in this field. Existing technologies often employ a "single flexible diacrylate monomer + thermal initiator" system to form a polymer coating on the lithium metal surface through in-situ polymerization. For example, polyethylene glycol diacrylate (PEGDA) or diethylene glycol diacrylate (DEGDA) can be used as monomers, and azobisisobutyronitrile (AIBN) as an initiator to form a cross-linked network coating on the lithium surface through in-situ polymerization. These techniques utilize the flexible segments of the diacrylate to adapt to changes in lithium volume and leverage its C=O and C–O polar groups to promote lithium-ion migration.
[0004] However, the above-mentioned single flexible diacrylate system has the following technical defects: 1. The segments of the flexible diacrylate monomer (such as PEGDA) only interact with the lithium surface through weak physical adsorption and cannot form chemically bonded strong polar / bonding functional groups with lithium. During cycling, the coating is easy to peel off from the lithium substrate; 2. Such monomers do not contain ionic functional groups and rely only on the dipole interaction of neutral C=O and C–O groups to conduct lithium. They cannot build a continuous ion transport network, resulting in uneven distribution of lithium ions at the interface, local current concentration and dendrite induction; 3. The cross-linked network formed by a single monomer is difficult to balance mechanical strength, volumetric flexibility and ion conduction.
[0005] Therefore, providing a polymer coating that can simultaneously achieve tight chemical bonding, flexible volume adaptation, and uniform ion conduction on the surface of lithium metal remains a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0006] In view of this, the present invention proposes a polymer coating for lithium metal anodes based on in-situ polymerization, its preparation method, and its application, thereby solving the above-mentioned problems. The technical solution of the present invention is implemented as follows: A polymer coating for a lithium metal anode based on in-situ polymerization, characterized in that it is formed by in-situ polymerization of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine on the surface of a lithium metal anode; The mass ratio of polycaprolactone diacrylate, N-hydroxymethylacrylamide, and N,N'-bis(acryloyl)cystamine is 12-120:20-40:5-15.
[0007] The structural formula of the monomer polycaprolactone diacrylate of this invention is as follows: .
[0008] The structural formula of the monomer N-hydroxymethylacrylamide of this invention is as follows: .
[0009] The structural formula of the monomer N,N'-bis(acryloyl)cystamine of the present invention is as follows: .
[0010] The three monomers of this invention each have their own functional roles, are non-substitutable, and indispensable, forming a ternary synergistic effect. Specifically: Polycaprolactone diacrylate, as a flexible monomer, has flexible segments that work together with carbonate and ether-based lithium-conducting units in the molecular chain to adapt to volume changes during lithium deposition / stripping and to provide a basic ion transport path; N-hydroxymethylacrylamide, as a polar monomer, has hydroxyl and amide groups that react with the lithium surface to generate O-Li and N-Li chemical bonds, enabling the coating to form a chemical bond with the lithium substrate and become integrated, fundamentally avoiding interface stripping; N,N'-bis(acryloyl)cysteine, as an ionic crosslinking agent, enhances the mechanical strength of the coating through crosslinking and introduces lithium-ion functional groups to construct a continuous ion transport network, reducing interface impedance, guiding uniform lithium ion deposition, and forcing lithium to undergo layered deposition instead of dendritic growth.
[0011] Furthermore, the number average molecular weight of the polycaprolactone diacrylate is 500-5000.
[0012] Furthermore, the number average molecular weight of the polycaprolactone diacrylate is 1000.
[0013] The polyester skeleton in the polycaprolactone diacrylate of this invention is resistant to swelling and has stable interface over long cycles. It is significantly superior to the existing polyethylene glycol diacrylate (PEGDA) system in terms of swelling rate, impedance growth rate and coating integrity after cycling.
[0014] Furthermore, the thickness of the polymer coating is 5-15 μm.
[0015] A method for preparing a polymer coating for a lithium metal anode based on in-situ polymerization, the specific preparation steps of which include: S1. Polycaprolactone diacrylate, N-hydroxymethylacrylamide, N,N'-bis(acryloyl)cysteine and initiator are added to an organic solvent and stirred to obtain a precursor solution; S2. Under an inert atmosphere, the lithium metal anode is introduced into the precursor solution and stirred to react, so that the surface of the lithium metal anode polymerizes in situ to form a coating. The coating is then removed, washed, and dried to obtain the lithium metal anode polymer coating.
[0016] Furthermore, in step S1, the organic solvent is dimethyl carbonate or ethylene glycol dimethyl ether, with a water content of <10 ppm.
[0017] The ethylene glycol dimethyl ether of this invention has good compatibility with lithium surfaces, which can reduce side reactions during polymerization and improve monomer solubility. It is suitable for low-temperature scenarios and can still polymerize to form a uniform coating at -20°C, thus improving low-temperature cycling performance.
[0018] Furthermore, in step S1, the initiator is azobisisobutyronitrile, and its mass is 0.09%-0.5% of the total mass of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine.
[0019] The initiation method of the present invention can also be ultraviolet light-assisted in-situ polymerization, which is initiated by irradiating with 365nm ultraviolet light (power 10 W) for 1 hour in an argon glove box.
[0020] Furthermore, in step S1, the total mass concentration of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine in the precursor solution is 5-16 wt%.
[0021] Furthermore, in step S2, the stirring reaction is carried out at 20-40°C and 250-350 rpm for 0.5-3 hours.
[0022] Application of an in-situ polymer coating for lithium metal anodes in lithium metal batteries.
[0023] Compared with the prior art, the beneficial effects of the present invention are: 1. The polymer coating for the lithium metal anode of this invention is formed by in-situ polymerization of three monomers on the surface of the lithium metal anode. It exhibits strong interfacial bonding; the polar monomers form O-Li and N-Li chemical bonds with the lithium surface, chemically bonding the coating to the lithium substrate and resulting in high interfacial peel strength, fundamentally preventing interfacial peeling during cycling. It also provides uniform ion conduction and excellent dendrite suppression. The ionic crosslinking agent constructs a continuous ion transport network, reducing interfacial impedance and guiding lithium ions to diffuse uniformly to the lithium surface, achieving layered deposition instead of dendrite growth. Simultaneously, it blocks direct contact between the electrolyte and lithium, reducing side reactions. The flexible monomers, polar monomers, and ionic crosslinking agent complement each other, as neither single-component nor two-component systems can simultaneously achieve interfacial bonding, volume adaptation, and ion conduction. Test examples verify that the lithium metal anode modified with the polymer coating of this invention maintains a capacity retention of 62% after 600 cycles at 1C rate, with no short circuits observed during cycling, significantly improving the cycling stability and safety of the lithium metal anode.
[0024] 2. The polycaprolactone diacrylate of the present invention has a number average molecular weight of 500-5000. When the number average molecular weight is 500, although the cycle capacity retention rate is high, the discharge specific capacity decreases significantly. When the number average molecular weight is 5000, the cycle capacity retention rate decreases. Only when the number average molecular weight is 1000 does the coating achieve the optimal balance between cycle capacity retention rate and discharge specific capacity.
[0025] 3. The process of this invention is simple and low-cost. It adopts normal temperature and pressure reaction conditions, requires no complicated equipment, meets the needs of industrial mass production, and has good application prospects. Detailed Implementation
[0026] To better understand the technical content of this invention, specific embodiments are provided below to further illustrate the invention.
[0027] Unless otherwise specified, the experimental methods used in the embodiments of this invention are all conventional methods.
[0028] Unless otherwise specified, all materials and reagents used in the embodiments of this invention are commercially available.
[0029] The lithium foil of this invention has a thickness of 50 μm, a purity of 99.99%, and no oxide spots on its surface.
[0030] Example 1 A method for preparing a polymer coating for a lithium metal anode based on in-situ polymerization, the specific preparation steps of which include: S1. Add 60 mg of polycaprolactone diacrylate (number average molecular weight Mn of 1000), 30 mg of N-hydroxymethylacrylamide, 10 mg of N,N'-bis(acryloyl)cystamine and 0.15 mg of azobisisobutyronitrile to 900 mg of dimethyl carbonate (water content <10 ppm), and stir for 20 min in an argon glove box (water and oxygen content <0.1 ppm) to obtain the precursor solution; S2. Cut lithium foil into 15 mm diameter electrode sheets, wipe the surface twice with dimethyl carbonate to remove residual oil, and let it stand for 5 min in an argon glove box (water oxygen content < 0.1 ppm) to obtain lithium electrode sheets. Immerse them completely in the precursor solution and react with magnetic stirring at 25℃ and 300 rpm for 2 h. A milky white uniform coating gradually forms on the lithium surface. Remove the lithium electrode sheets, rinse the surface with dimethyl carbonate, and dry them in a vacuum drying oven at 40℃ for 1 h to obtain a metallic lithium anode with a surface polymer coating thickness of 8 μm.
[0031] Example 2 Based on Example 1, the number-average molecular weight Mn of polycaprolactone diacrylate was adjusted to 5000.
[0032] Specifically, in step S1, 12 mg of polycaprolactone diacrylate (number average molecular weight Mn of 5000), 30 mg of N-hydroxymethylacrylamide, 10 mg of N,N'-bis(acryloyl)cysteine and 0.15 mg of azobisisobutyronitrile were added to 900 mg of dimethyl carbonate (water content <10 ppm), and stirred for 20 min in an argon glove box (water and oxygen content <0.1 ppm) to obtain the precursor solution; Everything else is the same as in Example 1.
[0033] Example 3 Based on Example 1, the number-average molecular weight Mn of polycaprolactone diacrylate was adjusted to 500.
[0034] Specifically, in step S1, 120 mg of polycaprolactone diacrylate (number average molecular weight Mn of 500), 30 mg of N-hydroxymethylacrylamide, 10 mg of N,N'-bis(acryloyl)cysteine and 0.15 mg of azobisisobutyronitrile were added to 900 mg of dimethyl carbonate (water content <10 ppm), and stirred for 20 min in an argon glove box (water and oxygen content <0.1 ppm) to obtain the precursor solution; Everything else is the same as in Example 1.
[0035] Application Example 1 Using lithium metal with a polymer coating prepared in Example 1 as the negative electrode, and with NCM811 / NCM955 high-nickel positive electrode (nickel content > 80%), Celgard 2325 separator, and 1 mol / L LiPF6-EC / DEC (volume ratio 1:1, containing 2-5% fluoroethylene carbonate) electrolyte, CR2032 coin-type lithium metal batteries were assembled in an argon glove box (water and oxygen content < 0.1 ppm).
[0036] Application Example 2 Using lithium metal with a surface polymer coating prepared in Example 2 as the negative electrode, and with NCM811 / NCM955 high-nickel positive electrode (nickel content > 80%), Celgard 2325 separator, and 1 mol / L LiPF6-EC / DEC (volume ratio 1:1, containing 2-5% fluoroethylene carbonate) electrolyte, a CR2032 coin cell lithium metal battery was assembled in an argon glove box (water and oxygen content < 0.1 ppm).
[0037] Application Example 3 Using lithium metal with a surface polymer coating prepared in Example 3 as the negative electrode, and with NCM811 / NCM955 high-nickel positive electrode (nickel content > 80%), Celgard 2325 separator, and 1 mol / L LiPF6-EC / DEC (volume ratio 1:1, containing 2-5% fluoroethylene carbonate) electrolyte, a CR2032 coin cell lithium metal battery was assembled in an argon glove box (water and oxygen content < 0.1 ppm).
[0038] Test Example 1 The CR2032 coin cell lithium metal batteries obtained in Examples 1-3 were subjected to charge-discharge cycles at a 1C rate and a voltage range of 2.5-4.3 V for performance testing. The results are shown in Table 1.
[0039] Table 1
[0040] As can be seen from Table 1, the number-average molecular weight Mn of the monomer polycaprolactone diacrylate of the present invention has a significant nonlinear effect on the rate capability and cycle performance of the modified interface coating. When Mn=500, the chain is short and the crosslinking density is high, which is beneficial to maintaining the capacity retention rate but hinders ion migration, resulting in a significant decrease in discharge specific capacity. When Mn=5000, the chain is too long and the crosslinking density is insufficient, resulting in a decrease in mechanical strength and a decrease in cycle capacity retention rate. When Mn=1000, the optimal balance is achieved between flexible chain segments, crosslinking density and ion conduction, resulting in excellent discharge specific capacity while maintaining a high cycle capacity retention rate.
[0041] Furthermore, after cycling, the CR2032 coin lithium metal batteries obtained in Examples 1-3 were observed by scanning electron microscopy, and the lithium surface showed a uniform layered deposition morphology with no obvious dendrites.
[0042] Application Comparative Example 1 The difference from Application Example 1 is that only polycaprolactone diacrylate is used, and N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine are missing; otherwise, they are the same as Application Example 1.
[0043] Application Comparative Example 2 The difference from Application Example 1 is that N,N'-bis(acryloyl)cystamine is missing, otherwise it is the same as Application Example 1.
[0044] Application Comparative Example 3 The difference from Application Example 1 is that polycaprolactone diacrylate is replaced with polyethylene glycol diacrylate, otherwise it is the same as Application Example 1.
[0045] Application Comparative Example 4 Blank control, with bare lithium metal as the negative electrode.
[0046] Test Example 2 The CR2032 coin cell lithium metal batteries obtained in Application Example 1 and Comparative Examples 1-4 were subjected to charge-discharge cycles at a 1C rate and a voltage range of 2.5-4.3 V for performance testing. The results are shown in Table 2.
[0047] Table 2
[0048] As can be seen from Table 2, in Application Example 1 of the present invention, the capacity retention rate can reach 62% after 600 cycles at 1C rate, and no short circuit phenomenon occurred during the cycle, which significantly improves the cycle stability and safety of lithium metal anode.
[0049] Comparative Example 1 lacks N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine. The coating only exhibits physical adsorption with the lithium surface and lacks O-Li / N-Li chemical bonds, resulting in low interfacial peel strength. In addition, it lacks a continuous ion transport network, leading to uneven lithium ion distribution. The capacity retention rate is only about 40% after 600 cycles, and a short circuit occurs after about 450 cycles. After cycling, the lithium surface exhibits dendritic uneven deposition.
[0050] Comparative Example 2, lacking N,N'-bis(acryloyl)cysteine, failed to construct a continuous ion transport network in its coating, resulting in increased interfacial impedance, uneven lithium-ion distribution, and a capacity retention of approximately 46% after 600 cycles. Localized uneven deposition of lithium ions appeared on the lithium surface after cycling. This indicates that N,N'-bis(acryloyl)cysteine plays a crucial role in reducing interfacial impedance, guiding uniform lithium-ion deposition, and inhibiting dendrite growth.
[0051] The bare metal lithium anode battery in Comparative Example 4 exhibited significant capacity decay and short circuit after approximately 300 cycles, with a cycle life far lower than that of Application Example 1 of this invention.
[0052] Test Example 3 The batteries from Application Example 1 and Application Comparative Example 3 were tested; 1. Swelling resistance / dimensional stability: Films were formed on inert copper foil under the same conditions, immersed in 1 mol / L LiPF6-EC / DEC electrolyte, and allowed to stand at 25℃ for 24 h. The film thickness / mass change was measured, and the swelling rate (%) or thickness change (μm) was recorded. 2. Interfacial impedance before and after cycling: Electrochemical impedance spectroscopy (EIS) was measured before the first cycle and after 100 cycles. The interfacial impedance RInt was recorded, and the impedance growth rate (%) was recorded. 3. Coating integrity after cycling: After 600 cycles, the battery was disassembled and the lithium surface coating and deposition morphology were observed by SEM. Cracks / peeling, layering / dendritic formation were recorded.
[0053] The results are shown in Table 3.
[0054] Table 3
[0055] As shown in Table 3, the swelling rate of the polymer coating prepared in Application Example 1 of this invention is only 4%, significantly lower than the 14% of Application Example 3. After 100 cycles, the interfacial impedance growth rate is only 31%, far lower than the 76% of Application Example 3. After 600 cycles, the coating remains intact without cracking or peeling. In contrast, the polyether skeleton of Application Example 3 is electrolyte-loving and easily swells, resulting in significant volume expansion of the coating in the electrolyte. After cycling, local cracking and peeling occur, and the interfacial impedance increases significantly. These results indicate that this invention uses polycaprolactone diacrylate, which, due to the anti-swelling properties of its polyester skeleton, allows the polymer coating to maintain structural integrity and interfacial stability during long cycles. Therefore, it is significantly superior to the existing polyethylene glycol diacrylate system in terms of swelling rate, impedance growth rate, and coating integrity after cycling, which is beneficial for improving the cycling stability of lithium metal anodes.
[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A lithium metal anode polymer coating based on in-situ polymerization, characterized in that, It is formed by in-situ polymerization of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine on the surface of a lithium metal anode. The mass ratio of polycaprolactone diacrylate, N-hydroxymethylacrylamide, and N,N'-bis(acryloyl)cystamine is 12-120:20-40:5-15.
2. The lithium metal anode polymer coating based on in-situ polymerization as described in claim 1, characterized in that, The number average molecular weight of the polycaprolactone diacrylate is 500-5000.
3. The lithium metal anode polymer coating based on in-situ polymerization as described in claim 1, characterized in that, The number-average molecular weight of the polycaprolactone diacrylate is 1000.
4. The lithium metal anode polymer coating based on in-situ polymerization as described in claim 1, characterized in that, The thickness of the polymer coating is 5-15 μm.
5. A method for preparing a lithium metal anode polymer coating based on in-situ polymerization as described in any one of claims 1-4, characterized in that, The specific preparation steps include: S1. Polycaprolactone diacrylate, N-hydroxymethylacrylamide, N,N'-bis(acryloyl)cysteine and initiator are added to an organic solvent and stirred to obtain a precursor solution; S2. Under an inert atmosphere, the lithium metal anode is introduced into the precursor solution and stirred to react, so that the surface of the lithium metal anode polymerizes in situ to form a coating. The coating is then removed, washed, and dried to obtain the lithium metal anode polymer coating.
6. The method for preparing a lithium metal anode polymer coating based on in-situ polymerization as described in claim 5, characterized in that, In step S1, the organic solvent is dimethyl carbonate or ethylene glycol dimethyl ether, with a water content of <10 ppm.
7. The method for preparing a lithium metal anode polymer coating based on in-situ polymerization as described in claim 5, characterized in that, In step S1, the initiator is azobisisobutyronitrile, and its mass is 0.09%-0.5% of the total mass of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine.
8. The method for preparing a lithium metal anode polymer coating based on in-situ polymerization as described in claim 5, characterized in that, In step S1, the total mass concentration of polycaprolactone diacrylate, N-hydroxymethylacrylamide and N,N'-bis(acryloyl)cysteine in the precursor solution is 5-16 wt%.
9. The method for preparing a lithium metal anode polymer coating based on in-situ polymerization as described in claim 5, characterized in that, In step S2, the stirring reaction is carried out at 20-40℃ and 250-350rpm for 0.5-3h.
10. The application of the in-situ polymerization-based lithium metal anode polymer coating as described in any one of claims 1-4 in lithium metal batteries.