A positive electrode composite material and a preparation method thereof, a full-solid-state lithium battery, and an electric device

By introducing lithium halide and nitrogen-containing heterocyclic compound additives into the cathode composite material, an organic-inorganic composite CEI buffer layer with high Li⁺ conductivity and a wide electrochemical stability window is formed, which solves the interfacial stability problem between the sulfide solid electrolyte and the cathode active material, and improves the cycle stability and rate performance of the all-solid-state battery.

CN123143401APending Publication Date: 2026-11-20CHERY AUTOMOBILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611340073.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The interfacial chemistry and electrochemical stability issues between sulfide solid electrolytes and positive electrode active materials limit the performance and lifespan of all-solid-state batteries. Existing modification strategies suffer from problems such as complex processes, high costs, difficulty in ensuring interface uniformity, low Li⁺ conductivity, and increased interfacial impedance.

Method used

The cathode composite material is used, which includes cathode active material, sulfide solid electrolyte, conductive additives and functional additives. The functional additives include lithium halide and nitrogen-containing heterocyclic compounds. By coating the surface of the cathode active material with lithium halide and mixing it with nitrogen-containing heterocyclic compounds, an organic-inorganic composite CEI buffer layer with high Li⁺ conductivity, wide electrochemical stability window and mechanical flexibility is formed.

Benefits of technology

It effectively suppresses interfacial side reactions, reduces interfacial impedance, and improves the cycle stability and rate performance of all-solid-state batteries. It also improves interfacial stability and mechanical flexibility through chemical coordination and redox buffering mechanisms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143401A_ABST
    Figure CN123143401A_ABST
Patent Text Reader

Abstract

The application discloses a positive electrode composite material and a preparation method thereof, a full-solid-state lithium battery and an electric device. The positive electrode composite material comprises a positive electrode active material, a sulfide solid electrolyte, a conductive additive and a functional additive. The functional additive comprises at least one of a lithium halide additive and a nitrogen-containing heterocyclic compound additive. By introducing the specific functional additives, lithium halide salt and nitrogen-containing heterocyclic compound, into the positive electrode composite material, a composite CEI buffer layer with high Li + conductivity, a wide electrochemical stability window and good mechanical flexibility can be constructed in situ at the contact interface between the positive electrode active material particles and the sulfide solid electrolyte particles, thereby effectively inhibiting the interface side reaction, reducing the interface impedance, and improving the cycle stability and rate performance of the full-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and more specifically, to a positive electrode composite material and its preparation method, an all-solid-state lithium battery, and an electrical device. Background Technology

[0002] Sulfide solid electrolytes have become the most promising solid electrolyte system for industrialization due to their unique comprehensive performance. Although sulfide solid electrolytes have significant advantages in terms of ionic conductivity and processability, the interfacial chemistry and electrochemical stability between them and positive electrode active materials (especially high-voltage layered oxides such as NCM and LCO) have become the core technical challenges restricting the performance and lifespan of sulfide-based all-solid-state batteries.

[0003] To address the interfacial problems of sulfide solid electrolytes, academia and industry have mainly explored the following modification strategies, but all have limitations to varying degrees: (1) Coating the surface of positive electrode particles: A thin layer of oxide (such as LiNbO3, Li2ZrO3, Al2O3, Li4Ti5O3) is deposited on the surface of the positive electrode active material particles. 12 (e.g., Al2O3) is currently the most mature interface modification method, and its effectiveness has been verified in various systems. However, this method has the following problems: ① The coating process is complex, usually requiring ALD or wet chemical coating followed by high-temperature annealing, resulting in high cost, numerous steps, and difficulty in scaling up; ② The uniformity of the coating layer is difficult to guarantee, with some uncoated areas still exposed to the electrolyte; ③ Oxide coating layers (such as Al2O3, with an ionic conductivity of -10) -9 Li (S / cm) + The conductivity is much lower than that of the sulfide electrolyte bulk, introducing additional Li at the interface. + ④ The thickness of the coating layer needs to be precisely controlled, usually 2nm-10nm. Too thick a layer will significantly increase the interface impedance, while too thin a layer will have limited protective effect.

[0004] (2) Electrolyte bulk doping modification: Electrochemical stability is improved by introducing doping elements (such as halogen doping or metal ion doping) into the sulfide electrolyte bulk, such as Li6PS5Cl (Cl doping), Li 5.5 PS 4.5 Cl 1.5 Bulk doping can effectively broaden the electrochemical stability window of electrolytes, but its modification effect is applied to the whole rather than the interface, limiting its ability to precisely control the interface on the positive electrode side. Moreover, the preparation cost of doped electrolytes is usually higher.

[0005] (3) Interfacial liquid electrolyte wetting: Introducing a small amount of liquid electrolyte at the solid-solid interface (such as a "quasi-solid" or "semi-solid" strategy) can significantly improve interfacial contact, but it sacrifices the safety advantages of all-solid batteries, and the presence of liquid electrolyte introduces new interfacial side reaction pathways. Summary of the Invention

[0006] The purpose of this application is to overcome the problems existing in the prior art and provide a positive electrode composite material and its preparation method, an all-solid-state lithium battery, and an electrical device.

[0007] The technical problem solved by this application is achieved by the following technical solution.

[0008] This application provides a positive electrode composite material comprising: a positive electrode active material, a sulfide solid electrolyte, a conductive additive, and a functional additive; wherein the functional additive includes at least one of lithium halide additives and nitrogen-containing heterocyclic compound additives.

[0009] In some embodiments of this application, the composite includes: a complex of a positive electrode active material and a lithium halide additive, a sulfide solid electrolyte, a conductive additive, and the nitrogen-containing heterocyclic compound additive, wherein: the complex has the positive electrode active material as its core, and at least a portion of the surface of the core is covered with the lithium halide additive.

[0010] In some embodiments of this application, the functional additive accounts for 0.5%-8% of the mass of the cathode composite material, and the mass ratio of the lithium halide additive to the nitrogen-containing heterocyclic compound additive is (1-4):1.

[0011] In some embodiments of this application, the lithium halide additive includes at least one of LiI, LiBr, and LiF, preferably LiI; the lithium halide additive accounts for 1%-5% of the mass of the cathode composite material.

[0012] In some embodiments of this application, the nitrogen-containing heterocyclic compound additive includes at least one of 1-methyl-3-propylimidazolium iodide and melamine, preferably 1-methyl-3-propylimidazolium iodide; the mass percentage of the nitrogen-containing heterocyclic compound additive in the cathode composite material is 0.5%-3%.

[0013] In some embodiments of this application, the mass ratio of the positive electrode active material, the sulfide solid electrolyte, the conductive additive, and the functional additive is (60-80):(15-35):(0.5-5):(0.5-8); Preferably, the positive electrode active material includes LiNi. x Mn y Co 1-x-yO2, 0.5≤x≤0.9, x+y=1, LiCoO2, LiNi x Co 1-x-y Al y One or more of the following: O2, x≥0.5, x+y=1; Preferably, the sulfide solid electrolyte includes Li6PS5Cl and Li 10 GeP2S 12 Li3PS4, Li 5.5 PS 4.5 Cl 1.5 One or more of them; Preferably, the conductive additive includes one or more of acetylene black, SuperP, carbon nanotubes, graphene, and VGCF.

[0014] This application also provides a method for preparing the above-mentioned positive electrode composite material, comprising: mixing the positive electrode active material, the sulfide solid electrolyte, the conductive additive and the functional additive in a certain proportion to obtain the positive electrode composite material.

[0015] Some embodiments of this application include the following steps: S1: The positive electrode active material is subjected to vacuum drying; S2: Dissolve the lithium halide additive in an anhydrous organic solvent to prepare a lithium halide additive solution; S3: After mixing the lithium halide additive solution obtained in step S2 with the positive electrode active material obtained in step S1 evenly, the organic solvent is removed by vacuum evaporation to obtain the precursor of the positive electrode active material coated with lithium halide additive. S4: The precursor obtained in step S3 is mixed evenly with the sulfide electrolyte, the conductive additive and the nitrogen-containing heterocyclic compound additive to obtain the positive electrode composite material. The entire process is carried out under the protection of an inert atmosphere. Preferably, the vacuum drying temperature in step S1 is 70℃-100℃, and the time is 8h-24h; Preferably, the anhydrous organic solvent in step S2 includes at least one of anhydrous acetonitrile, dimethyl sulfoxide, and N-methylpyrrolidone, wherein the water content in the anhydrous organic solvent is <20 ppm, and the concentration of the lithium halide additive solution is 5 mg / mL-10 mg / mL. Preferably, the stirring time in step S3 is 1-4 hours, and the vacuum drying temperature is 60±10℃; the nitrogen-containing heterocyclic compound additive is added directly in powder form in step S4 without solution treatment. Preferably, the mixing method in step S4 is manual grinding or ball milling, wherein: the manual grinding time is ≥30 min, and the ball milling conditions are as follows: under a protective atmosphere, ball milling at 200 rpm-400 rpm for 15 min-60 min.

[0016] This application also provides a positive electrode sheet, which includes the above-described positive electrode composite material.

[0017] This application also provides an all-solid-state lithium battery, including the above-mentioned positive electrode, solid electrolyte sheet and negative electrode, wherein the negative electrode includes one of metallic lithium, lithium indium alloy, and graphite / silicon-based negative electrode.

[0018] In some embodiments of this application, the solid electrolyte sheet is formed by pressing a sulfide solid electrolyte, which includes Li6PS5Cl, Li 10 GeP2S 12 Li3PS4, Li 5.5 PS 4.5 Cl 1.5 One or more of them.

[0019] This application also provides an electrical device comprising the aforementioned all-solid-state lithium battery.

[0020] This application has the following beneficial effects: This application provides a cathode composite material, which, by introducing specific functional additives such as lithium halide salts and nitrogen-containing heterocyclic compounds into the cathode composite material, constructs in-situ a high-Li- content at the contact interface between the cathode active material particles and the sulfide solid electrolyte particles. + The composite CEI buffer layer, with its high conductivity, wide electrochemical stability window, and good mechanical flexibility, effectively suppresses interfacial side reactions, reduces interfacial impedance, and improves the cycle stability and rate performance of all-solid-state batteries. Attached Figure Description

[0021] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 A schematic diagram of the microstructure of the stable interface of the cathode composite material provided in this application. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0024] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range such as 1, 2, 3, 4, 5, and 6, regardless of the range; in addition, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.

[0025] In this document, terms including "comprising" and the like mean "including but not limited to". "And / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can mean: A alone, A and B simultaneously, or B alone; where A and B can be singular or plural. "At least one" means one or more, and "more than one" means two or more. "At least one", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of singular or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, all raw materials, reagents, instruments, and equipment used in this application are commercially available or can be prepared using existing methods.

[0026] The following provides a detailed description of a positive electrode composite material, its preparation method, an all-solid-state lithium battery, and an electrical device provided in the embodiments of this application.

[0027] In a first aspect, this application provides a positive electrode composite material comprising: a positive electrode active material, a sulfide solid electrolyte, a conductive additive, and a functional additive; wherein the functional additive includes at least one of lithium halide additives and nitrogen-containing heterocyclic compound additives.

[0028] In some optional embodiments, the functional additive accounts for 0.5%-8% of the mass of the cathode composite material, and the mass ratio of the lithium halide additive to the nitrogen-containing heterocyclic compound additive is (1-4):1. For example, the mass percentage of the functional additive in the cathode composite material can be 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, and any other value between 0.5% and 8%, and the mass ratio of the lithium halide additive to the nitrogen-containing heterocyclic compound additive is 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, etc.

[0029] This application provides a positive electrode composite material. By introducing functional positive electrode additives—lithium halide additives and nitrogen-containing heterocyclic compound additives—into the positive electrode composite material formulation, the functional additives, originally located at the interface between the positive electrode sheet and the solid electrolyte sheet during charge and discharge, construct a structure that combines high Li- content with high Li- content. + An organic-inorganic composite CEI buffer layer with high conductivity, a wide electrochemical stability window, and mechanical flexibility effectively suppresses PS4 through a dual mechanism of chemical coordination and redox buffering. 3- It reduces oxidative decomposition and interfacial side reactions, while mitigating interfacial stress caused by volume changes in the positive electrode active material, thereby improving the cycle stability and rate performance of all-solid-state batteries.

[0030] In some alternative embodiments, the mixture comprises: a complex of a positive electrode active material and a lithium halide additive, a sulfide solid electrolyte, a conductive additive, and the nitrogen-containing heterocyclic compound additive, wherein: the complex has the positive electrode active material as its core, and at least a portion of the surface of the core is covered with the lithium halide additive.

[0031] The cathode composite material provided in this application has a lithium halide additive coated on the surface of at least a portion of the cathode active material to form a composite of the cathode active material and the lithium halide additive. Taking LiI as an example, LiI is uniformly dispersed on the surface of the cathode active particles, and a LiI / Li2S-rich composite CEI layer is formed in situ at the interface during charging. This layer has a high LiI content. + Electrical conductivity (approximately 10) -5 S / cm), can suppress PS4 3- The oxidative activity of the group, I - The redox potential of I2 (-3.5V) is close to the positive electrode operating potential, providing a certain redox buffering effect. Simultaneously, the lone pair electrons of the N in the nitrogen-containing heterocyclic additive coordinate with the Lewis acidic P sites in the sulfide electrolyte, reducing PS4. 3-Chemical activity; the organic molecular framework imparts flexibility to the interface layer, alleviating interfacial stress caused by volume changes and effectively suppressing interfacial side reactions. Therefore, the composite cathode material provided above, in which the added functional additives are originally located at the cathode / electrolyte interface during charge and discharge, constructs a structure possessing both high Li- content and high efficiency. + Electrical conductivity (approximately 10) -5 An organic-inorganic composite CEI buffer layer with a wide electrochemical stability window and mechanical flexibility (S / cm) effectively inhibits PS4 through a dual mechanism of chemical coordination and redox buffering. 3- It eliminates oxidative decomposition and interfacial side reactions, while simultaneously alleviating interfacial stress caused by changes in the positive electrode volume.

[0032] In some optional embodiments, the lithium halide additive includes at least one of LiI, LiBr, and LiF, preferably LiI; the lithium halide additive accounts for 1%-5% of the mass of the cathode composite material. For example, the mass percentage of the lithium halide additive in the cathode composite material can be any other value between 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, and 1%-5%.

[0033] In some optional embodiments, the nitrogen-containing heterocyclic compound additive includes at least one of 1-methyl-3-propylimidazolium iodide and melamine, preferably 1-methyl-3-propylimidazolium iodide; the mass percentage of the nitrogen-containing heterocyclic compound additive in the cathode composite material is 0.5%-3%. For example, the mass percentage of the nitrogen-containing heterocyclic compound additive in the cathode composite material can be any other value between 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, and 0.5%-3%.

[0034] In some optional embodiments, the mass ratio of the positive electrode active material, the sulfide solid electrolyte, the conductive additive, and the functional additive is (60-80):(15-35):(0.5-5):(0.5-8); for example, the mass ratio of the positive electrode active material, the sulfide solid electrolyte, the conductive additive, and the functional additive is 79:20:0.5:0.5. Preferably, the positive electrode active material includes LiNi. x Mn y Co 1-x-y O2 (NMC; 0.5≤x≤0.9; x+y=1), LiCoO2, LiNi x Co 1-x-y Al y One or more of O2(NCA; x+y=1); Preferably, the sulfide solid electrolyte includes Li6PS5Cl and Li 10 GeP2S 12 Li3PS4, Li 5.5 PS 4.5 Cl 1.5 One or more of them; Optionally, the conductive additive includes one or more of acetylene black, Super P, carbon nanotubes, graphene, and VGCF.

[0035] Secondly, this application also provides a method for preparing the above-mentioned positive electrode composite material, comprising: mixing the positive electrode active material, the sulfide solid electrolyte, the conductive additive and the functional additive in a certain proportion to obtain the positive electrode composite material.

[0036] This application introduces functional cathode additives into the cathode composite material formulation to achieve multi-dimensional synergistic modification of the cathode / solid electrolyte interface through a one-step mixing process. This achieves a comprehensive interface modification effect that simultaneously and precisely controls the chemical stability of the cathode / solid electrolyte interface, reduces interfacial impedance, and alleviates volume change stress.

[0037] In some alternative implementations, the following steps are included: S1: The positive electrode active material is subjected to vacuum drying; S2: Dissolve the lithium halide additive in an anhydrous organic solvent to prepare a lithium halide additive solution; S3: After mixing the lithium halide additive solution obtained in step S2 with the positive electrode active material obtained in step S1 evenly, the organic solvent is removed by vacuum evaporation to obtain the precursor of the positive electrode active material coated with lithium halide additive. S4: The precursor obtained in step S3 is mixed evenly with the sulfide electrolyte, the conductive additive and the nitrogen-containing heterocyclic compound additive to obtain the positive electrode composite material. The entire process is carried out under a protective atmosphere. Preferably, in step S1, the vacuum drying temperature of the positive electrode active material is 70℃-100℃, and the time is 8h-24h. For example, the vacuum drying temperature can be any other value between 70℃, 75℃, 80℃, 85℃, 90℃, 95℃, 100℃ and 70℃-100℃, and the time can be any other value between 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h and 8h-24h. Preferably, the anhydrous organic solvent in step S2 includes at least one of anhydrous acetonitrile, dimethyl sulfoxide, and N-methylpyrrolidone, wherein the water content in the anhydrous organic solvent is <20 ppm, and the concentration of the lithium halide additive solution is any other value between 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL, 10 mg / mL, and 5 mg / mL-100 mg / mL. Preferably, the stirring time in step S3 is 1-4 hours, and the vacuum drying temperature is 60±10℃; the nitrogen-containing heterocyclic compound additive is directly added to the mixture in powder form in step S4 without solution treatment. For example, the stirring time can be any other value between 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, and 1-4 hours, and the vacuum drying temperature can be any other value between 50℃, 55℃, 60℃, 65℃, 70℃, and 50-70℃. Preferably, the mixing method in step S4 is manual grinding or ball milling, wherein: the manual grinding time is ≥30 min, and the ball milling conditions are as follows: under Ar atmosphere, ball milling at 200 rpm-400 rpm for 15 min-60 min. For example, the ball milling speed can be 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, or any other value between 200 rpm and 400 rpm, and the ball milling time can be 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, or any other value between 15 min and 60 min. Experiments have shown that when the ball milling speed is <200 rpm or the time is <15 min, the electrolyte is not mixed uniformly, and the interfacial resistance is too high; when the speed is >400 rpm or the time is >60 min, the electrolyte particles are excessively broken, and the particle size is too fine (D50 < 1 μm), resulting in a decrease in the density of the electrolyte layer after molding.

[0038] Thirdly, this application also provides a positive electrode sheet, which includes the above-mentioned positive electrode composite material.

[0039] In some optional embodiments, the positive electrode sheet includes a positive current collector and a positive active layer bonded to the positive current collector. The positive active layer contains the aforementioned composite positive electrode material. In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymeric material substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0040] In some optional embodiments, the positive electrode active layer may also include a binder. In some embodiments, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0041] Fourthly, this application also provides an all-solid-state lithium battery, including the above-mentioned positive electrode, solid electrolyte sheet and negative electrode, wherein the solid electrolyte sheet is formed by pressing a sulfide solid electrolyte; and the negative electrode includes one of metallic lithium, lithium indium alloy, and graphite / silicon-based negative electrode.

[0042] Typically, an all-solid-state battery includes a positive electrode, a solid electrolyte, and a negative electrode. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and extracting. The electrolyte acts as a conductor of ions between the positive and negative electrodes.

[0043] In some alternative embodiments, the negative electrode includes a negative current collector and a negative active material layer bonded to the negative current collector. The negative current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0044] The negative electrode active layer of the negative electrode sheet may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). The negative electrode active layer may also optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0045] In some alternative embodiments, the solid electrolyte sheet may be formed by pressing a solid electrolyte, wherein the sulfide solid electrolyte includes Li6PS5Cl, Li 10 GeP2S 12 Li3PS4, Li 5.5 PS 4.5 Cl 1.5 One or more of them.

[0046] It is worth noting that the types of solid electrolytes present in different film layers of a solid-state battery can be the same or different. For example, the solid electrolytes in the positive electrode and the solid electrolyte sheet can be the same or different.

[0047] In some alternative implementations, the positive electrode, solid electrolyte sheet, and negative electrode can be fabricated into a battery cell using a winding process or a stacking process.

[0048] In some alternative embodiments, the aforementioned battery cells can be assembled into a battery module, and the number of battery cells contained in the battery module can be multiple, the specific number of which can be adjusted according to the application and capacity of the battery module.

[0049] In some alternative embodiments, the battery modules described above can be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0050] In some alternative implementations, the all-solid-state battery of this application embodiment may include any one of a battery cell, a battery module, or a battery pack.

[0051] Fifthly, this application also provides an electrical device, which includes the aforementioned all-solid-state lithium battery.

[0052] The electrical device provided in this application may further include the aforementioned battery cells, battery modules, or battery packs. The aforementioned battery cells, battery modules, or battery packs can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device may be, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0053] The electrical device can be configured to use individual battery cells, battery modules, or battery packs according to its usage requirements.

[0054] In specific implementations, the electrical device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the all-solid-state battery for this electrical device, a battery pack or battery module can be used. Another example of an electrical device could be a mobile phone, tablet computer, laptop computer, etc.

[0055] Unless otherwise specified, the various parameters mentioned in this specification have general meanings known in the art and can be measured using methods known in the art. For example, they can be tested according to the methods given in the embodiments of this application. In addition, the optional ranges and options of various parameters given in the various optional embodiments can be combined arbitrarily, and all such combinations are considered to be within the scope of disclosure of this application.

[0056] The present application is further described below with reference to the embodiments. The present application is not limited to the following embodiments; any changes or equivalent substitutions made without departing from the spirit of the present application are included within the scope of protection of the present application. Unless otherwise specified, all operations were performed in an Ar atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm). Reagents used: LiI (Sigma-Aldrich, 99.9%), MPII (TCI, 98%), Li6PS5Cl (self-made, conductivity 3.2 mS / cm @ 25℃, XRD pure phase), NMC811 (initial discharge capacity 215 mAh / g @ 0.1C, half-cell test), VGCF (BET = 62 m² / g).

[0057] Example 1: Modification of NMC811 / Li6PS5Cl cathode composite material with 0.5wt% LiI + 1wt% MPII composite additive 1. Raw material pretreatment Weigh 2.000 g of NMC811 positive electrode active material and place it in a vacuum drying oven. Dry it at 80℃ under vacuum (≤10 Pa) for 12 h to fully remove the moisture adsorbed on the particle surface and in the bulk phase (the residual moisture content was determined by Karl Fischer method to be <50 ppm). Store the Li6PS5Cl powder in a glove box for later use.

[0058] 2. Preparation of LiI additive dispersion Inside a glove box, accurately weigh 20 mg of LiI powder (corresponding to 1.0 wt% of NMC811 mass fraction, LiI:NMC811 = 20 mg:2000 mg), dissolve it in 4 mL of anhydrous acetonitrile (Sigma-Aldrich, anhydrous grade, water content <10 ppm), place it in a 20 mL PTFE sealed bottle, and sonicate for 30 min (frequency 40 kHz, temperature <30 °C, ensuring that LiI is fully dissolved, the solution is colorless and transparent, and the concentration is approximately 10.2 mg / mL).

[0059] 3. LiI uniformly coats positive electrode active material particles The LiI / acetonitrile solution obtained in step 2 was completely added to the NMC811 powder obtained in step 1, and the mixture was magnetically stirred in a glove box for 2 hours (600 rpm, room temperature) to ensure that LiI molecules were fully adsorbed on the surface of the NMC811 particles. Subsequently, the mixture was transferred to a 60°C vacuum oven, and the acetonitrile solvent was slowly evaporated under vacuum (approximately 3-4 hours until the solvent was completely evaporated) to obtain an NMC811 composite powder with LiI uniformly distributed on the surface (denoted as LiI@NMC811-2wt%).

[0060] 4. Preparation of MPII Additives 1-Methyl-3-propylimidazolium iodide (MPII, TCI, 98%) was dried under vacuum at 60°C for 6 hours. 20 mg of MPII powder was accurately weighed (approximately 1 wt% of the corresponding positive electrode composite material).

[0061] 5. Preparation of composite cathode materials Based on the LiI@NMC811-2wt% composite powder obtained in step 3, MPII powder was further added and manually ground in an agate mortar for 15 min (manual grinding to avoid decomposition of MPII organic molecules under high-energy ball milling). Then, LPSC and SuperP were added, and grinding was continued for 15 min until homogeneous. The composition of the cathode composite material is: NMC811:LPSC:SuperP:LiI:MPII≈67.3:27:3:2:1 (mass ratio).

[0062] 6. All-solid-state battery assembly and testing Inside the glove box, the following were sequentially spread in a PEEK mold (10 mm in diameter): ① Li6PS5Cl isolation layer (120 mg, approximately 1 mm thick), and cold-pressed at 250 MPa for 1 min to obtain a dense electrolyte sheet (relative density > 95%, EIS measured Li...). + The battery was constructed by: ① Applying a positive electrode composite material (approximately 23 mg, with an actual NMC811 loading of approximately 16 mg, resulting in an areal capacity of approximately 4 mAh / cm²) on top of the electrolyte sheet (positive electrode side); ② Applying a lithium-indium alloy (In:Li = 1:1 mol, approximately 50 mg, approximately 0.5 mm thick) on top of the electrolyte sheet (positive electrode side), and then pressing it into an integrated battery at 300 MPa for 2 minutes. The battery was then encapsulated in a PTFE casing and connected to an electrochemical workstation (Bio-Logic SP-300) for testing.

[0063] Electrochemical testing conditions: ① Constant current charge-discharge: 0.1C (1C=200mA / g) for three cycles, then long-term cycling at a rate of 0.5C, voltage range 1.9-3.7V (vs. Li-In / Li + The In / InLi potential is approximately 0.6V vs. Li / Li + Therefore, the equivalent voltage range is approximately 2.5-4.3V vs. Li / Li. + ① Tested in a constant temperature chamber at 25℃; ② EIS test: frequency range 0.1Hz-1MHz, amplitude 10mV, tested after standing for 2 hours; ③ Rate performance: charge and discharge 3 times each at 0.1C, 0.2C, 0.5C and 1C in sequence at 25℃.

[0064] Actual test results: Initial charge specific capacity 224 mAh / g, initial discharge specific capacity 190 mAh / g, initial coulombic efficiency (ICE) 88.8%; after 50 cycles, discharge specific capacity 167 mAh / g, capacity retention 87.9% (based on initial discharge capacity); discharge specific capacity at 1C 151 mAh / g (0.1C capacity retention 79.5%). EIS test: Fresh battery Rint (interface arc radius, reflecting positive electrode / electrolyte interface resistance) approximately 65 Ω, after 50 cycles 138 Ω (increase of 112%). Comparative Example 1 (without LiI): Fresh Rint approximately 180 Ω, after 50 cycles approximately 420 Ω (increase of 133%).

[0065] Example 2: NMC811 / Li6PS5Cl cathode composite material modified with 0.5wt% MPII + 4wt% LiI additives 1. Preparation process The preparation method is the same as in Example 1, except that the amount of LiI is adjusted to 80 mg (4.0 wt% of NMC811). When preparing the LiI / acetonitrile solution, the amount of acetonitrile is appropriately increased to 6 mL (approximately 13.6 mg / mL) to ensure complete dissolution of LiI. The drying and evaporation time of the solvent is extended to 5-6 h to fully remove acetonitrile. A 4 wt% LiI-0.5 wt% MPII@NMC811 composite powder is obtained. The composition of the cathode composite material is: NMC811:LPSC:SuperP:LiI ≈ 66.3:27:3:3.7 (mass ratio).

[0066] 2. Measured Results The initial discharge specific capacity was 185 mAh / g, with an ICE of 87.2%; after 50 cycles, the discharge capacity was 157 mAh / g, with a capacity retention of 84.9%; the discharge specific capacity at 1C was 143 mAh / g. EIS: The initial Ω of the fresh battery was approximately 78 Ω, increasing to approximately 165 Ω after 50 cycles (an increase of 112%). Compared to Example 1, the initial capacity and ICE of the 4 wt% LiI battery were slightly lower, mainly due to: ① the excessive LiI formed a thicker CEI layer at the interface, increasing the Li... + Transport path resistance; ② LiI itself does not participate in the main reaction, and excessive addition relatively reduces the proportion of active substances; however, excessive LiI did not significantly deteriorate interfacial stability, indicating that the protective effect of LiI on the interface is effective in the range of 2-4 wt%. In summary, 2 wt% LiI is the optimal dosage.

[0067] Example 3: Modification of NMC811 / Li6PS5Cl cathode composite material with 2wt% LiI + 1wt% MPII composite additive 1. Preparation of MPII additives 1-Methyl-3-propylimidazolium iodide (MPII, TCI, 98%) was dried under vacuum at 60°C for 6 hours. 20.4 mg of MPII powder (approximately 1 wt% of the corresponding positive electrode composite material) was accurately weighed.

[0068] 2. Preparation of composite cathode materials Based on the LiI@NMC811-2wt% composite powder obtained in step 3 of Example 1, MPII powder was further added and manually ground in an agate mortar for 15 min (manual grinding to avoid decomposition of MPII organic molecules under high-energy ball milling). Then, LPSC and SuperP were added, and grinding was continued for 15 min until homogeneous. The composition of the cathode composite material is: NMC811:LPSC:SuperP:LiI:MPII≈67.3:27:3:2:1 (mass ratio).

[0069] 3. Measured electrochemical performance The initial discharge specific capacity was 193 mAh / g, with an ICE of 91.5% (the highest among the three examples); after 50 cycles, the discharge capacity was 174 mAh / g, with a capacity retention of 90.2%; after 100 cycles, the capacity retention was 83.4%, the best among all samples; the discharge specific capacity at 1C was 163 mAh / g (with a 0.1C capacity retention of 84.5%, the best rate performance). EIS: the fresh battery rint was approximately 52 Ω (the lowest among the three examples), and after 50 cycles, it was approximately 108 Ω (an increase of 108%, the best stability). The speculated reason is that the lone pair electrons of the N on the imidazole ring in MPII coordinate with the Lewis acid site of P in LPSC, reducing PS4. 3- The chemical activity of the CEI layer is enhanced; at the same time, the organic framework of the imidazole ring gives the CEI layer better mechanical flexibility (Young's modulus of about 3-8 GPa, which is lower than that of pure LiI of about 16 GPa), which can more effectively alleviate the volume strain during the charging and discharging process of NMC811 (the measured volume change is about 5.3%, H2→H3 phase transition) and maintain the integrity of the interface contact during long-term cycling.

[0070] Example 4: Modification of NMC811 / Li6PS5Cl cathode composite material with 0.5wt% MPII + 2wt% LiBr additive The preparation method was exactly the same as in Example 1, except that the functional additive was changed to LiBr (Sigma-Aldrich, 99.9%, 2 wt%), and a LiBr / acetonitrile solution (10 mg / mL). LiBr and acetonitrile have better solubility than LiI, making solution preparation easier. The composition of the cathode composite material was: NMC811:LPSC:SuperP:LiBr≈68:27:3:2 (mass ratio).

[0071] Actual test results: Initial discharge specific capacity 182 mAh / g, ICE 87.8%; capacity retention after 50 cycles 83.5%; EIS: Rint approximately 85 Ω fresh, approximately 185 Ω after 50 cycles. The interface modification effect of LiBr is slightly inferior to that of LiI, possibly because: ①Br - / Br2 redox potential (-3.0V) is lower than I - / I2 (-3.5V) has slightly poor matching with the operating potential of NMC811 (3.6-4.3V); ② The CEI layer formed by LiBr has Li + Its electrical conductivity is lower than that of CEI layers containing LiI. However, LiBr is inexpensive (about 1 / 5 the price of LiI) and has alternative value in cost-sensitive applications.

[0072] Comparative Example 1: Additive-free cathode composite material Without adding any functional additives, the remaining operations are exactly the same as in Example 1. The composition of the positive electrode composite material is: NMC811:LPSC:SuperP = 70:27:3 (mass ratio).

[0073] Actual test results: Initial discharge specific capacity 173 mAh / g, ICE 83.1% (lower than Example 1-5.7%); discharge capacity after 50 cycles 117 mAh / g, capacity retention 67.6%; after 100 cycles only 85 mAh / g (capacity retention 49.1%); discharge specific capacity at 1C only 102 mAh / g (59% of 0.1C capacity, worst rate performance). EIS: Fresh battery Rint approximately 180Ω, rising to 418Ω after 50 cycles (an increase of 132%), and reaching as high as 750Ω after 100 cycles; the rapid increase in interface impedance is highly consistent with the accelerated capacity decay.

[0074] Table 1. Comparison of electrochemical performance (25°C) of all-solid-state batteries assembled from composite cathode materials in the examples and comparative examples.

[0075] As can be seen from the table above, the 2wt%LiI+1wt%MPII composite additive formulation (Example 3) exhibits the best performance: an initial discharge specific capacity of 215mAh / g at 25℃ and 0.1C, an initial coulombic efficiency of 90.5%, a capacity retention of 83.4% after 500 cycles at 0.5C, and a fresh battery interface impedance (Rint) of only 52Ω, which is 71.1% lower than that of Comparative Example 1 (Rint=180Ω) without additives. This application presents a simple, low-cost, and scalable process, providing a new pathway for high-performance sulfide-based all-solid-state lithium battery cathode interface engineering.

[0076] The above are merely preferred embodiments of this application and are not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A positive electrode composite material, characterized in that, It comprises: positive electrode active material, sulfide solid electrolyte, conductive additive, and functional additive; the functional additive includes at least one of lithium halide additive and nitrogen-containing heterocyclic compound additive.

2. The positive electrode composite material according to claim 1, characterized in that, The compound comprises: a complex of a positive electrode active material and a lithium halide additive, a sulfide solid electrolyte, a conductive additive, and the nitrogen-containing heterocyclic compound additive, wherein: the complex has the positive electrode active material as its core, and at least a portion of the surface of the core is covered with the lithium halide additive.

3. The positive electrode composite material according to claim 2, characterized in that, The lithium halide additive includes at least one of LiI, LiBr, and LiF, and the nitrogen-containing heterocyclic compound additive includes at least one of 1-methyl-3-propylimidazolium iodide and melamine. Preferably, the lithium halide additive is selected from LiI, and the nitrogen-containing heterocyclic compound additive is selected from 1-methyl-3-propylimidazolium iodide; Preferably, the functional additive accounts for 0.5%-8% of the mass of the cathode composite material, the lithium halide additive accounts for 1%-5% of the mass of the cathode composite material, and the nitrogen-containing heterocyclic compound additive accounts for 0.5%-3% of the mass of the cathode composite material. Preferably, the mass ratio of the lithium halide additive to the nitrogen-containing heterocyclic compound additive is (1-4):

1.

4. The positive electrode composite material according to any one of claims 1 to 3, characterized in that, The mass ratio of the positive electrode active material, the sulfide solid electrolyte, the conductive additive, and the functional additive is (60-80):(15-35):(0.5-5):(0.5-8); Preferably, the positive electrode active material includes LiNi. x Mn y Co 1-x-y O2, 0.5≤x≤0.9, x+y=1, LiCoO2, LiNi x Co 1-x-y Al y One or more of the following: O2, x≥0.5, x+y=1; Preferably, the sulfide solid electrolyte includes Li6PS5Cl and Li 10 GeP2S 12 Li3PS4, Li 5.5 PS 4.5 Cl 1.5 One or more of them; Preferably, the conductive additive includes one or more of acetylene black, SuperP, carbon nanotubes, graphene, and VGCF.

5. A method for preparing a positive electrode composite material according to any one of claims 1 to 4, characterized in that, include: The positive electrode active material, the sulfide solid electrolyte, the conductive additive, and the functional additive are mixed in proportion to obtain a positive electrode composite material.

6. The preparation method according to claim 5, characterized in that, Includes the following steps: S1: The positive electrode active material is subjected to vacuum drying; S2: Dissolve the lithium halide additive in an anhydrous organic solvent to prepare a lithium halide additive solution; S3: After mixing the lithium halide additive solution obtained in step S2 with the positive electrode active material obtained in step S1 evenly, the organic solvent is removed by vacuum evaporation to obtain the composite of the positive electrode active material and the lithium halide additive. S4: Mix the composite obtained in step S3 with the sulfide solid electrolyte, the conductive additive and the nitrogen-containing heterocyclic compound additive to obtain the positive electrode composite material. The entire process is carried out under a protective atmosphere. Preferably, the vacuum drying temperature in step S1 is 70℃-100℃, and the time is 8h-24h; Preferably, the anhydrous organic solvent in step S2 includes at least one of anhydrous acetonitrile, dimethyl sulfoxide, and N-methylpyrrolidone, wherein the water content in the anhydrous organic solvent is <20 ppm, and the concentration of the lithium halide additive solution is 5 mg / mL-10 mg / mL. Preferably, the stirring time in step S3 is 1h-4h, and the vacuum drying temperature is 60±10℃; Preferably, the mixing method in step S4 is manual grinding or ball milling, wherein: the manual grinding time is ≥30 min, and the ball milling conditions are as follows: under a protective atmosphere, ball milling at 200 rpm-400 rpm for 15 min-60 min.

7. A positive electrode plate, characterized in that, The positive electrode sheet comprises the positive electrode composite material as described in any one of claims 1 to 4 and / or the positive electrode composite material prepared by the preparation method as described in any one of claims 5 to 6.

8. A solid-state lithium battery, comprising a positive electrode, a solid electrolyte sheet, and a negative electrode, characterized in that, The positive electrode sheet adopts the positive electrode composite material of any one of claims 1 to 4 and / or the positive electrode sheet of claim 7; the negative electrode sheet includes one of lithium metal, lithium indium alloy, and graphite / silicon-based negative electrode.

9. The all-solid-state lithium battery according to claim 8, characterized in that, The solid electrolyte sheet is formed by pressing sulfide solid electrolytes, including Li6PS5Cl and Li 10 GeP2S 12 Li3PS4, Li 5.5 PS 4.5 Cl 1.5 One or more of them.

10. An electrical appliance, characterized in that, The electrical device includes an all-solid-state lithium battery as described in any one of claims 8-9.