Self-repairing negative electrode binder, negative electrode sheet, and preparation method and application thereof

By using a self-healing binder composed of an acrylate copolymer containing carboxyl groups, catechol groups, and disulfide bonds and a metal salt in lithium-ion batteries, the problem of dynamic reversible cross-linking and strong interfacial anchoring of silicon-carbon anodes in lithium-ion batteries during cycling is solved, achieving high cycle stability and structural integrity of the battery.

CN123143408APending Publication Date: 2026-11-20HUIZHOU LITONGWEI ELECTRONIC TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611536074.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing silicon-carbon anode binders for lithium-ion batteries cannot achieve dynamic reversible cross-linking and strong interfacial anchoring during cycling, resulting in insufficient battery cycle stability and complex preparation processes.

Method used

A self-healing negative electrode binder composed of an acrylate copolymer containing carboxyl groups, catechol groups, and disulfide bonds, and a water-soluble salt of Zn²⁺ or Mg²⁺, forms a dynamic reversible network through interfacial hydrogen bonding anchoring of catechol groups, dynamic coordination crosslinking of carboxyl groups, and dynamic covalent exchange of disulfide bonds, thus buffering volume expansion stress.

Benefits of technology

It improves the cycle stability and structural integrity of lithium-ion batteries by reorganizing the network structure under stress through a self-repair mechanism, thus maintaining the integrity of the electrode structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The application discloses a self-repairing negative electrode binder, a negative electrode sheet and a preparation method and application thereof. The self-repairing negative electrode binder comprises components A and B with a mass ratio of 1: (0.02-0.08). The component A is an acrylic ester copolymer containing a carboxyl group, a catechol group and a disulfide bond. The weight average molecular weight of the component A is 80,000-150,000, the carboxyl group content is 4 mmol / g-7 mmol / g, the catechol group content is 0.5 mmol / g-1.5 mmol / g, and the disulfide bond content is 0.1 mmol / g-0.5 mmol / g. The component B is a water-soluble salt of Zn 2+ or Mg 2+ . The component A and the component B form a metal-carboxyl coordination bond, which is stable in an aqueous system, reversibly broken and recombined under the stress generated by silicon volume expansion, and self-repaired without external stimulation, thereby ensuring the cycle stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium battery materials technology, and in particular to a self-healing negative electrode binder, a negative electrode sheet, its preparation method and application. Background Technology

[0002] During charging and discharging, the silicon-carbon anode of lithium-ion batteries undergoes significant volume expansion. Binders are used to maintain the integrity of the electrode structure and inhibit the pulverization and shedding of active materials. Currently, silicon-carbon anode binders mainly employ two systems: one is a physical cross-linking network represented by polyallylamine hydrochloride and polyacrylic acid-polybenzimidazole; the other is a surface-linking binder that forms a chemically cross-linked coating layer on the surface of silicon-carbon materials through in-situ polymerization. However, the aforementioned physical cross-linking networks have low bond energies and are prone to irreversible breakage under the stress generated by the volume expansion of silicon, lacking self-repair capabilities. While chemically cross-linking networks have stronger bonding forces, they permanently fail after the cross-linking bonds break, and the preparation process is complex. More critically, existing aqueous binder systems cannot simultaneously achieve dynamic reversible cross-linking and strong interfacial anchoring, leading to irreversible damage to the network structure and interfacial debonding during cycling, resulting in insufficient battery cycle stability. Summary of the Invention

[0003] This application provides a self-healing negative electrode binder, a negative electrode sheet, its preparation method, and its application to solve the technical problem of insufficient battery cycle stability.

[0004] In a first aspect, this application provides a self-healing negative electrode adhesive, comprising component A and component B in a mass ratio of 1:(0.02~0.08); Component A is an acrylate copolymer containing carboxyl groups, catechol groups, and disulfide bonds; the weight-average molecular weight of component A is 80,000 to 150,000, the carboxyl content is 4 mmol / g to 7 mmol / g, the catechol group content is 0.5 mmol / g to 1.5 mmol / g, and the disulfide bond content is 0.1 mmol / g to 0.5 mmol / g. The B component is Zn. 2+ or Mg 2+ Water-soluble salts.

[0005] In some embodiments, component A is copolymerized from the following monomers in weight percentages: 55% to 65% acrylic acid, 25% to 35% butyl acrylate, 5% to 10% dopamine methacrylamide, and 1% to 3% disulfide-containing methacrylate monomers.

[0006] Among them, acrylic acid monomers provide carboxyl groups, and when the content is 55%~65%, sufficient coordination crosslinking sites and hydrophilicity can be ensured, while avoiding excessive hydrophilicity and pH sensitivity caused by excessive carboxyl content; butyl acrylate monomers provide flexibility, and its homopolymer glass transition temperature is about -50℃. When the content is 25%~35%, the copolymer can maintain appropriate chain segment mobility within the battery operating temperature range, which is beneficial for buffering the stress generated by silicon volume expansion; dopamine methacrylamide monomers provide catechol groups, and when the content is 5%~10%, sufficient hydrogen bond anchoring sites can be formed on the surface of silicon carbon particles, while avoiding an increase in catechol oxidation side reactions caused by excessive content; methacrylate monomer units containing disulfide bonds provide disulfide bonds, and when the content is 1%~3%, an appropriate amount of dynamic covalent bonds can be introduced without significantly affecting the mechanical properties of the copolymer.

[0007] In some embodiments, the disulfide-containing methacrylate monomer is 2-(2-pyridyldithio)ethyl methacrylate, which contains methacrylate double bonds and pyridyl disulfide bonds, and can be introduced into the polymer backbone through free radical copolymerization; the pyridyl disulfide bonds have low exchange activation energy and can undergo disulfide bond exchange reaction under stress, which helps the dynamic reorganization of the network structure.

[0008] In some embodiments, component A is prepared by the following steps: Under nitrogen protection, deionized water, emulsifier, acrylic acid, butyl acrylate, dopamine methacrylamide, and disulfide-bonded methacrylate monomers were mixed, the pH was adjusted to 5.5-6.5, an initiator was added, and the polymerization reaction was carried out at 65℃-75℃ for 4-6 hours. After demulsification, washing, and drying, component A was obtained.

[0009] The process employs emulsion free radical copolymerization with water as the dispersion medium. The emulsifier forms micelles to solubilize the hydrophobic monomer butyl acrylate, ensuring a uniform copolymer composition. Nitrogen protection prevents the oxidation of the catechol group in dopamine methacrylamide to quinone. The pH is adjusted to 5.5-6.5 to partially neutralize acrylic acid, increasing its solubility in the aqueous phase, and to avoid accelerating the oxidation rate of catechol under alkaline conditions. The polymerization temperature of 65℃-75℃ ensures a moderate decomposition rate of the initiator ammonium persulfate, preventing explosive polymerization. The reaction time of 4-6 hours ensures a sufficiently high monomer conversion rate.

[0010] In some embodiments, the emulsifier is sodium dodecyl sulfate, and the amount of the emulsifier is 1% to 3% of the total mass of the monomers; the initiator is ammonium persulfate, and the amount of the initiator is 0.5% to 1.5% of the total mass of the monomers.

[0011] In some embodiments, component B is at least one of zinc acetate, zinc sulfate, and magnesium acetate.

[0012] Zinc acetate, zinc sulfate, and magnesium acetate are all water-soluble metal salts that can dissociate in aqueous slurries. or It forms a coordination crosslink with the carboxyl group in component A; acetate and sulfate are inert anions, do not participate in side reactions, and will not introduce impurity ions that are harmful to battery performance.

[0013] Secondly, this application also provides a silicon-carbon negative electrode sheet, including a current collector and a negative electrode slurry layer disposed on the current collector, wherein the negative electrode slurry layer is formed by coating and drying the negative electrode slurry; the negative electrode slurry includes silicon-carbon active material, conductive electrode, deionized water and self-healing negative electrode binder as described in the first aspect.

[0014] The current collector, which can be copper foil with a thickness of 8 μm to 12 μm, is used to support the negative electrode slurry layer and collect current. Silicon-carbon active material serves as the negative electrode active material, providing lithium-ion storage capacity. A conductive agent is used to construct electronic conduction pathways between the active materials and between the active materials and the current collector. Deionized water is used as the dispersion medium to uniformly disperse the components and form a coatable slurry. The aforementioned self-healing negative electrode binder is used to bond the active material and conductive agent together and combine them with the current collector. Simultaneously, during cycling, it maintains the integrity of the electrode structure through a self-healing mechanism of dynamic coordination bonds and disulfide bonds.

[0015] Optionally, the silicon-carbon active material is a composite of artificial graphite and nano-silicon. The artificial graphite provides stable cycling performance and conductivity, while the nano-silicon provides high specific capacity. The nano-silicon accounts for 5% to 20% of the total mass of the silicon-carbon active material, which can control the volume expansion within the range that the binder network can withstand while ensuring high capacity. The particle size of the nano-silicon is 50 nm to 500 nm, which can shorten the lithium-ion diffusion path and avoid excessive specific surface area and increased side reactions caused by excessively small particle size.

[0016] Optionally, the conductive agent is at least one of conductive carbon black, carbon nanotubes, and graphene. Conductive carbon black has a high specific surface area and good conductivity, carbon nanotubes have a one-dimensional tubular structure and excellent electronic conductivity, and graphene has a two-dimensional sheet structure and extremely high carrier mobility.

[0017] Thirdly, this application also provides a method for preparing a silicon-carbon negative electrode sheet as described in the second aspect, including... Adjust the pH of component A to 6.5-7.5 with ammonia water to prepare an aqueous dispersion. Add silicon carbide active material and stir for 30-60 minutes. Then add conductive agent and adjust the pH to 5.0-6.0 with acetic acid. Add component B and stir for 1-2 hours. Add deionized water until the solid content is 45%-55% to obtain the negative electrode slurry. The negative electrode slurry is coated onto the current collector, followed by three-stage gradient drying and vacuum heat treatment to obtain the silicon-carbon negative electrode sheet.

[0018] First, adjust the pH of component A to 6.5-7.5 with ammonia water to neutralize the carboxyl groups in component A into ammonium carboxylate salts, improving the solubility and dispersion of component A in water and forming a uniform aqueous dispersion. After adding silicon carbon active material, stir for 30-60 minutes to allow the catechol groups in component A to fully contact with the hydroxyl groups on the surface of silicon carbon particles and form hydrogen bonds for anchoring, thus achieving interface modification of the active material by the binder. Then, add a conductive agent and stir evenly, and adjust the pH to 5.0-6.0 with acetic acid. At this point, the carboxyl groups are restored to their protonated form, and this pH range can also prevent the formation of hydroxide precipitates from subsequently added metal ions. After adding component B, stir for 1-2 hours to allow the metal ions to fully coordinate with the carboxyl groups. Add deionized water to bring the solid content to 45%-55%, which ensures that the slurry has suitable coating rheological properties.

[0019] In some embodiments, the three-stage gradient drying includes: a first stage drying temperature of 60℃~80℃, a drying rate of 1.5 g / (m²·s)~3.0 g / (m²·s), and a time of 60 s~120 s; The second stage of drying is carried out at a temperature of 80℃~100℃, a drying rate of 0.5 g / (m²·s)~1.5 g / (m²·s), and a time of 30 s~60 s. The third stage of drying is carried out at a temperature of 100℃~115℃, a drying rate of 2.0 g / (m²·s)~4.0 g / (m²·s), a time of 60 s~120 s, and in a nitrogen or vacuum environment.

[0020] The process involves three stages: The first stage employs a high drying rate and a low temperature to evaporate most of the moisture in the slurry quickly, while preventing excessive heat that could cause surface crusting. The second stage uses a lower drying rate to allow the remaining moisture to evaporate slowly, giving the binder molecular chains sufficient time to rearrange and preventing binder migration to the coating surface, thus achieving a uniform distribution along the electrode thickness. The third stage uses a higher drying rate and a higher temperature to rapidly remove residual moisture and complete the drying process. The third stage drying environment is a nitrogen or vacuum environment to prevent the copper foil from oxidizing at high temperatures.

[0021] Optionally, the vacuum heat treatment is performed at a temperature of 80°C to 100°C for a time of 0.5 h to 2 h to further promote the coordination and cross-linking reaction between the carboxyl groups in component A and the metal ions in component B. At the same time, the vacuum environment can prevent the copper foil from oxidizing and the adhesive from degrading.

[0022] Fourthly, this application also provides the application of a silicon-carbon negative electrode sheet prepared by the method described in the second aspect or the preparation method described in the third aspect in a lithium-ion battery.

[0023] The lithium-ion battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the negative electrode is the aforementioned silicon-carbon negative electrode sheet. The silicon-carbon negative electrode sheet of the present invention effectively buffers the volume expansion of silicon during battery charge-discharge cycles and maintains the integrity of the electrode structure through interfacial anchoring of the silicon-carbon active material by the catechol groups in component A, dynamic coordination crosslinking of carboxyl groups with metal ions in component B, and dynamic covalent exchange of disulfide bonds, thereby improving the cycle stability of the lithium-ion battery.

[0024] Compared with the prior art, this application also has the following beneficial effects: The carboxyl groups in component A provide sites for coordination and crosslinking with metal ions in component B, while also imparting hydrophilicity and ion conductivity to the copolymer; the catechol groups can form strong hydrogen bonds with the hydroxyl groups on the surface of the silicon-carbon active material, achieving interfacial anchoring of the binder to the silicon-carbon particles; the disulfide bonds, as dynamic covalent bonds, can undergo exchange reactions under stress, assisting in the reorganization of the network structure. Component B... or It forms a metal-carboxyl coordination bond with the carboxyl group in component A. This coordination bond is stable in the aqueous system and has a moderate bond energy. It can be reversibly broken and recombined under the stress generated by the volume expansion of silicon, and can achieve self-repair without external stimulation, thereby ensuring the cycle stability of the battery. Detailed Implementation

[0025] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0026] As used herein, the terms “prepared from” and “comprising” are synonymous. The terms “comprising,” “including,” “having,” “containing,” or any other variations thereof, as used herein, are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0027] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, it should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Unless otherwise specified, the raw materials used in the following examples and comparative examples are commercially available industrial products, and all conditions not otherwise specified are conventional.

[0029] Preparation Example 1 In a reactor equipped with a stirrer, condenser, and nitrogen inlet, 500 parts by weight of deionized water and 2 parts of sodium dodecyl sulfate were added, and nitrogen was introduced to remove oxygen. 60 parts of acrylic acid, 30 parts of butyl acrylate, 8 parts of dopamine methacrylamide, and 2 parts of 2-(2-pyridyldithio)ethyl methacrylate were added sequentially, and the pH was adjusted to 5.8 with ammonia. The temperature was raised to 70°C, and 0.8 parts of ammonium persulfate were added. The polymerization reaction was carried out for 5 hours under nitrogen protection. After the reaction was completed, the pH was adjusted to 4.5 with hydrochloric acid to demulsify, filtered, washed three times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain component A.

[0030] The weight-average molecular weight of component A was determined to be 120,000 by gel permeation chromatography; the carboxyl content was determined to be 5.5 mmol / g by acid-base titration; the catechol group content was determined to be 0.9 mmol / g by ultraviolet spectrophotometry; and the disulfide bond content was determined to be 0.3 mmol / g by disulfide bond specific reduction-ultraviolet detection method.

[0031] Preparation Example 2 In a reactor equipped with a stirrer, condenser, and nitrogen inlet, 500 parts of deionized water and 1.5 parts of sodium dodecyl sulfate were added, and nitrogen was introduced to remove oxygen. Then, 55 parts of acrylic acid, 35 parts of butyl acrylate, 6 parts of dopamine methacrylamide, and 1.5 parts of 2-(2-pyridyldithio)ethyl methacrylate were added sequentially, and the pH was adjusted to 6.0 with ammonia. The temperature was raised to 65°C, and 0.6 parts of ammonium persulfate were added. The polymerization reaction was carried out under nitrogen protection for 6 hours. After the reaction, the pH was adjusted to 4.5 with hydrochloric acid to demulsify, the mixture was filtered, washed three times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain component A.

[0032] The weight-average molecular weight of component A was determined to be 90,000 by gel permeation chromatography; the carboxyl content was determined to be 5.0 mmol / g by acid-base titration; the catechol group content was determined to be 0.5 mmol / g by ultraviolet spectrophotometry; and the disulfide bond content was determined to be 0.1 mmol / g by disulfide bond specific reduction-ultraviolet detection method.

[0033] Preparation Example 3 In a reactor equipped with a stirrer, condenser, and nitrogen inlet, 500 parts of deionized water and 2.5 parts of sodium dodecyl sulfate were added, and nitrogen was introduced to remove oxygen. Then, 65 parts of acrylic acid, 25 parts of butyl acrylate, 7 parts of dopamine methacrylamide, and 3 parts of 2-(2-pyridyldithio)ethyl methacrylate were added sequentially, and the pH was adjusted to 5.5 with ammonia. The temperature was raised to 75°C, and 1.2 parts of ammonium persulfate were added. The polymerization reaction was carried out under nitrogen protection for 4 hours. After the reaction, the pH was adjusted to 4.5 with hydrochloric acid to demulsify, the mixture was filtered, washed three times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain component A.

[0034] The weight-average molecular weight of component A was determined to be 145,000 by gel permeation chromatography; the carboxyl content was determined to be 6.5 mmol / g by acid-base titration; the catechol group content was determined to be 1.2 mmol / g by ultraviolet spectrophotometry; and the disulfide bond content was determined to be 0.5 mmol / g by disulfide bond specific reduction-ultraviolet detection method.

[0035] Comparative Preparation Example 1 In a reactor equipped with a stirrer, condenser, and nitrogen inlet, 500 parts of deionized water and 2 parts of sodium dodecyl sulfate were added, and nitrogen was introduced to remove oxygen. 60 parts of acrylic acid, 30 parts of butyl acrylate, 8 parts of dopamine methacrylamide, and 2 parts of methyl methacrylate were added sequentially, and the pH was adjusted to 5.8 with ammonia. The temperature was raised to 70°C, and 0.8 parts of ammonium persulfate were added. The polymerization reaction was carried out for 5 hours under nitrogen protection. After the reaction was completed, the pH was adjusted to 4.5 with hydrochloric acid to demulsify, filtered, washed three times with deionized water, and vacuum dried at 60°C for 12 hours to obtain control component A.

[0036] According to gel permeation chromatography, the weight-average molecular weight of component A was 120,000; according to acid-base titration, the carboxyl content was 5.5 mmol / g; according to ultraviolet spectrophotometry, the catechol group content was 0.9 mmol / g; and it contained no disulfide bonds.

[0037] Comparative Preparation Example 2 In a reactor equipped with a stirrer, condenser, and nitrogen inlet, 500 parts of deionized water and 2 parts of sodium dodecyl sulfate were added, and nitrogen was introduced to remove oxygen. Then, 60 parts of acrylic acid, 30 parts of butyl acrylate, 8 parts of methyl methacrylate, and 2 parts of 2-(2-pyridyldithio)ethyl methacrylate were added sequentially, and the pH was adjusted to 5.8 with ammonia. The temperature was raised to 70°C, and 0.8 parts of ammonium persulfate were added. The polymerization reaction was carried out under nitrogen protection for 5 hours. After the reaction, the pH was adjusted to 4.5 with hydrochloric acid to demulsify, the mixture was filtered, washed three times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain control component A.

[0038] According to gel permeation chromatography, the weight-average molecular weight of component A was 118,000; according to acid-base titration, the carboxyl content was 5.5 mmol / g; according to disulfide bond specific reduction-UV detection method, the disulfide bond content was 0.3 mmol / g; and it did not contain catechol groups.

[0039] Comparative preparation example 3 In a reactor equipped with a stirrer, condenser, and nitrogen inlet, 500 parts of deionized water and 2 parts of sodium dodecyl sulfate were added, and nitrogen was introduced to remove oxygen. Then, 60 parts of butyl acrylate, 8 parts of dopamine methacrylamide, 2 parts of 2-(2-pyridyldithio)ethyl methacrylate, and 30 parts of hydroxyethyl methacrylate were added sequentially. The pH was adjusted to 5.8 with ammonia. The temperature was raised to 70°C, and 0.8 parts of ammonium persulfate were added. The polymerization reaction was carried out under nitrogen protection for 5 hours. After the reaction, the pH was adjusted to 4.5 with hydrochloric acid to demulsify, the mixture was filtered, washed three times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain control component A.

[0040] According to gel permeation chromatography, the weight-average molecular weight of component A was 122,000; according to ultraviolet spectrophotometry, the catechol group content was 0.9 mmol / g; according to disulfide bond specific reduction-ultraviolet detection method, the disulfide bond content was 0.3 mmol / g; and it did not contain carboxyl groups.

[0041] Comparative preparation example 4 The difference between Comparative Preparation Example 4 and Preparation Example 1 is that bis(2-methacryloyloxyethyl) disulfide was used instead of 2-(2-pyridyldithio)ethyl methacrylate. The weight-average molecular weight of Comparative Preparation A was 121,000, as determined by gel permeation chromatography; the carboxyl group content was 5.5 mmol / g, as determined by acid-base titration; the catechol group content was 0.9 mmol / g, as determined by ultraviolet spectrophotometry; and the disulfide bond content was 0.3 mmol / g, as determined by disulfide bond-specific reduction-ultraviolet detection. Example 1

[0042] The self-healing negative electrode binder comprises component A and component B in a mass ratio of 1:0.05. Component A is the component A obtained in Preparation Example 1, and component B is zinc acetate.

[0043] Preparation method of silicon-carbon negative electrode sheet: Adjust the pH of component A to 7.0 with ammonia to prepare a 5 wt% aqueous dispersion; add silicon-carbon active material (10% by mass of nano-silicon, 100 nm particle size, with the remainder being artificial graphite), and stir for 45 minutes; add conductive carbon black Super P Li, adjust the pH to 5.5 with acetic acid, add component B zinc acetate, stir for 1.5 hours, and add deionized water until the solid content is 50% to obtain the negative electrode slurry; based on the total mass of the negative electrode slurry as 100%, the silicon-carbon active material is 92.5%, the conductive carbon black is 1.5%, component A is 5%, component B (calculated as Zn²⁺) is 0.25%, and the remainder is deionized water; The negative electrode paste was coated onto a 10 μm thick copper foil, with a coating amount of 200 g / m. 2 The process then involves a three-stage gradient drying process: the first stage is dried at 70℃ with a drying rate of 2 g / (m²). 2 The first drying stage (drying time) is 90 s; the second drying stage has a temperature of 90℃ and a drying rate of 1 g / (m²). 2 The drying time for the first stage is 45 s; the drying temperature for the third stage is 110℃, and the drying rate is 3 g / (m²). 2 The drying process is carried out in a nitrogen atmosphere for 90 seconds, followed by vacuum heat treatment at 90°C for 1 hour to obtain a silicon-carbon negative electrode sheet. Example 2

[0044] The preparation method of the silicon-carbon negative electrode sheet is the same as in Example 1, except that: component A is the same as component A obtained in Preparation Example 2, component B is zinc sulfate, and the mass ratio of A to B is 1:0.02; based on the total mass of the negative electrode slurry as 100%, the silicon-carbon active material is 93%, the conductive carbon black is 2%, component A is 4.5%, and component B is Zn 2+ The content was calculated as 0.09%, with the remainder being deionized water; in the three-stage gradient drying process, the first stage drying temperature was 60℃, and the drying rate was 1.5 g / (m²). 2 The first drying stage (drying time) was 120 s; the second drying stage was at a temperature of 80℃ and a drying rate of 0.5 g / (m²). 2 The drying time for the first stage is 60 s; the drying temperature for the third stage is 100℃, and the drying rate is 2.0 g / (m²). 2 •s), time is 120 s; vacuum heat treatment at 80℃ for 2h. Example 3

[0045] The preparation method of the silicon-carbon negative electrode sheet is the same as in Example 1, except that: component A is the same as component A obtained in Preparation Example 3, component B is magnesium acetate, and the mass ratio of A to B is 1:0.08; based on the total mass of the negative electrode slurry as 100%, the silicon-carbon active material is 90%, the conductive agent is carbon nanotubes 1%, component A is 5%, and component B is Mg 2+ The content is calculated as 0.4%, with the remainder being deionized water; in the three-stage gradient drying, the first stage drying temperature is 80℃, and the drying rate is 3.0 g / (m²). 2 The first drying stage (drying time) was 60 s; the second drying stage was at a temperature of 100℃ and a drying rate of 1.5 g / (m²). 2 The drying time for the first stage is 30 s; the drying temperature for the third stage is 115℃, and the drying rate is 4.0 g / (m²). 2 •s), time is 60 s; vacuum heat treatment at 100℃ for 0.5h. Example 4

[0046] The preparation method of the silicon-carbon negative electrode sheet is the same as in Example 1, except that: the mass ratio of A to B is 1:0.04; based on the total mass of the negative electrode slurry as 100%, the silicon-carbon active material is 94%, the conductive agent is graphene 1%, component A is 3%, and component B is Zn 2+ The content was calculated as 0.09%, with the remainder being deionized water; in the three-stage gradient drying process, the first stage drying temperature was 75℃, and the drying rate was 2.5 g / (m²). 2 The first drying stage (drying time) was 90 s; the second drying stage was at a temperature of 85℃ and a drying rate of 1.0 g / (m²). 2 The drying time for the first stage is 45 s; the drying temperature for the third stage is 105℃, and the drying rate is 3.0 g / (m²). 2 •s), time is 90 s; vacuum heat treatment at 85℃ for 1.5h. Example 5

[0047] The preparation method of the silicon-carbon negative electrode sheet is the same as in Example 1, except that: component A is the component A obtained in Preparation Example 2, component B is a mixture of zinc acetate and magnesium acetate (molar ratio 1:1), and the mass ratio of A:B is 1:0.06; based on the total mass of the negative electrode slurry as 100%, the silicon-carbon active material is 91%, the conductive agent is a mixture of conductive carbon black and carbon nanotubes (mass ratio 1:1) 2%, component A is 4.5%, component B is 0.27% based on metal ions, and the balance is deionized water; vacuum heat treatment at 95°C for 1 hour. Example 6

[0048] The preparation method of the silicon-carbon negative electrode sheet is the same as in Example 1, except that: component A is the same as component A obtained in Preparation Example 3, component B is zinc sulfate, and the mass ratio of A to B is 1:0.03; based on the total mass of the negative electrode slurry as 100%, the silicon-carbon active material is 93.5%, the conductive carbon black is 1.5%, component A is 4%, and component B is Zn 2+ The content is 0.12%, with the remainder being deionized water; vacuum heat treatment at 90℃ for 1 hour.

[0049] Comparative Example 1 The difference from Example 1 is that the A component of Comparative Example 1 is the same as the Comparative A component obtained in Comparative Preparation Example 1.

[0050] Comparative Example 2 The difference from Example 1 is that the A component of Comparative Example 2 is the same as the Comparative A component obtained in Comparative Preparation Example 2.

[0051] Comparative Example 3 The difference from Example 1 is that the A component of Comparative Example 3 is the same as the Comparative A component obtained in Comparative Preparation Example 3.

[0052] Comparative Example 4 The difference from Example 1 is that the A component of Comparative Example 4 is the same as the Comparative A component obtained in Comparative Preparation Example 4.

[0053] Comparative Example 5 The difference from Example 1 is that component A in Comparative Example 5 was replaced with an equal amount of polyacrylic acid (weight average molecular weight 120,000, carboxyl content 5.5 mmol / g).

[0054] Comparative Example 6 The difference from Example 1 is that component B in Comparative Example 6 is replaced with an equal amount of sodium chloride.

[0055] Comparative Example 7 The difference from Example 1 is that component B in Comparative Example 7 was replaced with an equal amount of aluminum nitrate.

[0056] Comparative Example 8 The difference from Example 1 is that Comparative Example 8 does not add component B, but only uses component A as a binder. The amount of component A is the same as the total amount of components A and B in Example 1.

[0057] Comparative Example 9 The difference from Example 1 is that the three-stage gradient drying is replaced by constant temperature drying at 90°C for 300 seconds.

[0058] Performance testing 1. Electrode peel strength test Referring to GB / T 2792-2014 "Test Method for Peel Strength of Adhesive Tape", the negative electrode sheet was cut into 24 mm × 200 mm samples. The peel force between the electrode coating and the copper foil was tested by peeling at 180° with a tensile speed of 300 mm / min. The peel force (N / m) was recorded.

[0059] 2. Button cell assembly and electrochemical performance testing The negative electrode was punched into a 14 mm diameter disc, with a lithium metal sheet as the counter electrode, Celgard 2400 as the separator, and 1 mol / L LiPF6 in EC / DEC / EMC (volume ratio 1:1:1) electrolyte to assemble a CR2032 coin cell. After standing for 2 hours, charge and discharge tests were conducted at a 0.1C rate, with a voltage range of 0.01 V to 1.5 V. The initial coulombic efficiency was the ratio of the initial charge capacity to the initial discharge capacity. Cyclic performance tests were conducted at a 0.5C rate, and the capacity retention rate after 500 cycles was recorded.

[0060] 3. Electrode Rebound Rate Test The negative electrode sheet was cut into 100 mm × 100 mm samples, and the initial thickness was measured using a micrometer. After the electrode sheet was charged and discharged 50 times at a rate of 0.5C, the battery was removed, the electrode sheet thickness was measured, and the rebound rate was calculated as (thickness after cycles - initial thickness) / initial thickness × 100%.

[0061] Table 1 Performance test results of the examples and comparative examples

[0062] As demonstrated in Examples 1 to 6, the self-healing negative electrode binder of the present invention exhibits excellent performance in terms of peel strength, initial coulombic efficiency, cycle capacity retention, and electrode rebound rate. Example 1 shows the best overall performance, indicating that the binder achieves optimal dual dynamic network synergy when the A:B mass ratio is 1:0.05, zinc acetate is used as component B, the three-stage gradient drying parameters are 70℃ / 2.0 / 90s, 90℃ / 1.0 / 45s, 110℃ / 3.0 / 90s, and vacuum heat treatment at 90℃ / 1h.

[0063] The capacity retention rate of Comparative Example 1 decreased to 78.5% after 500 cycles, and the peel strength decreased to 28.3 N / m. This indicates that the disulfide bond, as a dynamic covalent bond, plays an important role in maintaining the integrity of the electrode structure by reversibly exchanging and reorganizing through an auxiliary network during cycling.

[0064] The peel strength of Comparative Example 2 decreased to 24.1 N / m, and the cycle retention rate decreased to 72.3%, indicating that the strong hydrogen bond anchoring of the catechol group on the surface of silicon carbon particles is the key to achieving interface stability. Without this anchoring effect, the adhesive and the active material are only physically adsorbed, and they are prone to debonding during cycling.

[0065] The peel strength of Comparative Example 3 decreased to 22.6 N / m, and the cycle retention rate decreased to 68.7%, indicating that the carboxyl group is not only an essential site for forming coordination crosslinks with the metal ions of component B, but also provides hydrophilicity and ion conduction ability. Without the carboxyl group, the coordination network cannot be formed, and the overall performance of the adhesive is greatly reduced.

[0066] Comparative Example 4 (using a common alkyl disulfide monomer instead of 2-(2-pyridyldithio)ethyl methacrylate) exhibited a capacity retention of 80.4% after 500 cycles and a peel strength of 29.6 N / m, both significantly lower than Example 1. This indicates that while common alkyl disulfide bonds can provide some dynamic covalent exchange capacity, their high activation energy results in a slow exchange reaction rate within the battery operating temperature range (-20℃ to 60℃), limiting their self-healing effect. In contrast, the pyridyl disulfide bond in 2-(2-pyridyldithio)ethyl methacrylate, due to the electron-withdrawing effect of the pyridine ring reducing the electron cloud density of the disulfide bond, facilitates the thiol-disulfide bond exchange reaction. Under battery conditions, it can achieve rapid dynamic recombination without an external catalyst, thus more effectively buffering the stress generated by silicon volume expansion and maintaining the integrity of the electrode structure.

[0067] The cycle retention rate of Comparative Example 5 decreased to 65.4%, and the peel strength decreased to 21.5 N / m. This indicates that ordinary polyacrylic acid does not contain catechol anchoring groups and disulfide dynamic covalent bonds. The synergistic effect of interface anchoring and dynamic self-repair cannot be achieved by relying solely on the coordination crosslinking of carboxyl groups and metal ions.

[0068] The cycle retention rate of Comparative Example 6 decreased to 74.6%, indicating that... Without forming effective coordination crosslinks with carboxyl groups, a dynamic network cannot be constructed, proving that... / The necessity of coordination with the carboxyl group.

[0069] The cycle retention rate of Comparative Example 7 decreased to 73.8%, indicating that the trivalent... It forms irreversible coordination with carboxyl groups, and the network lacks dynamic reversibility, making it unable to release stress through coordination bond breakage and recombination during silicon volume expansion.

[0070] The peel strength of Comparative Example 8 was 27.1 N / m, and the cycle retention rate was 76.2%, indicating that the physical hydrogen bonds and covalent disulfide bonds in component A alone are insufficient to maintain the network structure. Metal-carboxyl coordination crosslinking is indispensable for improving cohesive strength and self-healing ability.

[0071] Comparative Example 9 showed a cycle retention rate of 82.1% and a peel strength of 30.2 N / m, indicating that the three-stage gradient drying significantly improves electrode performance by controlling the solvent evaporation rate to inhibit the migration of binder to the surface and ensuring uniform distribution of binder in the electrode thickness direction.

[0072] In summary, the self-healing anode binder of the present invention effectively solves the technical problem that existing waterborne silicon-carbon anode binders cannot simultaneously achieve dynamic reversible crosslinking and strong interfacial anchoring through the interfacial anchoring of catechol groups in component A, the dynamic coordination crosslinking of carboxyl groups and metal ions in component B, and the dynamic covalent exchange of pyridyl disulfide bonds provided by 2-(2-pyridyldithio)ethyl methacrylate, combined with a three-stage gradient drying process. This significantly improves the cycle stability and structural integrity of silicon-carbon anodes.

[0073] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0074] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit the scope of protection of this application. In particular, it should be noted that any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application for those skilled in the art.

Claims

1. A self-healing negative electrode adhesive, characterized in that, It includes component A and component B with a mass ratio of 1:(0.02~0.08); Component A is an acrylate copolymer containing carboxyl groups, catechol groups, and disulfide bonds; the weight-average molecular weight of component A is 80,000 to 150,000, the carboxyl content is 4 mmol / g to 7 mmol / g, the catechol group content is 0.5 mmol / g to 1.5 mmol / g, and the disulfide bond content is 0.1 mmol / g to 0.5 mmol / g. The B component is Zn. 2+ or Mg 2+ Water-soluble salts.

2. The self-healing negative electrode adhesive as described in claim 1, characterized in that, Component A is copolymerized from the following monomers in the indicated mass percentages: 55%~65% acrylic acid, 25%~35% butyl acrylate, 5%~10% dopamine methacrylamide, and 1%~3% disulfide-containing methacrylate monomers.

3. The self-healing negative electrode adhesive as described in claim 2, characterized in that, The disulfide-containing methacrylate monomer is 2-(2-pyridyldithio)ethyl methacrylate.

4. The self-healing negative electrode adhesive as described in claim 2, characterized in that, Component A is prepared by the following steps: Under nitrogen protection, deionized water, emulsifier, acrylic acid, butyl acrylate, dopamine methacrylamide, and disulfide-bonded methacrylate monomers were mixed, the pH was adjusted to 5.5-6.5, an initiator was added, and the polymerization reaction was carried out at 65℃-75℃ for 4-6 hours. After demulsification, washing, and drying, component A was obtained.

5. The self-healing negative electrode adhesive as described in claim 4, characterized in that, The emulsifier is sodium dodecyl sulfate, and the amount of the emulsifier is 1% to 3% of the total mass of the monomers; the initiator is ammonium persulfate, and the amount of the initiator is 0.5% to 1.5% of the total mass of the monomers.

6. The self-healing negative electrode adhesive as described in claim 1, characterized in that, Component B is at least one of zinc acetate, zinc sulfate, and magnesium acetate.

7. A silicon-carbon negative electrode sheet, characterized in that, It includes a current collector and a negative electrode slurry layer disposed on the current collector, the negative electrode slurry layer being formed by coating and drying the negative electrode slurry; the negative electrode slurry includes silicon-carbon active material, conductive electrode, deionized water and self-healing negative electrode binder as described in any one of claims 1 to 6.

8. A method for preparing a silicon-carbon negative electrode sheet as described in claim 7, characterized in that, include Adjust the pH of component A to 6.5-7.5 with ammonia water to prepare an aqueous dispersion. Add silicon carbide active material and stir for 30-60 minutes. Then add conductive agent and adjust the pH to 5.0-6.0 with acetic acid. Add component B and stir for 1-2 hours. Add deionized water until the solid content is 45%-55% to obtain the negative electrode slurry. The negative electrode slurry is coated onto the current collector, followed by three-stage gradient drying and vacuum heat treatment to obtain the silicon-carbon negative electrode sheet.

9. The method for preparing the silicon-carbon negative electrode sheet as described in claim 8, characterized in that, The three-stage gradient drying includes: the first stage drying temperature is 60℃~80℃, the drying rate is 1.5 g / (m²·s)~3.0 g / (m²·s), and the time is 60 s~120 s; The second stage of drying is performed at a temperature of 80℃~100℃, a drying rate of 0.5 g / (m²·s)~1.5 g / (m²·s), and a time of 30s~60s. The third stage of drying is carried out at a temperature of 100℃~115℃, a drying rate of 2.0 g / (m²·s)~4.0 g / (m²·s), a time of 60 s~120 s, and in a nitrogen or vacuum environment.

10. The application of a silicon-carbon anode sheet as described in claim 7 or a silicon-carbon anode sheet prepared by the preparation method described in claims 8 to 9 in a lithium-ion battery.