A lithium negative electrode mixed conductive interface layer and a preparation method and application thereof
By constructing a hybrid conductive interface layer composed of non-lithiated metal nanoparticles and lithium compounds on the surface of the negative electrode of a lithium metal battery, the problem that existing interface layer materials cannot simultaneously achieve lithium-ion transport and electric field regulation is solved, thus achieving the effects of lithium dendrite suppression and battery life extension.
Patent Information
- Application Number
- CN202611638117.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-20
AI Technical Summary
Existing lithium metal battery anode surface interface layer materials cannot simultaneously achieve efficient lithium-ion transport and interface electric field regulation, leading to lithium dendrite growth and affecting battery life and safety.
A hybrid conductive interface layer combining non-lithiated metal nanoparticles and lithium compounds is employed. Through in-situ conversion reaction, non-lithiated metal nanoparticles are uniformly dispersed in the lithium compound, forming a functional synergy of local electron conduction and long-range electron blocking, thereby inhibiting lithium dendrite growth.
It effectively reduces interface impedance, extends the cycle life of lithium metal batteries, improves battery safety and stability, simplifies the manufacturing process, and has good prospects for industrialization.
Smart Images

Figure CN123143409A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium battery technology, and relates to a lithium anode hybrid conductive interface layer, its preparation method and application. Background Technology
[0002] Lithium metal batteries, with their ultra-high theoretical specific capacity and extremely low electrochemical potential of lithium metal anodes, have become a core candidate system for next-generation high-energy-density energy storage devices, showing broad application prospects in new energy storage, power batteries, and other fields. However, during battery cycling, lithium metal anodes are prone to lithium dendrite formation due to factors such as uneven lithium-ion flux distribution and interfacial electric field distortion. This not only causes continuous loss of active lithium and a gradual decline in battery coulombic efficiency, significantly shortening battery life, but may also puncture the separator, leading to safety accidents such as short circuits and thermal runaway, greatly hindering the commercialization of lithium metal batteries.
[0003] Currently, constructing an artificial interface layer on the surface of a lithium metal anode is the mainstream and effective method to improve the electrode-electrolyte interface state and suppress lithium dendrite growth. An ideal artificial interface layer needs to possess both efficient lithium-ion transport and interfacial electric field modulation capabilities to reduce interfacial impedance and achieve uniform lithium deposition. However, existing single-functional interface layer materials such as LiF and Li3N only possess lithium-ion conduction properties and cannot regulate interfacial electronic behavior, which easily leads to local lithium-ion aggregation and still induces lithium dendrite nucleation and growth.
[0004] Existing hybrid conductive interface layers mostly employ lithium alloyed metals such as In, Sn, and Ag, which present numerous drawbacks in practical applications. The lithium alloys formed by these metals are brittle, significantly reducing the creep performance of lithium metal. Furthermore, the metal elements readily diffuse into the lithium bulk phase, and the alloying process completely eliminates the self-healing ability of lithium metal to repair interface defects through plastic deformation, failing to meet the requirements for long-term stable interface protection. Therefore, developing a novel hybrid conductive interface layer with both excellent ionic and electronic conductivity is a pressing technical challenge in this field. Summary of the Invention
[0005] The main objective of this invention is to overcome the deficiencies in the prior art and provide a lithium anode hybrid conductive interface layer, its preparation method, and its application.
[0006] To achieve the above objectives, the specific technical solution is as follows: The first aspect of the present invention provides a lithium anode hybrid conductive interface layer comprising non-lithiated metal nanoparticles and a lithium compound, wherein the non-lithiated metal is selected from at least one of Ni, Fe, and Cu; The non-lithiated metal nanoparticles are dispersed in the lithium compound, and the non-lithiated metal nanoparticles do not form a continuous electronic conductive network. The non-lithiated metal nanoparticles constitute 1% to 15% of the volume of the hybrid conductive interface layer.
[0007] This invention selects metals such as Ni, Cu, and Fe, which do not form alloys with lithium, as the electronically conductive components. These metals are almost insoluble in lithium and do not undergo significant alloying reactions during battery cycling, thus effectively avoiding interface degradation caused by alloying. This helps maintain the creep capacity of lithium metal and allows lithium metal to repair interface contact defects through plastic deformation. It avoids the problems of interface porosity accumulation and contact failure caused by alloying in the prior art, and helps improve the structural integrity and stability of the interface during long-term cycling.
[0008] This invention uniformly disperses non-lithiated metal nanoparticles in a lithium compound matrix, with the non-lithiated metal nanoparticles isolated from each other and not forming a continuous electronic conductive network. The non-lithiated metal nanoparticles homogenize the electric field in a local area, while the lithium compound matrix undertakes the functions of rapid ion transport and electron blocking. The two are spatially separated and functionally complementary, realizing the functional synergy of ion conduction and electronic conduction at the interface layer, inhibiting lithium dendrite growth, reducing interface impedance, and significantly extending the cycle life of lithium metal batteries.
[0009] In this invention, the metal volume fraction refers to the percentage of the metal nanoparticle volume in the total volume of the mixed conductive interface layer. The total volume of the mixed conductive interface layer includes the metal nanoparticles, the lithium compound matrix, incompletely converted precursor residues, and micropores. Since the degree of in-situ conversion reaction is affected by the type of precursor, loading amount, initiation method, and initiation conditions, the actual generated metal nanoparticle volume fraction can be controlled within the range of 1% to 15%.
[0010] This invention clarifies the volume fraction of non-lithiated metal nanoparticles in the mixed conductive interface layer, moving from qualitative to quantitative controllability; when the non-lithiated metal nanoparticles are less than 1%, the number of metal particles is insufficient and cannot effectively homogenize the electric field; when they are more than 15%, the spacing between metal particles is too small, which may form local connections and increase the risk of electron tunneling.
[0011] Furthermore, the particle size of the non-lithiated metal nanoparticles is 1–100 nm, preferably 5–50 nm.
[0012] The non-lithiated metal nanoparticles of the present invention are selected within the above-mentioned particle size range, which ensures that they are uniformly dispersed and isolated from each other in the lithium compound matrix, and do not form a continuous electronic conductive network. This enables the mixed conductive interface layer to stably achieve a uniform local electric field and block electron tunneling.
[0013] Furthermore, the thickness of the hybrid conductive interface layer is 100 nm to 10 μm, preferably 500 nm to 5 μm.
[0014] The thickness range of the mixed conductive interface layer in this invention allows the non-lithiated metal nanoparticles to fully exert their role in homogenizing the electric field and inhibiting lithium dendrite growth. This avoids the situation where the interface layer is too thin to block lithium dendrite penetration, and also avoids the situation where the interface layer is too thick to excessively increase the overall impedance of the battery, thus ensuring that lithium ions have a stable and efficient transmission channel.
[0015] Furthermore, the lithium compound is selected from at least one of lithium nitride, lithium oxide, lithium fluoride, lithium chloride, lithium bromide, and lithium iodide.
[0016] The lithium compound used in this invention has good lithium-ion conductivity and chemical stability, which can enhance the physical inhibition of lithium dendrite growth by the interface layer and ensure the cycle stability and safety of lithium metal batteries.
[0017] A second aspect of the present invention provides a method for preparing the above-mentioned lithium anode hybrid conductive interface layer, comprising the following steps: S1: Under an inert atmosphere, a non-lithiated metal active material containing at least one metal element selected from Ni, Fe, and Cu is loaded onto the surface of a lithium metal substrate; S2: Initiate an in-situ conversion reaction between the non-lithiated metal active material and the lithium metal matrix to obtain a mixed conductive interface layer.
[0018] This invention utilizes an in-situ conversion reaction to achieve a one-step conversion of non-lithiated metal active materials into a functional interface layer, generating an interface layer composed of non-lithiated metal nanoparticles and lithium compounds. Because the reaction occurs in situ on the lithium metal surface, the generated metal nanoparticles are uniformly dispersed in the lithium compound matrix, resulting in tight interfacial bonding and high structural stability. This avoids the problems of interfacial inhomogeneity and insufficient long-term stability caused by physical mixing or stepwise preparation.
[0019] Further, in step S1, the inert atmosphere is selected from any one of helium, neon or argon, preferably argon.
[0020] Further, in step S1, the non-lithiated metal active material is a compound or mixture formed by at least one metal element selected from Ni, Fe, and Cu and at least one non-metal element selected from N, O, F, Cl, Br, and I, and the metals can be selected independently.
[0021] This invention utilizes non-lithiated metal active materials formed by metallic elements from Ni, Fe, and Cu and non-metallic elements from N, O, F, Cl, Br, and I. These materials can form a uniform and stable phase on the surface of a lithium metal matrix. During subsequent in-situ conversion reactions, they can directly react with the lithium metal matrix to generate corresponding lithium compounds. The metal components are reduced to elemental non-lithiated metal nanoparticles that are uniformly dispersed in the lithium compounds. No additional reactants are required, and the target mixed conductive interface layer can be generated in one step, greatly simplifying the preparation process while ensuring that the components of the generated interface layer are uniformly distributed and tightly bonded.
[0022] Further, the non-lithiated metal active material can be one or more of the following: nitrides, oxides, fluorides, chlorides, bromides, iodides, or oxyhalides of nickel, iron, and copper; as an example, it can be selected from one or more of Ni3N, NiO, Ni2O3, NiF2, NiCl2, NiBr2, NiI2, NiOCl, NiOF, Fe2N, FeO, Fe3O4, Fe2O3, FeF3, FeCl2, FeCl3, FeBr2, FeBr3, FeI2, FeOCl, FeOF, Cu3N, Cu2O, CuO, CuF2, CuCl, CuCl2, CuBr, CuBr2, CuI, and Cu2OCl2.
[0023] Preferably, the non-lithiated metal active material is selected from one or more of NiF2, NiCl2, NiBr2, NiI2, NiO, Ni2O3, Fe2O3, Fe3O4, FeOCl, FeF3, FeCl2, FeBr3, FeI2, CuO, Cu2O, CuCl2, CuBr2, CuI, and Cu2OCl2.
[0024] Further, in step S1, the loading method is at least one of electroplating, vapor deposition, spraying, blade coating, spin coating, chemical vapor deposition, or rolling, preferably blade coating or spin coating.
[0025] This invention employs various simple methods such as spin coating, blade coating, and roller coating to load non-lithiated metal active materials onto the surface of a lithium metal substrate. It does not require harsh conditions such as high temperature and high vacuum, and while ensuring the quality of the interface layer, it has good prospects for industrialization and is highly compatible with existing battery manufacturing processes.
[0026] As one implementation method, the precursor solution or suspension of the non-lithiated metal active material is loaded onto the surface of a lithium sheet by spin coating and then dried to obtain an active material coating.
[0027] The spin coating speed is 1000–3000 rpm; the acceleration is 800–1200 rpm / s; the spin coating time is 45–90 s; the drop volume is 80–150 μL; and a single spin coating or multiple spin coatings (2–5 times) are selected according to the target interface layer thickness.
[0028] As one embodiment, the preparation method of the precursor solution or suspension of the non-lithiated metal active material is as follows: in an inert atmosphere, the non-lithiated metal active material is added to a solvent and stirred and dispersed for 0.5 to 5 hours to obtain a uniform precursor solution or suspension.
[0029] Further, the solvent is selected from at least one of tetrahydrofuran (THF), 1,2-dimethoxyethane (DME), 1,3-dioxolane (DOL), and cyclohexane; the mass fraction of the active substance in the precursor solution or suspension is 0.5 wt% to 40 wt%, preferably 1 wt% to 30 wt%.
[0030] When the active substance is completely dissolved in the solvent, its mass fraction is preferably 1 wt% to 20 wt%; when the active substance is dispersed in the solvent in a suspended form, its mass fraction is preferably 0.5 wt% to 15 wt%.
[0031] Furthermore, the drying temperature is 40–120°C, and the time is 0.5–24 h.
[0032] Further, in step S2, the initiation method is at least one of thermal initiation, mechanical initiation, and electrochemical initiation, preferably thermal initiation.
[0033] This invention loads a non-lithiated metal active material onto the surface of a lithium metal substrate, and then, through thermal initiation, mechanical initiation, or electrochemical initiation, causes the non-lithiated metal active material to undergo an in-situ conversion reaction with lithium metal, thereby generating an interface layer composed of non-lithiated metal nanoparticles and lithium compounds in one step.
[0034] As one implementation method, thermal initiation provides activation energy for the reaction by heating, prompting the active material to undergo an in-situ conversion reaction with lithium metal.
[0035] The general formula for the in-situ transformation reaction is: M a X b + (b·y)Li → aM + bLi y X, wherein M is at least one of Ni, Fe, and Cu, and X is at least one of N, O, F, Cl, Br, and I.
[0036] Furthermore, the heating temperature for thermal initiation is 40–300°C, preferably 60–180°C; the heating time is 0.5–48 h, preferably 1–12 h.
[0037] A third aspect of the present invention provides a lithium metal anode, comprising a lithium metal substrate and a mixed conductive interface layer covering at least one surface of the lithium metal substrate; wherein the mixed conductive interface layer is the mixed conductive interface layer of the first aspect or the mixed conductive interface layer prepared by the preparation method of the second aspect.
[0038] A fourth aspect of the present invention provides a battery, said battery being a lithium metal battery, comprising a lithium metal negative electrode as described in the third aspect.
[0039] In one embodiment, the battery is a lithium metal all-solid-state battery.
[0040] Compared with the prior art, the present invention has the following significant advantages: This invention employs non-lithiated metals as the electronically conductive component, effectively avoiding interface degradation caused by alloying. Through a structural design that isolates the non-lithiated metal nanoparticles from each other, a continuous electronically conductive network is not formed, achieving a synergistic effect of localized electron conduction, long-range electron blocking, and rapid ion transport. A quantitative relationship between metal volume fraction and interfacial electrochemical performance is established, enabling the technical solution to move from qualitative to quantitatively controllable methods. An in-situ conversion reaction is used to achieve a one-step conversion of the non-lithiated metal active material into a functional interface layer, resulting in tight interfacial bonding and high structural stability. Furthermore, the preparation method is simple, highly compatible with existing battery manufacturing processes, and possesses excellent industrialization prospects while ensuring the quality of the interface layer. Attached Figure Description
[0041] To more clearly illustrate the technical solutions in this invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0042] Figure 1 This is a schematic diagram of the structure of the lithium anode hybrid conductive interface layer of the present invention; Figure 2 This is a scanning electron microscope image of the surface morphology of the lithium anode hybrid conductive interface layer prepared in Example 1 of the present invention; Figure 3 This is a cross-sectional scanning electron microscope image of the lithium anode hybrid conductive interface layer prepared in Example 1 of this invention; Figure 4 This is a cycle performance diagram of Embodiment 1 and Comparative Example 1 of the present invention. Detailed Implementation
[0043] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0044] The technical solution of the present invention will be described in detail below through embodiments and comparative examples. It should be noted that the following embodiments are only used to help understand the technical solution of the present invention and do not constitute any limitation on the scope of protection of the present invention.
[0045] Unless otherwise specified, specific techniques or conditions in the embodiments of this invention shall be performed in accordance with the techniques or conditions described in the literature in this field, or in accordance with the product instructions. Devices, instruments, reagents, etc., whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels. All raw materials used in this invention are readily available in the domestic market.
[0046] Example 1 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The lithium anode hybrid conductive interface layer has a thickness of 2 μm and comprises Ni nanoparticles and lithium fluoride. The Ni nanoparticles are uniformly dispersed in the lithium fluoride, and the Ni nanoparticles do not form a continuous electronic conductive network. The Ni nanoparticles constitute 5% of the volume of the hybrid conductive interface layer, and the particle size of the Ni nanoparticles is 10–30 nm. A schematic diagram of the structure is shown below. Figure 1 As shown.
[0047] The specific preparation method of the lithium anode hybrid conductive interface layer is as follows: S1: In an argon glove box (oxygen level <0.1 ppm), NiF2 powder was added to THF and magnetically stirred for 3 hours to obtain a uniform suspension with a mass fraction of 8 wt%. This suspension was then spin-coated onto the surface of a lithium wafer. The coated lithium wafer was then dried in an 80°C vacuum drying oven for 6 hours to remove the THF solvent, resulting in a lithium wafer with a NiF2 coating. The spin-coating speed was 2000 rpm, the acceleration was 1000 rpm / s, each spin-coating session lasted 60 seconds, and the drop volume was 100 μL. Multiple spin-coating sessions were performed. S2: The dried lithium sheet with NiF2 coating is placed on a heating stage and kept at 120℃ for 4 h. After the reaction is completed, a lithium metal anode with a mixed conductive interface layer of about 5% Ni volume fraction and a thickness of 2 μm is obtained.
[0048] Example 2 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The difference from Embodiment 1 is that the Ni nanoparticles account for 8% of the volume of the hybrid conductive interface layer; in the preparation method, the mass fraction of NiF2 suspension is 13 wt%, and the other conditions are the same as in Embodiment 1.
[0049] Example 3 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The difference from Embodiment 1 is that the Ni nanoparticles account for 2% of the volume of the hybrid conductive interface layer; in the preparation method, the mass fraction of the NiF2 suspension is 5 wt%, and the other conditions are the same as in Embodiment 1.
[0050] Example 4 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The difference from Embodiment 1 is that the hybrid conductive interface layer with a thickness of 500 nm is obtained by controlling the number of spin coatings, while the other conditions are the same as in Embodiment 1.
[0051] Example 5 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The difference from Embodiment 1 is that the hybrid conductive interface layer with a thickness of 5 μm is obtained by controlling the number of spin coatings, and the other conditions are the same as in Embodiment 1.
[0052] Example 6 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The difference from Embodiment 1 is that the lithium anode hybrid conductive interface layer comprises Fe nanoparticles and a lithium compound, wherein the lithium compound is a mixture of lithium oxide and lithium chloride (molar ratio 4:1); the Fe nanoparticles constitute 5% of the volume of the hybrid conductive interface layer; and the particle size of the Fe nanoparticles is 5–15 nm. In the preparation method, in step S1, the non-lithiated metal active material is an Fe₂O₃ / FeOCl composite (molar ratio 1:1), and the mass fraction of the suspension is 20 wt%. In step S2, the temperature is maintained at 100°C for 2 h. The remaining conditions are the same as in Embodiment 1.
[0053] Example 7 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method. The difference from Embodiment 1 is that the lithium anode hybrid conductive interface layer comprises non-lithiated metal nanoparticles and a lithium compound. The non-lithiated metal nanoparticles are Ni nanoparticles and Cu nanoparticles (molar ratio 1:1); the lithium compound is a mixture of lithium fluoride and lithium chloride (molar ratio 1:1); the total volume of the Ni nanoparticles and Cu nanoparticles is 5% of the volume of the hybrid conductive interface layer; the particle size of the Ni nanoparticles is 10–30 nm, and the particle size of the Cu nanoparticles is 5–40 nm. In the preparation method, in step S1, the non-lithiated metal active material is a mixture of NiF2 and CuCl2 in a molar ratio of 1:1, and the mass fraction of the suspension is 20 wt%. In step S2, the temperature is maintained at 140°C for 4 h. The remaining conditions are the same as in Embodiment 1.
[0054] Example 8 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method, which is consistent with Example 1, except that in step S2, the temperature is maintained at 80℃ for 12 h, while the other conditions are the same as in Example 1. After the reaction, a hybrid conductive interface layer in which Ni nanoparticles are dispersed in a LiF matrix is obtained.
[0055] Example 9 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method, which is consistent with Example 1, except that in step S2, the temperature is maintained at 160℃ for 1 h, while the other conditions are the same as in Example 1. After the reaction, a hybrid conductive interface layer in which Ni nanoparticles are dispersed in a LiF matrix is obtained.
[0056] Example 10 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method, which is consistent with Example 1, except that in step S1, a NiF2 suspension is loaded onto the lithium sheet surface using a blade coating method. The final interface layer thickness is 2 μm by controlling the blade gap and the number of coatings. All other conditions are the same as in Example 1. After the reaction, a hybrid conductive interface layer in which Ni nanoparticles are dispersed in a LiF matrix is obtained.
[0057] Example 11 This embodiment provides a lithium anode hybrid conductive interface layer and its preparation method, which is consistent with Embodiment 1, except that heating is not performed in step S2. Instead, lithium sheets with NiF2 coating are assembled into a symmetrical battery at 0.1 mA / cm². 2 The reaction was repeated for 3 cycles to initiate an in-situ conversion reaction between NiF2 and lithium metal via electrochemical initiation, with all other conditions remaining the same as in Example 1. After the reaction, a mixed conductive interface layer in which Ni nanoparticles were dispersed in a LiF matrix was obtained.
[0058] Comparative Example 1 The lithium wafers in this comparative example were not modified with any interface layer. Subsequently, the fresh lithium wafers were directly assembled into lithium metal batteries in an argon glove box.
[0059] Comparative Example 2 This comparative example provides a method for preparing a lithium anode hybrid conductive interface layer. The difference from Example 1 is that step S2 does not involve heating; the layer is simply placed at room temperature for 4 hours. All other conditions are the same as in Example 1.
[0060] Comparative Example 3 This comparative example provides a method for preparing a lithium anode hybrid conductive interface layer. The difference from Example 1 is that the active material in step S1 is nano-nickel powder (average particle size 50 nm). The remaining conditions are the same as in Example 1.
[0061] Comparative Example 4 This comparative example provides a method for preparing a lithium anode hybrid conductive interface layer. The difference from Example 1 is that the active material in step S1 is LiF powder, and the other conditions are the same as in Example 1.
[0062] Comparative Example 5 This comparative example provides a method for preparing a lithium anode hybrid conductive interface layer. The difference from Example 1 is that the mass fraction of NiF2 suspension is 0.5 wt%, the volume fraction of Ni in the interface layer is 0.3%, and the other conditions are the same as in Example 1.
[0063] Comparative Example 6 This comparative example provides a method for preparing a lithium anode hybrid conductive interface layer. The difference from Example 1 is that the mass fraction of NiF2 suspension is 35 wt%, Ni accounts for 22% of the volume fraction of the interface layer, and the other conditions are the same as in Example 1.
[0064] Electrochemical performance testing: The battery mold, with a diameter of 10 mm, was used for assembly in a high-purity argon glove box.
[0065] Electrochemical performance tests were conducted on symmetrical lithium metal anode assemblies with mixed conductive interface layers prepared using the examples or comparative examples: (1) Weigh 100 mg of Li6PS5Cl sulfide solid electrolyte powder and cold press it at 400 MPa for 2 min to form a dense electrolyte sheet; (2) Take two lithium metal anodes prepared by the above-mentioned examples or comparative examples, and place the side with the mixed conductive interface layer on the upper and lower surfaces of the electrolyte sheet respectively. (3) Place copper current collectors on the outside of the lithium metal anodes on both sides and press them lightly for 2 minutes under a pressure of 50 MPa to ensure close contact between the layers. (4) Finally, tighten the mold screws and use the AC impedance method (EIS, frequency range 1 MHz–0.1 Hz, disturbance voltage 10 mV) to measure its interface impedance at 25℃; test its critical current density (CCD).
[0066] Electrochemical performance tests were conducted on full cells assembled with lithium metal anodes having mixed conductive interface layers, prepared using the examples or comparative examples: (1) Weigh 100 mg of Li6PS5Cl sulfide solid electrolyte powder and cold press it at 400 MPa for 2 min to form a dense electrolyte sheet; (2) The pre-prepared positive electrode composite film (with the composition of LZO@NCM811 : Li6PS5Cl : VGCF : PTFE = 70 : 26 : 3 : 1, and an areal specific capacity of 2.4 mAh cm⁻¹) was used. -2 Place the positive electrode layer on the upper surface of the electrolyte sheet, then place the aluminum current collector on top of it, and press it under a pressure of 400 MPa for 2 minutes to make the positive electrode layer and the electrolyte in close contact. (3) Place the side of the lithium metal anode with the mixed conductive interface layer obtained in the above experimental section on the lower surface of the electrolyte sheet, and then place the copper current collector on top of it. Press lightly under 50 MPa pressure for 2 minutes to ensure good contact. (4) Finally, tighten the mold screws, activate at 0.05C for 3 turns, and then perform a cycle performance test at 0.5C (voltage range 2.8-4.3V).
[0067] The test performance results of the lithium anode hybrid conductive interface layer and the lithium anode assembled batteries of each embodiment and comparative example are shown in Table 1.
[0068] Table 1. Battery performance results of the lithium anode hybrid conductive interface layer and its lithium anode assembly in each embodiment and comparative example.
[0069] Test Result Analysis: The lithium anode hybrid conductive interface layer prepared in Example 1 was characterized by scanning electron microscopy, and its surface SEM image shows ( Figure 2 Ni nanoparticles and lithium fluoride are uniformly distributed on the lithium metal surface; its cross-sectional SEM image shows ( Figure 3 The thickness of the hybrid conductive interface layer is approximately 2 μm.
[0070] As can be seen from the data in Table 1 for Example 1, Comparative Examples 3 and 4, although Ni powder alone can play a certain role in homogenizing the electric field, the interfacial resistance is still as high as 85 Ω·cm. 2 The CCD has a capacity of only 2.7 mA / cm². 2The capacity retention rate after 200 cycles is only 27%; when using the LiF layer alone, although it can provide some chemical stability, the interfacial resistance is 95 Ω·cm. 2 The CCD has an A / cm² of only 2.5 mA. 2 The capacitance retention rate is only 25% after 200 cycles. However, the combination of the two reduces the interface resistance to 15 Ω·cm. 2 The CCD has been upgraded to 6.0 mA / cm². 2 The capacity retention rate is as high as 87% after 200 cycles. This fully verifies the core advantages of the hybrid conductive interface layer design: the uniform electric field of Ni reduces the local current density, and LiF provides fast ion channels and blocks electron tunneling and side reactions. Both are indispensable.
[0071] As can be seen from the data in Table 1 for Examples 1, 2, and 3, and Comparative Examples 5 and 6, when the Ni volume fraction increases from 2% to 5%, the interface resistance increases from 22 Ω·cm. 2 Reduced to 15 Ω·cm 2 The CCD efficiency was increased from 4.8 to 6.0 mA / cm². 2 The capacitance retention rate increased from 83% to 87%; when it was further increased to 8%, the interface resistance rose slightly to 20 Ω·cm. 2 The CCD and capacity retention rate decreased slightly. This may be because the electric field homogenization is insufficient when the Ni content is low; when the Ni content is high, the conductive pathways increase, and local electron channels may begin to appear. When the Ni content is too low, as in Comparative Example 5, the interface resistance is 85 Ω·cm. 2 The CCD has an A / cm² value of 2.4 mA. 2 The capacity retention rate is only 24%, indicating that Ni content below 1% is almost ineffective in providing a uniform electric field. When the Ni content is too high, as in Comparative Example 6, the interface resistance is 65 Ω·cm. 2 The CCD has an A / cm² value of 3.0 mA. 2 The capacity retention rate was 32%, which is much lower than that of the example, indicating that excessive Ni may cause some particles to come into contact with each other and form electron channels, thus weakening the electron blocking function of LiF.
[0072] As shown in Table 1, the data from Examples 1, 4, and 5 indicate that the 500 nm interface layer has the shortest ion transport path, the lowest interface resistance, and the highest CCD performance. However, due to its thinness, it is slightly less resistant to volume changes during long cycles, and the capacity retention rate drops slightly to 80% after 200 cycles. The 2 μm layer provides good ion transport while maintaining sufficient mechanical stability, resulting in the best overall performance. The 5 μm layer has an excessively long ion transport path, leading to an interface resistance as high as 28 Ω·cm. 2 The CCD voltage dropped to 4.6 mA / cm. 2The retention rate dropped to 82%. This set of data indicates that if the interface layer is too thin, it will affect long-term stability, while if it is too thick, it will sacrifice ion transport efficiency.
[0073] As can be seen from the data of Examples 1, 6 and 7 in Table 1, different non-lithiated metals also have excellent electrochemical performance, and the combination of multiple non-lithiated metals can provide complementary electronic conduction functions, verifying the feasibility of the multi-metal strategy.
[0074] As shown by the data in Table 1 for Examples 1, 8, and 9, the thermal initiation temperature and time have a significant impact on the interface layer performance. Too low a thermal initiation temperature leads to incomplete conversion, while too high a temperature or too short a time affects interface uniformity. Due to incomplete conversion at 80°C, the Ni nanoparticle volume fraction in Example 8 was 4%.
[0075] As can be seen from the data of Examples 1, 10 and 11 in Table 1, a hybrid conductive interface layer with good performance can also be obtained by changing the load method or the triggering method.
[0076] As shown in Table 1, the data from Example 1 and Comparative Example 2 indicate that, due to the lack of thermal initiation in Comparative Example 2, NiF2 failed to transform into a Ni / LiF composite layer. The interface resistance, CCD, and capacity retention of Comparative Example 2 are almost identical to those of the bare lithium in Comparative Example 1, demonstrating that the unconverted NiF2 coating cannot form an effective interface layer. The cycling data of Example 1 and Comparative Example 1 at 0.5C are as follows: Figure 4 As shown, this verifies the core role of the initiation step in this invention. Only by initiating the in-situ conversion reaction between the active material and lithium metal can a synergistic conductive interface be generated.
[0077] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A lithium anode hybrid conductive interface layer, characterized in that, It includes non-lithiated metal nanoparticles and lithium compounds, wherein the non-lithiated metal is selected from at least one of Ni, Fe, and Cu; The non-lithiated metal nanoparticles are dispersed in the lithium compound, and the non-lithiated metal nanoparticles do not form a continuous electronic conductive network. The non-lithiated metal nanoparticles constitute 1% to 15% of the volume of the hybrid conductive interface layer.
2. The lithium anode hybrid conductive interface layer according to claim 1, characterized in that, The particle size of the non-lithiated metal nanoparticles is 1–100 nm.
3. The lithium anode hybrid conductive interface layer according to claim 1 or 2, characterized in that, The thickness of the hybrid conductive interface layer is 100 nm to 10 μm.
4. The lithium anode hybrid conductive interface layer according to claim 1 or 2, characterized in that, The lithium compound is selected from at least one of lithium nitride, lithium oxide, lithium fluoride, lithium chloride, lithium bromide, and lithium iodide.
5. A method for preparing a lithium anode hybrid conductive interface layer as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1: Under an inert atmosphere, a non-lithiated metal active material containing at least one metal element selected from Ni, Fe, and Cu is loaded onto the surface of a lithium metal substrate; S2: Initiate an in-situ conversion reaction between the non-lithiated metal active material and the lithium metal matrix to obtain a lithium anode mixed conductive interface layer.
6. The preparation method according to claim 5, characterized in that, In step S1, the non-lithiated metal active material is a compound or mixture formed by at least one metal element selected from Ni, Fe, and Cu and at least one non-metal element selected from N, O, F, Cl, Br, and I.
7. The preparation method according to claim 6, characterized in that, The non-lithiated metal active material is selected from one or more of NiF2, NiCl2, NiBr2, NiI2, NiO, Ni2O3, Fe2O3, Fe3O4, FeOCl, FeF3, FeCl2, FeBr3, FeI2, CuO, Cu2O, CuCl2, CuBr2, CuI, and Cu2OCl2.
8. The preparation method according to claim 5, characterized in that, In step S1, the loading method is at least one of electroplating, vapor deposition, spraying, blade coating, spin coating, chemical vapor deposition, or rolling. And / or, in step S2, the initiation method is at least one of thermal initiation, mechanical initiation, and electrochemical initiation.
9. A lithium metal anode, characterized in that, The lithium metal substrate includes a lithium metal substrate on at least one surface of which a mixed conductive interface layer is loaded; the mixed conductive interface layer is the lithium anode mixed conductive interface layer according to any one of claims 1 to 4 or the lithium anode mixed conductive interface layer prepared by any one of claims 5 to 8.
10. A battery, characterized in that, The battery is a lithium metal battery, including the lithium metal negative electrode as described in claim 9.