Functionalized modified metal organic framework-proton exchange membrane composite membrane, preparation method and application thereof
By covalently grafting acidic and proton acceptor groups onto the surface of MOF, the interfacial compatibility problem between MOF and PEM matrix was solved, resulting in a composite membrane with high proton conductivity and excellent mechanical properties at high temperatures, suitable for high-temperature proton exchange membrane water electrolysis and fuel cells.
Patent Information
- Application Number
- CN202611106276.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-20
AI Technical Summary
Existing perfluorosulfonic acid membranes exhibit decreased proton conductivity and poor mechanical strength at high temperatures, and the MOF filler has poor interfacial compatibility with the PEM matrix, resulting in poor long-term stability of the composite membrane.
By covalently grafting bifunctional organic molecules with acidic and proton acceptor groups onto the surface of MOFs, hydrogen bonds are formed with the PEM matrix through acid-base interactions, achieving nanoscale uniform dispersion and interfacial bonding of MOFs in the PEM matrix, and constructing a continuous proton conduction network.
It significantly improves the proton conductivity, mechanical properties and long-term stability of composite membranes, and is suitable for various MOF and PEM materials, as well as high-temperature proton exchange membrane water electrolysis and fuel cells.
Smart Images

Figure CN123143457A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical technology, specifically relating to a metal-organic framework-proton exchange membrane composite membrane, its preparation method and application, and particularly to a bifunctional MOF-enhanced proton exchange membrane for high-temperature water electrolysis or high-temperature fuel cells. Background Technology
[0002] Hydrogen energy, as a zero-carbon energy carrier, is one of the key pathways to achieving carbon neutrality. "Green hydrogen," produced by electrolyzing water using renewable energy, is currently the most promising hydrogen production technology. Among various water electrolysis technologies, proton exchange membrane (PEM) water electrolysis (PEMWE) has become a research and industrialization hotspot due to its advantages such as high current density, high efficiency, fast response speed, high gas purity, and direct coupling with the volatility of renewable energy sources. Similarly, proton exchange membrane fuel cells (PEMFCs), as an important end-use device for hydrogen energy, also rely on high-performance proton exchange membranes.
[0003] The core component of both PEMWE and PEMFC technologies is the proton exchange membrane. Currently, the most widely used membrane material in commercial applications is the perfluorosulfonic acid membrane (such as Nafion). However, the proton conductivity of this type of membrane material is highly dependent on the water content within the membrane. Under high-temperature (e.g., above 100 °C) and / or low-humidity conditions, water molecules evaporate rapidly, leading to a sharp decrease in proton conductivity. Furthermore, perfluorosulfonic acid membranes exhibit decreased mechanical strength and a lower glass transition temperature at high temperatures, severely limiting their application in high-efficiency high-temperature PEMWE and HT-PEMFC. Increasing the operating temperature (e.g., 120-200 °C) can significantly improve reaction kinetics, simplify the thermal management system, and increase energy utilization efficiency. Therefore, developing novel proton exchange membranes that can operate stably at high temperatures and maintain high proton conductivity is crucial to overcoming the technological bottlenecks of high-temperature PEM electrolyzers and fuel cells.
[0004] To overcome the insufficient high-temperature performance of perfluorosulfonic acid (PFSA) membranes, researchers have explored various modification strategies, such as combining them with inorganic or organic fillers to prepare composite membranes. Among these, metal-organic frameworks (MOFs) are considered highly promising fillers due to their ultra-high specific surface area, designable pore structures, and modifiable surface chemistry. However, directly combining unmodified or monofunctionalized MOFs with PEM matrices faces significant challenges. First, MOF particles exhibit poor interfacial compatibility with hydrophobic / hydrophilic polymer matrices, easily leading to aggregation, disrupting the inherent microphase separation structure of PEM, and even forming proton-blocking channels. Second, the lack of strong interactions between MOFs and PEM results in poor long-term operational stability of the composite membrane. To address these issues, researchers have attempted functionalization modification of MOFs, but existing methods are typically limited to synthesizing complex organic ligands containing functional groups, or monofunctional modification struggles to simultaneously solve the problems of interfacial compatibility and proton conduction efficiency.
[0005] Therefore, there is an urgent need to develop a new interface design strategy that can simultaneously achieve nanoscale uniform dispersion of MOF fillers in PEM matrix, construct efficient interfacial proton conduction channels, and significantly enhance the interfacial bonding force between fillers and matrix, thereby preparing high-temperature proton exchange membranes with high proton conductivity, excellent mechanical properties, and long-term stability. Summary of the Invention
[0006] The purpose of this invention is to provide a high-temperature proton exchange membrane-functionalized metal-organic framework-proton exchange membrane composite membrane with high proton conductivity, excellent mechanical properties and long-term stability, as well as its preparation method and application.
[0007] This invention provides a functionalized modified metal-organic framework-proton exchange membrane composite membrane. By covalently grafting bifunctional organic molecules with both acidic groups (such as sulfonic acid groups, carboxyl groups, and phosphate groups) and proton acceptor groups (such as amino and imidazole groups) onto the MOF surface, and utilizing hydrogen bonds and / or acid-base pair interactions between the acid-base groups and the ionic groups (such as sulfonic acid groups) in the PEM matrix, the problems of MOF filler aggregation and interfacial compatibility are solved, and a continuous proton conduction network is constructed, thereby significantly improving the overall performance of the composite membrane at high temperatures. This invention also achieves nanoscale uniform dispersion of MOF fillers in the PEM matrix, constructs efficient interfacial proton conduction channels, and significantly enhances the interfacial bonding force between the filler and the matrix, thus obtaining a high-temperature proton exchange membrane with high proton conductivity, excellent mechanical properties, and long-term stability.
[0008] The functionalized modified metal-organic framework-proton exchange membrane composite membrane provided by this invention is obtained by uniformly dispersing a bifunctionalized modified metal-organic framework (F-MOF) as a filler in a proton exchange membrane (PEM) matrix; wherein:
[0009] The metal-organic framework (MOF) is a porous crystalline material formed by the coordination connection of metal ions or metal oxygen clusters with organic ligands. Its surface contains active groups (such as hydroxyl, amino or coordination unsaturated sites) that can be chemically modified and can serve as reactive sites.
[0010] The bifunctional modification is achieved by grafting an organic molecule containing both acidic groups and proton acceptor groups onto the surface-active groups of the MOF via covalent bonds.
[0011] The proton exchange membrane is a polymer membrane containing acidic ionic groups (preferably sulfonic acid groups);
[0012] The F-MOF filler forms hydrogen bonds and / or acid-base pairs with the ionic groups in the PEM matrix through acidic groups and / or proton acceptor groups on its surface, inducing optimization of the micro-phase separation structure of the PEM matrix, forming wider, more ordered and interconnected hydrophilic ion channels. At the same time, it significantly enhances the mechanical strength and dimensional stability of the composite membrane through physical constraints and interfacial bonding, and endows the composite membrane with excellent proton conductivity and water retention capacity at high temperatures.
[0013] Optionally, the metal element in the MOF is selected from one or more of zirconium (Zr), aluminum (Al), chromium (Cr), iron (Fe), titanium (Ti), copper (Cu), zinc (Zn), hafnium (Hf), cobalt (Co), nickel (Ni), and lanthanides. Preferably, the MOF is a zirconium-based MOF, selected from the NU-1000, UiO-66, UiO-67, MIL-140 series, or PCN-222.
[0014] Optionally, the acidic group is selected from one or more of sulfonic acid group (-SO3H), carboxyl group (-COOH), phosphate group (-PO3H2), and phosphonic acid group (-PO(OH)2); the proton acceptor group is selected from one or more of amino group (-NH2), secondary amino group (-NH-), imino group, imidazolyl group, pyridyl group, and quaternary ammonium group.
[0015] Optionally, the bifunctional organic molecule should have one end capable of reacting with MOF surface-active groups (e.g., through silanization or nucleophilic substitution), and the other end or side chain should contain the aforementioned acidic groups and / or proton acceptor groups. Preferably, the organic molecule is a combination of 3-aminopropyltriethoxysilane (APTS) and 1,3-propanesulfonyl lactone (1,3-PS); or a combination of APTS and sodium 2-bromoethanesulfonate; or a combination of APTS and succinic anhydride; or a combination of (3-aminopropyl)triethoxysilane and 2-bromoethylphosphoric acid; or a silane coupling agent containing both amino and sulfonic acid groups can be used directly.
[0016] Optionally, the proton exchange membrane is a polymer membrane containing sulfonic acid groups, selected from one of the following: perfluorosulfonic acid resin membrane (such as Nafion®), sulfonated polyarylene ether sulfone membrane (SPAES), sulfonated polyether ether ketone membrane (SPEEK), sulfonated polyimide membrane (SPI), and sulfonated polyphenylene sulfone membrane; or a phosphoric acid doped polymer membrane, selected from one of the following: phosphoric acid doped polybenzimidazole membrane (PBI / PA) and phosphoric acid doped polybenzoxazine membrane; or a composite membrane composed of the above polymers and inorganic / organic fillers.
[0017] This invention also provides a method for preparing the metal-organic framework-proton exchange membrane composite membrane, the specific steps of which are as follows:
[0018] (1) Synthesize or provide MOF precursors and prepare activated MOFs by solvothermal, hydrothermal or microwave methods;
[0019] (2) Disperse the MOF in an anhydrous organic solvent, add a silane coupling agent containing a proton acceptor group or an organic small molecule containing a proton acceptor group, and heat the reaction to obtain a proton acceptor group-functionalized MOF, denoted as B-MOF;
[0020] (3) Disperse B-MOF in an organic solvent, add small organic molecules containing acidic groups (such as sulcinolone, halosulfonate, acid anhydride, halocarboxylic acid, halophosphoric acid, etc.), heat to react, and obtain bifunctionalized MOF, denoted as F-MOF;
[0021] (4) Dissolve the proton exchange membrane resin in an organic solvent to obtain a PEM solution;
[0022] (5) F-MOF is added to PEM solution in a certain proportion, and after ultrasonic dispersion and stirring, a uniform composite film casting solution is obtained;
[0023] (6) The composite film casting solution is formed into a film by solution casting, blade coating or spin coating, and then dried and annealed to obtain a composite film.
[0024] Optionally, in step (2), the mass ratio of the MOF to the silane coupling agent containing the proton acceptor group is 1:(0.1-5), preferably 1:(1-3), the reaction temperature is room temperature to 120°C, and the time is 6-48 hours.
[0025] Optionally, in step (3), the mass ratio of B-MOF to the small organic molecule containing acidic groups is 1:(0.5-10), preferably 1:(1-5), the reaction temperature is 30℃-150℃, and the time is 4-48 hours.
[0026] Optionally, the amount of F-MOF added in step (5) is 0.1%-10% of the mass of PEM resin, preferably 0.5%-3%.
[0027] The present invention also provides the application of the above-mentioned composite membrane in the preparation of membrane electrodes and electrochemical devices.
[0028] The membrane electrode assembly (MEA) includes an anode catalyst layer, a cathode catalyst layer, and the composite membrane sandwiched between them. The anode and cathode catalysts are coated onto both sides of the composite membrane by ultrasonic spraying, brushing, screen printing, or transfer printing.
[0029] The electrochemical device is a proton exchange membrane water electrolyzer (PEMWE), a proton exchange membrane fuel cell (PEMFC), or a proton exchange membrane carbon dioxide reduction electrolyzer, using the composite membrane as a solid electrolyte; it includes components such as the membrane electrode, gas diffusion layer, bipolar plate, and end plate. This device can operate stably within a temperature range of 100-200 °C, achieving efficient energy conversion or chemical synthesis.
[0030] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0031] (1) This invention proposes an interface design strategy of "dual-functional grafting and acid-base synergy". By covalently introducing flexible segments containing both acidic groups and proton acceptor groups on the surface of MOF, the MOF filler becomes a "multifunctional crosslinking node" with natural affinity to the PEM matrix.
[0032] (2) This strategy tightly binds the “inorganic” MOF filler and the “organic / polymer” matrix together at the molecular level through strong hydrogen bonds and / or acid-base pair interactions, thus completely solving the long-standing problem of MOF filler agglomeration and interfacial incompatibility that has plagued the field.
[0033] (3) More importantly, this interfacial interaction drives the rearrangement of molecular chains within the PEM matrix, inducing the fusion and interconnection of hydrophilic ionic phases, forming proton transport channels that are wider and more interconnected than pure PEM. This optimization of the microstructure directly leads to a leap in macroscopic performance: taking Nafion as an example, the proton conductivity of the composite membrane reaches 154.7 mS cm⁻¹ at 100 °C. −1 It is twice that of pure Nafion membrane. (4) At the same time, due to the physical constraints of MOF filler and strong interfacial bonding, the composite membrane has a significantly increased water absorption rate while its swelling rate has decreased significantly. The mechanical strength and glass transition temperature have been improved, achieving a synergistic improvement of "high conductivity" and "high stability". (5) The dual-functionalization strategy described in this invention has universality and can be applied to a variety of MOF materials (not limited to zirconium-based) and a variety of proton exchange membrane materials (not limited to perfluorosulfonic acid membranes), providing a universal material platform for designing the next generation of high-temperature proton exchange membranes. Attached Figure Description
[0034] Figure 1 This is a schematic diagram of the S / N-NU-1000 synthesis process provided in an embodiment of the present invention.
[0035] Figure 2 This is a schematic diagram of the S / N-Nafion composite membrane preparation process provided in the embodiments of the present invention.
[0036] Figure 3These are the Fourier transform infrared spectra of S / N-NU-1000 and NU-1000 provided in the embodiments of the present invention.
[0037] Figure 4 The X-ray photoelectron spectrum of S / N-NU-1000 and the X-ray photoelectron spectrum of S 2p provided in the embodiments of the present invention are shown.
[0038] Figure 5 This is a scanning electron microscope and energy dispersive spectroscopy (EDS) elemental distribution map of the S / N-NU-1000 provided in an embodiment of the present invention.
[0039] Figure 6 These are the X-ray diffraction spectra of S / N-NU-1000 and NU-1000 provided in the embodiments of the present invention.
[0040] Figure 7 The N2 adsorption-desorption curves and pore size distributions of S / N-NU-1000 and NU-1000 provided in the embodiments of the present invention are shown.
[0041] Figure 8 These are the mechanical tensile curves of each membrane provided in the embodiments of the present invention.
[0042] Figure 9 These are differential scanning calorimetry curves of various membranes provided in the embodiments of the present invention.
[0043] Figure 10 This is a graph showing the variation of the proton conductivity of each membrane as a function of temperature and relative humidity, provided in the embodiments of the present invention.
[0044] Figure 11 These are the proton conductivity versus temperature and Arrhenius plots of the various membranes provided in the embodiments of the present invention.
[0045] Figure 12 These are the Fourier transform infrared spectra and X-ray photoelectron spectra of S / N-Nafion and R-Nafion provided in the embodiments of the present invention.
[0046] Figure 13 These are small-angle X-ray scattering patterns of S / N-Nafion and R-Nafion provided in embodiments of the present invention.
[0047] Figure 14 These are atomic force microscopy phase images of S / N-Nafion and R-Nafion provided in embodiments of the present invention.
[0048] Figure 15 These are the radial distribution functions and mean square displacement plots of water from molecular dynamics simulations of S / N-Nafion and R-Nafion provided in this embodiment of the invention.
[0049] Figure 16 The polarization curves of the high-temperature water electrolyzers based on S / N-Nafion, NU-Nafion and R-Nafion provided in the embodiments of the present invention at 60 ℃ and 120 ℃ are shown.
[0050] Figure 17 The high-temperature water electrolyzer based on various membranes provided in this embodiment of the invention operates at 120 °C and 1.0 A cm⁻¹. -2 The following is a chart showing the long-term stability test results. Detailed Implementation
[0051] The present invention will be further described below with reference to the embodiments and accompanying drawings.
[0052] It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0053] Example 1: Construction of a bifunctional NU-1000 / Nafion composite membrane and its application in hydrogen production via water electrolysis.
[0054] This embodiment provides a bifunctionalized modified metal-organic framework material (taking S / N-NU-1000 as an example) and its preparation method, wherein the MOF material is mesoporous NU-1000, the acidic group is sulfonic acid group (-SO3H), and the proton acceptor group is secondary amine group (-NH-).
[0055] (I) The preparation of NU-1000 specifically includes the following steps:
[0056] Specifically, 388 mg of ZrOCl2·8H2O and 10.8 g of benzoic acid were placed in a 100 mL pressure-resistant bottle, and 32 mL of anhydrous DMF was added. The mixture was dissolved by sonication. The mixture was heated in an 80 °C oven for 1 hour, cooled, and then 160 mg of H4TBAPy was added. The mixture was then sonicated for 20 minutes. The reaction flask was placed in a 100 °C oven for 15 hours. After the reaction was completed, the pale yellow solid was collected by centrifugation, washed successively with DMF and acetone, and then activated under vacuum at 120 °C for 12 hours to obtain activated NU-1000 powder.
[0057] The preparation method of bifunctional MOF (S / N-NU-1000) specifically includes the following steps:
[0058] Under argon protection, 100 mg of activated NU-1000 was rapidly transferred to a pressure-resistant bottle containing 30 mL of anhydrous DMF and dispersed by stirring. 41 mg of APTS was diluted with 10 mL of anhydrous DMF and slowly injected into the NU-1000 suspension under an argon flow. After sealing, the mixture was stirred in an oil bath at 80 °C for 24 hours. After the reaction was complete, the solid was collected by centrifugation, washed repeatedly with DMF and acetone, and dried under vacuum at 60 °C for 12 hours to obtain amino-functionalized N-NU-1000.
[0059] 100 mg N-NU-1000 was dispersed in 30 mL of anhydrous DMF, and 131.24 mg of 1,3-PS was added. The mixture was stirred at 40 °C for 12 hours. After the reaction was complete, the solid was collected by centrifugation, washed three times with DMF and acetone, and dried under vacuum at 60 °C for 12 hours to obtain sulfonated modified S / N-NU-1000.
[0060] The schematic diagram of the synthesis route of S / N-NU-1000 obtained in this embodiment is shown below. Figure 1 .
[0061] (II) Preparation of the bifunctionalized NU-1000 / Nafion composite membrane, specifically including the following steps:
[0062] Nafion resin (D2020) was dried at 60 °C, cut into pieces, placed in 1 M H2SO4 solution, acidified in a water bath at 60 °C for 24 hours, then washed with deionized water until neutral, and vacuum dried at 60 °C for later use.
[0063] Take 1 g of dry Nafion resin, add 6 mL of DMAc, and stir in an 80 ℃ water bath for 2 hours until completely dissolved to obtain a Nafion solution (approximately 14 wt%).
[0064] The S / N-NU-1000 powder obtained above was added to the Nafion solution at a ratio of 1.5 wt% (relative to the mass of Nafion resin), ultrasonically dispersed for 30 minutes, and then stirred for 24 hours to obtain a uniform composite film casting solution.
[0065] The casting solution was cast onto a clean glass plate and dried at 60 °C for 1 hour, followed by annealing at 80 °C for 12 hours. After cooling, the glass plate was placed in deionized water to peel off the membrane. The resulting membrane was then treated in 3 vol% H2O2 solution and 0.5 M H2SO4 solution at 80 °C for 1 hour each to remove organic impurities, yielding the S / N-Nafion composite membrane.
[0066] For comparison, pure Nafion membranes without fillers (R-Nafion) and composite membranes with unmodified NU-1000 added (NU-Nafion) were prepared using the same method.
[0067] A schematic diagram of the preparation of S / N-Nafion obtained in this embodiment is shown below. Figure 2 .
[0068] (III) Fabrication of a membrane electrode assembly (MEA) for hydrogen production via water electrolysis, comprising the following steps:
[0069] Catalyst-coated membrane (CCM) technology was employed, using S / N-Nafion as the solid electrolyte membrane, to coat Ir-based catalysts (0.5~1.0 mg). Ir cm -2 The Pt / C catalyst (0.1~0.3 mg) was sprayed onto the anode side of the membrane. Pt cm -2 The coating is sprayed onto the cathode side and hot-pressed to obtain a water electrolysis hydrogen production membrane electrode (MEA).
[0070] (iv) Preparation of PEM water electrolysis hydrogen production device (PEMWE): MEA, titanium felt (anode), carbon paper (cathode), and titanium plate with flow field are assembled into a single electrolysis cell with an active area of 5 cm². 2 .
[0071] (v) In this embodiment, using commonly used analytical methods such as X-ray diffraction (XRD), differential scanning calorimetry (DSC), scanning electron microscopy (SEM), small-angle X-ray diffraction (SAXS), atomic force microscopy (AFM), energy dispersive spectroscopy (EDS), X-ray photoelectron spectroscopy (XPS), thermogravimetric analysis (TG), Fourier transform infrared spectroscopy (FTIR), and mechanical property testing, the structure, mechanical properties, and thermal properties of S / N-NU-1000 and S / N-Nafion were characterized.
[0072] Figure 3 FTIR spectra show that S / N-NU-1000 at 1047 cm⁻¹ -1 and 1183 cm -1 A new absorption peak appears at the point, which is attributed to the characteristic vibration of -SO3H, proving that the sulfonic acid group was successfully grafted.
[0073] Figure 4 In the XPS spectrum, the S 2p spectrum of S / N-NU-1000 showed characteristic double peaks at 167.9 eV and 169.3 eV, further confirming the presence of -SO3H.
[0074] Figure 5The SEM-EDS elemental distribution map shows that the S element is uniformly distributed in S / N-NU-1000.
[0075] Figure 6 XRD and Figure 7 The nitrogen adsorption results showed that the crystal structure and mesoporous framework of the MOF were maintained after grafting modification.
[0076] Figure 8 The stress-strain curves show that the tensile strength of the S / N-Nafion membrane (28.01 MPa) is higher than that of NU-Nafion (26.27 MPa) and R-Nafion (25.17 MPa). Figure 9 The DSC results show that the glass transition temperature (T0) of the S / N-Nafion film is... g The temperature reaches 141.7 °C, far exceeding the 98.2 °C of R-Nafion. The significant enhancement in mechanical properties and thermal stability is attributed to the strong hydrogen bond network formed between S / N-NU-1000 and the Nafion matrix, which effectively restricts the movement of Nafion molecular chains.
[0077] Figure 10 The proton conductivity of the composite membrane was demonstrated; at 100 °C and 100% RH, the proton conductivity of the S / N-Nafion membrane reached 154.7 mS / cm. -1 It is R-Nafion (75.6 mS cm⁻¹) -1 More than twice that of the standard. Even under low humidity conditions of 100 °C and 40% RH, the conductivity of the S / N-Nafion membrane (3.6 mS / cm) is... -1 It is still R-Nafion (0.6 mS cm) -1 6 times that of ).
[0078] Figure 11 The Arrhenius plot shows the activation energy (E) of the S / N-Nafion membrane. a Only 22.4 kJ mol -1 It is much lower than that of R-Nafion (38.7 kJ mol). -1 This indicates that the proton transport energy barrier has been significantly reduced.
[0079] Figure 12 FTIR analysis of a showed that the S / N-Nafion membrane located at 3400 cm⁻¹ -1 The broad OH stretching vibration peaks on both sides show a significant red shift, while the intensity of the -SO3H stretching vibration peak is relatively weakened. Figure 12XPS analysis of b showed that the binding energy of the -SO3H group in the S / N-Nafion film shifted to a lower value, and both characterizations together confirmed that a strong hydrogen bond was formed between S / N-NU-1000 and Nafion.
[0080] Figure 13 The SAXS results showed that the ion cluster spacing of the S / N-Nafion membrane (4.94 nm) was greater than that of the R-Nafion membrane (4.76 nm), indicating that the hydrophilic ion channels were broadened.
[0081] Figure 14 The AFM phase diagrams visually demonstrate that the S / N-Nafion membrane has a clearer and more interconnected hydrophilic / hydrophobic microphase separation structure.
[0082] Figure 15 Molecular dynamics simulations further confirmed that water molecules in the S / N-Nafion membrane form a more ordered and denser hydration layer around sulfonate ions, which is conducive to proton hopping and transport via the Grotthuss mechanism.
[0083] Water electrolysis tests were conducted at temperatures of 60℃ and 120℃, respectively. Figure 16 As shown, at 3.0 A cm -2 At the specified current density, the electrolyzer using the S / N-Nafion membrane achieved the lowest operating voltage: 1.72 V at 60 °C and 1.59 V at 120 °C. In contrast, the electrolyzer using the R-Nafion membrane required higher voltages under the same conditions (1.85 V and 1.71 V, respectively).
[0084] Figure 17 The electrolytic cell was demonstrated at 120 °C and 1.0 A cm⁻¹. -2 The S / N-Nafion-PEMWE exhibited stable voltage over 300 hours of continuous operation, with a voltage decay rate of only 6.0 µV h. -1 The results are far superior to those of the comparative samples. This fully demonstrates the great potential of the composite membrane provided by the present invention in the application of water electrolysis for hydrogen production at medium temperature (60 °C) and high temperature (120 °C).
[0085] Example 2: Expansion of different functionalized molecules.
[0086] Referring to the method in Example 1, NU-1000 can be replaced with other zirconium-based MOFs containing hydroxyl groups on their surface, such as MOF-808 or UiO-66, to achieve similar bifunctional modification. In the surface functionalization step, the APTS / 1,3-PS system can be replaced with a 3-aminopropyltriethoxysilane and 2-bromoethanesulfonate system, or a silane coupling agent containing both amino and sulfonic acid groups can be used directly to achieve similar bifunctional modification. When these functionalized MOFs are combined with Nafion, the resulting composite films exhibit significantly better proton conductivity, mechanical properties, and thermal stability than pure Nafion films.
Claims
1. A functionalized modified metal-organic framework-proton exchange membrane composite membrane, characterized in that, It consists of bifunctionalized metal-organic frameworks (F-MOFs) uniformly dispersed in a proton exchange membrane (PEM) matrix; wherein: The metal-organic framework (MOF) is a porous crystalline material formed by the coordination and connection of metal ions or metal oxygen clusters with organic ligands, and its surface contains active groups that can be chemically modified. The bifunctional modification is achieved by grafting an organic molecule containing both acidic groups and proton acceptor groups onto the surface-active groups of the MOF via covalent bonds. The proton exchange membrane is a polymer membrane containing acidic ionic groups; The F-MOF filler forms hydrogen bonds and / or acid-base pairs with the ionic groups in the PEM matrix through acidic groups and / or proton acceptor groups on its surface, inducing optimization of the micro-phase separation structure of the PEM matrix and forming wider and more interconnected hydrophilic ion channels. This results in the composite membrane having excellent proton conductivity and water retention capacity at high temperatures while maintaining or improving the mechanical strength of the membrane material.
2. The composite membrane according to claim 1, characterized in that, The metal element in the MOF is selected from one or more of zirconium, aluminum, chromium, iron, titanium, copper, zinc, hafnium, cobalt, nickel, and lanthanides.
3. The composite membrane according to claim 1, characterized in that, The acidic group is selected from one or more of sulfonic acid group, carboxyl group, phosphate group, and phosphonic acid group; the proton acceptor group is selected from one or more of amino group, secondary amino group, imino group, imidazolyl group, pyridyl group, and quaternary ammonium group.
4. The composite membrane according to claim 1, characterized in that, The organic molecule is a bifunctional molecule grafted onto the surface-active group of MOF via silanization or nucleophilic substitution. The organic molecule is selected from a combination of 3-aminopropyltriethoxysilane and 1,3-propanesulfonyl lactone, or a combination of 3-aminopropyltriethoxysilane and sodium 2-bromoethanesulfonate, or a combination of 3-aminopropyltriethoxysilane and succinic anhydride, or a combination of (3-aminopropyl)triethoxysilane and 2-bromoethylphosphoric acid, or a silane coupling agent containing both amino and sulfonic acid groups, or a silane coupling agent containing both imidazole and sulfonic acid groups.
5. The composite membrane according to claim 1, characterized in that, The proton exchange membrane is a polymer membrane containing sulfonic acid groups, selected from one of perfluorosulfonic acid resin membrane, sulfonated polyarylene ether sulfone membrane, sulfonated polyether ether ketone membrane, sulfonated polyimide membrane, and sulfonated polyphenylsulfone membrane; or it is a phosphoric acid-doped polymer membrane, selected from one of phosphoric acid-doped polybenzimidazole membrane and phosphoric acid-doped polybenzoxazine membrane; or it is a composite membrane composed of the above polymers and inorganic / organic fillers.
6. The method for preparing the metal-organic framework-proton exchange membrane composite membrane as described in any one of claims 1-5, characterized in that, The specific steps are as follows: (1) Synthesize or provide MOF precursors and prepare activated MOFs by solvothermal method, hydrothermal method or microwave method; (2) Disperse the MOF in an anhydrous organic solvent, add a silane coupling agent containing a proton acceptor group or an organic small molecule containing a proton acceptor group, and heat the reaction to obtain a proton acceptor group-functionalized MOF, denoted as B-MOF; (3) Disperse B-MOF in an organic solvent, add small organic molecules containing acidic groups, and heat to react to obtain bifunctionalized MOF, denoted as F-MOF; (4) Dissolve the proton exchange membrane resin in an organic solvent to obtain a PEM solution; (5) F-MOF was added to the PEM solution, and after ultrasonic dispersion and stirring, a uniform composite film casting solution was obtained; (6) The composite film casting solution is formed into a film by solution casting, blade coating or spin coating, and then dried and annealed to obtain a composite film.
7. The preparation method according to claim 6, characterized in that: In step (2), the mass ratio of the MOF to the silane coupling agent containing the proton acceptor group is 1:(0.1-5); the organic solvent is anhydrous N,N-dimethylformamide, anhydrous ethanol or toluene; the heating reaction temperature is room temperature to 120°C; and the time is 6-48 hours. In step (3), the mass ratio of B-MOF to the small organic molecule containing acidic groups is 1:(0.5-10); the organic solvent is N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran or toluene; the heating reaction temperature is 30℃-150℃ and the time is 4-48 hours. In step (4), the organic solvent is N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone or a mixture thereof; the dissolution temperature is 60℃-120℃; In step (5), the amount of F-MOF added is 0.1%-10% of the mass of PEM resin; In step (6), the drying process is a step-by-step heating drying process, and the annealing temperature is 100℃-200℃.
8. A membrane electrode, characterized in that, It includes an anode catalyst layer, a cathode catalyst layer, and a metal-organic framework-proton exchange membrane composite membrane as described in any one of claims 1-5 sandwiched between the two.
9. The method for preparing the membrane electrode as described in claim 8, characterized in that, This includes coating the anolyte catalyst and the cathode catalyst onto both sides of the composite membrane by ultrasonic spraying, brushing, screen printing or transfer methods to form a membrane electrode.
10. An electrochemical device, characterized in that, The device contains a metal-organic framework-proton exchange membrane composite membrane as described in any one of claims 1-5 as a solid electrolyte; the electrochemical device is a proton exchange membrane water electrolyzer, a proton exchange membrane fuel cell, or a proton exchange membrane carbon dioxide reduction electrolyzer.